A composite modified polyvinyl alcohol acetal resin, its preparation method and application
By introducing α-ester units and ethylene units into the preparation method of composite modified polyvinyl acetal resin, the problems of plasticizer migration, high solution viscosity and poor dispersibility of inorganic powder in existing resins are solved, achieving low viscosity stability and high thermal decomposition resistance, which is suitable for electronic ceramic casting and bonding of precision electronic components.
Patent Information
- Application Number
- CN202610898776.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-22
- Publication Date
- 2026-11-10
AI Technical Summary
Existing polyvinyl acetal resins suffer from problems such as plasticizer migration, excessively high solution viscosity, poor dispersibility of inorganic powders, and thermal decomposition residues, making it difficult to meet the application requirements of industrial production and precision electronics.
Composite modified polyvinyl alcohol acetal resin was prepared by introducing α-ester units and ethylene units for composite modification, controlling the degree of acetalization to 22-80 mol%, and using a water-ethanol mixed solvent system for graft copolymerization and acetalization reaction.
It achieves excellent flexibility, low viscosity, high viscosity stability, superior inorganic powder dispersibility and high thermal decomposition without the need for external plasticizers, making it suitable for electronic ceramic casting and precision electronic component bonding, thus improving yield and performance stability.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, and in particular to a composite modified polyvinyl alcohol acetal resin, its preparation method, and its applications. Background Technology
[0002] Polyvinyl acetal resin, due to its excellent film-forming properties, adhesion, and organic solvent solubility, is widely used in industrial fields such as electronic ceramic casting, coatings, adhesives, and thermal imaging photosensitive materials. To address the insufficient flexibility of traditional polyvinyl acetal resin, existing technologies typically employ the addition of external plasticizers. However, external plasticizers are prone to migration during use, leading to performance degradation of resin products after long-term use. Furthermore, traditional polyvinyl acetal resins generally suffer from high solution viscosity and poor viscosity stability, making it difficult to perfectly adapt to the requirements of industrial casting processes for slurry delivery and coating. Moreover, its dispersibility for inorganic powders is insufficient, resulting in defects such as powder agglomeration and interlayer delamination in the prepared ceramic cast films.
[0003] To address the aforementioned issues, existing technologies have proposed various single-modification schemes. For example, Japanese Patent JP2014189681A discloses a modified polyvinyl acetal resin containing α-ester units. This resin achieves internal plasticization by controlling the α-ester unit content to 25-48% and the degree of acetalization to ≥22%, thus eliminating the need for external plasticizers. However, the resin solution viscosity in this technical solution remains relatively high, posing difficulties for slurry delivery and coating operations in industrial production. Another Japanese Patent JP2003183325A discloses a modified polyvinyl acetal resin containing ethylene units, with an ethylene unit content of 1-20%. While this technical solution can significantly reduce the viscosity of the resin solution, the resulting resin lacks flexibility and still requires the addition of plasticizers to meet the peelability requirements of products such as ceramic cast films, thus still posing a risk of plasticizer migration.
[0004] Furthermore, the aforementioned single-modified polyvinyl acetal resins also suffer from the problem of excessive thermal decomposition residues. When applied in the sintering process of electronic ceramics, the residual carbon in the resin can easily lead to defects such as porosity or poor conductivity inside the ceramic components. Simultaneously, these resins have poor moisture resistance; when used as adhesives in high-humidity environments, the bonding strength decreases significantly, thus limiting their application in the field of precision electronics.
[0005] Therefore, there is an urgent need to develop a polyvinyl alcohol acetal resin that can comprehensively solve the problems mentioned above, such as plasticizer migration, excessively high solution viscosity, poor dispersibility of inorganic powders, and thermal decomposition residues. Summary of the Invention
[0006] The purpose of this invention is to address the problems existing in the prior art by providing a composite modified polyvinyl acetal resin, its preparation method, and its application. By simultaneously introducing α-ester units and ethylene units for composite modification, the resulting resin exhibits excellent comprehensive properties.
