Micro-foamed rubber sealing strip for automobiles and method for manufacturing the same
By compounding EPDM rubber with high and low ethylene content, and using modified nano-silica and micro-foaming technology, a lightweight micro-foamed automotive rubber sealing strip with strong weather resistance was prepared. This solved the problems of high material density and poor weather resistance of the sealing strip, and achieved the material's lightweight and improved weather resistance.
Patent Information
- Application Number
- CN202611419317.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-10
AI Technical Summary
Existing automotive sealing strips have high density and high material consumption, making it difficult to meet the needs of modern automobiles for lightweighting and comfort upgrades, and they cannot maintain weather resistance and aging resistance in extreme outdoor environments.
It uses a blend of EPDM rubber with high and low ethylene content, combined with modified nano-silica, functional additives and micro-foaming agents to form a microporous structure, which enhances the material's cold resistance, elasticity and flame retardancy, while reducing density.
It achieves lightweighting of materials and improves weather resistance, ozone resistance and UV resistance, meeting the lightweighting and comfort upgrade requirements of new energy vehicles.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of weather-resistant sealant materials, specifically relating to a micro-foamed automotive rubber sealing strip and its preparation method. Background Technology
[0002] Automotive sealing strips are key components ensuring vehicle sealing, sound insulation, vibration reduction, and waterproofing / dustproofing. Traditional solid rubber sealing strips have high density, high material usage, and high compressive load, making them difficult to meet the demands of modern automobiles for lightweighting and improved comfort. Driven by industry trends of energy conservation and emission reduction, the development of new energy vehicles, and increasingly stringent NVH performance requirements, micro-foamed rubber technology has become an important upgrade direction for sealing systems.
[0003] This technology uses ethylene propylene diene monomer (EPDM) rubber as the main base material. Through controlled microfoaming, a uniform closed-cell structure is formed, effectively reducing material density, weight, and optimizing resilience and sealing performance. Simultaneously, it improves sound insulation and vibration damping, reduces door closing force, and improves compression set. Microfoamed rubber meets the vehicle's durability requirements, such as weather resistance and aging resistance, while achieving lightweighting and cost optimization. It has been widely used in vehicle body sealing systems such as doors, windows, and sunroofs, becoming a mainstream technology solution in the automotive sealing field.
[0004] Specialized sealing rubber must have a hardness (Shore A) of 70-80, tensile strength ≥8MPa, elongation at break ≥200%, and specific gravity of 0.8-1.0g / cm³. 3 Key performance indicators include compression set (80℃×24h) ≤25%. Existing materials, while meeting basic performance requirements, have a high specific gravity, failing to meet the requirements for lightweighting.
[0005] Therefore, there is an urgent need to develop a special material that combines weather resistance, ozone resistance, high and low temperature resistance, adaptability to extreme outdoor environments, and lightweight material. Summary of the Invention
[0006] The purpose of this invention is to overcome the defects of the prior art and provide a micro-foamed automotive rubber sealing strip and its preparation method. This material has excellent resistance to high and low temperatures, ozone, ultraviolet rays, and wind and rain, and is suitable for extreme outdoor environments, meeting the needs of lightweighting and comfort upgrades for new energy vehicles.
[0007] This invention provides the following technical solution:
[0008] This invention provides a micro-foamed rubber sealing strip for automobiles, which, by weight, comprises: 10-40 parts of EP 4045M rubber, 60-90 parts of S5890F rubber, 10-30 parts of modified reinforcing filler, 150-180 parts of reinforcing filler, 70-90 parts of plasticizer, 1-3 parts of vulcanizing agent, 3-8 parts of vulcanization activator, 2-4 parts of accelerator, 15-21 parts of functional additive, and 5-7 parts of microfoaming agent;
[0009] The modified reinforcing filler is modified nano-silica, and the preparation method is as follows: nano-silica is dispersed in an organic solvent, vinyl silane is added, heated to react, and then filtered, dried and ground to obtain the modified nano-silica.
[0010] This invention uses a blend of two types of EPDM rubber with different ethylene contents (high and low) to balance cold resistance, elasticity, and processing performance. Modified nano-silica is grafted with vinyl groups, which allow the nano-silica to participate in the vulcanization crosslinking network, improving its dispersibility and interfacial bonding in the rubber matrix, and enhancing the rubber's tensile strength and abrasion resistance. A vulcanization activator activates the vulcanization process and improves the compound's heat resistance. A microfoaming agent creates a microporous structure within the material, ensuring lightweight construction.
[0011] Furthermore, the mass ratio of nano-silica to vinylsilane is (5~8):(1~3); the particle size of nano-silica is 30~50nm; the organic solvent is one of ethanol, methanol or toluene; and the heating temperature is 80~90℃.
