Preparation method of low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables
The shrinkage rate and mechanical properties of LSZH polyolefin material were improved by using a three-layer composite interface structure and gradient temperature-controlled vulcanization process. This solved the problems of large shrinkage rate, deterioration of mechanical properties and poor processing performance in the existing technology, and achieved a cable insulation material with high flame retardancy, low shrinkage and high flexibility.
Patent Information
- Application Number
- CN202611162669.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-10
AI Technical Summary
Existing LSZH polyolefin materials suffer from problems such as large shrinkage, deterioration of mechanical properties, and poor processing performance during the crosslinking process. In particular, the high amount of inorganic flame retardant leads to insulation layer shrinkage, reduced material strength, and processing difficulties.
A modified inorganic flame-retardant filler with a three-layer composite interface structure, including a polydopamine adhesive layer, a flexible polyetheramine stress transition layer, and a nano-silica lubricating layer, combined with a hyperbranched stress buffer and a gradient temperature-controlled vulcanization process, improves the interfacial bonding and cross-linking process between the inorganic filler and the polyolefin matrix.
It achieves a balance between low shrinkage, high flame retardancy, and excellent mechanical properties, improves the molding stability and processing performance of cable insulation materials, avoids insulation layer shrinkage and warping defects, and maintains the flexibility and strength of the material.
Smart Images

Figure CN123062822A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable material technology, specifically to a method for preparing low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables. Background Technology
[0002] Halogen-free, low-smoke flame-retardant (LSZH) polyolefin cable materials are widely used in cable insulation and sheathing in densely populated areas such as rail transit and high-rise buildings due to their low smoke emission and absence of toxic hydrogen halide gas release during combustion. Currently, LSZH polyolefin materials mainly achieve their flame-retardant effect by adding large amounts of inorganic flame retardants (such as aluminum hydroxide and magnesium hydroxide). However, high filler content (typically as high as 60%-70%) can lead to the following serious problems: 1. Large shrinkage rate: During the peroxide crosslinking process, due to the large difference in thermal expansion coefficients between the inorganic filler and the polymer matrix, and the volume shrinkage that accompanies the formation of the crosslinking network, the cable insulation layer generates large internal stress after cooling. This is macroscopically manifested as insulation layer shrinkage, and may even lead to the insulation layer peeling off from the conductor and dimensional deviations.
[0003] 2. Deterioration of mechanical properties: The addition of a large amount of rigid inorganic filler disrupts the continuity of the polymer matrix, resulting in a sharp decrease in the tensile strength and elongation at break of the material.
[0004] 3. Poor processing performance: The melt viscosity is high, the extruded surface is rough, and scorching is likely to occur.
[0005] Existing technologies typically alleviate these problems by adding anti-shrinkage agents or improving filler dispersion, but this often results in one aspect being neglected while another is achieved, making it difficult to strike a balance between low shrinkage, high flame retardancy, and excellent mechanical properties. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables, so as to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution: 1. A low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables, characterized in that, by weight, it comprises the following components: 100 parts of polyolefin matrix resin; 120-160 parts of modified inorganic flame-retardant filler; 3-8 parts of hyperbranched stress buffer; 1.5-3.0 parts of cross-linking agent; 1.0-2.5 parts of co-cross-linking agent; 0.5-1.5 parts of antioxidant; and 1.0-3.0 parts of processing aid; The surface of the modified inorganic flame-retardant filler has a composite interface structure consisting of a polydopamine adhesive layer, a flexible polyetheramine stress transition layer, and a nano-silica lubricating layer arranged sequentially from the inside to the outside; the hyperbranched stress buffer is at least one of terminal epoxy hyperbranched polyester or terminal hydroxyl hyperbranched polyamide, with a number average molecular weight of 2000-5000, a branching degree of 60%-85%, and an epoxy / hydroxyl functionality ≥6. The modified inorganic flame-retardant filler is a mixture of magnesium hydroxide and aluminum hydroxide in a mass ratio of 2:1, with D50 = 1.0-2.0 μm and D97 ≤ 3.0 μm, avoiding local stress concentration caused by oversized particles; Preferably, the polyolefin matrix resin is a blend of ethylene-octene copolymer (POE) and ethylene-vinyl acetate copolymer (EVA) in a weight ratio of 30:70; the EVA has a vinyl acetate content of 25-28% and a melt index of 2.0-3.0 g / 10 min (190℃ / 2.16 kg), with a narrow range of control to balance flexibility and water absorption shrinkage defects.
