A method for preparing a self-assembled hole transport material containing nitrogen-containing heterocyclic linking units and its photovoltaic application.
By leveraging the intramolecular non-covalent interactions between the nitrogen heterocyclic linking unit and the end group, and the steric hindrance effect of the triphenylamine end group, the problems of easy aggregation and poor film formation of HTSAMs were solved, enabling efficient and stable operation of perovskite solar cells.
Patent Information
- Application Number
- CN202611487365.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-10
AI Technical Summary
Existing self-assembled hole transport materials (HTSAMs) are prone to aggregation and have poor film-forming properties, resulting in poor performance of perovskite solar cells. In particular, the strong intermolecular π-π interactions, molecular aggregation, and interface defects lead to nonradiative recombination, which affects device performance.
A self-assembled hole transport material containing nitrogen-containing heterocyclic linking units is used. A coplanar conjugated molecular framework is formed through intramolecular non-covalent interactions between the nitrogen-containing heterocyclic linking units and the end groups. Combined with the steric hindrance effect of the triphenylamine end groups, molecular aggregation is suppressed, and uniform and dense film stacking is achieved.
It improves the π-π interaction between molecules, enhances the ordered stacking and film formation of the film, optimizes the interface properties and the crystal quality of the perovskite film, and improves the photoelectric conversion efficiency and device stability of perovskite solar cells.
Smart Images

Figure CN123062489A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic materials technology, and relates to a method for preparing a self-assembled hole transport material containing nitrogen-containing heterocyclic linking units and its photovoltaic application. Specifically, it relates to the preparation of a self-assembled hole transport material containing nitrogen-containing heterocyclic linking units and its application in perovskite solar cells. Background Technology
[0002] Perovskite solar cells have attracted significant attention from researchers in the photovoltaic field in recent years due to their simple fabrication process and excellent photoelectric conversion efficiency. Among them, self-assembled monolayers (HTSAMs), as an emerging type of hole transport material, have powerfully promoted the development of perovskite solar cells due to their advantages such as low cost, tunable work function, ability to control perovskite crystallization, and optimization of interfacial charge dynamics. However, traditional HTSAMs generally suffer from problems such as molecular aggregation and poor film coverage, which interfere with the perovskite film crystallization process, generate numerous interfacial defects, and induce severe nonradiative recombination, ultimately significantly weakening device performance.
[0003] Currently, most commercially available HTSAMs materials use carbazole derivatives as end groups. The strong intermolecular π-π interactions induced by these highly conjugated segments are a key factor in molecular aggregation. Therefore, weakening intermolecular π-π interactions is a common strategy to achieve uniform coverage of HTSAMs on the substrate. Existing optimization methods mainly focus on end group modification, including introducing sterically hindered groups and constructing a three-dimensional π-conjugated framework. However, both have significant drawbacks: excessive molecular steric hindrance hinders orderly stacking, forming amorphous structures with disordered orientations, resulting in van der Waals gaps at the interface, where holes can only be transported via tunneling, significantly reducing hole transport efficiency. Furthermore, end group conjugation modification easily induces rearrangement of the highest occupied molecular orbital energy levels of HTSAMs, causing energy level mismatch with the perovskite layer, exacerbating interfacial charge recombination, and adding complexity to molecular design. Therefore, limiting modifications to end groups cannot simultaneously solve the three major problems of molecular aggregation, disordered stacking, and energy level mismatch. In contrast, conjugation regulation of the linking groups of HTSAMs can effectively overcome these bottlenecks. Compared to traditional alkyl chains, aromatic linking groups can precisely regulate intermolecular forces and optimize charge transport capabilities, synergistically balancing molecular anti-aggregation and ordered stacking characteristics. Furthermore, the conjugation regulation of linking groups has less impact on molecular energy level perturbation, effectively solving the challenges of HTSAMs molecular design.
[0004] Based on the aforementioned problems in the prior art, this invention aims to study two types of HTSAMs molecules based on nitrogen heterocyclic linking units, to solve the technical problems of easy aggregation and poor film formation of existing self-assembled hole transport materials, and to improve some of the shortcomings of this type of HTSAMs molecules in the application performance of perovskite solar cells. Summary of the Invention
[0005] To address the problems of poor performance in perovskite solar cells caused by the easy aggregation, poor film formation, and numerous interface defects of existing HTSAMs molecules, this invention provides a method for preparing self-assembled hole transport materials containing nitrogen-containing heterocyclic linking units and their photovoltaic applications. This method is based on HTSAMs molecules with conjugated nitrogen-containing heterocyclic linking units. The intramolecular non-covalent interactions between the nitrogen-containing heterocyclic linking units and the end groups induce a coplanar structure of the molecular framework. This highly conjugated structure enhances the intermolecular π-π interactions, achieving the uniform, dense, and ordered stacking thin film characteristics of HTSAMs. Based on this, the invention provides a method for molecule synthesis and its application in perovskite solar cells, enabling efficient and stable device operation.
[0006] To achieve the above objectives, the present invention provides a self-assembled hole transport material containing a nitrogen heterocyclic linking unit. The molecular structure of the self-assembled hole transport material includes a nitrogen heterocyclic linking unit, a triphenylamine end group covalently bonded to at least one end of the nitrogen heterocyclic linking unit, and a conjugated bridging unit located between the nitrogen heterocyclic linking unit and the triphenylamine end group. The nitrogen heterocyclic linking unit and the conjugated bridging unit form a coplanar conjugated molecular skeleton through intramolecular non-covalent interactions to enhance intermolecular π-π stacking. The triphenylamine end group has a propeller-shaped spatial torsion conformation, which inhibits excessive aggregation of molecules in the solution phase through steric hindrance effect, enabling the self-assembled hole transport material to self-assemble into a uniform and dense film.
[0007] Furthermore, the nitrogen-containing heterocyclic linking unit is a nitrogen-containing six-membered heterocycle selected from at least one of pyridine, pyrimidine, pyrazine, triazine, quinoline and their substituted derivatives; the intramolecular non-covalent interaction is an intramolecular CH…N hydrogen bond; the conjugated bridging unit is selected from at least one of thiophene, furan, benzene ring, selenophene and their substituted derivatives.