[0007] To achieve the above objectives, the present invention provides a method for preparing a composite modified polyvinyl acetal resin, comprising the following steps: S1. Polyvinyl alcohol, solvent, α-ester monomer, ethylene comonomer and initiator are mixed and graft copolymerization reaction is carried out to obtain copolymerized modified polyvinyl alcohol solution; the mass ratio of polyvinyl alcohol, α-ester monomer and ethylene comonomer is 100:(30-80):(5-30); S2. A copolymerized modified polyvinyl alcohol solution, an acid catalyst, and an acetalizing agent are mixed and subjected to an acetalization reaction to obtain a composite modified polyvinyl alcohol acetal resin; the degree of acetalization of the composite modified polyvinyl alcohol acetal resin is 22-80 mol.
[0008] In an optional embodiment, in S1, the polyvinyl alcohol has a degree of alcoholysis ≥ 80 mol% and a degree of polymerization of 200-3500; the solvent includes water and ethanol in a volume ratio of 1:(0.5-2); the α-ester monomer includes at least one of vinyl acetate and vinyl propionate; the ethylene comonomer includes ethylene-vinyl acetate copolymer with a degree of polymerization of 500-1500, a degree of alcoholysis of 80-90 mol%, and an ethylene content of 10-30 wt%; the initiator includes at least one of ammonium persulfate and potassium persulfate.
[0009] In an optional embodiment, in S1, the mass ratio of polyvinyl alcohol to initiator is 100:(0.5-3); the mass ratio of polyvinyl alcohol to solvent is 100:(800-1200).
[0010] In an optional embodiment, in S1, the stirring speed of the graft copolymerization reaction is 200-300 r / min, the temperature is 60-80℃, and the time is 2-4 h.
[0011] In an optional embodiment, in S2, the copolymerized modified polyvinyl alcohol solution is first cooled to 20-30°C, then an acid catalyst is added, followed by the addition of an acetalizing agent.
[0012] In an optional embodiment, in S2, the acid catalyst includes at least one of hydrochloric acid solution and sulfuric acid solution; the acetalizing agent includes at least one of n-butyraldehyde and acetaldehyde. When the acetalizing agent includes both n-butyraldehyde and acetaldehyde, their mass ratio is (1-3):1.
[0013] In an optional embodiment, in S2, the mass ratio of the acid catalyst to the polyvinyl alcohol in S1 is (1-5):100; and the mass ratio of the acetalizing agent to the polyvinyl alcohol in S1 is (30-75):100.
[0014] In an optional embodiment, in S2, the stirring speed of the acetalization reaction is 200-300 r / min, the temperature is 20-60℃, and the time is 3-5 h.
[0015] In an optional embodiment, S2, after the acetalization reaction is completed, includes neutralization, precipitation, washing, and drying in sequence. Specifically, an alkaline solution is added to the reaction solution obtained from the acetalization reaction, and the solution is neutralized to pH 7-8 at a stirring speed of 100-200 r / min; then, 2-5 times the volume of deionized water is added, and the mixture is stirred at a stirring speed of 150-200 r / min for 10-20 min to precipitate a solid; the solid is washed 2-3 times with deionized water at 25-30℃ and with a conductivity ≤10 μS / cm; finally, the solid is vacuum dried at 45-55℃ and 45-55 mmHg for 12-16 h to obtain the composite modified polyvinyl alcohol acetal resin.
[0016] In one optional embodiment, the alkaline solution includes at least one of sodium hydroxide solution and potassium hydroxide solution, and the concentration of the alkaline solution is 0.5-2 mol / L.
[0017] The present invention also provides a composite modified polyvinyl acetal resin, which is prepared according to the preparation method described above.
[0018] The present invention also provides the application of the aforementioned composite modified polyvinyl acetal resin in the preparation of electronic ceramic casting slurry or as an adhesive for bonding precision electronic components.
[0019] In an optional embodiment, when used to prepare electronic ceramic casting slurry, the mass ratio of composite modified polyvinyl acetal resin to inorganic ceramic powder is 1:(8-12), and the solid content of the resulting electronic ceramic casting slurry is 55-65 wt%. The inorganic ceramic powder includes at least one of barium titanate, alumina, and zirconium oxide, and has an average particle size of 0.1-0.5 μm.