[0008] Preferably, the modified inorganic flame retardant filler is composed of magnesium hydroxide and aluminum hydroxide in a mass ratio of 2:1, with an average particle size of 1.0-2.5μm, a particle size D97≤3μm, complete three-layer coating without peeling, and a total coating thickness of 80-150nm.
[0009] Preferably, the preparation steps of the modified inorganic flame retardant filler are as follows: S1. Inorganic filler is dispersed in pH 8.0-9.0 Tris-HCl buffer solution, and dopamine hydrochloride is added and stirred at room temperature for 8-15 hours; solid-liquid separation, water washing, and vacuum drying are performed to form a polydopamine rigid bonding bottom layer, achieving a strong bond between the inorganic powder and the organic intermediate layer; S2. Polydopamine-coated powder is dispersed in an alcohol-water mixed solvent, and terminal amino polyether (Mn=800-2000) is added and reacted at 50-70℃ for 4-8h; long-chain flexible polyether amine molecules are grafted onto the surface of dopamine as a stress buffer transition layer to buffer the difference in modulus between the filler and the matrix. S3. Polyetheramine grafted powder is dispersed in ethanol, and then hydrolyzed at room temperature with tetraethyl orthosilicate and ammonia for 2-5 hours; a nano-SiO2 lubricating thin layer is formed on the surface, which reduces melt friction resistance and improves processing fluidity; Each step involves thorough rinsing to prevent acid and alkali residues from dissolving the underlying coating structure; a neutral water rinsing buffer step is added between steps to isolate the alternating acid and alkali environments from damaging the preceding coating layer.
[0010] Limited ratio: Inorganic filler: Buffer solution: Dopamine hydrochloride = 100:200:1.5; Dopamine powder: Alcohol-water solvent: Polyether = 10:120:2; Polyether powder: Ethanol: Tetraethyl orthosilicate: Ammonia = 10:80:2.5:0.5.
[0011] Preferably, after each reaction step (S1, S2, S3) is completed, the powder system is neutralized and washed multiple times with deionized water until the pH of the powder system is stabilized at 6.5-7.5 before proceeding to the next coating step, thus avoiding the alternating erosion of the three-layer composite structure by strong acids and strong alkalis.
[0012] Preferably, the hyperbranched stress buffer has a number-average molecular weight of 2000-5000, a branching degree of 60%-85%, and a terminal epoxy / hydroxyl functionality ≥6; the crosslinking agent is dicumyl peroxide or di-tert-butyl peroxide; the co-crosslinking agent is at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, and 1,4-butanediol dimethacrylate; and the antioxidant is a hindered phenol + sulfide compound system to inhibit high-temperature vulcanization and long-term thermo-oxidative aging.
[0013] A method for preparing a low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables includes the following steps: Step 1, Preparation of modified inorganic flame retardant filler: Prepare a three-layer coated filler according to the method of claims 4 and 5, and wash with neutralizing water in each step to protect the integrity of the coating layer; Step 2, basic masterbatch mixing: polyolefin matrix, three-layer modified filler, hyperbranched buffer, antioxidant, and processing aids are premixed in a high-speed mixer; then transferred to a closed internal mixer and mixed at 110-130℃ for 8-12 minutes; twin-screw extrusion granulation is performed at a die head temperature of 100-120℃ and a screw speed of 200-400 r / min; the entire process is sealed and dust-proof, and no peroxide crosslinking agents are added during the high-temperature stage to prevent scorching; Step 3, low-temperature compounding of the crosslinking system: The base masterbatch is naturally cooled to below 40°C, then transferred to a light-proof, sealed low-temperature mixing equipment and mixed at 60-80°C for 3-5 minutes. After adding the crosslinking agent and co-crosslinking agent, it is quickly compressed into tablets and granules. The entire process is carried out in the dark and with temperature control to prevent the peroxide from decomposing and becoming ineffective prematurely. Step four: Extrusion molding and multi-gradient temperature vulcanization, three-stage progressive cooling: The finished material is extruded onto a copper conductor by a single screw extruder and fed into a high-pressure steam vulcanization pipe at a steam pressure of 0.8-1.2 MPa. Three-stage stepped temperature vulcanization: Preheating section: 150-160℃, hold for 1-2 minutes to slowly soften the melt and release extrusion shear stress; The primary vulcanization is carried out at 180-190℃ for 2-3 minutes to allow the peroxides to fully decompose and build a cross-linked network. The homogenization stage is set at 170-175℃ for 1-2 minutes to balance the internal and external crosslinking densities and eliminate local crosslinking inhomogeneity. Gradient three-stage cooling: Pre-cool with 60-70℃ warm water for 1-2 minutes; transition with 35-45℃ medium-temperature water for 1 minute; set with 20-25℃ cold water to room temperature; gradually release the dual internal stress of cross-linking chemical shrinkage and thermal shrinkage through multiple slow cooling stages to avoid delamination and warping defects caused by sudden temperature changes.
