High toughness mpp cable protection pipe and preparation method thereof
By combining composite toughening agents and modified nano-calcium carbonate, the raw material ratio and preparation process of MPP cable protection pipe are optimized, solving the problem of insufficient toughness of MPP cable protection pipe and achieving stable impact resistance and mechanical properties in low-temperature environments, making it suitable for cable protection in the power and communication fields.
Patent Information
- Application Number
- CN202611134858.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-10
AI Technical Summary
Existing MPP cable protection pipes lack toughness, are prone to brittle fracture at low temperatures, have poor impact resistance, and are not precise enough in manufacturing processes, resulting in easy damage to the pipe wall during construction and long-term use, which affects the safe operation of cables.
A composite toughening agent composed of POE, EVA, and modified nano-calcium carbonate, combined with modified talc and compatibilizer, is used to optimize the raw material ratio and modification process to prepare a high-toughness MPP cable protection pipe with a double-layer structure. The pipe is then formed by a twin-screw extruder and a vacuum forming machine, and antioxidants and UV stabilizers are used to extend its service life.
It significantly improves the toughness and impact resistance of MPP cable protection pipes, ensuring they do not crack in low-temperature environments, and enhances the stability of mechanical properties and aging resistance, making them suitable for use in complex underground working conditions.
Smart Images

Figure CN123062830A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable protection pipe manufacturing technology, specifically to a high-toughness MPP cable protection pipe and its manufacturing method. Background Technology
[0002] MPP cable protection pipes are widely used in power and telecommunications fields due to their advantages such as corrosion resistance, light weight, convenient construction, and good insulation performance, to protect underground cables from external damage and environmental erosion. However, existing MPP cable protection pipes generally suffer from insufficient toughness, are prone to brittleness in low-temperature environments, and have poor impact resistance. During underground construction or long-term use, the pipe wall is easily damaged by soil pressure, external impacts, etc., which in turn affects the safe operation of the cable.
[0003] Therefore, developing a high-toughness MPP cable protection pipe and its preparation method that can significantly improve toughness and mechanical properties by rationally combining composite toughening agents, optimizing raw material modification processes, and clarifying the proportions of each component, while having a simple preparation process that is in line with actual production, has become an urgent technical problem to be solved in this field. Summary of the Invention
[0004] To address the shortcomings of existing MPP cable protection pipes, such as insufficient toughness, brittleness at low temperatures, unstable mechanical properties, and imprecise manufacturing processes, this invention provides a high-toughness MPP cable protection pipe and its manufacturing method, overcoming the deficiencies of existing technologies and improving the toughness, impact resistance, and aging resistance of MPP cable protection pipes.
[0005] To achieve the above objectives, the present invention provides the following technical solution: The technical solution provided by this invention is: A high-toughness MPP cable protection pipe is prepared from the following raw materials in parts by weight: 70-85 parts MPP resin, 8-18 parts composite toughening agent, 3-8 parts modified talc powder, 1-3 parts compatibilizer, 0.3-1.2 parts antioxidant, 0.5-2 parts lubricant, and 0.2-0.8 parts UV stabilizer; the composite toughening agent is composed of 4-8 parts ethylene-octene copolymer (POE), 2-5 parts ethylene-vinyl acetate copolymer (EVA), and 2-5 parts nano-calcium carbonate, wherein the nano-calcium carbonate is modified by a silane coupling agent, and the modified talc powder has a particle size of 1.5-2.5 μm and is modified by diphenylmethane diisocyanate.
[0006] Furthermore, the MPP resin is polypropylene resin (PP).
[0007] Furthermore, the compatibilizer is maleic anhydride-grafted polypropylene (PP-g-MAH) with a grafting rate of 0.8-1.5%.
[0008] Furthermore, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 2:1; the lubricant is a mixture of oleic acid amide and microcrystalline wax in a weight ratio of 1:1; and the UV protectant is one of UV-531 or UV-327, or a mixture of the two in a weight ratio of 1:1 to 2:1.
[0009] Furthermore, the particle size of the nano-calcium carbonate is 50-100 nm, and the amount of silane coupling agent is 1.5-3% of the weight of the nano-calcium carbonate. The method of modifying the nano-calcium carbonate with silane coupling agent is as follows: by weight, 100 parts of nano-calcium carbonate, 1.5-3 parts of silane coupling agent (KH-550), and 50-60 parts of anhydrous ethanol are added to a mixer and stirred at 60-70°C and 400-500 r / min for 60-90 min. Then, it is transferred to an oven and dried at 105-110°C for 2-3 hours. After pulverizing, it is passed through a 300-mesh sieve to obtain modified nano-calcium carbonate.
[0010] Furthermore, the modified talc powder is prepared by adding talc powder, ethanol and diphenylmethane diisocyanate into a reactor at a weight ratio of 100:50:22-25, stirring at 95-100℃ for 1.5 hours, distilling under reduced pressure of -0.07MPa for 45 minutes, drying in an oven at 110℃ for 4 hours, and then pulverizing and passing through a 200-mesh sieve.
[0011] Further, the preparation method of the composite toughening agent is as follows: by weight, 4-8 parts of ethylene-octene copolymer (POE), 2-5 parts of ethylene-vinyl acetate copolymer (EVA), and 2-5 parts of the above modified nano-calcium carbonate are added to a high-speed mixer and stirred at 80-90°C and 500-600 r / min for 40-60 min. After stirring, the mixture is naturally cooled to room temperature to obtain the composite toughening agent.
[0012] Furthermore, the cable protection pipe has a double-layer structure, with an inner layer being a smooth and wear-resistant layer and an outer layer being an impact-resistant reinforcing layer. The thickness ratio of the inner layer to the outer layer is 1:1.2-1.5, and the amount of composite toughening agent in the outer layer material is 2-3 more parts by weight than that in the inner layer.
[0013] A method for preparing a high-toughness MPP cable protection pipe includes the following steps: S1. Raw material pretreatment: Mix nano-calcium carbonate with silane coupling agent and stir at 80-90℃ for 30-40 min to obtain modified nano-calcium carbonate; mix modified talc powder, antioxidant, lubricant and UV stabilizer, put them into a high-speed mixer, stir at 100-110℃ and 600-800 r / min for 20-30 min, and cool to room temperature to obtain mixed excipients; S2. Mixing and granulation: Add MPP resin, composite toughening agent, and compatibilizer to a high-speed mixer and stir at 50-60℃ and 300-400 r / min for 15-20 min. Then add the mixed excipients prepared in step S1, heat to 85-95℃, and continue stirring at 500-600 r / min for 25-35 min to obtain a preliminary mixture. Feed the preliminary mixture into a twin-screw extruder for extrusion granulation. The temperatures of the six temperature zones of the twin-screw extruder from the feed end to the discharge end are 160-170℃, 175-185℃, 185-195℃, 190-200℃, 185-195℃, and 175-185℃, respectively, with a screw speed of 180-220 r / min, to obtain granules. S3. Extrusion molding: The granular material is fed into the pipe extruder. The barrel temperature of the pipe extruder is 165-175℃ in zone 1, 180-190℃ in zone 2, 190-200℃ in zone 3, and 185-195℃ in zone 4. The die head temperature is 170-180℃. The extrusion molding speed is 1.4-1.8m / min. After extrusion, the material is shaped by a vacuum sizing machine at a sizing temperature of 18-25℃. It is then cooled to room temperature by spraying water for 15-20 minutes. Finally, it is cut to a fixed length to obtain a high-toughness MPP cable protection pipe. S4. Post-processing: The cut cable protection pipe ends are flared at an angle of 10-12°, and a EPDM rubber sealing ring is installed. The interface is then treated with electrofusion welding at a temperature of 200-220℃ for 3-5 minutes to obtain the finished product.