[0008] Furthermore, the functional end group of the triphenylamine is any one of unsubstituted triphenylamine, alkyl-substituted triphenylamine, alkoxy-substituted triphenylamine, or aryl-substituted triphenylamine, and the three benzene rings of the triphenylamine are in a propeller-like twisted conformation relative to the central nitrogen atom.
[0009] The second aspect of the present invention provides a method for preparing a self-assembled hole transport material containing nitrogen-containing heterocyclic linking units, wherein an arylboronic acid / boronic acid ester / halide monomer with a triphenylamine structure is cross-coupled with a halide / boronic acid / boronic acid ester monomer with a nitrogen-containing heterocycle through a Suzuki coupling reaction, a Stille coupling reaction, or a Heck coupling reaction, and the self-assembled hole transport material is obtained after purification.
[0010] Furthermore, the structural formula of the self-assembled hole transport material includes the following two: In the formula, the nitrogen heterocyclic linking units in (a) and (b) are pyridine and thiadiazolidine, respectively, and the corresponding names of the two molecules are PyPA and TPyPA.
[0011] Furthermore, it includes the following steps: S1. Synthesis of the target PyPA molecule: S11. Under a nitrogen atmosphere, 4-boronic acid triphenylamine, 5-bromo-2-iodopyridine, potassium carbonate, and tetra(triphenylphosphine)palladium were dissolved in a mixed solution of ethanol / deionized water / toluene (ethanol:deionized water:toluene = 1:1:3), and the mixture was refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, and purified by extraction, drying, and silica gel chromatography to obtain intermediate 1a. S12. Dissolve intermediate 1a obtained in step S11, diethyl phosphite, triethylamine and tetra(triphenylphosphine)palladium in toluene, reflux for 12 hours, cool to room temperature after the reaction is completed, and obtain intermediate 2a by extraction, drying and silica gel chromatography. S13. Under a nitrogen atmosphere, intermediate 2a was dissolved in dichloromethane and added to a round-bottom flask. Trimethylbromosilane was then slowly added dropwise to the solution, and the mixture was stirred at room temperature for 12 hours. After the reaction was completed, the solution was concentrated under reduced pressure and recrystallized with dichloromethane and / or methanol solution. The target PyPA molecule was obtained after purification. S2. Synthesis of the target TPyPA molecule: S21. Under a nitrogen atmosphere, 4-boronic acid triphenylamine, 4,7-dibromo-[1,2,5]thiadiazo[3,4-c]pyridine, potassium carbonate, and tetra(triphenylphosphine)palladium were dissolved in a mixed solution of ethanol / deionized water / toluene (ethanol:deionized water:toluene = 1:1:3), and the mixture was refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, and purified by extraction, drying, and silica gel chromatography to obtain intermediate 1b. S22. Dissolve intermediate 1b obtained in step S21, diethyl phosphite, triethylamine and tetra(triphenylphosphine)palladium in toluene, reflux for 12 hours, cool to room temperature after the reaction is completed, and obtain intermediate 2b by extraction, drying and silica gel chromatography. S23. Under a nitrogen atmosphere, intermediate 2b was dissolved in dichloromethane and added to a round-bottom flask. Trimethylbromosilane was then slowly added dropwise to the solution, and the mixture was stirred at room temperature for 12 hours. After the reaction was completed, the solution was concentrated under reduced pressure and recrystallized with dichloromethane and / or methanol solution. The purified solution yielded the target TPyPA molecule.
[0012] Further, in step S11, the molar ratio of 4-boronic acid triphenylamine, 5-bromo-2-iodopyridine, potassium carbonate, and tetrakis(triphenylphosphine)palladium is 1.0:1.2:4.0:0.05; in step S12, the molar ratio of intermediate 1a, diethyl phosphite, triethylamine, and tetrakis(triphenylphosphine)palladium is 1.0:2.0:10.0:0.05; in step S13, each millimole of intermediate 2a corresponds to 3 milliliters of trimethylbromosilane.
[0013] Further, in step S21, the molar ratio of 4-boronic acid triphenylamine, 4,7-dibromo-[1,2,5]thiadiazo[3,4-c]pyridine, potassium carbonate, and tetra(triphenylphosphine)palladium is 1.0:1.0:4.0:0.05; in step S22, the molar ratio of intermediate 1b, diethyl phosphite, triethylamine, and tetra(triphenylphosphine)palladium is 1.0:2.0:10.0:0.05; in step S23, each millimole of intermediate 2b corresponds to 3 milliliters of trimethylbromosilane.
[0014] A third aspect of the present invention provides a self-assembly functional thin film, which is prepared by self-assembly of the self-assembly hole transport material described in the present invention through solution processing; the self-assembly functional thin film is a uniform and dense nanoscale thin film, and there is ordered intermolecular π-π stacking inside the film.
[0015] A fourth aspect of the present invention provides a perovskite optoelectronic device comprising the self-assembly functional thin film described in the present invention; the self-assembly functional thin film is disposed at the buried interface between the perovskite light-absorbing layer and the charge transport layer, and is used to regulate the crystallization of the perovskite thin film, optimize the interface energy level matching, and improve the interface contact performance.
[0016] Furthermore, the perovskite optoelectronic device is a perovskite solar cell, a perovskite light-emitting diode, or a perovskite photodetector; the self-assembled functional thin film serves as a hole interface modification layer and is disposed between the perovskite light-absorbing layer and the hole transport layer.
[0017] The fifth aspect of this invention provides a method for fabricating the perovskite optoelectronic device described herein, comprising the following steps: (1) Deposit a first charge transport layer on a conductive substrate; (2) The self-assembled hole transport material is prepared into a precursor solution, deposited on the surface of the first charge transport layer by solution method, and then annealed to form a self-assembled functional film. (3) A perovskite light-absorbing layer is prepared on the surface of the self-assembled functional thin film; (4) A second charge transport layer and a counter electrode are sequentially deposited on the surface of the perovskite light absorption layer to obtain a perovskite optoelectronic device.