[0014] Preferably, in step two, the mixing temperature is 110-130℃ and the mixing time is 8-12 minutes; the twin-screw extruder head is 100-120℃ and the speed is 200-400 r / min; the mixing chamber is protected by nitrogen micro-positive pressure to inhibit the thermal and oxidative degradation of the high-temperature matrix.
[0015] Preferably, in step three, the low-temperature mixing equipment is sealed and protected from light, the temperature is 60-80℃, the mixing time is 3-5 minutes, and after discharge, the material is sealed and stored at low temperature to prevent premature decomposition of the crosslinking agent.
[0016] Preferably, the stepped vulcanization is equipped with 0.8-1.2MPa saturated steam; the gradient cooling is set with three temperature-controlled water tanks to gradually reduce the temperature difference and release residual stress.
[0017] Compared with the prior art, the beneficial effects of the present invention are: 1. The three-layer gradient coating filler of this invention reduces shrinkage defects at the interface source: the inner polydopamine layer is a high-adhesion bonding layer that firmly bonds the inorganic powder; the middle long-chain polyetheramine flexible layer serves as a stress buffer transition zone, compensating for the huge difference in modulus and thermal expansion coefficient between the inorganic filler and the polyolefin matrix, and dissipating the chemical shrinkage stress generated by the crosslinking reaction; the outer nano-SiO2 thin layer reduces filler friction and improves melt fluidity; the process adds a neutralization water washing buffer to avoid alternating acid and alkali damage to the complete three-layer coating structure, solving the problems of interface debonding and stress concentration of traditional single-layer fillers.
[0018] 2. The hyperbranched three-dimensional dendritic structure of this invention is interspersed in the gaps between polyolefin molecular chains, which mainly alleviates thermal shrinkage during the melt cooling stage; together with the middle layer of polyetheramine flexible layer, it dissipates cross-linking internal stress; it can significantly reduce volume shrinkage during the molding and cooling stage, and the two work together to achieve an overall low shrinkage effect; at the same time, the terminal epoxy groups can form hydrogen bonds with the hydroxyl groups on the filler surface, further strengthening the interfacial bonding and inhibiting long-term thermal cycling shrinkage cracking.
[0019] 3. This invention eliminates processing defects through segmented low-temperature mixing and gradient temperature-controlled vulcanization cooling: First, the filler is uniformly dispersed at high temperature, and then the masterbatch is fully cooled before the peroxide is mixed in at low temperature, completely avoiding the decomposition and scorching of the high-temperature crosslinking agent; the vulcanization adopts a three-stage step heating to avoid uneven local crosslinking density; the innovative three-stage progressive gradient cooling significantly reduces the single temperature difference compared to the traditional two-stage cooling, releases multi-layer residual internal stress in stages, and significantly improves the dimensional stability of the finished insulation, eliminating insulation peeling, warping, and dimensional deviation problems.
[0020] 4. The present invention simultaneously improves processing performance and mechanical properties: the nano-silica lubricating layer on the surface of the filler reduces the viscosity of the high-filler melt and makes the extruded surface smooth; the three-layer composite structure greatly improves the dispersibility of the filler, and with the POE / EVA compound matrix and hyperbranched compressive buffer system, it still maintains excellent tensile strength and elongation at break under the condition of a maximum filler filling amount of 160 parts and high flame retardancy, taking into account the triple properties of high flame retardancy, low shrinkage and high flexibility. Attached Figure Description
[0021] Figure 1 This is a flowchart illustrating the steps of preparing the low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables according to the present invention. Detailed Implementation
[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Please see Figure 1 The present invention provides the following technical solution: Example 1
[0024] A low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables, formulated in parts by weight: 100 parts of polyolefin matrix resin, 140 parts of three-layer composite interface modified inorganic flame retardant filler, 5 parts of terminal epoxy hyperbranched polyester, 2.2 parts of dicumyl peroxide crosslinking agent, 1.8 parts of triallyl isocyanurate co-crosslinking agent, 1.0 part of hindered phenol + thioether compound antioxidant, and 2.0 parts of polyethylene low molecular weight wax + oleamide + methylphenyl organosilicon compound processing aid.