[0020] In an optional embodiment, when used as an adhesive for bonding precision electronic components, the composite modified polyvinyl acetal resin is compounded with other resins, including at least one of epoxy resin and phenolic resin; the mass ratio of the composite modified polyvinyl acetal resin to the other resins is (3-7):(3-7); the adhesive is cured at 100-140°C for 1-2 hours. The bonding substrate for the precision electronic components includes at least one of copper foil, aluminum foil, ceramic substrate, and epoxy resin substrate.
[0021] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention modifies polyvinyl acetal resin by simultaneously introducing α-ester units and ethylene units. The α-ester unit can reduce intermolecular hydrogen bonding, achieving internal plasticization of the resin. Good flexibility can be obtained without the addition of external plasticizers, fundamentally avoiding performance degradation caused by plasticizer migration. The ethylene unit can reduce the viscosity of the resin solution and improve viscosity stability, making it easy to transport and coat the slurry in industrial casting processes. The synergistic effect of the two makes the resin have the characteristics of internal plasticization, low viscosity, and high viscosity stability.
[0022] (2) The present invention controls the degree of acetalization of the resin to be 22-80 mol%, and the molar ratio of the degree of acetalization to the content of α-ester units is ≥0.32, thereby ensuring the good solubility of the resin in organic solvents, the balance of adhesive strength and flexibility, and avoiding the excessive hydrophilicity and decreased dispersibility of inorganic powder caused by excessively low acetalization, as well as the increased brittleness and poor peelability caused by excessively high acetalization.
[0023] (3) The composite modified polyvinyl alcohol acetal resin of the present invention has a thermal decomposition residual carbon rate of 0% at 700℃. When applied to electronic ceramics sintering, no residual carbon is generated, which avoids defects such as pores or poor conductivity inside the ceramic components and improves the yield and performance stability of the ceramic components.
[0024] (4) The composite modified polyvinyl alcohol acetal resin of the present invention has excellent dispersibility for inorganic ceramic powders such as barium titanate and alumina. The ceramic casting slurry prepared by it has no powder agglomeration, the casting film surface is flat, the interlayer adhesion is good, and there is no peeling phenomenon. It can realize the thinning of ceramic film (thickness ≤3μm) and multi-layer stacking (≥500 layers).
[0025] (5) The preparation method of the present invention uses a water-ethanol mixed solvent system, the reaction conditions are mild, and it is compatible with the existing industrial production process of polyvinyl acetal resin. No new core equipment is required. It can be achieved by simply adjusting the monomer ratio and reaction parameters. It is easy to industrialize, and the raw materials are all commercially available conventional chemical raw materials, so the cost is controllable. Detailed Implementation
[0026] The following embodiments are provided to better understand the present invention and are not intended to limit the implementation methods. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0027] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0028] In the following embodiments and comparative examples of the present invention, "parts" refers to "parts by mass".
[0029] Example 1 This embodiment provides a method for preparing a composite modified polyvinyl acetal resin, including the following steps: 100 parts of polyvinyl alcohol (90 mol% degree of hydrolysis, 800% degree of polymerization) were dissolved in 900 parts of solvent, including water and ethanol in a 1:1 volume ratio, and stirred at 88°C until completely dissolved. 50 parts of an α-ester monomer (vinyl acetate), 10 parts of an ethylene comonomer (ethylene-vinyl acetate copolymer EVA, with a degree of polymerization of 1000, a degree of hydrolysis of 85 mol%, and an ethylene content of 20 wt%), and 1 part of an initiator (ammonium persulfate) were added to the resulting solution. Graft copolymerization was carried out at 250 r / min and 70°C for 3 h to obtain a copolymerized modified polyvinyl alcohol solution.
[0030] The copolymerized polyvinyl alcohol solution was cooled to 25°C, then 3 parts of acid catalyst (1 mol / L hydrochloric acid solution) were added, followed by dropwise addition of 40 parts of acetalizing agent (n-butyraldehyde). The acetalization reaction was carried out for 4 hours at a stirring speed of 250 r / min and a temperature of 40°C. Samples were taken during the reaction to determine the reaction process. 13 C-NMR was used to monitor the degree of acetalization in real time, and the degree of acetalization was controlled at 50 mol.