[0018] Compared with existing inventions, the beneficial effects of the present invention are: (1) This invention uses triphenylamine as the end group and nitrogen heterocycle as the linking group. Utilizing the steric hindrance effect of triphenylamine, the strong π-π interactions between the end groups of HTSAMs in solution can be weakened, effectively enhancing the anti-agglomeration property of the molecules and ensuring good solubility. Simultaneously, the intramolecular non-covalent interactions between the nitrogen heterocycle and the conjugated bridging unit can induce overall coplanarization of the molecular skeleton, increasing the degree of molecular conjugation, resulting in strong intermolecular interactions in the solid film and exhibiting a dense and ordered stacking. Thanks to this structure, the two molecules are uniformly dispersed in methanol solution without agglomeration, and can form a dense HTSAMs layer on the ITO substrate, further optimizing the buried interface properties and the crystallinity of the perovskite film, while also exhibiting good energy level matching with the perovskite layer.
[0019] (2) The two HTSAMs molecules designed in this invention use pyridine and thiadiazopyridine as linking groups, respectively. Compared with pyridine, thiadiazopyridine exhibits stronger intramolecular non-covalent interactions with the end groups. The TPyPA invented in this way has better film-forming performance. The perovskite solar cell designed in this way has a photoelectric conversion efficiency of up to 22.91% and exhibits excellent device stability, which is significantly better than PyPA. Attached Figure Description
[0020] Figure 1 This is the proton NMR spectrum of PyPA.
[0021] Figure 2 This is the 1H NMR spectrum of TPyPA.
[0022] Figure 3 Dynamic light scattering (DLS) of PyPA and TPyPA solutions.
[0023] Figure 4 Atomic force microscopy (AFM) images of PyPA and TPyPA deposited on ITO substrates; (a) ITO / PyPA, (b) ITO / TPyPA.
[0024] Figure 5 X-ray photoelectron spectra (XPS) of PyPA and TPyPA deposited on ITO substrates; (a) In 3d, (b) P 2p.
[0025] Figure 6 Wetness tests of perovskite precursor solutions on PyPA and TPyPA films; (a) ITO / PyPA, (b) ITO / TPyPA.
[0026] Figure 7Scanning electron microscope (SEM) images of perovskite films deposited on PyPA and TPyPA films; (a) ITO / PyPA / PVK, (b) ITO / TPyPA / PVK.
[0027] Figure 8 (a) Photoluminescence (PL) and (b) Time-resolved PL spectra of perovskite films deposited on PyPA and TPyPA films.
[0028] Figure 9 Current-voltage curves of perovskite devices based on PyPA and TPyPA.
[0029] Figure 10 The stability curves of perovskite devices based on PyPA and TPyPA under different conditions are shown: (a) 65°C, nitrogen atmosphere, (b) 25°C, 50-70% humidity, air atmosphere. Detailed Implementation
[0030] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0031] According to a first aspect of the present invention, an HTSAMs material based on nitrogen heterocyclic linking units is provided.
[0032] In one embodiment of the present invention, the HTSAMs material has a triphenylamine end group, a nitrogen heterocycle as a linking group, a phosphonic acid group as an anchoring group, and a benzene ring as a conjugated bridging group, and its structural formula includes the following two types: In the formula, the linking groups of the two molecules are pyridine and thiadiazolidine, respectively, named PyPA and TPyPA.
[0033] According to a second aspect of the present invention, a method for preparing HTSAMs is provided.
[0034] In one embodiment of the present invention, the method for preparing the HTSAMs material based on nitrogen heterocyclic linking units includes the following steps: S1. Synthesis of the target PyPA molecule: S11. Under a nitrogen atmosphere, triphenylamine 4-borate, 5-bromo-2-iodopyridine, potassium carbonate, and tetrakis(triphenylphosphine)palladium were dissolved in a mixed solution of ethanol / deionized water / toluene (ethanol:deionized water:toluene = 1:1:3), and the mixture was refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, extracted, dried, and purified by silica gel chromatography to obtain intermediate 1a. S12. Dissolve intermediate 1a obtained in step S11, diethyl phosphite, triethylamine and tetra(triphenylphosphine)palladium in toluene, reflux for 12 hours, cool to room temperature after the reaction is completed, and obtain intermediate 2a by extraction, drying and silica gel chromatography. S13. Under a nitrogen atmosphere, intermediate 2a was dissolved in dichloromethane and added to a round-bottom flask. Trimethylbromosilane was then slowly added dropwise to the solution, and the mixture was stirred at room temperature for 12 hours. After the reaction was completed, the solution was concentrated under reduced pressure and recrystallized from dichloromethane and / or methanol solution. The purified product was the target PyPA molecule. S2. Synthesis of the target TPyPA molecule: S21. Under a nitrogen atmosphere, triphenylamine 4-borate, 4,7-dibromo-[1,2,5]thiadiazo[3,4-c]pyridine, potassium carbonate, and tetra(triphenylphosphine)palladium were dissolved in a mixed solution of ethanol / deionized water / toluene (ethanol:deionized water:toluene = 1:1:3), and the mixture was refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, extracted, dried, and purified by silica gel chromatography to obtain intermediate 1b. S22. Dissolve intermediate 1b obtained in step S21, diethyl phosphite, triethylamine and tetra(triphenylphosphine)palladium in toluene, reflux for 12 hours, cool to room temperature after the reaction is completed, and obtain intermediate 2b by extraction, drying and silica gel chromatography. S23. Under a nitrogen atmosphere, intermediate 2b was dissolved in dichloromethane and added to a round-bottom flask. Trimethylbromosilane was then slowly added dropwise to the solution, and the mixture was stirred at room temperature for 12 hours. After the reaction was completed, the solution was concentrated under reduced pressure and recrystallized from dichloromethane and / or methanol solution. The purified product was the target TPyPA molecule.