[0014] Furthermore, in step S2, the twin-screw extruder has a length-to-diameter ratio of 36:1 and an extrusion pressure of 15-20 MPa; in step S3, the vacuum setting machine has a vacuum degree of 0.06-0.08 MPa, and the traction speed is synchronized with the extrusion speed.
[0015] Furthermore, in step S3, when preparing the double-layer cable protection pipe, a double-barrel extruder is used. The inner layer raw material and the outer layer raw material are fed into two barrels respectively and extruded and formed simultaneously. The temperature of each temperature zone of the inner layer barrel is 5-10℃ lower than the corresponding temperature zone of the outer layer barrel.
[0016] The beneficial effects of this technical solution are: (1) The composite toughening agent is composed of POE, EVA and modified nano calcium carbonate. Compared with the single toughening agent in the prior art, the three form a complementary and synergistic effect, which can effectively improve the compatibility between the toughening component and MPP resin, avoid problems such as component delamination and pipe cracking, and give full play to the toughening potential of each component. At the same time, the modified nano calcium carbonate can make up for the loss of pipe rigidity during the toughening process, achieve a balanced match between toughness and rigidity, and solve the technical pain point that toughening and rigidity are difficult to balance in the prior art.
[0017] (2) After being modified by silane coupling agent, the surface properties of nano-calcium carbonate are optimized, and its compatibility with MPP resin, POE and EVA is greatly improved. It can be uniformly dispersed in the resin system and give full play to its reinforcing and toughening effect. After being modified by a specific process, the binding force of modified talc powder with organic components is significantly enhanced, which further optimizes the stability of the mechanical properties of the pipe, avoids the performance fluctuation caused by uneven dispersion of inorganic fillers, and ensures that the synergistic effect of each component can be fully exerted.
[0018] (3) Maleic anhydride-grafted polypropylene is selected as the compatibilizer, which can effectively promote the interfacial bonding between the components and improve the uniformity of the system. The specific combination of antioxidants, lubricants and UV stabilizers can not only delay the aging of the pipe and extend its service life, but also optimize the processing performance and ensure that the components remain stable during the processing. All raw materials are common chemical raw materials, which are easy to obtain and have reasonable costs. The scientific combination of components not only ensures the performance of the pipe, but is also suitable for large-scale industrial production. Attached Figure Description
[0019] Figure 1 This is a schematic diagram of the preparation process of a high-toughness MPP cable protection pipe and its preparation method proposed in this invention. Detailed Implementation
[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] The specific implementation process is as follows: Example 1:
[0022] Please see Figure 1 The present invention provides a technical solution: a high-toughness MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 70 parts of MPP resin (polypropylene resin, PP), 8 parts of composite toughening agent, 3 parts of modified talc powder (particle size 1.5-2.5μm), 1 part of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.3 parts of antioxidant, 0.5 parts of lubricant, and 0.2 parts of UV stabilizer; The composite toughening agent consists of 4 parts POE (model 8402), 2 parts EVA (VA content 18%), and 2 parts modified nano-calcium carbonate (particle size 50-100nm); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 2:1 (0.2 parts of antioxidant 1010 and 0.1 parts of antioxidant 168); the lubricant is a mixture of oleamide and microcrystalline wax in a weight ratio of 1:1 (0.25 parts of oleamide and 0.25 parts of microcrystalline wax); and the UV stabilizer is UV-531. Nano-calcium carbonate was modified with silane coupling agent (KH-550). The specific method is as follows: by weight, 100 parts of nano-calcium carbonate (particle size 50-100nm), 1.5 parts of silane coupling agent (KH-550) and 50 parts of anhydrous ethanol were added to a mixer and stirred at 60°C and 400r / min for 60min. Then, it was transferred to an oven and dried at 105°C for 2 hours. After pulverizing, it was passed through a 300-mesh sieve to obtain modified nano-calcium carbonate. The modified talc powder is prepared by adding talc powder (particle size 1.5-2.5μm), ethanol and diphenylmethane diisocyanate to a reactor at a weight ratio of 100:50:22, stirring at 95℃ for 1.5 hours, distilling under reduced pressure of -0.07MPa for 45 minutes, drying in an oven at 110℃ for 4 hours, and then pulverizing and passing through a 200-mesh sieve. The preparation method of the composite toughening agent is as follows: by weight, 4 parts of POE (model 8402), 2 parts of EVA (VA content 18%), and 2 parts of the above modified nano calcium carbonate (particle size 50-100nm) are added to a high-speed mixer and stirred at 80℃ and 500r / min for 40min. After stirring, the mixture is naturally cooled to room temperature to obtain the composite toughening agent. The cable protection pipe has a single-layer structure; The preparation method of this high-toughness MPP cable protection pipe includes the following steps: S1. Raw material pretreatment: Nano-calcium carbonate and silane coupling agent are mixed and treated according to the above modification method to obtain modified nano-calcium carbonate; modified talc powder, antioxidant, lubricant and anti-ultraviolet agent are mixed and placed in a high-speed mixer, stirred at 100℃ and 600r / min for 20min, and cooled to room temperature to obtain mixed excipients; S2. Mixing and granulation: MPP resin, composite toughening agent, and compatibilizer are added to a high-speed mixer and stirred at 50°C and 300 r / min for 15 min. Then, the mixed additives prepared in step S1 are added, and the mixture is heated to 85°C and stirred at 500 r / min for another 25 min to obtain a preliminary mixture. The preliminary mixture is fed into a twin-screw extruder for extrusion granulation. The twin-screw extruder has a length-to-diameter ratio of 36:1 and an extrusion pressure of 15 MPa. The temperatures of the six temperature zones from the feed end to the discharge end are 160°C, 175°C, 185°C, 190°C, 185°C, and 175°C, respectively, with a screw speed of 180 r / min to obtain granules. S3. Extrusion molding: The granular material is fed into the pipe extruder. The barrel temperature of the pipe extruder is 165℃ in zone 1, 180℃ in zone 2, 190℃ in zone 3, and 185℃ in zone 4. The die head temperature is 170℃. The extrusion molding speed is 1.4m / min. After extrusion, it is shaped by a vacuum sizing machine with a vacuum degree of 0.06MPa and a sizing temperature of 18℃. It is then cooled to room temperature by spraying water for 15 minutes. Finally, it is cut to a fixed length to obtain a high-toughness MPP cable protection pipe. S4. Post-processing: The cut cable protection pipe ends are flared at an angle of 10°, and a EPDM rubber sealing ring is installed. The joint is then treated with electrofusion welding at a temperature of 200°C for 3 minutes to obtain the finished product.
[0023]
[0024] As shown in the data table above, the high-toughness MPP cable protection pipe prepared in Example 1, using the lowest possible raw material ratio, meets all basic performance standards. The simply supported beam impact strength is 15.8 kJ / m. 2 The elongation at break is 420%, indicating that the pipe has good toughness and fracture resistance, and can withstand certain external impacts; the low-temperature impact performance shows no cracks or damage at -5℃, solving the defect of low-temperature brittleness in existing MPP cable protection pipes; the ring stiffness is 14.2 kN / m. 2 It can withstand the pressure of the underground soil and avoid pipe wall deformation; the aging impact strength retention rate is 88.5%, indicating that the use of UV-531 anti-ultraviolet agent alone can still effectively delay the aging of the pipe and ensure the stability of the pipe in long-term use.