[0031] After the acetalization reaction was completed, an alkaline solution (1 mol / L sodium hydroxide solution) was added to the reaction solution, and the solution was neutralized to pH 7 while stirring at 150 rpm. Then, three times the volume of deionized water was added, and the mixture was stirred at 180 rpm for 15 min, precipitating a solid. The solid was washed three times with running deionized water (28℃, conductivity ≤10 μS / cm). Finally, it was vacuum dried at 50℃ and 50 mmHg for 12 h to obtain the composite modified polyvinyl alcohol acetal resin, denoted as P1.
[0032] Example 2 This embodiment provides a method for preparing a composite modified polyvinyl acetal resin, including the following steps: 100 parts of polyvinyl alcohol (degree of hydrolysis 98 mol%, degree of polymerization 2000) were dissolved in 1000 parts of solvent, including water and ethanol in a volume ratio of 1:2, and stirred at 90°C until completely dissolved. 60 parts of α-ester monomer (vinyl propionate), 15 parts of ethylene comonomer (ethylene-vinyl acetate copolymer EVA, degree of polymerization 1000, degree of hydrolysis 85 mol%, ethylene content 20 wt%), and 2 parts of initiator (ammonium persulfate) were added to the resulting solution. Graft copolymerization was carried out at 200 r / min and 75°C for 2.5 h to obtain a copolymerized modified polyvinyl alcohol solution.
[0033] The copolymerized modified polyvinyl alcohol solution was cooled to 20°C, then 4 parts of acid catalyst (1 mol / L hydrochloric acid solution) were added, followed by dropwise addition of 50 parts of acetalizing reagent (butyraldehyde and acetaldehyde, with a mass ratio of 3:1). The acetalization reaction was carried out for 5 hours at a stirring speed of 200 r / min and a temperature of 30°C. Samples were taken during the reaction to determine the reaction process. 13 C-NMR was used to monitor the degree of acetalization in real time, and the degree of acetalization was controlled at 60 mol.
[0034] After the acetalization reaction was completed, an alkaline solution (1 mol / L sodium hydroxide solution) was added to the reaction solution, and the solution was neutralized to pH 8 under a stirring speed of 150 r / min. Then, four times the volume of deionized water was added, and the mixture was stirred at 180 r / min for 10 min, precipitating a solid. The solid was washed twice with running deionized water at 28℃ with a conductivity ≤10 μS / cm. Finally, it was vacuum dried at 50℃ and 50 mmHg for 14 h to obtain the composite modified polyvinyl alcohol acetal resin, denoted as P2.
[0035] Example 3 This embodiment provides a method for preparing a composite modified polyvinyl acetal resin, including the following steps: 100 parts of polyvinyl alcohol (90 mol% degree of hydrolysis, 800% degree of polymerization) were dissolved in 800 parts of solvent, including water and ethanol in a volume ratio of 1:0.5, and stirred at 86°C until completely dissolved. 30 parts of α-ester monomers (vinyl acetate and vinyl propionate in a 1:1 mass ratio), 5 parts of ethylene comonomers (ethylene-vinyl acetate copolymer EVA, with a degree of polymerization of 1000, a degree of hydrolysis of 85 mol%, and an ethylene content of 20 wt%), and 0.5 parts of initiator (ammonium persulfate) were added to the resulting solution. Graft copolymerization was carried out at 300 r / min and 65°C for 4 h to obtain a copolymerized modified polyvinyl alcohol solution.
[0036] The copolymerized modified polyvinyl alcohol solution was cooled to 30°C, then 2 parts of acid catalyst (1 mol / L sulfuric acid solution) were added, followed by dropwise addition of 30 parts of acetalizing reagent (butyraldehyde and acetaldehyde, in a mass ratio of 1:1). The acetalization reaction was carried out for 3 hours at a stirring speed of 300 r / min and a temperature of 50°C. Samples were taken during the reaction to determine the reaction process. 13 C-NMR was used to monitor the degree of acetalization in real time, and the degree of acetalization was controlled at 40 mol.
[0037] After the acetalization reaction was completed, an alkaline solution (1 mol / L potassium hydroxide solution) was added to the reaction solution, and the solution was neutralized to pH 7 while stirring at 150 rpm. Then, twice the volume of deionized water was added, and the mixture was stirred at 180 rpm for 20 min, precipitating a solid. The solid was washed three times with running deionized water (28℃, conductivity ≤10 μS / cm). Finally, it was vacuum dried at 50℃ and 50 mmHg for 16 h to obtain the composite modified polyvinyl alcohol acetal resin, denoted as P3.