[0025] The matrix is composed of ethylene-octene copolymer elastomer and ethylene-vinyl acetate copolymer in a weight ratio of 30:70; the ethylene-vinyl acetate copolymer has a vinyl acetate monomer content of 28% and a melt index of 2.2 g / 10 min; the inorganic flame retardant filler is composed of magnesium hydroxide powder and aluminum hydroxide powder in a weight ratio of 2:1, with a median particle size of 1.8 micrometers and an upper limit of 2.6 micrometers for large particles; the hyperbranched polyester has a number average molecular weight of 3500, a branching degree of 75%, and an epoxy functionality of 8; after each coating reaction of the three-layer coated filler, it is neutralized and washed with deionized water until the system is neutral, and the total coating thickness of the filler is 120 nanometers.
[0026] Complete preparation process of three-layer composite interface modified inorganic flame retardant fillers: S1 mixes magnesium hydroxide powder, aluminum hydroxide powder mixed filler, tris(hydroxymethyl)aminomethane-hydrochloric acid buffer, and dopamine hydrochloride in a mass ratio of 100:200:1.5. The pH of the buffer is controlled at 8.5. The mixture is stirred at room temperature for 12 hours. After the reaction is completed, the mixture is washed with water and vacuum dried to form a polydopamine adhesive underlayer on the powder surface. S2 mixes polydopamine-coated powder, ethanol-deionized mixed solvent, and amino-terminated polyether with a number average molecular weight of 1200 in a ratio of 10:120:2, reacts at a constant temperature of 60 degrees Celsius for 6 hours, and then neutralizes and washes with water after the reaction. S3 mixes polyether grafted modified powder, anhydrous ethanol, tetraethyl orthosilicate, and ammonia catalyst in a ratio of 10:80:2.5:0.5, hydrolyzes at room temperature for 3 hours, washes thoroughly with water until neutral, and then vacuum dries to obtain a complete three-layer composite coated flame retardant powder.
[0027] Complete finished product preparation steps: Step 1: Prepare a three-layer composite interface modified inorganic flame retardant filler that meets the standards after neutralization and water washing according to the above procedures; Step 2: Add ethylene-octene copolymer elastomer, ethylene-vinyl acetate copolymer matrix, three-layer modified flame retardant filler, terminal epoxy hyperbranched polyester, hindered phenol sulfide composite antioxidant, and compounded processing aids to a high-speed mixer for premixing until uniform; transfer to a nitrogen micro-positive pressure closed mixing equipment and mix at 120 degrees Celsius for 10 minutes; feed the discharged material into a twin-screw extruder, with a die head temperature of 110 degrees Celsius and a screw speed of 300 rpm for extrusion granulation to obtain basic insulation masterbatch; Step 3: The basic insulating masterbatch is naturally cooled to 38 degrees Celsius and then transferred to a light-proof, sealed low-temperature mixing equipment. It is mixed at 70 degrees Celsius for 4 minutes, while simultaneously adding dicumyl peroxide crosslinking agent and triallyl isocyanurate co-crosslinking agent. After the low-temperature mixing is completed, it is quickly pressed into tablets and granulated. The finished particles are sealed and stored in the dark. Step 4: The insulating masterbatch is fed into a single-screw extruder and evenly extruded onto the surface of the oxygen-free copper conductor. The cable is then fed into a saturated steam vulcanization pipeline with an internal saturated steam pressure of 1.0 MPa. The three-stage stepped temperature vulcanization process is as follows: 155°C preheating for 1.5 minutes → 185°C main vulcanization for 2.5 minutes → 172°C homogenization for 1.5 minutes. After vulcanization, the cable enters a three-stage gradient cooling water tank: 65°C warm water precooling for 1.5 minutes → 40°C medium-temperature water transition cooling for 1 minute → 23°C room temperature cold water setting to room temperature.
