A high-performance silicon nitride ceramic, its preparation method and application

High-density silicon nitride ceramics with high mechanical properties were prepared by low-temperature discharge plasma sintering and ZrH2 in-situ reaction, which solved the problems of high energy consumption in high-temperature processes and insufficient densification in low-temperature sintering, enabling their application in engine parts and cutting tools.

CN123062276APending Publication Date: 2026-11-10GUANGDONG UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611565269.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing high-performance silicon nitride ceramic preparation processes suffer from high energy consumption, high cost, and abnormal grain growth. Low-temperature sintering results in insufficient densification and suppression of β-phase transformation, leading to insufficient mechanical properties and limiting its application in engine components and cutting tools.

Method used

A mixture of α-Si3N4 powder, MgO powder, Yb2O3 powder and ZrH2 powder is sintered by discharge plasma at a low temperature of 1600~1700℃. ZrN is generated through the in-situ reaction of ZrH2, which promotes the transformation of α-Si3N4 to β-Si3N4 phase, forming an interlocked bimodal microstructure and improving the density and mechanical properties of the ceramic.

Benefits of technology

Silicon nitride ceramics with high density (greater than 98.7%), high hardness (15.8~18.2 GPa) and high fracture toughness (6.6~8.8 MPa·m-2) were prepared at low temperature, which significantly reduced energy consumption and improved mechanical properties and structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062276A_ABST
    Figure CN123062276A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of ceramic material production technology, and discloses a high-performance silicon nitride ceramic, its preparation method, and its application. The method involves ball milling and mixing α-Si3N4 powder, MgO powder, Yb2O3 powder, ZrH2 powder, and anhydrous ethanol, followed by rotary drying and sieving to obtain a mixed powder. The mixed powder is then pre-pressed and sintered under a nitrogen atmosphere at 30-50 MPa pressure and 1600-1700℃ using spark plasma sintering. The mass ratio of α-Si3N4 powder, Yb2O3 powder, MgO powder, and ZrH2 powder is 90:1. x :(10~ x :(10~25) x =2~8. This invention introduces ZrH2 as a second phase, in-situ nitriding to generate ZrN and promoting silicon nitride phase transformation to achieve toughening, improve fracture strength, and obtain silicon nitride ceramics with excellent mechanical properties, which can be used in cutting tools, engine parts and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ceramic material production technology, specifically relating to a high-performance silicon nitride ceramic, its preparation method, and its application. Background Technology

[0002] Silicon nitride (Si3N4), with its excellent comprehensive properties, is considered an ideal candidate material for key components of next-generation high-performance engines (such as turbine rotors and bearing rings) and advanced cutting tools. Its high hardness, low density, and excellent thermal stability ensure that components maintain dimensional stability and long-term durability under high-speed and high-temperature conditions. Among various performance indicators, high fracture toughness is particularly critical. It not only determines whether engine components can maintain structural integrity under extreme mechanical loads and thermal shocks, but also directly relates to the ability of cutting tools to resist chipping during unsteady machining processes such as intermittent cutting, thus affecting the service life and reliability of the entire component and tool.