[0035] In the preferred embodiment, in step S11, the molar ratio of 4-boronic acid triphenylamine, 5-bromo-2-iodopyridine, potassium carbonate, and tetrakis(triphenylphosphine)palladium is 1.0:1.2:4.0:0.05.
[0036] In the preferred embodiment, in steps S11, S12 and S13, the solvent used for extraction is dichloromethane.
[0037] In the preferred embodiment, in step S11, the eluent used for silica gel chromatography purification is a mixed solution of dichloromethane and petroleum ether in a 1:4 ratio.
[0038] In the preferred embodiment, in step S12, the molar ratio of intermediate 1a, diethyl phosphite, triethylamine, and tetra(triphenylphosphine)palladium is 1.0:2.0:9.0:0.05.
[0039] In the preferred embodiment, in step S12, the eluent used for silica gel chromatography purification is a mixed solution of dichloromethane and ethyl acetate in a 10:1 ratio.
[0040] In the preferred embodiment, in step S13, each 1 mmol of intermediate 2a corresponds to 3 ml of trimethylbromosilane.
[0041] In the preferred embodiment, in step S21, the molar ratio of 4-boronic acid triphenylamine, 4,7-dibromo-[1,2,5]thiadiazolo[3,4-c]pyridine, potassium carbonate, and tetra(triphenylphosphine)palladium is 1.0:1.2:4.0:0.05.
[0042] In the preferred embodiment, in steps S21, S22 and S23, the solvent for extraction is dichloromethane.
[0043] In the preferred embodiment, in step S21, the eluent used for silica gel chromatography purification is a mixed solution of dichloromethane and petroleum ether in a 1:3 ratio.
[0044] In the optimized scheme, in step S22, the molar ratio of intermediate 1b, diethyl phosphite, triethylamine, and tetra(triphenylphosphine)palladium is 1.0:2.0:9.0:0.05.
[0045] In the preferred embodiment, in step S22, the silica gel chromatography uses a mixed solution of dichloromethane and ethyl acetate in an 8:1 ratio as the eluent.
[0046] In the preferred embodiment, in step S23, each 1 mmol of intermediate 2b corresponds to 3 ml of trimethylbromosilane.
[0047] In the preferred embodiment, the drying is performed using anhydrous magnesium sulfate.
[0048] According to a third aspect of the present invention, an HTSAMs thin film is provided, which is prepared by self-assembly of the HTSAMs material by solution processing; the HTSAMs thin film is a uniform and dense nanoscale film with a root mean square roughness (RMS) ≤ 5 nm and ordered intermolecular π-π stacking exists inside the film.
[0049] According to a fourth aspect of the present invention, a perovskite solar cell is provided.
[0050] In one embodiment of the present invention, the perovskite solar cell is fabricated using an inverted structure, and the device structure is ITO / HTSAMs / PVK / PEAI / PCBM / BCP / Ag, wherein the HTSAMs are selected from PyPA or TPyPA.
[0051] A method for preparing the perovskite solar cell is provided according to a fifth aspect of the present invention.
[0052] In one embodiment of the present invention, the method for preparing the perovskite solar cell includes the following steps: S3, ITO substrate cleaning: ultrasonically cleaned sequentially with detergent, ultrapure water, anhydrous ethanol, acetone, and isopropanol, dried with nitrogen, treated with ultraviolet ozone, and transferred to a glove box filled with nitrogen. S4. Preparation of HTSAMs layer: The HTSAMs material is dissolved in anhydrous methanol to prepare an HTSAMs solution, which is then spin-coated onto the ITO substrate described in step S3 and annealed. S5. Preparation of perovskite layer: Lead iodide (PbI2), cesium iodide (CsI), methylammonium iodide (MAI), formamidinium iodide (FAI), and methylammonium chloride (MACl) are dissolved in a mixed solution of N,N-dimethylformamide / dimethyl sulfoxide to obtain a perovskite precursor solution. The perovskite precursor solution is then spin-coated onto the HTSAMs layer described in step S4 using a two-step method, during which chlorobenzene anti-solvent is added dropwise, followed by annealing.
[0053] S6. Electron transport layer and electrode preparation: The perovskite layer described in step S5 is spin-coated sequentially with an isopropanol solution containing phenylethyl ammonium iodide (PEAI), a chlorobenzene solution containing methyl [6,6]-phenyl-C61-butyrate (PCBM), and an ethanol solution containing 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP), and then annealed. Finally, a silver electrode is deposited by vapor deposition.
[0054] In the preferred embodiment, in step S3, the ultrasonic cleaning time is 15-30 minutes, and the ultraviolet ozone irradiation time is 15 minutes.
[0055] In the preferred embodiment, in step S4, the concentration of HTSAMs is 1 mg / ml.
[0056] In the preferred embodiment, in step S4, the spin coating speed is 5000 rpm and the time is 30 s.
[0057] In the preferred embodiment, in step S4, the annealing temperature is 100°C and the time is 10 min.
[0058] In the preferred embodiment, in step S5, the PbI2 mass concentration is 0.705 g / ml.
[0059] In the preferred embodiment, in step S5, the CsI mass concentration is 0.020 g / ml.
[0060] In the preferred embodiment, in step S5, the mass concentration of MAI is 0.024 g / ml.
[0061] In the preferred embodiment, in step S5, the FAI concentration is 0.219 g / ml.
[0062] In the preferred embodiment, in step S5, the mass concentration of MACl is 0.025 g / ml.
[0063] In a preferred embodiment, in step S5, the volume ratio of the N,N-dimethylformamide / dimethyl sulfoxide mixed solution is 4:1.
[0064] In the preferred embodiment, in step S5, the two-step spin coating method consists of first rotating at 1000 rpm for 10 seconds, and then rotating at 5000 rpm for 30 seconds. In the preferred embodiment, during step S5, chlorobenzene antisolvent is added dropwise, and 150 μl of chlorobenzene is added dropwise after spin coating for 30 s.
[0065] In the preferred embodiment, in step S5, the annealing temperature is 100°C and the time is 30 min.
[0066] In the preferred embodiment, in step S6, the PEAI concentration is 1.5 mg / ml.