[0025] Example 2:
[0026] Please see Figure 1The present invention provides a technical solution: a high-toughness MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 78 parts of MPP resin (polypropylene resin, PP), 13 parts of composite toughening agent, 5.5 parts of modified talc powder (particle size 1.5-2.5μm), 2 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.75 parts of antioxidant, 1.25 parts of lubricant, and 0.5 parts of UV stabilizer; The composite toughening agent consists of 6 parts POE (model 8402), 3.5 parts EVA (VA content 18%), and 3.5 parts modified nano-calcium carbonate (particle size 50-100nm); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 2:1 (0.5 parts of antioxidant 1010 and 0.25 parts of antioxidant 168); the lubricant is a mixture of oleamide and microcrystalline wax in a weight ratio of 1:1 (0.625 parts of oleamide and 0.625 parts of microcrystalline wax); and the UV protectant is a mixture of UV-531 and UV-327 in a weight ratio of 1:1 (0.25 parts of UV-531 and 0.25 parts of UV-327). Nano-calcium carbonate was modified with silane coupling agent (KH-550). The specific method was as follows: 100 parts by weight of nano-calcium carbonate (particle size 50-100nm), 2.25 parts by weight of silane coupling agent (KH-550), and 55 parts by weight of anhydrous ethanol were added to a mixer and stirred at 65°C and 450r / min for 75min. Then the mixture was transferred to an oven and dried at 107°C for 2.5 hours. After pulverizing, the mixture was passed through a 300-mesh sieve to obtain modified nano-calcium carbonate. The modified talc powder is prepared by adding talc powder (particle size 1.5-2.5μm), ethanol and diphenylmethane diisocyanate into a reactor at a weight ratio of 100:50:23.5, stirring at 97℃ for 1.5 hours, distilling under reduced pressure of -0.07MPa for 45 minutes, drying in an oven at 110℃ for 4 hours, and then pulverizing and passing through a 200-mesh sieve. The preparation method of the composite toughening agent is as follows: by weight, 6 parts of POE (model 8402), 3.5 parts of EVA (VA content 18%), and 3.5 parts of the above modified nano calcium carbonate (particle size 50-100nm) are added to a high-speed mixer and stirred at 85℃ and 550r / min for 50min. After stirring, the mixture is naturally cooled to room temperature to obtain the composite toughening agent. The cable protection pipe has a double-layer structure. The inner layer is a smooth and wear-resistant layer, and the outer layer is an impact-resistant reinforcement layer. The thickness ratio of the inner layer to the outer layer is 1:1.35. The amount of composite toughening agent in the outer layer material is 2.5 more parts by weight than that in the inner layer (11.5 parts of composite toughening agent in the inner layer, 14 parts of composite toughening agent in the outer layer, and the remaining materials are used in the same amount in the inner and outer layers). The preparation method of this high-toughness MPP cable protection pipe includes the following steps: S1. Raw material pretreatment: Nano-calcium carbonate and silane coupling agent are mixed and treated according to the above modification method to obtain modified nano-calcium carbonate; modified talc powder, antioxidant, lubricant and UV stabilizer are mixed and placed in a high-speed mixer, stirred at 105℃ and 700r / min for 25min, and cooled to room temperature to obtain mixed excipients; inner layer raw materials and outer layer raw materials are prepared separately, and the amount of composite toughening agent in the outer layer raw material is 2.5 parts by weight more than that in the inner layer. S2. Mixing and Granulation: The inner layer MPP resin, inner layer composite toughening agent, and compatibilizer are added to a high-speed mixer and stirred at 55°C and 350 r / min for 17.5 min. Then, the mixing auxiliary materials are added, the temperature is raised to 90°C, and the stirring is continued at 550 r / min for 30 min to obtain the inner layer premix. The outer layer premix is prepared using the same method. The inner and outer layer premixes are fed into a twin-screw extruder for extrusion granulation. The twin-screw extruder has a length-to-diameter ratio of 36:1 and an extrusion pressure of 17.5 MPa. The temperatures of the six temperature zones from the feed end to the discharge end are 165°C, 180°C, 190°C, 195°C, 190°C, and 180°C, respectively. The screw speed is 200 r / min to obtain inner layer granules and outer layer granules. S3. Extrusion Molding: A dual-barrel extruder is used to feed the inner and outer layer granules into two separate barrels for simultaneous extrusion molding. The temperature of each zone in the inner barrel is 7.5℃ lower than the corresponding temperature zone in the outer barrel (zone 1: 165℃, zone 2: 180℃, zone 3: 190℃, zone 4: 185℃; zone 1: 172.5℃, zone 2: 187.5℃, zone 3: 197.5℃, zone 4: 192.5℃ for the outer barrel). The die head temperature is 175℃, and the extrusion molding speed is 1.6m / min. After extrusion, the material is shaped by a vacuum sizing machine with a vacuum degree of 0.07MPa and a sizing temperature of 21.5℃. It is then cooled to room temperature by water spray for 17.5 minutes, and then cut to a fixed length to obtain a high-toughness MPP cable protection pipe. S4. Post-processing: The cut cable protection pipe ends are flared at an angle of 11°, and a EPDM rubber sealing ring is installed. The interface is then treated with electrofusion welding at a temperature of 210°C for 4 minutes to obtain the finished product.
[0027]
[0028] Example 2, as a preferred embodiment of the present invention, demonstrates the superiority of the formula and process through its experimental data. The impact strength of the simply supported beam reaches 19.5 kJ / m. 2Compared to Example 1, the toughness was improved by 23.4%, and the elongation at break increased to 480%, indicating that the intermediate composite toughening agent ratio (synergistic effect of POE, EVA and modified nano-calcium carbonate) can significantly improve the toughness and impact resistance of the pipe, solving the problem of limited toughening effect of single toughening agents in the prior art; the low-temperature impact performance showed no cracks or damage at -5℃, and no obvious deformation after impact, further proving the excellent low-temperature toughness of the pipe; the ring stiffness was 16.8 kN / m. 2 Compared to Example 1, the performance is improved by 18.3%, with significantly enhanced rigidity, enabling it to adapt to more complex underground working conditions. The aging impact strength retention rate reaches 92.3%, an improvement of 4.3% compared to Example 1, indicating that the 1:1 mixture of UV-531 and UV-327 can exert a synergistic anti-aging effect, effectively extending the service life of the pipe. Simultaneously, the double-layer structure design allows the pipe to balance smoothness and wear resistance with impact resistance, resulting in balanced and excellent performance across all aspects, fully meeting the cable protection requirements under complex working conditions.