[0003] However, current high-performance silicon nitride products heavily rely on high-temperature sintering processes exceeding 1800℃, a route with inherent drawbacks such as high energy consumption, high cost, and abnormal grain growth. For example, Chinese patent CN113480319A discloses the preparation of high-performance silicon nitride ceramics with a flexural strength as high as 830MPa at 1800~2000℃, but its process cost is significantly high. To reduce energy consumption and cost, researchers have attempted to lower the sintering temperature by optimizing the composite sintering aid system, but lowering the temperature often induces new technical contradictions: in the low-temperature range below 1700℃, the sintering driving force is severely insufficient, leading to inadequate densification of the ceramic body, and the residual micropores significantly weaken its thermal conductivity and electrical insulation strength; more importantly, the low-temperature environment greatly inhibits the phase transformation kinetics of silicon nitride from the equiaxed α phase to the long rod-shaped β phase, and hinders the full growth of β grains. It is precisely this interlocking microstructure of long rod-shaped β grains that constitutes the source of the high toughness of silicon nitride ceramics. In addition, Yi-Xin Wang et al., in their study on HfN-induced phase transformation and fracture toughness improvement of α / β-Si3N4 ceramics (Yi-Xin Wang et al. HfN-induced phase transformation and fracture toughness improvement of α / β-Si3N4ceramics, Journal of Alloys and Compounds. 1057 (2026) 186893), found that the addition of ZrN inhibited the α→β-Si3N4 phase transformation, with a β-silicon nitride content of only 25.3% and a fracture toughness of only 5.6±0.1 MPa·m. -2The limited availability of silicon nitride ceramics restricts their application in fields such as cutting tools. Therefore, developing new methods for preparing silicon nitride ceramics that combine low-temperature processing with high toughness is crucial and has become a key technical bottleneck that needs to be addressed to promote the large-scale application of silicon nitride ceramics in engine components and cutting tools. Summary of the Invention

[0004] To address the aforementioned technical problems, the primary objective of this invention is to provide a method for preparing high-performance silicon nitride ceramics.

[0005] Another object of the present invention is to provide high-performance silicon nitride ceramics prepared by the above method.

[0006] Another object of the present invention is to provide applications of the above-mentioned high-performance silicon nitride ceramics.

[0007] The objective of this invention is achieved through the following technical solution:

[0008] A high-performance silicon nitride ceramic is prepared by ball milling, mixing, rotary drying, and sieving α-Si3N4 powder, MgO powder, Yb2O3 powder, ZrH2 powder, and anhydrous ethanol to obtain a mixed powder. The mixed powder is then pre-pressed and sintered under a nitrogen atmosphere at 30-50 MPa pressure and 1600-1700℃ using discharge plasma sintering. The mass ratio of α-Si3N4 powder, Yb2O3 powder, MgO powder, and ZrH2 powder is 90:x:(10-x):(10-25); x = 2-8.

[0009] Preferably, the α-Si3N4 powder has a purity of 98wt% or higher and a particle size of 0.3~1µm, the MgO powder has a purity of 99.8wt% or higher and a particle size of 50~100nm, the Yb2O3 powder has a purity of 99.8wt% or higher and a particle size of 50~100nm, and the ZrH2 powder has a purity of 99.9wt% or higher and a particle size of 1~10µm.

[0010] Preferably, the silicon nitride ceramic has a density greater than 98.7%, a hardness of 15.8~18.2 GPa, a flexural strength of 673~773 MPa, and a fracture toughness of 6.6~8.8 MPa·m. -2 .

[0011] The method for preparing the high-performance silicon nitride ceramic specifically includes the following steps:

[0012] S1. Mix α-Si3N4 powder, MgO powder, Yb2O3 powder, ZrH2 powder and anhydrous ethanol and ball mill them, then dry them by rotary evaporation. After they are completely dried, they are sieved to obtain a mixed powder.

[0013] S2. Place the mixed powder into a graphite mold and pre-press it under a pressure of 20~30MPa;

[0014] S3. Place the pre-pressed graphite mold into a spark plasma sintering furnace, introduce nitrogen gas, heat it to 1600-1700℃ at a rate of 100-200℃, apply an axial pressure of 30-50MPa at the same time, hold it at that temperature for 5-20 minutes, and then cool it down to 800℃ and let it cool naturally to room temperature to obtain high-performance silicon nitride ceramics.

[0015] Preferably, the ball milling method in step S1 is a planetary ball mill or a roller ball mill, the ball milling speed is 250~300 r / min, the ball milling time is 18~24 h; the rotary evaporation drying temperature is 45~65℃; and the sieve aperture is 100~200 mesh.

[0016] Preferably, the pre-compression time in step S2 is 2 to 5 minutes.

[0017] The application of the high-performance silicon nitride ceramics in the fields of cutting tools or engine components.