[0067] In the preferred embodiment, in step S6, the PCBM mass concentration is 20 mg / ml.
[0068] In the preferred embodiment, in step S6, the BCP concentration is 0.5 mg / ml.
[0069] In the preferred embodiment, in step S6, the spin coating speed of the PEAI solution is 4000 rpm and the time is 30 s.
[0070] In the preferred embodiment, in step S6, the PEAI annealing temperature is 100°C and the time is 5 min.
[0071] In the preferred embodiment, in step S6, the spin coating speed of the PCBM solution is 2000 rpm and the time is 30 s.
[0072] In the preferred embodiment, in step S6, the PCBM annealing temperature is 100°C and the time is 30 min.
[0073] In the preferred embodiment, in step S6, the spin coating speed of the BCP solution is 4000 rpm and the time is 30 s.
[0074] In the preferred embodiment, in step S6, the BCP annealing temperature is 90°C and the time is 5 min.
[0075] In the preferred embodiment, in step S6, the evaporation rate of the silver electrode is 0.5~1 A / s. In a preferred embodiment, in step S6, the thickness of the silver electrode is 100 nm.
[0076] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0077] Unless otherwise specified, the raw materials used in the following embodiments are all disclosed in the prior art, such as those that can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0078] Example 1 An HTSAMs material, with pyridine as the linking group, has the following structural formula: The HTSAMs material is prepared by the following steps: S1. Synthesis of the target PyPA molecule: S11. A mixture of 1.16 g (4 mmol) of triphenylamine 4-borate, 1.41 g (5 mmol) of 5-bromo-2-iodopyridine, 2.30 g (16.2 mmol) of potassium carbonate, and 0.23 g (0.20 mmol) of tetra(triphenylphosphine)palladium was placed in a sealed three-necked flask. The system was purged with nitrogen several times to ensure nitrogen protection. Then, 30 mL of toluene, 10 mL of ethanol, and 10 mL of deionized water were added sequentially using a syringe. The mixture was then reacted at 90°C for 12 hours, and the reaction was detected by thin-layer chromatography. After the reaction was complete, the organic solvent was evaporated by rotary evaporation. The reaction solution was poured into 75 ml of saturated sodium chloride solution and extracted twice with 50 ml of dichloromethane. The organic phase was dried over anhydrous magnesium sulfate, filtered, and concentrated under reduced pressure. The crude product was purified by silica gel column chromatography (eluent: dichloromethane: petroleum ether = 1:4) to give 1.46 g of a white solid product (intermediate 1a), with a yield of 91%. The reaction formula is as follows: S12. The intermediate 1a (1.20 g, 3 mmol) obtained in step S11, diethyl phosphite (830 mg, 6 mmol), triethylamine (3 ml), and tetrakis(triphenylphosphine)palladium (0.17 g, 0.15 mmol) were mixed in a sealed three-necked flask, and the nitrogen gas was purged several times to ensure the system was under nitrogen protection. Then, 30 ml of toluene was added via syringe. The reaction was then carried out at 90°C for 12 hours, and the reaction was detected by thin-layer chromatography. After the reaction was completed, the organic solvent was evaporated by rotary evaporation, and the reaction solution was poured into 50 ml of saturated sodium chloride solution and extracted twice with 50 ml of dichloromethane. The organic phase was dried with anhydrous magnesium sulfate, filtered, and concentrated under reduced pressure. The crude product was purified by silica gel column chromatography (eluent: ethyl acetate: dichloromethane = 1:10) to give 0.90 g of milky white solid product (intermediate 2a), with a yield of 65%. The reaction formula is as follows: S13. Dissolve intermediate 2a (0.46 g, 1 mmol) obtained in step S12 in 20 mL of dichloromethane and transfer the solution to a round-bottom flask. Seal the flask and purge with nitrogen several times to ensure the system is under nitrogen protection. Then, slowly add 3 mL of trimethylbromosilane dropwise to the system using a syringe. Stir at room temperature for 12 hours. After the reaction is complete, evaporate the organic phase by rotary evaporation, wash with plenty of water, extract the product with dichloromethane, dry with anhydrous magnesium sulfate, recrystallize with methanol, filter the product, and dry under vacuum to finally obtain 0.34 g of a light green solid product (PyPA), with a yield of 85%. The reaction formula is as follows: The prepared PyPA 1H NMR spectrum is as follows Figure 1 As shown, its hydrogen NMR spectrum resolution data is as follows: 1 ¹H NMR (600 MHz, DMSO) δ 8.81 (d, J = 6.4 Hz, 1H), 8.04 (d, J = 8.8 Hz, 3H), 7.97 (d, J = 8.3 Hz, 1H), 7.36 (t, J = 7.9 Hz, 4H), 7.16 – 7.06 (m, 6H), 7.03 (d, J = 8.9 Hz, 2H), indicating that the preparation method provided by this invention can successfully prepare PyPA.