[0012] Furthermore, the functional additive is a mixture of magnesium hydroxide and 6-hydroxyhexyl-2-hexyldecanoate, wherein the mass ratio of magnesium hydroxide to 6-hydroxyhexyl-2-hexyldecanoate is 3~6:1.
[0013] When magnesium hydroxide decomposes upon heating, it releases water vapor, absorbs heat, and dilutes flammable gases. This enhances its flame-retardant properties. Furthermore, the hydroxyl groups on the surface of magnesium hydroxide and the polar hydroxyl groups of 6-hydroxyhexyl-2-hexyldecanoate form hydrogen bonds, creating a coating layer on the surface of the filler particles. This effectively reduces the agglomeration of fillers and additives. In addition, the long-chain alkyl groups of 6-hydroxyhexyl-2-hexyldecanoate have good compatibility with the molecular chains of EPDM rubber, which can reduce the surface energy of the filler-rubber interface and further promote the bonding between the filler and the EPDM rubber matrix.
[0014] Furthermore, the reinforcing filler is carbon black. As a highly efficient reinforcing agent, carbon black provides excellent mechanical strength, elasticity, and processing properties.
[0015] Furthermore, the plasticizer is a hydrogenated paraffin-based white oil with a flash point greater than 260°C.
[0016] Furthermore, the vulcanizing agent is sulfur.
[0017] Furthermore, the vulcanizing activator is a mixture of zinc oxide and stearic acid, wherein the zinc oxide is 2 to 6 parts and the stearic acid is 1 to 2 parts.
[0018] Furthermore, the accelerator is one or more of accelerators M, CZ, BZ, TT, TRA, and TDEC.
[0019] Furthermore, the microfoaming agent is one or more of acrylic polymer microspheres, SuperFoam GE, and OBSH.
[0020] This invention also provides a method for preparing the above-mentioned micro-foamed automotive rubber sealing strip, comprising the following steps:
[0021] S1. Put EPDM rubber into an internal mixer and plasticize for 40-60 seconds; add modified reinforcing filler, reinforcing filler, vulcanization activator and plasticizer, and mix for 180-240 seconds; control the temperature at 150-160℃, and discharge the rubber to obtain a premixed rubber.
[0022] S2. After cooling a section of premixed rubber, put it back into the internal mixer, add vulcanizing agent, accelerator, functional additive and micro foaming agent, mix for 60-90 seconds and discharge the final rubber in the range of 80-90℃, place the final rubber in the mold and vulcanize it at 165-175℃ for 20-35 minutes, cool it after vulcanization to obtain the micro foamed automotive rubber sealing strip.
[0023] The present invention has the following beneficial effects:
[0024] 1. This invention utilizes EPDM rubbers with high and low ethylene content and molecular weight in a synergistic manner, taking into account cold resistance, elasticity, and processing performance; it employs modified nano-silica with vinyl grafts on its surface, allowing it to participate in the vulcanization crosslinking network, improving its dispersibility and interfacial bonding performance in the rubber matrix; the addition of functional additives enhances the flame retardant properties of the material, and can further effectively reduce the agglomeration of fillers and additives, promote the bonding between fillers and EPDM rubber matrix, and improve the strength of the material; the use of a micro-foaming system ensures the achievement of lightweight material.
[0025] 2. The preparation process of this invention is highly controllable and suitable for large-scale production of automotive sealing strips. Detailed Implementation
[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] This invention provides a micro-foamed automotive rubber sealing strip, which, by weight, comprises: 10-40 parts of EP4045M rubber, 60-90 parts of S5890F rubber, 10-30 parts of modified reinforcing filler, 150-180 parts of reinforcing filler, 70-90 parts of plasticizer, 1-3 parts of vulcanizing agent, 3-8 parts of vulcanization activator, 2-4 parts of accelerator, 15-21 parts of functional additive, and 5-7 parts of microfoaming agent;
[0028] The modified reinforcing filler is modified nano-silica, and the preparation method is as follows: nano-silica is dispersed in an organic solvent, vinyl silane is added, heated to react, and then filtered, dried and ground to obtain modified nano-silica.
[0029] In a preferred embodiment, the mass ratio of nano-silica to vinylsilane is (5~8):(1~3); the particle size of nano-silica is 30~50nm; the organic solvent is one of ethanol, methanol or toluene; and the heating temperature is 80~90℃.
[0030] In a preferred embodiment, the functional additive is a mixture of magnesium hydroxide and 6-hydroxyhexyl-2-hexyldecanoate, wherein the mass ratio of magnesium hydroxide to 6-hydroxyhexyl-2-hexyldecanoate is 3 to 6:1.
[0031] In a preferred embodiment, the reinforcing filler is carbon black.
[0032] In a preferred embodiment, the plasticizer is a hydrogenated paraffin-based white oil with a flash point greater than 260°C.