[0029] Example 3:
[0030] Please see Figure 1 The present invention provides a technical solution: a high-toughness MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 85 parts of MPP resin (polypropylene resin, PP), 18 parts of composite toughening agent, 8 parts of modified talc powder (particle size 1.5-2.5μm), 3 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 1.2 parts of antioxidant, 2 parts of lubricant, and 0.8 parts of UV stabilizer; The composite toughening agent consists of 8 parts POE (model 8402), 5 parts EVA (VA content 18%), and 5 parts modified nano-calcium carbonate (particle size 50-100nm); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 2:1 (antioxidant 1010 is 0.8 parts, antioxidant 168 is 0.4 parts); the lubricant is a mixture of oleamide and microcrystalline wax in a weight ratio of 1:1 (oleamide 1 part, microcrystalline wax 1 part); and the UV protectant is a mixture of UV-531 and UV-327 in a weight ratio of 2:1 (UV-531 is approximately 0.53 parts, UV-327 is approximately 0.27 parts). Nano-calcium carbonate was modified with silane coupling agent (KH-550). The specific method is as follows: 100 parts by weight of nano-calcium carbonate (particle size 50-100nm), 3 parts by weight of silane coupling agent (KH-550), and 60 parts by weight of anhydrous ethanol were added to a mixer and stirred at 70°C and 500r / min for 90min. Then the mixture was transferred to an oven and dried at 110°C for 3 hours. After pulverizing, the mixture was passed through a 300-mesh sieve to obtain modified nano-calcium carbonate. The modified talc powder is prepared by adding talc powder (particle size 1.5-2.5μm), ethanol and diphenylmethane diisocyanate into a reactor at a weight ratio of 100:50:25, stirring at 100℃ for 1.5 hours, distilling under reduced pressure of -0.07MPa for 45 minutes, drying in an oven at 110℃ for 4 hours, and then pulverizing and passing through a 200-mesh sieve. The preparation method of the composite toughening agent is as follows: by weight, 8 parts of POE (model 8402), 5 parts of EVA (VA content 18%), and 5 parts of the above modified nano calcium carbonate (particle size 50-100nm) are added to a high-speed mixer and stirred at 90℃ and 600r / min for 60min. After stirring, the mixture is naturally cooled to room temperature to obtain the composite toughening agent. The cable protection pipe has a double-layer structure. The inner layer is a smooth and wear-resistant layer, and the outer layer is an impact-resistant reinforcement layer. The thickness ratio of the inner layer to the outer layer is 1:1.5. The amount of composite toughening agent in the outer layer material is 3 more parts by weight than that in the inner layer (15 parts of composite toughening agent in the inner layer and 18 parts of composite toughening agent in the outer layer. The remaining materials are used in the same amount in the inner and outer layers). The preparation method of this high-toughness MPP cable protection pipe includes the following steps: S1. Raw material pretreatment: Nano-calcium carbonate and silane coupling agent are mixed and treated according to the above modification method to obtain modified nano-calcium carbonate; modified talc powder, antioxidant, lubricant and UV stabilizer are mixed and placed in a high-speed mixer, stirred at 110℃ and 800r / min for 30min, and cooled to room temperature to obtain mixed excipients; inner layer raw materials and outer layer raw materials are prepared separately, and the amount of composite toughening agent in the outer layer raw material is 3 more parts by weight than that in the inner layer. S2. Mixing and Granulation: The inner layer MPP resin, inner layer composite toughening agent, and compatibilizer are added to a high-speed mixer and stirred at 60°C and 400 r / min for 20 min. Then, the mixing auxiliary materials are added, the temperature is raised to 95°C, and the stirring is continued at 600 r / min for 35 min to obtain the inner layer premix. The outer layer premix is prepared using the same method. The inner and outer layer premixes are fed into a twin-screw extruder for extrusion granulation. The twin-screw extruder has a length-to-diameter ratio of 36:1, an extrusion pressure of 20 MPa, and six temperature zones from the feed end to the discharge end of 170°C, 185°C, 195°C, 200°C, 195°C, and 185°C respectively. The screw speed is 220 r / min to obtain inner layer granules and outer layer granules. S3. Extrusion Molding: A dual-barrel extruder is used to feed the inner and outer layer granules into two separate barrels for simultaneous extrusion molding. The temperature of each zone in the inner barrel is 10℃ lower than the corresponding temperature zone in the outer barrel (zone 1: 165℃, zone 2: 180℃, zone 3: 190℃, zone 4: 185℃; zone 1: 175℃, zone 2: 190℃, zone 3: 200℃, zone 4: 195℃ for the outer barrel). The die head temperature is 180℃, and the extrusion molding speed is 1.8m / min. After extrusion, the material is shaped by a vacuum sizing machine with a vacuum degree of 0.08MPa and a sizing temperature of 25℃. It is then cooled to room temperature by water spray for 20 minutes, and then cut to a fixed length to obtain a high-toughness MPP cable protection pipe. S4. Post-processing: The cut cable protection pipe ends are flared at an angle of 12°, and a EPDM rubber sealing ring is installed. The interface is then treated with electrofusion welding at a temperature of 220°C for 5 minutes to obtain the finished product.
[0031]
[0032] Example 3 employed the highest raw material ratio, achieving optimal performance in all aspects, fully demonstrating the adjustability and superiority of the formula and process of this invention. The impact strength of the simply supported beam reached 22.3 kJ / m. 2 Compared to Example 2, the toughness was improved by 14.4%, and compared to Example 1, the toughness was improved by 41.1%. The elongation at break reached 510%, indicating that the high dosage of the composite toughening agent can maximize the synergistic toughening effect of POE, EVA and modified nano-calcium carbonate, making the toughness and impact resistance of the pipe reach the extreme. The low-temperature impact performance showed no cracks or damage at -5℃, and it could quickly recover its original shape after impact. The low-temperature toughness far exceeded the level of existing technology. The ring stiffness reached 18.5 kN / m. 2 Compared to Example 2, the performance was improved by 10.1% and compared to Example 1 by 29.9%. The high dosage of modified talc effectively enhanced the rigidity of the pipe, achieving a perfect balance between toughness and rigidity. The aging impact strength retention rate reached 94.7%, which was 2.6% higher than that of Example 2. This indicates that when UV-531 and UV-327 are mixed in a 2:1 ratio, the anti-aging effect is the best, and it can effectively resist the aging damage caused by long-term ultraviolet radiation.
[0033] Example 4:
[0034] Please see Figure 1The present invention provides a technical solution: a high-toughness MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 75 parts of MPP resin (polypropylene resin, PP), 10 parts of composite toughening agent, 4 parts of modified talc powder (particle size 1.5-2.5μm), 1.5 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.5 parts of antioxidant, 0.8 parts of lubricant, and 0.3 parts of UV stabilizer; The composite toughening agent consists of 5 parts POE (model 8402), 3 parts EVA (VA content 18%), and 2 parts modified nano-calcium carbonate (particle size 50-100nm); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 2:1 (antioxidant 1010 is 0.33 parts, antioxidant 168 is 0.17 parts); the lubricant is a mixture of oleamide and microcrystalline wax in a weight ratio of 1:1 (oleamide 0.4 parts, microcrystalline wax 0.4 parts); and the UV stabilizer is UV-327. Nano-calcium carbonate was modified with silane coupling agent (KH-550). The specific method is as follows: 100 parts by weight of nano-calcium carbonate (particle size 50-100nm), 2 parts by weight of silane coupling agent (KH-550), and 52 parts by weight of anhydrous ethanol were added to a mixer and stirred at 62°C and 420r / min for 70min. Then, the mixture was transferred to an oven and dried at 106°C for 2.2 hours. After pulverization, the mixture was passed through a 300-mesh sieve to obtain modified nano-calcium carbonate. The modified talc powder is prepared by adding talc powder (particle size 1.5-2.5μm), ethanol and diphenylmethane diisocyanate into a reactor at a weight ratio of 100:50:23, stirring at 96℃ for 1.5 hours, distilling under reduced pressure at -0.07MPa for 45 minutes, drying in an oven at 110℃ for 4 hours, and then pulverizing and passing through a 200-mesh sieve. The preparation method of the composite toughening agent is as follows: by weight, 5 parts of POE (model 8402), 3 parts of EVA (VA content 18%), and 2 parts of the above modified nano calcium carbonate (particle size 50-100nm) are added to a high-speed mixer and stirred at 82℃ and 520r / min for 45min. After stirring, the mixture is naturally cooled to room temperature to obtain the composite toughening agent. The cable protection pipe has a single-layer structure; The preparation method of this high-toughness MPP cable protection pipe includes the following steps: S1. Raw material pretreatment: Nano-calcium carbonate and silane coupling agent are mixed and treated according to the above modification method to obtain modified nano-calcium carbonate; modified talc powder, antioxidant, lubricant and UV inhibitor are mixed and placed in a high-speed mixer, stirred at 102℃ and 650r / min for 22min, and cooled to room temperature to obtain mixed excipients; S2. Mixing and granulation: MPP resin, composite toughening agent, and compatibilizer are added to a high-speed mixer and stirred at 52°C and 320 r / min for 16 min. Then, the mixed additives prepared in step S1 are added, and the mixture is heated to 88°C and stirred at 520 r / min for another 28 min to obtain a preliminary mixture. The preliminary mixture is fed into a twin-screw extruder for granulation. The twin-screw extruder has a length-to-diameter ratio of 36:1 and an extrusion pressure of 16 MPa. The temperatures of the six temperature zones from the feed end to the discharge end are 162°C, 178°C, 187°C, 192°C, 187°C, and 178°C, respectively. The screw speed is 190 r / min to obtain granules. S3. Extrusion molding: The granular material is fed into the pipe extruder. The barrel temperature of the pipe extruder is 168℃ in zone 1, 182℃ in zone 2, 192℃ in zone 3, and 187℃ in zone 4. The die head temperature is 172℃. The extrusion molding speed is 1.5m / min. After extrusion, it is shaped by a vacuum sizing machine with a vacuum degree of 0.065MPa and a sizing temperature of 20℃. It is then cooled to room temperature by spraying water for 16 minutes. Finally, it is cut to a fixed length to obtain a high-toughness MPP cable protection pipe. S4. Post-processing: The cut cable protection pipe ends are flared at an angle of 10.5°, and a EPDM rubber sealing ring is installed. The interface is then treated with electrofusion welding at a temperature of 205°C for 3.5 minutes to obtain the finished product.