[0079] Example 2 A type of HTSAMs material, with thiadiazopyridine as the linking group, has the following structural formula: The HTSAMs material is prepared by the following steps: S2. Synthesis of the target TPyPA molecule: S21. A mixture of 1.16 g (4 mmol) of triphenylamine 4-borate, 1.47 g (5 mmol) of 4,7-dibromo-[1,2,5]thiadiazo[3,4-c]pyridine, 2.30 g (16.2 mmol) of potassium carbonate, and 0.23 g (0.20 mmol) of tetra(triphenylphosphine)palladium was placed in a sealed three-necked flask. The system was purged with nitrogen several times to ensure nitrogen protection. Then, 30 mL of toluene, 10 mL of ethanol, and 10 mL of deionized water were added sequentially using a syringe. The reaction was then carried out at 100°C for 12 hours, and the reaction was detected by thin-layer chromatography. After the reaction was complete, the organic solvent was evaporated by rotary evaporation. The reaction solution was poured into 75 ml of saturated sodium chloride solution and extracted twice with 50 ml of dichloromethane. The organic phase was dried over anhydrous magnesium sulfate, filtered, and concentrated under reduced pressure. The crude product was purified by silica gel column chromatography (eluent: dichloromethane: petroleum ether = 1:3) to give 1.43 g of orange solid product (intermediate 1b), with a yield of 74%. The reaction formula is as follows: S22. The intermediate 1b (1.38 g, 3 mmol) obtained in step S21, diethyl phosphite (830 mg, 6 mmol), triethylamine (3 ml), and tetrakis(triphenylphosphine)palladium (0.17 g, 0.15 mmol) were mixed in a sealed three-necked flask, and the nitrogen gas was purged several times to ensure the system was under nitrogen protection. Then, 30 ml of toluene was added via syringe. The reaction was then carried out at 90°C for 12 hours, and the reaction was detected by thin-layer chromatography. After the reaction was completed, the organic solvent was evaporated by rotary evaporation, and the reaction solution was poured into 50 ml of saturated sodium chloride solution and extracted twice with 50 ml of dichloromethane. The organic phase was dried over anhydrous magnesium sulfate, filtered, and concentrated under reduced pressure. The crude product was purified by silica gel column chromatography (eluent: ethyl acetate: dichloromethane = 1:8) to give 1.05 g of orange solid product (intermediate 2b), with a yield of 68%. The reaction formula is as follows: S23. Dissolve intermediate 2b (0.52 g, 1 mmol) obtained in step S22 in 20 mL of dichloromethane and transfer the solution to a round-bottom flask. Seal the flask and purge with nitrogen several times to ensure the system is under nitrogen protection. Then, slowly add 3 mL of trimethylbromosilane dropwise to the system using a syringe. Stir at room temperature for 12 hours. After the reaction is complete, evaporate the organic phase by rotary evaporation, wash with plenty of water, extract the product with dichloromethane, dry with anhydrous magnesium sulfate, recrystallize with methanol, filter the product, and dry under vacuum to finally obtain 0.37 g of a red solid product (TPyPA), with a yield of 80%. The reaction formula is as follows: The prepared TPyPA 1H NMR spectrum is as follows Figure 2 As shown, its hydrogen NMR spectrum resolution data is as follows: 1 ¹H NMR (600 MHz, DMSO) δ 8.09 (dd, J = 15.1, 7.1 Hz, 1H), 7.92 (d, J = 8.5 Hz, 2H), 7.79 (s, 1H), 7.65 – 7.53 (m, 1H), 7.35 (t, J = 7.8 Hz, 3H), 7.10 (dt, J = 15.9, 7.7 Hz, 7H), indicating that the preparation method provided by this invention can successfully prepare TPyPA.
[0080] Example 3 A perovskite solar cell based on HTSAMs prepared in Example 1 is disclosed, which adopts an inverted structure and has a device structure of ITO / PyPA / PVK / PEAI / PCBM / BCP / Ag.
[0081] The method for preparing the perovskite solar cell includes the following steps: S3. ITO Substrate Cleaning: Place the ITO conductive glass in a cleaning rack and then into a beaker. Add soapy water to the beaker to cover the substrate, and clean it in an ultrasonic cleaner for 15 minutes. Then, discard the soapy water, add deionized water to cover the substrate, and clean it in an ultrasonic cleaner for 15 minutes. Repeat this process several times to ensure no soapy water residue remains. Next, add acetone to cover the substrate and clean it in an ultrasonic cleaner for 15 minutes. Repeat this process twice. Then, add isopropanol to cover the substrate and clean it in an ultrasonic cleaner for 15 minutes. Repeat this process twice. Finally, add anhydrous ethanol and clean it in an ultrasonic cleaner for 15 minutes. Repeat this process twice. Finally, store the ITO substrate in an ethanol solution. Before each use, dry the ITO with a nitrogen gun.
[0082] After drying, the ITO substrates are irradiated in a UV ozone cleaner for 15 minutes to remove residual solvent and improve ITO wettability. The treated ITO substrates are then placed in a nitrogen-filled glove box for later use.
[0083] S4. PyPA Layer Preparation: Weigh 1.0 mg of the PyPA prepared in Example 1 using an electronic balance and place it in a 5 mL glass bottle. Then add methanol to prepare a 1.0 mg / mL HTSAMs solution. Place the ITO substrate prepared in step S3 on a spin coater. Use a pipette to evenly spread 50 μL of the HTSAMs solution evenly over the ITO substrate. Set the spin coater speed to 5000 rpm and the time to 30 s. After spin coating, place the substrate on a heating stage and heat-anneal at 100°C for 10 minutes. The HTSAMs layer is thus obtained. The entire process is carried out in a nitrogen-filled glove box.
[0084] S5. Preparation of the perovskite layer: Weigh 19.48 mg of lead iodide, 23.85 mg of methylammonium iodide, 219.26 mg of formamidinium iodide, and 25.0 mg of methylammonium chloride using an electronic balance and place them in a 5 mL brown glass bottle. Add 800 μL of N,N-dimethylformamide and 200 μL of dimethyl sulfoxide, and stir thoroughly on a shaker for at least 8 hours to prepare a perovskite precursor solution. Then, place the substrate prepared in step S4 on a spin coater, and use a pipette to evenly spread 60 μL of the perovskite precursor solution onto the prepared HTSAMs layer. Use a two-step spin coating method, setting the spin coater speed to 1000 rpm for 10 s, then increasing the speed to 5000 rpm for 30 s. At the 30th second of spin coating, add 150 μL of chlorobenzene. Finally, the treated substrate was placed on a heating stage and heat-annealed at 100°C for 30 minutes to obtain the perovskite layer. The entire process was carried out in a glove box filled with nitrogen.