[0033] In a preferred embodiment, the vulcanizing agent is sulfur.
[0034] In a preferred embodiment, the vulcanizing activator is a mixture of zinc oxide and stearic acid, wherein the zinc oxide is 2 to 6 parts and the stearic acid is 1 to 2 parts.
[0035] In a preferred embodiment, the accelerator is one or more of the following accelerators: M, CZ, BZ, TT, TRA, and TDEC.
[0036] As a preferred embodiment, the microfoaming agent is one or more of acrylic polymer microspheres, SuperFoam GE, and OBSH.
[0037] This invention also provides a method for preparing the micro-foamed automotive rubber sealing strip, comprising the following steps:
[0038] S1. Put EPDM rubber into an internal mixer and plasticize for 40-60 seconds; add modified reinforcing filler, reinforcing filler, vulcanization activator and plasticizer, and mix for 180-240 seconds; control the temperature at 150-160℃, and discharge the rubber to obtain a premixed rubber.
[0039] S2. After cooling a section of premixed rubber, put it back into the internal mixer, add vulcanizing agent, accelerator, functional additive and micro foaming agent, mix for 60-90 seconds and discharge the final rubber in the range of 80-90℃, place the final rubber in the mold and vulcanize it at 165-175℃ for 20-35 minutes, cool it after vulcanization to obtain micro foamed automotive rubber sealing strip.
[0040] The present invention will be further illustrated below through specific embodiments:
[0041] The materials or reagents used in the following examples (such as EP 4045M rubber - Sinopec Shanghai Mitsui, S5890F rubber - Korean SK, vinylsilane, 6-hydroxyhexyl-2-hexyldecanoate, nano silica, carbon black, hydrogenated paraffinic white oil, accelerator, microfoaming agent, etc.) can all be purchased commercially.
[0042] Example 1:
[0043] The microfoamed automotive rubber sealing strip prepared in this embodiment comprises, by weight, the following components: 15 parts of EP 4045M rubber, 85 parts of S5890F rubber, 25 parts of modified reinforcing filler, 155 parts of reinforcing filler (carbon black), 75 parts of plasticizer (hydrogenated paraffinic white oil, flash point 265℃), 3 parts of vulcanizing agent (sulfur), 6 parts of vulcanization activator (4 parts of zinc oxide and 2 parts of stearic acid), 4 parts of accelerator (accelerator M), 20 parts of functional additive (15 parts of magnesium hydroxide and 5 parts of 6-hydroxyhexyl-2-hexyldecanoate), and 7 parts of microfoaming agent (acrylic polymer microspheres).
[0044] The specific preparation process is as follows:
[0045] 50 mg of nano-silica with an average particle size of 40 nm was selected, dispersed in 100 mL of ethanol, and 15 mg of vinylsilane was added. The mixture was heated and stirred at 85 °C for 20 min. After filtration, drying and grinding, modified nano-silica was obtained.
[0046] 4045M rubber and S5890F rubber were put into an internal mixer and plasticized for 60 seconds; modified reinforcing filler, reinforcing filler, vulcanization activator and plasticizer were added and mixed for 240 seconds; the temperature was controlled at 160℃ and the rubber was discharged to obtain a premixed rubber.
[0047] After cooling a premixed rubber, it is put back into the internal mixer, and vulcanizing agent, accelerator, functional additive and micro foaming agent are added. The mixture is mixed for 90 seconds and discharged in the range of 80-90℃ to obtain the final rubber. The final rubber is placed in a mold and vulcanized at 170℃ for 30 minutes. After vulcanization, it is cooled to obtain a micro foamed automotive rubber sealing strip sample.
[0048] Example 2:
[0049] The preparation process in this embodiment is the same as in Example 1. The micro-foamed automotive rubber sealing strip prepared has the following components by mass: 25 parts of EP 4045M rubber, 75 parts of S5890F rubber, 20 parts of modified reinforcing filler, 165 parts of reinforcing filler (carbon black), 80 parts of plasticizer (hydrogenated paraffinic white oil, flash point 265℃), 2 parts of vulcanizing agent (sulfur), 8 parts of vulcanization activator (6 parts of zinc oxide and 2 parts of stearic acid), 3 parts of accelerator (accelerator M), 20 parts of functional additive (15 parts of magnesium hydroxide and 5 parts of 6-hydroxyhexyl-2-hexyldecanoate), and 6 parts of microfoaming agent (acrylic polymer microspheres).