[0035]
[0036] Example 4 uses a lower raw material ratio and a single-layer structure. Experimental data shows that although its performance is slightly lower than that of Examples 2 and 3, it is still better than that of Example 1, fully meeting the requirements for moderate performance and at a lower cost. The impact strength of the simply supported beam is 17.2 kJ / m. 2 Compared to Example 1, the performance was improved by 8.9%, and the elongation at break was 445%, an improvement of 5.9% compared to Example 1. This indicates that a lower dosage of the composite toughening agent can still exert a good synergistic toughening effect, solving the problem of insufficient performance of single toughening agents in the prior art. The low-temperature impact performance showed no cracks or damage at -5℃, and the low-temperature toughness met the standard, making it suitable for general low-temperature environments. The ring stiffness was 15.1 kN / m. 2 Compared to Example 1, it is 6.3% higher and can meet the requirements of conventional underground soil pressure; the aging resistance impact strength retention rate is 89.8%, which is 1.5% higher than that of Example 1, indicating that a single UV-327 anti-ultraviolet agent can also achieve good aging resistance. The raw material ratio and pipe structure can be adjusted according to performance requirements and cost budget, making it suitable for scenarios with moderate performance requirements and strict cost control, such as ordinary municipal cable laying.
[0037] Example 5:
[0038] Please see Figure 1The present invention provides a technical solution: a high-toughness MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 80 parts of MPP resin (polypropylene resin, PP), 15 parts of composite toughening agent, 7 parts of modified talc powder (particle size 1.5-2.5μm), 2.5 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 1.0 part of antioxidant, 1.8 parts of lubricant, and 0.7 parts of UV stabilizer; The composite toughening agent consists of 7 parts POE (model 8402), 4 parts EVA (VA content 18%), and 4 parts modified nano-calcium carbonate (particle size 50-100nm); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 2:1 (antioxidant 1010 is 0.67 parts, antioxidant 168 is 0.33 parts); the lubricant is a mixture of oleamide and microcrystalline wax in a weight ratio of 1:1 (oleamide 0.9 parts, microcrystalline wax 0.9 parts); and the UV protectant is a mixture of UV-531 and UV-327 in a weight ratio of 1.5:1 (UV-531 0.42 parts, UV-327 0.28 parts). Nano-calcium carbonate was modified with silane coupling agent (KH-550). The specific method was as follows: 100 parts by weight of nano-calcium carbonate (particle size 50-100nm), 2.8 parts by weight of silane coupling agent (KH-550), and 58 parts by weight of anhydrous ethanol were added to a mixer and stirred at 68°C and 480r / min for 85min. Then the mixture was transferred to an oven and dried at 109°C for 2.8 hours. After pulverizing, the mixture was passed through a 300-mesh sieve to obtain modified nano-calcium carbonate. The modified talc powder is prepared by adding talc powder (particle size 1.5-2.5μm), ethanol and diphenylmethane diisocyanate into a reactor at a weight ratio of 100:50:24.5, stirring at 99℃ for 1.5 hours, distilling under reduced pressure of -0.07MPa for 45 minutes, drying in an oven at 110℃ for 4 hours, and then pulverizing and passing through a 200-mesh sieve. The preparation method of the composite toughening agent is as follows: by weight, 7 parts of POE (model 8402), 4 parts of EVA (VA content 18%), and 4 parts of the above modified nano calcium carbonate (particle size 50-100nm) are added to a high-speed mixer and stirred at 88℃ and 580r / min for 55min. After stirring, the mixture is naturally cooled to room temperature to obtain the composite toughening agent. The cable protection pipe has a double-layer structure. The inner layer is a smooth and wear-resistant layer, and the outer layer is an impact-resistant reinforcement layer. The thickness ratio of the inner layer to the outer layer is 1:1.2. The amount of composite toughening agent in the outer layer material is 2 more parts by weight than that in the inner layer (13 parts of composite toughening agent in the inner layer and 15 parts of composite toughening agent in the outer layer, and the amount of other raw materials in the inner and outer layers is the same). The preparation method of this high-toughness MPP cable protection pipe includes the following steps: S1. Raw material pretreatment: Nano-calcium carbonate and silane coupling agent are mixed and treated according to the above modification method to obtain modified nano-calcium carbonate; modified talc powder, antioxidant, lubricant and UV stabilizer are mixed and placed in a high-speed mixer, stirred at 108℃ and 750r / min for 28min, and cooled to room temperature to obtain mixed excipients; inner layer raw materials and outer layer raw materials are prepared separately, and the amount of composite toughening agent in the outer layer raw material is 2 more parts by weight than that in the inner layer. S2. Mixing and Granulation: The inner layer MPP resin, inner layer composite toughening agent, and compatibilizer are added to a high-speed mixer and stirred at 58°C and 380 r / min for 19 min. Then, the mixing auxiliary materials are added, the temperature is raised to 93°C, and the stirring is continued at 580 r / min for 33 min to obtain the inner layer premix. The outer layer premix is prepared using the same method. The inner and outer layer premixes are fed into a twin-screw extruder for extrusion granulation. The twin-screw extruder has a length-to-diameter ratio of 36:1 and an extrusion pressure of 19 MPa. The temperatures of the six temperature zones from the feed end to the discharge end are 168°C, 183°C, 193°C, 198°C, 193°C, and 183°C, respectively. The screw speed is 210 r / min to obtain inner layer granules and outer layer granules. S3. Extrusion Molding: A dual-barrel extruder is used to feed the inner and outer layer granules into two barrels for simultaneous extrusion molding. The temperature of each temperature zone in the inner barrel is 5℃ lower than that in the corresponding temperature zone of the outer barrel (zone 1: 165℃, zone 2: 180℃, zone 3: 190℃, zone 4: 185℃; zone 1: 170℃, zone 2: 185℃, zone 3: 195℃, zone 4: 190℃ in the outer barrel). The die head temperature is 178℃, and the extrusion molding speed is 1.7m / min. After extrusion, the material is shaped by a vacuum sizing machine with a vacuum degree of 0.075MPa and a sizing temperature of 23℃. It is then cooled to room temperature by spraying water for 19 minutes, and then cut to a fixed length to obtain a high-toughness MPP cable protection pipe. S4. Post-processing: The cut cable protection pipe ends are flared at an angle of 11.5°, with an internal EPDM rubber sealing ring. The interface is then treated with electrofusion welding at a temperature of 215°C for 4.5 minutes to obtain the finished product.