[0038] Example 4 This embodiment provides a method for preparing a composite modified polyvinyl acetal resin, including the following steps: 100 parts of polyvinyl alcohol (degree of hydrolysis 98 mol%, degree of polymerization 2000) were dissolved in 1100 parts of solvent, including water and ethanol, in a volume ratio of 1:1.5, and stirred at 88°C until completely dissolved. 80 parts of α-ester monomer (vinyl acetate), 30 parts of ethylene comonomer (ethylene-vinyl acetate copolymer EVA, degree of polymerization 1000, degree of hydrolysis 85 mol%, ethylene content 20 wt%), and 3 parts of initiator (ammonium persulfate) were added to the resulting solution. Graft copolymerization was carried out at 250 r / min and 80°C for 2 h to obtain a copolymerized modified polyvinyl alcohol solution.
[0039] The copolymerized modified polyvinyl alcohol solution was cooled to 25°C, then 5 parts of acid catalyst (1 mol / L sulfuric acid solution) were added, followed by dropwise addition of 75 parts of acetalizing reagent (butyraldehyde and acetaldehyde, with a mass ratio of 2:1). The acetalization reaction was carried out for 3.5 hours at a stirring speed of 250 r / min and a temperature of 60°C. During the reaction, samples were taken for analysis. 13 C-NMR was used to monitor the degree of acetalization in real time, and the degree of acetalization was controlled at 70 mol.
[0040] After the acetalization reaction was completed, an alkaline solution (1 mol / L sodium hydroxide solution) was added to the reaction solution, and the solution was neutralized to pH 7.5 at a stirring speed of 150 r / min. Then, five times the volume of deionized water was added, and the mixture was stirred at a stirring speed of 180 r / min for 10 min, precipitating a solid. The solid was washed twice with running deionized water at 28℃ with a conductivity ≤10 μS / cm. Finally, it was vacuum dried at 50℃ and 50 mmHg for 13 h to obtain the composite modified polyvinyl alcohol acetal resin, denoted as P4.
[0041] Comparative Example 1 This comparative example provides a method for preparing a modified polyvinyl acetal resin, differing from Example 1 only in that the addition of ethylene comonomers is omitted. The remaining steps are exactly the same as in Example 1, and the resulting modified polyvinyl acetal resin is denoted as D1.
[0042] Comparative Example 2 This comparative example provides a method for preparing a modified polyvinyl acetal resin, which differs from Example 1 only in that the addition of α-ester monomers is omitted. The remaining steps are exactly the same as in Example 1, and the resulting modified polyvinyl acetal resin is designated as D2.
[0043] Comparative Example 3 This comparative example provides a method for preparing a modified polyvinyl acetal resin, differing from Example 1 only in that the amount of α-ester monomer added is changed to 100 parts. The remaining steps are exactly the same as in Example 1, and the resulting modified polyvinyl acetal resin is designated as D3.
[0044] Comparative Example 4 This comparative example provides a method for preparing a modified polyvinyl acetal resin, which differs from Example 1 only in that the degree of acetalization is controlled at 20 mol%. The remaining steps are exactly the same as in Example 1, and the obtained modified polyvinyl acetal resin is denoted as D4.
[0045] Experimental Example 1: Resin Composition and Basic Properties The resins prepared in the above embodiments and comparative examples were subjected to the following tests. The specific conditions for each test method are as follows.
[0046] (1) Structural unit content and degree of acetalization use 13 The 1 / 2 C-NMR spectrometry was used to determine the content of α-ester units (mol%), ethylene units (mol%), and degree of acetalization (mol%) in the resin. The molar ratio of degree of acetalization to α-ester unit content was also calculated based on the spectra.
[0047] (2) Glass transition temperature (Tg) The measurements were taken using a differential scanning calorimeter (DSC) at a heating rate of 10 °C / min.
[0048] The results of the resin composition and basic property tests are recorded in Table 1.
[0049] Table 1. Test results of resin composition and basic properties
[0050] Experiment Example 2: Performance Testing The resins prepared in the above embodiments and comparative examples were subjected to the following performance tests. The specific conditions for each performance test method are as follows.