[0018] This invention involves adding ZrH2 to remove hydrogen at high temperature, then reacting it with silicon nitride and surface SiO2 to generate in-situ ZrN and gaseous SiO. Under a nitrogen atmosphere, the generated SiO gas increases the atomic ratio of N and O in the liquid phase Mg-Yb-Si-ON at high temperature, reducing the viscosity of the Mg-Yb-Si-ON liquid phase, thereby promoting the transformation of the α-Si3N4 phase to the β-Si3N4 phase and obtaining high-performance bimodal microstructure silicon nitride ceramics.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. This invention adds ZrH2 as a second phase to silicon nitride ceramics, promoting the dissolution and precipitation of equiaxed α-Si3N4, transforming it into long rod-shaped β-Si3N4, forming an interlocked bimodal microstructure, and improving fracture toughness and strength.

[0021] 2. In this invention, ZrH2 is used as the second phase to obtain silicon nitride ceramics with high β content at a low temperature of 1600~1700℃, which significantly reduces energy consumption and avoids further coarsening of grains and reduction of mechanical properties caused by high temperature.

[0022] 3. This invention introduces ZrH2 to generate a ZrN second phase in situ during sintering, resulting in silicon nitride ceramics with a density greater than 98.7%, a hardness of 15.8~18.2 GPa, a flexural strength of 673~773 MPa, and a fracture toughness of 6.6~8.4 MPa·m. -2 This improves the mechanical properties of silicon nitride. Attached Figure Description

[0023] Figure 1 This is a scanning electron microscope (SEM) image of the silicon nitride ceramic of Example 1;

[0024] Figure 2 The image shows a scanning electron microscope (SEM) image of the silicon nitride ceramic in Comparative Example 1.

[0025] Figure 3 The image shows a scanning electron microscope (SEM) image of the silicon nitride ceramic in Comparative Example 2.

[0026] Figure 4 The XRD patterns of silicon nitride ceramics in Example 1, Comparative Examples 1 and 2 are shown. Detailed Implementation

[0027] The present invention will be further described below with reference to specific embodiments, but these should not be construed as limiting the invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in this technical field.

[0028] The α-Si3N4 powder used in the embodiments of the present invention has a purity of 98wt% or higher and a particle size of 0.3~1µm; the MgO powder has a purity of 99.8wt% or higher and a particle size of 50~100nm; the Yb2O3 powder has a purity of 99.8wt% or higher and a particle size of 50~100nm; and the ZrH2 powder has a purity of 99.9wt% or higher and a particle size of 1~10µm.

[0029] In the examples, the β-Si3N4 phase content was determined by... The calculation yields, where I α(201) I α(210) I β(200) I β(120) These represent the peak intensities of the four peaks.

[0030] Example 1

[0031] 1. α-Si3N4 powder, Yb2O3 powder, MgO powder, ZrH2 powder and anhydrous ethanol in a mass ratio of 90:6:4:15 were ball-milled in a roller mill at 300 r / min for 24 h. Then, the mixture was dried by rotary evaporation at 50 °C. After complete drying, the mixture was passed through a 100-mesh sieve to obtain a mixed powder.

[0032] 2. Place the mixed powder into a graphite mold in a spark plasma sintering furnace, apply an axial pressure of 20 MPa using a manual hydraulic press and hold the pressure for 5 minutes to perform pre-pressing molding;

[0033] 3. The pre-pressed graphite mold is placed in a spark plasma sintering furnace. Under a nitrogen atmosphere, the temperature is increased to 1700℃ at a rate of 100℃ / min, while an axial pressure of 30MPa is applied. The temperature is held for 10min, and then the temperature is decreased to 800℃ at a rate of 100℃ / min and naturally cooled to room temperature to obtain silicon nitride ceramic, labeled as 1700-15ZrH2.

[0034] The silicon nitride ceramic microstructure prepared in this embodiment is as follows: Figure 1 As shown, by Figure 1 It is known that a large number of long rod-shaped β-Si3N4 atoms are present. The β-Si3N4 content is 97.5%, and its relative density is 98.8%. The flexural strength is 710 MPa, and the fracture toughness is 8.0 MPa·m. -2 The hardness is 16.4 GPa, indicating that the silicon nitride ceramic has excellent mechanical properties.