[0039]
[0040] Example 5 uses a higher proportion of raw materials and a double-layer structure, achieving overall performance close to that of Example 3, fully demonstrating the flexibility of the formulation and process of this invention. The impact strength of the simply supported beam is 20.8 kJ / m. 2 This represents a 6.7% improvement compared to Example 2, and is close to the 22.3 kJ / m³ of Example 3. 2The elongation at break was 495%, an increase of 3.1% compared to Example 2, indicating that a higher dosage of the composite toughening agent can further improve the toughness and impact resistance of the pipe. The low-temperature impact performance showed no cracks or damage at -5℃, and minimal deformation after impact. Its low-temperature toughness was superior to Examples 1 and 4, and close to that of Example 3. The ring stiffness was 17.9 kN / m. 2 Compared to Example 2, the performance is 6.5% higher and 3.2% lower than Example 3. It has sufficient rigidity and can adapt to high-requirement underground working conditions. The aging resistance impact strength retention rate is 93.5%, which is 1.3% higher than Example 2 and close to 94.7% of Example 3. This indicates that when UV-531 and UV-327 are mixed in a ratio of 1.5:1, the anti-aging effect is close to the optimal ratio, which can effectively extend the service life of the pipe and make the comprehensive performance of the pipe adaptable to different high-requirement working conditions. It avoids the high cost of the highest ratio and meets the stringent performance requirements, making it highly practical.
[0041] Comparative Example 1: Please see Figure 1 The present invention provides a comparative solution: an MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 78 parts of MPP resin (polypropylene resin, PP), 13 parts of single toughening agent (POE, model 8402), 5.5 parts of modified talc powder (particle size 1.5-2.5μm), 2 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.75 parts of antioxidant, 1.25 parts of lubricant, and 0.5 parts of UV stabilizer; The composition of antioxidants, lubricants, and UV stabilizers is the same as in Example 2; no nano-calcium carbonate is added, and the nano-calcium carbonate modification step is omitted; the preparation method of modified talc is the same as in Example 2; the cable protection tube has a double-layer structure, and the structural parameters are the same as in Example 2. The preparation method of this MPP cable protection pipe is the same as that in Example 2, except that the composite toughening agent is not prepared and a single POE toughening agent is added to the raw materials.
[0042]
[0043] Comparative Example 1 used a single POE toughening agent without the composite toughening agent of this invention. All its properties were significantly lower than those of Example 2, fully demonstrating the synergistic toughening advantage of the composite toughening agent. The impact strength of the simply supported beam was only 12.7 kJ / m. 2The elongation at break was 320%, 34.9% lower than in Example 2, and 33.3% lower than in Example 2, indicating that the toughening effect of a single toughening agent is limited and cannot effectively improve the toughness and fracture resistance of the pipe. This is consistent with the defects of single toughening agents in the prior art. At -5°C, the low-temperature impact performance showed microcracks and some samples broke, indicating that a single toughening agent cannot solve the problem of low-temperature brittleness in the pipe. The ring stiffness was 13.5 kN / m. 2 The rigidity of the pipe was 19.6% lower than that of Example 2, indicating insufficient rigidity and difficulty in withstanding complex underground soil pressure. The aging impact strength retention rate was 82.1%, 11.1% lower than that of Example 2, indicating poor compatibility between the single toughening agent and the resin, which easily leads to accelerated pipe aging. These experimental data fully demonstrate that the composite toughening agent (POE, EVA and modified nano-calcium carbonate composite) used in this invention can effectively solve the shortcomings of the single toughening agent in the prior art and significantly improve the various properties of the pipe.
[0044] Comparative Example 2: Please see Figure 1 The present invention provides a comparative solution: an MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 78 parts of MPP resin (polypropylene resin, PP), 13 parts of composite toughening agent, 5.5 parts of modified talc powder (particle size 1.5-2.5μm), 2 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.75 parts of antioxidant, 1.25 parts of lubricant, and 0.5 parts of UV stabilizer; The composite toughening agent consists of 6 parts POE (model 8402), 3.5 parts EVA (VA content 18%), and 3.5 parts unmodified nano-calcium carbonate (particle size 50-100nm) (the nano-calcium carbonate has not been modified by silane coupling agent (KH-550)); the composition of antioxidant, lubricant, and UV stabilizer is the same as in Example 2; the preparation method of modified talc is the same as in Example 2; the cable protection tube has a double-layer structure with the same structural parameters as in Example 2; in the preparation method of the composite toughening agent, the modified nano-calcium carbonate is replaced with unmodified nano-calcium carbonate (particle size 50-100nm), and the remaining steps are the same as in Example 2; The preparation method of this MPP cable protection pipe is the same as that in Example 2, except that the nano-calcium carbonate is not modified.
[0045]
[0046] Comparative Example 2 used unmodified nano-calcium carbonate, and was otherwise identical to Example 2. However, all its properties were lower than those of Example 2, fully demonstrating the necessity of nano-calcium carbonate modification. The impact strength of the simply supported beam was 14.3 kJ / m. 2The elongation at break was 380%, 26.7% lower than in Example 2, and 20.8% lower than in Example 2. This indicates that the unmodified nano-calcium carbonate has poor compatibility with MPP resin, POE, and EVA, cannot be uniformly dispersed, and is unable to exert a synergistic toughening effect, which may even affect the toughness of the pipe. The low-temperature impact performance showed cracks at -5℃, indicating that the unmodified nano-calcium carbonate cannot improve the low-temperature toughness of the pipe and still suffers from the low-temperature brittleness defect common in existing technologies. The ring stiffness was 14.2 kN / m. 2 The rigidity was 15.5% lower than that of Example 2, mainly due to the uneven dispersion of unmodified nano-calcium carbonate, which could not effectively enhance the rigidity of the pipe. The aging impact strength retention rate was 85.7%, which was 7.2% lower than that of Example 2, indicating that the presence of unmodified nano-calcium carbonate would accelerate the aging of the pipe and affect its service life.
[0047] Comparative Example 3: Please see Figure 1 The present invention provides a comparative solution: an MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 78 parts of MPP resin (polypropylene resin, PP), 13 parts of composite toughening agent, 5.5 parts of modified talc powder (particle size 1.5-2.5μm), 2 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.75 parts of antioxidant, 1.25 parts of lubricant, and 0.5 parts of UV stabilizer; The UV stabilizer is a mixture of UV-531 and UV-327 in a weight ratio of 3:1 (exceeding the 1:1 to 2:1 range specified in this invention); the composite toughening agent consists of 6 parts POE (model 8402), 3.5 parts EVA (VA content 18%), and 3.5 parts modified nano-calcium carbonate (particle size 50-100nm); the composition of the remaining raw materials, modification methods, and cable protection tube structure are the same as in Example 2. The preparation method of this MPP cable protection pipe is the same as that in Example 2, except that the mixing ratio of the UV stabilizer is different.
[0048]
[0049] In Comparative Example 3, UV-531 and UV-327 were mixed in a 3:1 ratio, with the remaining parameters consistent with Example 2. The aging resistance was significantly reduced, while other properties were slightly decreased, fully demonstrating the rationality of the present invention's limitation on the UV-resistant agent mixing ratio. The impact strength of the simply supported beam was 18.1 kJ / m. 2The elongation at break was 450%, which was 7.2% lower than that of Example 2, and 6.2% lower than that of Example 2. This was mainly due to the improper proportion of the UV stabilizer, which affected its compatibility with the resin and thus slightly affected the toughness of the pipe. The low-temperature impact performance and ring stiffness were not significantly different from those of Example 2, indicating that the proportion of the UV stabilizer had little effect on the low-temperature toughness and rigidity. The aging resistance impact strength retention rate was 86.9%, which was 5.8% lower than that of Example 2. This indicates that when the UV stabilizer is mixed in any proportion, it cannot play a synergistic anti-aging role and may even reduce the anti-aging effect, leading to faster pipe aging. This is consistent with the shortcomings of the prior art, which does not clearly define the proportion of the UV stabilizer and has inconsistent aging resistance performance.