[0085] S6. Electron transport layer and electrode preparation: Weigh 1.5 mg of PEAI into a 5 mL glass bottle using an electronic balance, and add isopropanol to prepare a 1.5 mg / mL PEAI solution. Place the substrate prepared in step S5 on a spin coater, and use a pipette to evenly spread 30 μL of the PEAI solution onto the prepared substrate. Set the spin coater speed to 4000 rpm for 30 s. After spin coating, place the substrate on a heating stage and heat-anneal at 100°C for 10 minutes to obtain the PEAI layer. Weigh 20 mg of PCBM into a 5 mL glass bottle using an electronic balance, and add chlorobenzene to prepare a 20 mg / mL PCBM solution. Use a pipette to evenly spread 60 μL of the PCBM solution onto the above PEAI layer. Set the spin coater speed to 2000 rpm for 30 s. After spin coating, the substrate was placed on a heating stage and annealed at 100°C for 30 minutes to obtain the PCBM layer. 1 mg of BCP was weighed into a 5 mL glass bottle using an electronic balance, and anhydrous ethanol was added to prepare a 0.5 mg / mL BCP solution. 30 μL of the BCP solution was pipetted onto the PCBM layer and the spin coater was set to 4000 rpm for 30 s. After spin coating, the substrate was placed on a heating stage and annealed at 90°C for 5 minutes to obtain the BCP layer. The entire process was performed in a nitrogen-filled glove box. The treated substrate was then transferred to a vacuum deposition system, where 100 nm of Ag was deposited at a rate of 0.5–1 A / s.
[0086] Example 4 The method is basically the same as in Example 3, except that in step S4, the solution preparation method of the HTSAMs layer is to weigh 1 mg of TPyPA prepared in Example 2 using an electronic balance, and then add methanol to prepare a 1 mg / mL TPyPA solution.
[0087] Testing and Analysis The samples from Examples 1 and 2 were characterized and their performance was tested, such as... Figures 1-5 As shown.
[0088] like Figure 1 The image shows the 1H NMR spectrum of the PyPA molecule prepared in Example 1, indicating that the target HTSAMs molecule was successfully prepared.
[0089] like Figure 2 The image shows the 1H NMR spectrum of the TPyPA molecule prepared in Example 2, indicating that the target HTSAMs molecule was successfully prepared.
[0090] like Figure 3The image shows the dynamic light scattering (DLS) results for PyPA and TPyPA solutions, reflecting the particle size distribution of the two HTSAMs in methanol at a concentration of 0.5 mg / ml. The average particle sizes of PyPA and TPyPA in methanol solution are 667 and 718 nm, respectively, indicating that both molecules have good solubility.
[0091] like Figure 4 The images show atomic force microscopy (AFM) images of PyPA and TPyPA deposited on an ITO substrate. The RMS roughness of the PyPA and TPyPA films are 4.02 nm and 3.52 nm, respectively. TPyPA exhibits a more uniform and denser covering structure, which stems from stronger intramolecular non-covalent interactions between thiadiazopyridine and the end groups, promoting a coplanar molecular framework. This configuration further enhances stronger intermolecular π-π interactions in the TPyPA film stack.
[0092] like Figure 5 The image shows the X-ray photoelectron spectroscopy (XPS) spectra of PyPA and TPyPA deposited on an ITO substrate. Compared to a pure ITO substrate, after the adsorption of both HTSAMs, the 3d orbitals of In both showed a shift towards higher binding energies, indicating that both HTSAMs were successfully adsorbed on the ITO surface. Furthermore, the P 2p orbital binding energy of TPyPA is higher than that of PyPA, indicating that TPyPA has a stronger anchoring effect.
[0093] like Figure 6 The image shows the wettability test of the perovskite precursor solution on HTSAM films. The contact angles of the perovskite precursor solution on PyPA and TPyPA films are 51.8° and 49.2°, respectively. This indicates that TPyPA exhibits better wettability of the perovskite precursor solution, which is attributed to the highly compact packing structure and stronger polar groups of TPyPA.
[0094] like Figure 7 The images show scanning electron microscope (SEM) images of perovskite films deposited on two types of HTSAMs films. The perovskite film deposited on TPyPA film exhibits a larger grain size. No obvious voids were found. This demonstrates the promoting effect of dense TPyPA film on perovskite crystal growth.
[0095] like Figure 8 The images show the photoluminescence (PL) and time-resolved PL (TRPL) spectra of perovskite films deposited on two types of HTSAMs films. The TPyPA-based perovskite film exhibits significant fluorescence quenching and a shorter fluorescence lifetime. This indicates that the perovskite film has fewer defects and less nonradiative recombination, which is more conducive to carrier extraction / transport efficiency.
[0096] like Figure 9The figures show the current-voltage curves of perovskite devices based on PyPA and TPyPA. It can be seen that the device performance based on PyPA in Example 1 is as follows: Standard simulated sunlight (AM 1.5 G, 100 mW / cm²) 2 Under illumination, the open-circuit voltage is 1.16 V, and the short-circuit current is 23.11 mA / cm². 2 The fill factor is 76.95%, and the photoelectric conversion efficiency is 20.62%. The device performance of the TPyPA in Example 2 is as follows: under standard simulated sunlight (AM 1.5 G, 100 mW / cm²) irradiation, the open-circuit voltage is 1.17 V, and the short-circuit current is 24.98 mA / cm². 2 The fill factor is 78.34%, and the photoelectric conversion efficiency is 22.91%. Compared with PyPA, the device based on TPyPA has significantly better efficiency.
[0097] like Figure 10 The figures show the stability curves of perovskite devices based on PyPA and TPyPA under different conditions. Under unpackaged conditions, the TPyPA-based perovskite device exhibits better damp-heat stability.
[0098] The embodiments of this application have been described above with reference to the accompanying drawings. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are only for the purpose of helping to understand the core ideas of this application. However, this application is not limited to the specific embodiments described above, which are merely illustrative and not restrictive. Those skilled in the art, under the guidance of this application, can make many modifications without departing from the spirit and scope of the claims, all of which fall within the protection scope of this application.
Claims
1. A self-assembled hole transport material containing nitrogen-containing heterocyclic linking units, characterized in that, The molecular structure of the self-assembled hole transport material includes a nitrogen heterocyclic linking unit, a triphenylamine end group covalently bonded to at least one end of the nitrogen heterocyclic linking unit, and a conjugated bridging unit located between the nitrogen heterocyclic linking unit and the triphenylamine end group. The nitrogen heterocyclic linking unit and the conjugated bridging unit form a coplanar conjugated molecular skeleton through intramolecular non-covalent interactions to enhance intermolecular π-π stacking. The triphenylamine end group has a propeller-shaped spatial torsion conformation, which inhibits excessive aggregation of molecules in the solution phase through steric hindrance effect, enabling the self-assembled hole transport material to self-assemble into a uniform and dense film.