[0035] Example 2

[0036] The difference from Example 1 is that the mass ratio of α-Si3N4 powder, Yb2O3 powder, MgO powder, and ZrH2 powder in step 1 is 90:6:4:10.

[0037] The silicon nitride ceramic prepared in this embodiment has a β-Si3N4 content of 92.6%, contains a large number of long rod-shaped β-Si3N4, has a relative density of 98.9%, a flexural strength of 673 MPa, and a fracture toughness of 7.6 MPa·m. -2 The hardness is 16.8 GPa, indicating that the silicon nitride ceramic has excellent mechanical properties.

[0038] Example 3

[0039] The difference from Example 1 is that the mass ratio of α-Si3N4 powder, Yb2O3 powder, MgO powder, and ZrH2 powder in step 1 is 90:6:4:20.

[0040] The silicon nitride ceramic prepared in this embodiment has a 100% β-Si3N4 content, contains a large number of long rod-shaped β-Si3N4, has a relative density of 98.7%, a flexural strength of 773 MPa, and a fracture toughness of 8.4 MPa·m. -2 The hardness is 15.8 GPa, indicating that the silicon nitride ceramic has excellent mechanical properties.

[0041] Example 4

[0042] The difference from Example 1 is that the sintering temperature in step 3 is 1650°C.

[0043] The silicon nitride ceramic prepared in this embodiment has a β-Si3N4 content of 52.8%, a relative density of 99.3%, a flexural strength of 682 MPa, and a fracture toughness of 6.6 MPa·m. -2 The hardness is 18.2 GPa, indicating that this silicon nitride ceramic possesses excellent mechanical properties.

[0044] Comparative Example 1

[0045] The difference from Example 1 is that in step 1, the mass ratio of α-Si3N4 powder, Yb2O3 powder, and MgO powder is 90:6:4, resulting in silicon nitride ceramic, labeled as 1700-0ZrH2.

[0046] The microstructure of the silicon nitride ceramic in this comparative example is as follows: Figure 2 As shown, by Figure 2 It can be seen that a large number of long rod-shaped β-Si3N4 are present, but not as significantly as in the 1700-15ZrH2 sample. The β-Si3N4 content is 84.5%, lower than that of the 1700-15ZrH2 sample, its relative density is 99.2%, its flexural strength is 610 MPa, and its fracture toughness is 7.3 MPa·m. -2 The hardness was 17.1 GPa, indicating that the addition of ZrH2 can promote the transformation from α-Si3N4 to β-Si3N4, resulting in a more significant bimodal structure, thereby improving fracture toughness and bending strength.

[0047] Comparative Example 2

[0048] The difference from Example 1 is that ZrH2 in step 1 is replaced with ZrN to obtain silicon nitride ceramic, labeled as 1700-15ZrN.

[0049] The microstructure of the silicon nitride ceramic in this comparative example is as follows: Figure 3 As shown, by Figure 3 It can be seen that the content of long rod-shaped β-Si3N4 is relatively low, indicating that ZrN inhibits the transformation of α-Si3N4 to β-Si3N4. The β-Si3N4 content is 67.4%, its relative density is 99.3%, its flexural strength is 582 MPa, and its fracture toughness is 6.9 MPa·m. -2 The hardness is 17.9 GPa. The introduction of ZrN inhibits the transformation from α-Si3N4 to β-Si3N4, while ZrH2 promotes the phase transformation, resulting in a lower toughness than the silicon nitride ceramics of Comparative Example 1 and Example 1.