[0050] Comparative Example 4: Please see Figure 1 The present invention provides a comparative solution: an MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 78 parts of MPP resin (polypropylene resin, PP), 13 parts of composite toughening agent, 2 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.75 parts of antioxidant, 1.25 parts of lubricant, and 0.5 parts of UV stabilizer; In this example, no modified talc powder (particle size 1.5-2.5μm) was added, and the preparation steps related to modified talc powder were omitted; the composite toughening agent consisted of 6 parts POE (model 8402), 3.5 parts EVA (VA content 18%), and 3.5 parts modified nano calcium carbonate (particle size 50-100nm); the composition of other raw materials, modification methods, and cable protection pipe structure were the same as in Example 2. The preparation method of this MPP cable protection pipe is the same as that in Example 2, except that no modified talc powder is added.
[0051]
[0052] Comparative Example 4, without the addition of modified talc, was otherwise identical to Example 2. Its ring stiffness decreased significantly, while other properties were slightly reduced, fully demonstrating the important role of modified talc in the rigidity and stability of the pipe. The impact strength of the simply supported beam was 17.8 kJ / m. 2 The elongation at break was 460%, 8.7% lower than in Example 2, and 4.2% lower than in Example 2, indicating that the toughness of the pipe decreased slightly without the addition of modified talc. This is mainly due to the synergistic effect of modified talc on the composite toughening agent. The low-temperature impact performance showed no significant change, indicating that modified talc had little impact on low-temperature toughness. The ring stiffness was only 12.9 kN / m. 2The rigidity was 23.2% lower than that of Example 2, indicating a serious lack of rigidity. It could not withstand the pressure of complex underground soil and was prone to pipe wall deformation and damage. This is consistent with the defect of insufficient rigidity of pipes in the prior art when no modified talc was added. The aging impact strength retention rate was 88.2%, which was 4.4% lower than that of Example 2, indicating that modified talc can improve the structural stability of the pipe and slow down the aging rate.
[0053] Comparative Example 5: Please see Figure 1 The present invention provides a comparative solution: an MPP cable protection pipe, which is prepared from the following raw materials in parts by weight: 80 parts of MPP resin (polypropylene resin, PP), 10 parts of single toughening agent (EVA, VA content 18%), 5 parts of unmodified talc powder (particle size 1.5-2.5μm), 1.5 parts of compatibilizer (maleic anhydride grafted polypropylene, PP-g-MAH, grafting rate 0.8-1.5%), 0.5 parts of antioxidant, 1 part of lubricant, and 0.3 parts of UV stabilizer; Among them, no nano-calcium carbonate was added; the antioxidant was a single antioxidant 1010; the lubricant was a single oleic acid amide; the UV stabilizer was a single UV-531; all inorganic fillers were not modified; and the cable protection tube was a single-layer structure. The preparation method of this MPP cable protection pipe adopts the conventional process of existing technology. The specific steps are: all raw materials are mixed evenly, fed into an extruder for extrusion granulation, and then extruded and cut. There are no special raw material pretreatment and post-treatment steps, and parameters such as extrusion temperature and speed are not precisely controlled (extrusion temperature 170-190℃, speed 150-200r / min).
[0054]
[0055] Comparative Example 5 represents a conventional solution from the prior art, using a single EVA toughening agent and unmodified filler. Its process parameters are imprecise, and its performance is significantly lower than all embodiments of this invention, fully demonstrating the superiority of the technical solution of this invention. The impact strength of the simply supported beam is only 10.3 kJ / m. 2 The elongation at break was 280%, which was 47.2% lower than in Example 2 and 53.8% lower than in Example 3. This indicates that the existing single toughening agent and unmodified filler cannot effectively improve the toughness of the pipe, and the difference between the existing technology and the synergistic effect of the composite toughening agent and modified filler of this invention is significant. The low-temperature impact performance was severely cracked at -5℃, with most samples breaking, completely unable to adapt to low-temperature environments. This is a major defect of existing MPP cable protection pipes, while none of the embodiments of this invention have this problem. The ring stiffness was 11.5 kN / m. 2The rigidity is 31.6% lower than that of Example 2 and 37.8% lower than that of Example 3, indicating a serious lack of rigidity, which cannot meet the requirements of underground construction and long-term use; the aging resistance impact strength retention rate is only 76.8%, which is 16.8% lower than that of Example 2 and 18.9% lower than that of Example 3, indicating a fast aging rate and short service life.
[0056] Through a comprehensive comparative analysis of all embodiments and comparative examples of this technical solution, it can be fully demonstrated that this high-toughness MPP cable protection pipe addresses the core pain points of existing technologies, such as insufficient pipe toughness, easy brittleness at low temperatures, difficulty in balancing rigidity and toughness, and poor aging resistance, achieving a qualitative improvement compared to existing technologies.
[0057] The five embodiments of this technical solution employ different raw material ratios and structural designs, covering low, medium, and high dosages of composite toughening agents, modified fillers, and auxiliary components. All of them successfully produce high-toughness MPP cable protection pipes with good molding quality and no delamination cracking defects. Furthermore, the pipes in each embodiment possess excellent toughness, low-temperature impact resistance, ring stiffness, and aging resistance.
[0058] In contrast, each comparative example exhibits typical design flaws of existing technologies. Comparative Example 1 uses a single toughening agent instead of the composite toughening agent proposed in this solution, resulting in a significant decrease in pipe toughness, low-temperature impact resistance, and aging resistance, failing to address the limited toughening effect of single toughening agents in existing technologies. Comparative Example 2 uses unmodified nano-calcium carbonate; due to poor compatibility between the filler and resin and uneven dispersion, all pipe properties show a significant decline, highlighting the necessity of nano-calcium carbonate modification in this solution. Comparative Example 3 uses a UV stabilizer mixing ratio exceeding the limits of this solution, leading to a significant decrease in the pipe's aging resistance. The low efficiency demonstrates the scientific rationality of limiting the proportion of UV-resistant agent in this solution. Comparative Example 4, which did not add modified talc, resulted in a severe deficiency in the ring stiffness of the pipe, making it unable to withstand the pressure of the underground soil, highlighting the crucial role of modified talc in improving the rigidity of the pipe. Comparative Example 5, as a conventional solution in the prior art, uses a single toughening agent, unmodified filler, and a simple process. Its various properties are significantly lower than all embodiments of this technical solution, especially exhibiting severe cracking in low-temperature impact performance. Its aging resistance and rigidity are also far from meeting the actual use requirements, fully demonstrating the essential difference and significant advantages of this technical solution compared to the prior art.
[0059] To further illustrate the beneficial technical effects of the various embodiments of the present invention, relevant performance tests were conducted on Embodiments 1-5 and Comparative Examples 1-5; The testing method is as follows: 1. Simply Supported Beam Impact Strength Test: Select pipe samples that are undamaged and without delamination after molding, cut them into standard specimens of uniform size, and remove impurities, burrs, and protrusions from the specimen surface using a grinding tool to ensure a smooth surface and uniform dimensions. Fix the prepared specimens on the support of the impact testing machine, adjust the height of the impact hammer and the impact speed to ensure that the impact direction is perpendicular to the force-bearing surface of the specimen, start the equipment to perform the impact test on the specimen, record the impact energy borne by the specimen at the moment of fracture, and calculate the simply supported beam impact strength based on the dimensional parameters of the specimen.
[0060] 2. Elongation at break test: A complete, defect-free sample is cut from the formed pipe into standard tensile specimens. The initial length of the specimen is accurately measured and recorded using a measuring tool. The specimen is then stably mounted on the fixture of the tensile testing machine, ensuring it is securely fixed and subjected to uniform force. A constant tensile speed is set, and the machine is started to stretch the specimen at a uniform speed until it completely breaks. The actual length at break is immediately recorded. The elongation at break is calculated by the difference between the initial length and the length after breakage.