2. The self-assembled hole transport material according to claim 1, characterized in that, The nitrogen-containing heterocyclic linking unit is a nitrogen-containing six-membered heterocycle selected from at least one of pyridine, pyrimidine, pyrazine, triazine, quinoline and their substituted derivatives; the intramolecular non-covalent interaction is an intramolecular CH…N hydrogen bond; the conjugated bridging unit is selected from at least one of thiophene, furan, benzene ring, selenophene and their substituted derivatives.
3. A method for preparing a self-assembled hole transport material with nitrogen-containing heterocyclic linking units as described in claim 1, characterized in that, The self-assembled hole transport material is obtained by cross-coupling arylboronic acid / boronic acid ester / halide monomers with triphenylamine structures to halide / boronic acid / boronic acid ester monomers with nitrogen heterocycles via Suzuki coupling reaction, Stille coupling reaction or Heck coupling reaction, followed by purification.
4. The preparation method according to claim 3, characterized in that, The self-assembled hole transport material has the following two structural formulas: In the formula, the nitrogen heterocyclic linking units in (a) and (b) are pyridine and thiadiazolidine, respectively, and the corresponding names of the two molecules are PyPA and TPyPA.
5. The preparation method according to claim 4, characterized in that, Includes the following steps: S1. Synthesis of the target PyPA molecule: S11. Under a nitrogen atmosphere, 4-boronic acid triphenylamine, 5-bromo-2-iodopyridine, potassium carbonate, and tetra(triphenylphosphine)palladium were dissolved in a mixed solution of ethanol:deionized water:toluene = 1:1:
3. The mixture was refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature and purified by extraction, drying, and silica gel chromatography to obtain intermediate 1a. S12. Intermediate 1a, diethyl phosphite, triethylamine and tetra(triphenylphosphine)palladium were dissolved in toluene and refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature and purified by extraction, drying and silica gel chromatography to obtain intermediate 2a. S13. Under a nitrogen atmosphere, intermediate 2a was dissolved in dichloromethane and added to a round-bottom flask. Trimethylbromosilane was slowly added dropwise to the solution and stirred at room temperature for 12 hours. After the reaction was completed, the solution was concentrated under reduced pressure and recrystallized with dichloromethane and / or methanol solution. The target PyPA molecule was obtained after purification. S2. Synthesis of the target TPyPA molecule: S21. Under a nitrogen atmosphere, 4-boronic acid triphenylamine, 4,7-dibromo-[1,2,5]thiadiazo[3,4-c]pyridine, potassium carbonate, and tetra(triphenylphosphine)palladium were dissolved in a mixed solution of ethanol:deionized water:toluene = 1:1:
3. The mixture was refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature and purified by extraction, drying, and silica gel chromatography to obtain intermediate 1b. S22. Intermediate 1b, diethyl phosphite, triethylamine and tetra(triphenylphosphine)palladium were dissolved in toluene and refluxed for 12 hours. After the reaction was completed, the mixture was cooled to room temperature and purified by extraction, drying and silica gel chromatography to obtain intermediate 2b. S23. Under a nitrogen atmosphere, intermediate 2b was dissolved in dichloromethane and added to a round-bottom flask. Trimethylbromosilane was slowly added dropwise to the solution, and the mixture was stirred at room temperature for 12 hours. After the reaction was completed, the solution was concentrated under reduced pressure and recrystallized with dichloromethane and / or methanol solution. The purified solution yielded the target TPyPA molecule.
6. The preparation method according to claim 5, characterized in that, In step S11, the molar ratio of 4-boronic acid triphenylamine, 5-bromo-2-iodopyridine, potassium carbonate, and tetrakis(triphenylphosphine)palladium is 1.0:1.2:4.0:0.05; in step S12, the molar ratio of intermediate 1a, diethyl phosphite, triethylamine, and tetrakis(triphenylphosphine)palladium is 1.0:2.0:10.0:0.05; in step S13, each millimole of intermediate 2a corresponds to 3 milliliters of trimethylbromosilane.
7. The preparation method according to claim 5, characterized in that, In step S21, the molar ratio of 4-boronic acid triphenylamine, 4,7-dibromo-[1,2,5]thiadiazo[3,4-c]pyridine, potassium carbonate, and tetra(triphenylphosphine)palladium is 1.0:1.0:4.0:0.05; in step S22, the molar ratio of intermediate 1b, diethyl phosphite, triethylamine, and tetra(triphenylphosphine)palladium is 1.0:2.0:10.0:0.05; in step S23, each millimole of intermediate 2b corresponds to 3 milliliters of trimethylbromosilane.
8. A self-assembling functional thin film, characterized in that, The self-assembled hole transport material of claim 1 is prepared by solution processing; the self-assembled functional film is a uniform and dense nanoscale film with ordered intermolecular π-π stacking inside the film.
9. A perovskite optoelectronic device, characterized in that, The invention comprises the self-assembly functional thin film as described in claim 8; the self-assembly functional thin film is disposed at the buried interface between the perovskite light-absorbing layer and the charge transport layer, and is used to regulate the crystallization of the perovskite thin film, optimize the interface energy level matching, and improve the interface contact performance.
10. A method for fabricating the perovskite optoelectronic device according to claim 9, characterized in that, Includes the following steps: (1) Deposit a first charge transport layer on a conductive substrate; (2) The self-assembled hole transport material is prepared into a precursor solution, deposited on the surface of the first charge transport layer by solution method, and then annealed to form a self-assembled functional film. (3) A perovskite light-absorbing layer is prepared on the surface of the self-assembled functional thin film; (4) A second charge transport layer and a counter electrode are sequentially deposited on the surface of the perovskite light absorption layer to obtain a perovskite optoelectronic device.