[0028] The performance of the finished product in this embodiment is as follows: molding heat shrinkage rate ≤0.8%, oxygen index ≥33, elongation at break ≥200%, the surface of the extruded product is smooth without pitting, and there are no delamination or peeling defects after long-term thermal cycling at 85 degrees Celsius for 1000 hours. Example 2
[0029] Lightweight thin-walled insulation special formula, proportioned by weight: 100 parts of polyolefin matrix resin, 120 parts of three-layer composite interface modified inorganic flame retardant filler, 3 parts of hydroxyl-terminated hyperbranched polyamide, 1.5 parts of di-tert-butyl peroxide crosslinking agent, 1.0 part of trimethylolpropane trimethacrylate co-crosslinking agent, 0.5 parts of hindered phenol + thioether compound antioxidant, and 1.0 part of polyethylene low molecular weight wax + oleamide + methylphenyl organosilicon compound processing aid.
[0030] The number-average molecular weight of the hydroxyl-terminated hyperbranched polyamide is 2800, the branching degree is 65%, and the hydroxyl functionality is 7. The complete set of parameters and preparation process of the three-layer coating modification of the filler are completely consistent with those of Example 1.
[0031] Suitable for thin-walled, high-toughness, low-shrinkage cable insulation applications, the finished product has a heat shrinkage rate of ≤0.9%, and no cracking is observed during low-temperature bending tests.
[0032] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0033] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables, characterized in that, By weight, it comprises the following components: 100 parts polyolefin matrix resin; 120-160 parts modified inorganic flame retardant filler; 3-8 parts hyperbranched stress buffer; 1.5-3.0 parts crosslinking agent; 1.0-2.5 parts co-crosslinking agent; 0.5-1.5 parts antioxidant; and 1.0-3.0 parts processing aid. The surface of the modified inorganic flame-retardant filler has a composite interface structure consisting of a polydopamine adhesive layer, a flexible polyetheramine stress transition layer, and a nano-silica lubricating layer arranged sequentially from the inside to the outside; the hyperbranched stress buffer is at least one of terminal epoxy hyperbranched polyester or terminal hydroxyl hyperbranched polyamide, with a number average molecular weight of 2000-5000, a branching degree of 60%-85%, and an epoxy / hydroxyl functionality ≥6. The modified inorganic flame-retardant filler is a compound of magnesium hydroxide and aluminum hydroxide in a mass ratio of 2:1, with D50 = 1.0-2.0 μm and D97 ≤ 3.0 μm, avoiding local stress concentration caused by oversized particles.
2. The low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables according to claim 1, characterized in that, The polyolefin matrix resin is a blend of ethylene-octene copolymer and ethylene-vinyl acetate copolymer in a weight ratio of 30:70; the EVA has a vinyl acetate content of 25-28%.
3. The low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables according to claim 1, characterized in that, The modified inorganic flame retardant filler is composed of magnesium hydroxide and aluminum hydroxide in a mass ratio of 2:1, with an average particle size of 1.0-2.5μm, a particle size D97≤3μm, and complete three-layer coating without peeling, with a total coating thickness of 80-150nm.
4. The low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables according to claim 1, characterized in that, The preparation steps of the modified inorganic flame retardant filler are as follows: S1. Inorganic filler is dispersed in Tris-HCl buffer solution with pH 8.0-9.0, and dopamine hydrochloride is added and stirred at room temperature for 8-15 hours; solid-liquid separation, water washing, and vacuum drying are performed to form a polydopamine rigid bonding bottom layer, achieving a strong bond between the inorganic powder and the organic intermediate layer; S2. Polydopamine-coated powder is dispersed in an alcohol-water mixed solvent, and terminal amino polyether is added and reacted at 50-70℃ for 4-8 hours; long-chain flexible polyether amine molecules are grafted onto the dopamine surface as a stress buffer transition layer to buffer the difference in modulus between the filler and the matrix. S3. Polyetheramine grafted powder is dispersed in ethanol, and then hydrolyzed at room temperature with tetraethyl orthosilicate and ammonia for 2-5 hours; a nano-SiO2 lubricating thin layer is formed on the surface, which reduces melt friction resistance and improves processing fluidity; Each step involves thorough rinsing to prevent acid and alkali residues from dissolving the underlying coating structure; a neutral water rinsing buffer step is added between steps to isolate the alternating acid and alkali environments from damaging the preceding coating layer. The preparation ratios for each step are as follows: Inorganic filler: buffer solution: dopamine hydrochloride = 100:200:1.5; Dopamine powder: alcohol-water solvent: polyether = 10:120:2; Polyether powder: ethanol: tetraethyl orthosilicate: ammonia = 10:80:2.5:0.