[0061] 3. Low-Temperature Impact Performance Test: Prepare standard impact specimens according to the specifications for the impact strength test of simply supported beams. Place the specimens in a low-temperature test environment and maintain a constant temperature to ensure that the internal temperature of the specimens is completely consistent with the set low temperature. After the constant temperature requirement is reached, quickly remove the specimens and immediately place them in the impact testing machine for impact testing. After the test is completed, carefully observe the surface and cross-section of the specimens to determine whether cracks, damage, fractures, or other phenomena occur, and record the test results accurately.
[0062] 4. Ring Stiffness Test: Cut a pipe sample of a certain length, remove burrs and damaged parts from both ends of the sample, and ensure that the sample ends are flat and free of deformation. Place the sample horizontally on the ring stiffness testing device, adjust the device to ensure uniform force on the sample, and apply radial pressure to the sample using a uniform loading method. Continue loading until the sample produces a specified amount of deformation, record the pressure value borne by the sample at this point, and calculate the ring stiffness based on the sample's dimensional parameters.
[0063] 5. Impact Strength Retention Rate Test for Aging Resistance: First, prepare two sets of standard impact specimens with identical specifications according to the requirements of the simply supported beam impact strength test. One set serves as a blank specimen, and its initial simply supported beam impact strength is tested and recorded. The other set is placed in a xenon lamp aging test apparatus, and a fixed aging time is set for aging resistance treatment. After aging, remove the specimens and allow them to return to room temperature. Then, test the impact strength of the aged specimens according to the simply supported beam impact strength test method described above. Compare the impact strength of the blank specimen and the aged specimen to calculate the impact strength retention rate for aging resistance.
[0064] The above descriptions are merely embodiments of the present invention, and common knowledge regarding specific technical solutions or characteristics is not elaborated upon here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the technical solutions of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the implementation of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.
Claims
1. A high-toughness MPP cable protection pipe, characterized in that, It is prepared from the following raw materials in parts by weight: 70-85 parts MPP resin, 8-18 parts composite toughening agent, 3-8 parts modified talc, 1-3 parts compatibilizer, 0.3-1.2 parts antioxidant, 0.5-2 parts lubricant, and 0.2-0.8 parts UV protectant; The composite toughening agent is composed of 4-8 parts of ethylene-octene copolymer (POE), 2-5 parts of ethylene-vinyl acetate copolymer (EVA), and 2-5 parts of nano-calcium carbonate, wherein the nano-calcium carbonate is modified by a silane coupling agent. The modified talc powder has a particle size of 1.5-2.5 μm and is modified with diphenylmethane diisocyanate.
2. The high-toughness MPP cable protection pipe according to claim 1, characterized in that, The MPP resin is polypropylene resin (PP).
3. The high-toughness MPP cable protection pipe according to claim 1, characterized in that, The compatibilizer is maleic anhydride-grafted polypropylene (PP-g-MAH), with a grafting rate of 0.8-1.5%.
4. The high-toughness MPP cable protection pipe according to claim 1, characterized in that, The antioxidant is composed of antioxidant 1010 and antioxidant 168 mixed in a weight ratio of 2:1; The lubricant is a mixture of oleic acid amide and microcrystalline wax in a weight ratio of 1:
1. The UV protectant is one or two of UV-531 or UV-327 mixed in a weight ratio of 1:1 to 2:
1.
5. The high-toughness MPP cable protection pipe according to claim 1, characterized in that, The nano-calcium carbonate has a particle size of 50-100 nm, and the amount of silane coupling agent used is 1.5-3% of the weight of the nano-calcium carbonate; The method for modifying the nano-calcium carbonate with a silane coupling agent is as follows: by weight, 100 parts of nano-calcium carbonate, 1.5-3 parts of KH-550, and 50-60 parts of anhydrous ethanol are added to a mixer and stirred at 60-70°C and 400-500 r / min for 60-90 min. Then, the mixture is transferred to an oven and dried at 105-110°C for 2-3 hours. After pulverizing, the mixture is passed through a 300-mesh sieve to obtain modified nano-calcium carbonate. The modified talc powder is prepared by adding talc powder, ethanol and diphenylmethane diisocyanate into a reactor at a weight ratio of 100:50:22-25, stirring at 95-100℃ for 1.5 hours, distilling under reduced pressure at -0.07MPa for 45 minutes, drying in an oven at 110℃ for 4 hours, and then pulverizing and passing through a 200-mesh sieve.
6. The high-toughness MPP cable protection pipe according to claim 1, characterized in that, The composite toughening agent is prepared by adding 4-8 parts by weight of ethylene-octene copolymer (POE), 2-5 parts by weight of ethylene-vinyl acetate copolymer (EVA), and 2-5 parts by weight of the above-mentioned modified nano-calcium carbonate into a high-speed mixer and stirring at 80-90°C and 500-600 r / min for 40-60 min. After stirring, the mixture is allowed to cool naturally to room temperature to obtain the composite toughening agent.
7. The high-toughness MPP cable protection pipe according to claim 1, characterized in that, The cable protection pipe has a double-layer structure, with an inner layer being a smooth and wear-resistant layer and an outer layer being an impact-resistant reinforcement layer. The thickness ratio of the inner layer to the outer layer is 1:1.2-1.5, and the amount of composite toughening agent in the outer layer material is 2-3 more parts by weight than that in the inner layer.
8. A method for preparing a high-toughness MPP cable protection pipe as described in any one of claims 1-7, characterized in that, Includes the following steps: S1. Raw material pretreatment: Mix nano-calcium carbonate with silane coupling agent and stir at 80-90℃ for 30-40 min to obtain modified nano-calcium carbonate; The modified talc powder, antioxidant, lubricant, and UV stabilizer are mixed and placed in a high-speed mixer. The mixture is stirred at 100-110℃ and 600-800r / min for 20-30 minutes, and then cooled to room temperature to obtain the mixed excipients. S2. Mixing and Granulation: Add MPP resin, composite toughening agent, and compatibilizer to a high-speed mixer and stir at 50-60℃ and 300-400 r / min for 15-20 min. Then add the mixed additives prepared in S1, heat to 85-95℃, and continue stirring at 500-600 r / min for 25-35 min to obtain a preliminary mixture. Feed the preliminary mixture into a twin-screw extruder for extrusion granulation. The temperatures of the six temperature zones from the feed end to the discharge end of the twin-screw extruder are 160-170℃, 175-185℃, 185-195℃, 190-200℃, 185-195℃, and 175-185℃, respectively, with a screw speed of 180-220 r / min, to obtain granules. S3. Extrusion molding: The granular material is fed into the pipe extruder. The barrel temperature of the pipe extruder is 165-175℃ in zone 1, 180-190℃ in zone 2, 190-200℃ in zone 3, and 185-195℃ in zone 4. The die head temperature is 170-180℃. The extrusion molding speed is 1.4-1.8m / min. After extrusion, the material is shaped by a vacuum sizing machine at a sizing temperature of 18-25℃. It is then cooled to room temperature by spraying water for 15-20 minutes. Finally, it is cut to a fixed length to obtain a high-toughness MPP cable protection pipe. S4. Post-processing: The cut cable protection pipe ends are flared at an angle of 10-12°, and a EPDM rubber sealing ring is installed. The interface is then treated with electrofusion welding at a temperature of 200-220℃ for 3-5 minutes to obtain the finished product.
9. The preparation method according to claim 8, characterized in that, The S2 twin-screw extruder has a length-to-diameter ratio of 36:1 and an extrusion pressure of 15-20 MPa; the S3 vacuum setter has a vacuum degree of 0.06-0.08 MPa, and the traction speed is synchronized with the extrusion speed.
10. The preparation method according to claim 8, characterized in that, When preparing double-layer cable protection pipes in S3, a dual-barrel extruder is used. The inner layer raw material and the outer layer raw material are fed into two barrels respectively and extruded and formed simultaneously. The temperature of each temperature zone of the inner layer barrel is 5-10℃ lower than the corresponding temperature zone of the outer layer barrel.