[0051] (1) Solution viscosity and viscosity change rate The resin and solvent (ethanol and methyl ethyl ketone, volume ratio 1:1) were mixed to obtain a 10% resin solution. The initial viscosity was measured at 25°C using a rotational viscometer. After the solution was sealed and left at 25°C for one month, the viscosity was measured again. The viscosity change rate was calculated using the following formula: Viscosity change rate (%) = (Viscosity after standing - Initial viscosity) / Initial viscosity × 100%.
[0052] (2) Thermal decomposition The residual carbon rate (%) was determined using a TG / DTA thermogravimetric-differential thermal analyzer at a heating rate of 10℃ / min and a test temperature range of 30-700℃. The residual carbon rate (%) at 700℃ was recorded.
[0053] (3) Mechanical properties The resin was made into a 50 μm thick film, and the tensile strength (MPa) and elongation at break (%) were determined using a universal testing machine at a tensile speed of 10 mm / min.
[0054] (4) Dispersibility of inorganic powders Resin and barium titanate powder (average particle size 0.3 μm) were mixed at a mass ratio of 1:9, and an ethanol-methyl ethyl ketone mixed solvent (volume ratio 1:1) was added to prepare a casting slurry with a solid content of 60 wt%. The particle size distribution of the powder in the slurry was measured using a laser particle size analyzer. A particle size deviation ≤10% was considered as no agglomeration, based on the original particle size. Simultaneously, a 72-hour sedimentation test was conducted; a sedimentation volume ratio ≤5% was considered as stable. If both criteria were met, the dispersibility was deemed satisfactory.
[0055] (5) Plasticizer migration amount A resin-cast ceramic film (3 μm thick) was placed at 25°C and 60% relative humidity for 3 months. The mass of plasticizer migrating to the film surface was determined by gas chromatography. Migration amount (%) = mass of plasticizer migrating to the film surface / total mass of initially added plasticizer × 100%. Samples without added plasticizer were recorded as 0.
[0056] Special note: For Comparative Example 2, due to the insufficient flexibility of its resin, 10 wt% (based on resin mass) of dibutyl phthalate was added to the resin as a plasticizer. The resin with the added plasticizer was then used to prepare a ceramic cast film (3 μm thick), and the test was performed as described above.
[0057] (6) Bond strength and moisture resistance The resin and epoxy resin were compounded at a mass ratio of 5:5, and an appropriate amount of ethanol was added to prepare an adhesive. This adhesive was then applied between the copper foil and the epoxy resin substrate and cured (120℃, 1h). The initial bond strength (MPa) was then measured. The sample was placed at 25℃ and 90% relative humidity for 7 days, and the bond strength after moisture resistance was measured. The strength retention rate was calculated using the following formula: Strength retention rate (%) = Bond strength after moisture resistance / Initial bond strength × 100%.
[0058] (7) Peelability A ceramic cast film (3 μm thick) was laminated with a polyethylene terephthalate (PET) substrate. The 180° peel strength (N / 25 mm) between the film and the substrate was measured at a peel speed of 300 mm / min. Good peelability was defined as no film breakage during peeling and a peel strength of 5-15 N / 25 mm.
[0059] The performance test results are recorded in Table 2.
[0060] Table 2 Performance Test Results
[0061] As can be seen from Table 2, by simultaneously introducing α-ester units and ethylene units, and controlling the mass ratio of polyvinyl alcohol, α-ester monomers and ethylene comonomers to be 100:(30-80):(5-30), the degree of acetalization of the composite modified polyvinyl alcohol acetal resin is 22-80 mol%, which makes the resin have the characteristics of low viscosity, high viscosity stability, good flexibility, no plasticizer migration, high thermal decomposition, excellent inorganic powder dispersibility and good moisture resistance. Its comprehensive performance is significantly better than that of single modified resins and resins with composition ratios that exceed the scope of this invention.
[0062] Experiment Example 3: Application Performance Testing (1) Application of electronic ceramic casting Resin P1 prepared in Example 1 was mixed with barium titanate powder (average particle size 0.3 μm) at a mass ratio of 1:9, and an ethanol-methyl ethyl ketone mixed solvent (volume ratio 1:1) was added to prepare a casting slurry with a solid content of 60 wt%. A ceramic casting film with a thickness of 3 μm was prepared using a casting machine, dried, and stacked into 500 layers. After sintering, a multilayer ceramic capacitor was obtained. This capacitor has no internal pores or residual carbon, exhibits excellent dielectric properties, and has a yield rate of over 98%.