5.
5. The low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables according to claim 4, characterized in that, After each reaction step (S1, S2, S3) is completed, the powder system is neutralized and washed multiple times with deionized water until the pH of the powder system is stabilized at 6.5-7.5 before proceeding to the next coating step, thus avoiding the alternating erosion of the three-layer composite structure by strong acids and alkalis.
6. The low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables according to claim 1, characterized in that, The hyperbranched stress buffer has a number-average molecular weight of 2000-5000, a branching degree of 60%-85%, and a terminal epoxy / hydroxyl functionality of ≥6; the crosslinking agent is dicumyl peroxide or di-tert-butyl peroxide; the co-crosslinking agent is at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, and 1,4-butanediol dimethacrylate; the antioxidant is a hindered phenol + sulfide compound system to inhibit high-temperature vulcanization and long-term thermo-oxidative aging.
7. A method for preparing a low-shrinkage, halogen-free, low-smoke, flame-retardant cross-linked polyolefin insulation material for cables as described in any one of claims 1-6, characterized in that it comprises four steps: Step 1, Preparation of modified inorganic flame retardant filler: Prepare a three-layer coated filler according to the method of claims 4 and 5, and wash with neutralizing water in each step to protect the integrity of the coating layer; Step 2, basic masterbatch mixing: polyolefin matrix, three-layer modified filler, hyperbranched buffer, antioxidant, and processing aids are premixed in a high-speed mixer; then transferred to a closed internal mixer and mixed at 110-130℃ for 8-12 minutes; twin-screw extrusion granulation is performed at a die head temperature of 100-120℃ and a screw speed of 200-400 r / min; the entire process is sealed and dust-proof, and no peroxide crosslinking agents are added during the high-temperature stage to prevent scorching; Step 3, low-temperature compounding of the crosslinking system: The base masterbatch is naturally cooled to below 40°C, then transferred to a light-proof, sealed low-temperature mixing equipment and mixed at 60-80°C for 3-5 minutes. After adding the crosslinking agent and co-crosslinking agent, it is quickly compressed into tablets and granules. The entire process is carried out in the dark and with temperature control to prevent the peroxide from decomposing and becoming ineffective prematurely. Step four: Extrusion molding and multi-gradient temperature vulcanization, three-stage progressive cooling: The finished material is extruded onto a copper conductor by a single screw extruder and fed into a high-pressure steam vulcanization pipe at a steam pressure of 0.8-1.2 MPa. Three-stage stepped temperature vulcanization: Preheating section: 150-160℃, hold for 1-2 minutes to slowly soften the melt and release extrusion shear stress; The primary vulcanization is carried out at 180-190℃ for 2-3 minutes to allow the peroxides to fully decompose and build a cross-linked network. The homogenization stage is set at 170-175℃ for 1-2 minutes to balance the internal and external crosslinking densities and eliminate local crosslinking inhomogeneity. Gradient three-stage cooling: Pre-cool with 60-70℃ warm water for 1-2 minutes; transition with 35-45℃ medium-temperature water for 1 minute; set with 20-25℃ cold water to room temperature; gradually release the dual internal stress of cross-linking chemical shrinkage and thermal shrinkage through multiple slow cooling stages to avoid delamination and warping defects caused by sudden temperature changes.
8. According to the preparation method of claim 7, in step two, the mixing temperature is 110-130℃ and the mixing time is 8-12min; the twin-screw extruder head is 100-120℃ and the rotation speed is 200-400r / min; the mixing chamber is protected by nitrogen micro-positive pressure to inhibit the thermal and oxidative degradation of the high-temperature matrix.
9. According to the preparation method described in claim 7, in step three, the low-temperature mixing equipment is sealed and protected from light, the temperature is 60-80℃, the mixing time is 3-5 minutes, and after discharge, the material is sealed and protected from light and stored at low temperature to avoid premature decomposition of the crosslinking agent.
10. According to the preparation method of claim 7, the step vulcanization is accompanied by 0.8-1.2MPa saturated steam; the gradient cooling is set with a three-stage temperature-controlled water tank to gradually reduce the temperature difference and release residual stress.