[0050] Figure 4 The XRD patterns of silicon nitride ceramics in Examples 1, 1, and 2 are shown below. Figure 4It can be seen that the peak intensity of β-Si3N4 in 1700-15ZrN of Comparative Example 2 is lower than that in 1700-0ZrH2 of Comparative Example 1, while the peak intensity of β-Si3N4 in 1700-15ZrH2 of Example 1 is higher than that in 1700-0ZrH2 of Comparative Example 1. ZrN will inhibit the transformation of α-Si3N4 phase to β-Si3N4 phase. However, the introduction of ZrH2 reduces the viscosity of Mg-Yb-Si-ON liquid phase by generating ZrN through in-situ reaction, thereby promoting the transformation of α-Si3N4 phase to β-Si3N4 phase. Therefore, the introduction of ZrH2 can obtain silicon nitride ceramics with better comprehensive mechanical properties than ZrN.

[0051] Comparative Example 3

[0052] The difference from Example 4 is that the mass ratio of α-Si3N4 powder, Yb2O3 powder, and MgO powder in step 1 is 90:6:4.

[0053] In this embodiment, the silicon nitride ceramic has a β-Si3N4 content of 41.5%, a relative density of 99.6%, a flexural strength of 542 MPa, and a fracture toughness of 5.6 MPa·m. -2 The hardness was 19.1 GPa. Compared with Example 4, the introduction of ZrH2 can promote the transformation of α-Si3N4 to β-Si3N4, thereby improving fracture toughness and strength.

[0054] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations and simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A high-performance silicon nitride ceramic, characterized in that, The silicon nitride ceramic is prepared by ball milling, rotary drying, and sieving of α-Si3N4 powder, MgO powder, Yb2O3 powder, ZrH2 powder, and anhydrous ethanol to obtain a mixed powder. The mixed powder is then pre-pressed and sintered under a nitrogen atmosphere at 30-50 MPa pressure and 1600-1700℃ using spark plasma sintering. The mass ratio of α-Si3N4 powder, Yb2O3 powder, MgO powder, and ZrH2 powder is 90: x :(10~ x :(10~25) x =2~8.

2. The high-performance silicon nitride ceramic according to claim 1, characterized in that, The α-Si3N4 powder has a purity of ≥98wt% and a particle size of 0.3~1µm; the MgO powder has a purity of ≥99.8wt% and a particle size of 50~100nm; the Yb2O3 powder has a purity of ≥99.8wt% and a particle size of 50~100nm; and the ZrH2 powder has a purity of ≥99.9wt% and a particle size of 1~10µm.

3. The high-performance silicon nitride ceramic according to claim 1, characterized in that, The silicon nitride ceramic has a density greater than 98.7%, a hardness of 15.8~18.2 GPa, a flexural strength of 673~773 MPa, and a fracture toughness of 6.6~8.8 MPa·m. -2 .

4. The method for preparing high-performance silicon nitride ceramics according to any one of claims 1-3, characterized in that, Specifically, the following steps are included: S1. Mix α-Si3N4 powder, MgO powder, Yb2O3 powder, ZrH2 powder and anhydrous ethanol and ball mill them, then dry them by rotary evaporation. After they are completely dried, they are sieved to obtain a mixed powder. S2. Place the mixed powder into a graphite mold and pre-press it under a pressure of 20~30MPa; S3. Place the pre-pressed graphite mold into a spark plasma sintering furnace, introduce nitrogen gas, heat it to 1600-1700℃ at a rate of 100-200℃, apply an axial pressure of 30-50MPa at the same time, hold it at that temperature for 5-20 minutes, and then cool it down to 800℃ and let it cool naturally to room temperature to obtain high-performance silicon nitride ceramics.

5. The method for preparing high-performance silicon nitride ceramics according to claim 4, characterized in that, The ball milling method in step S1 is planetary ball milling or roller ball milling, the ball milling speed is 250~300 r / min, and the ball milling time is 18~24 h; the rotary evaporation drying temperature is 45~65℃; and the sieve aperture is 100~200 mesh.

6. The method for preparing high-performance silicon nitride ceramics according to claim 4, characterized in that, The pre-compression time in step S2 is 2~5 minutes.

7. The application of the high-performance silicon nitride ceramic according to any one of claims 1-3 in the field of cutting tools or engine components.

Citation Information

Patent Citations

  • Low-dielectric-constant silicon carbide and high-performance silicon nitride ceramic substrate and preparation method thereof