[0063] (2) Application of adhesives The resin P2 prepared in Example 2 was compounded with epoxy resin at a mass ratio of 5:5, and an appropriate amount of ethanol was added to make an adhesive. This adhesive was then applied between the copper foil and the epoxy resin substrate and cured at 120°C for 1 hour to obtain a bonded sample. The initial bond strength of this sample was 23 MPa. After being placed at 25°C and 90% relative humidity for 7 days, the bond strength retention rate was 88%, with no delamination or cracking. This sample can be used for bonding precision electronic components.
[0064] In summary, this invention achieves a combination of excellent flexibility, low viscosity, high viscosity stability, high thermal decomposition resistance, superior inorganic powder dispersibility, and good moisture resistance without the need for external plasticizers by synergistically combining the internal plasticizing effect of the α-ester unit with the low viscosity characteristics of the ethylene unit. The resin's preparation process is mild and compatible with existing industrial production, making it widely applicable in fields such as electronic ceramic casting and high moisture-resistant adhesives, demonstrating promising application prospects.
[0065] Finally, it should be noted that the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A method for preparing a composite modified polyvinyl acetal resin, characterized in that, Includes the following steps: S1. Polyvinyl alcohol, solvent, α-ester monomer, ethylene comonomer and initiator are mixed and graft copolymerization reaction is carried out to obtain copolymerized modified polyvinyl alcohol solution; the mass ratio of polyvinyl alcohol, α-ester monomer and ethylene comonomer is 100:(30-80):(5-30); S2. A copolymerized modified polyvinyl alcohol solution, an acid catalyst, and an acetalizing agent are mixed and subjected to an acetalization reaction to obtain a composite modified polyvinyl alcohol acetal resin; the degree of acetalization of the composite modified polyvinyl alcohol acetal resin is 22-80 mol.
2. The preparation method according to claim 1, characterized in that, In S1, the degree of alcoholysis of the polyvinyl alcohol is ≥80 mol%, and the degree of polymerization is 200-3500; the solvent includes water and ethanol, with a volume ratio of 1:(0.5-2); the α-ester monomer includes at least one of vinyl acetate and vinyl propionate; the ethylene comonomer includes ethylene-vinyl acetate copolymer, with a degree of polymerization of 500-1500, a degree of alcoholysis of 80-90 mol%, and an ethylene content of 10-30 wt%; the initiator includes at least one of ammonium persulfate and potassium persulfate.
3. The preparation method according to claim 1, characterized in that, In S1, the mass ratio of polyvinyl alcohol to initiator is 100:(0.5-3); the mass ratio of polyvinyl alcohol to solvent is 100:(800-1200).
4. The preparation method according to claim 1, characterized in that, In S1, the graft copolymerization reaction is carried out at a temperature of 60-80°C for 2-4 hours.
5. The preparation method according to claim 1, characterized in that, In S2, the acid catalyst includes at least one of hydrochloric acid solution and sulfuric acid solution; the acetalizing agent includes at least one of n-butyraldehyde and acetaldehyde.
6. The preparation method according to claim 1, characterized in that, In S2, the mass ratio of the acid catalyst to the polyvinyl alcohol in S1 is (1-5):100; the mass ratio of the acetalizing agent to the polyvinyl alcohol in S1 is (30-75):
100.
7. The preparation method according to claim 1, characterized in that, In S2, the acetalization reaction is carried out at a temperature of 20-60°C for 3-5 hours.
8. The preparation method according to claim 1, characterized in that, In S2, after the acetalization reaction is completed, the process also includes neutralization, precipitation, washing with water, and drying in sequence.
9. A composite modified polyvinyl acetal resin, characterized in that, Prepared by the preparation method according to any one of claims 1-8.
10. The application of the composite modified polyvinyl acetal resin according to claim 9 in the preparation of electronic ceramic casting slurry or as an adhesive for bonding precision electronic components.
Citation Information
Patent Citations
Modified polyvinyl acetal resin
JP2003183325A
Modified polyvinyl acetal resin
JP2014189681A