[0050] Example 3:
[0051] The preparation process in this embodiment is the same as in Example 1. The micro-foamed automotive rubber sealing strip prepared has the following components by mass: 35 parts of EP 4045M rubber, 65 parts of S5890F rubber, 15 parts of modified reinforcing filler, 175 parts of reinforcing filler (carbon black), 85 parts of plasticizer (hydrogenated paraffinic white oil, flash point 265℃), 1 part of vulcanizing agent (sulfur), 3 parts of vulcanization activator (2 parts of zinc oxide and 1 part of stearic acid), 2 parts of accelerator (accelerator CZ), 21 parts of functional additive (18 parts of magnesium hydroxide and 3 parts of 6-hydroxyhexyl-2-hexyldecanoate), and 5 parts of microfoaming agent (acrylic polymer microspheres).
[0052] Comparative Example 1:
[0053] No modified reinforcing filler was added; other components and preparation process were the same as in Example 1.
[0054] Comparative Example 2:
[0055] No functional additives were added; other ingredients and preparation process were the same as in Example 1.
[0056] Comparative Example 3:
[0057] No microfoaming agent was added; other components and preparation process were the same as in Example 1.
[0058] The performance of the samples prepared in Examples 1-3 and Comparative Examples 1-3 was tested, and the results are shown in Table 1:
[0059] Table 1. Performance characterization results of samples prepared in Examples 1-3 and Comparative Examples 1-3
[0060]
[0061] As can be seen from the table above, the rubber materials prepared in Examples 1-3 of this invention are significantly superior to the comparative examples in terms of compression resistance, media resistance, aging resistance, and specific gravity. By adding modified nano-silica, functional additives, micro-foaming agents, etc., the overall strength of the material is improved and the specific gravity of the material is reduced, which fully meets the requirements of automotive sealing strips in various scenarios.
[0062] The overall performance of the sample material obtained by this invention can reach:
[0063] 1. Hardness (Shore A): 75±5;
[0064] 2. Tensile strength ≥ 8 MPa;
[0065] 3. Elongation at break ≥ 200%;
[0066] 4. Compression set (80℃×24h) ≤25%;
[0067] 5. Volume change rate in media such as water ≤ 8%;
[0068] 6. Performance retention rate ≥85% after hot air aging (70℃×72h)
[0069] 7. Specific gravity 0.8-1.0 g / cm³ 3 .
[0070] This invention utilizes EPDM rubbers with varying ethylene content and molecular weights in a synergistic manner, achieving a balance between cold resistance, elasticity, and processing performance. Modified nano-silica with vinyl grafts on its surface participates in the vulcanization crosslinking network, improving its dispersibility and interfacial bonding within the rubber matrix. The addition of functional additives enhances the material's flame retardant properties and further reduces the agglomeration of fillers and additives, promoting the bonding between fillers and the EPDM rubber matrix and increasing the material's strength. The use of a micro-foaming system ensures the achievement of lightweight material design.
[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A micro-foamed rubber sealing strip for automobiles, characterized in that, By weight, its composition is as follows: 10-40 parts of EP 4045M rubber, 60-90 parts of S5890F rubber, 10-30 parts of modified reinforcing filler, 150-180 parts of reinforcing filler, 70-90 parts of plasticizer, 1-3 parts of vulcanizing agent, 3-8 parts of vulcanization activator, 2-4 parts of accelerator, 15-21 parts of functional additives, and 5-7 parts of microfoaming agent; The modified reinforcing filler is modified nano-silica, and the preparation method is as follows: nano-silica is dispersed in an organic solvent, vinyl silane is added, heated to react, and then filtered, dried and ground to obtain the modified nano-silica.
2. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The mass ratio of nano-silica to vinylsilane is (5~8):(1~3); the particle size of nano-silica is 30~50nm; the organic solvent is one of ethanol, methanol or toluene; and the heating temperature is 80~90℃.
3. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The functional additive is a mixture of magnesium hydroxide and 6-hydroxyhexyl-2-hexyldecanoate, with a mass ratio of magnesium hydroxide to 6-hydroxyhexyl-2-hexyldecanoate of 3 to 6:
1.
4. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The reinforcing filler is carbon black.
5. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The plasticizer is a hydrogenated paraffin-based white oil with a flash point greater than 260°C.
6. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The vulcanizing agent is sulfur.
7. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The vulcanizing activator is a mixture of zinc oxide and stearic acid, wherein zinc oxide is 2 to 6 parts and stearic acid is 1 to 2 parts.
8. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The accelerator is one or more of the following: accelerators M, CZ, BZ, TT, TRA, and TDEC.
9. The micro-foamed automotive rubber sealing strip as described in claim 1, characterized in that: The microfoaming agent is one or more of acrylic polymer microspheres, SuperFoam GE, and OBSH.
10. The method for preparing the micro-foamed automotive rubber sealing strip according to any one of claims 1 to 9, characterized in that: Includes the following steps: S1. Put EPDM rubber into a mixer and masticate for 40-60 seconds; Add modified reinforcing fillers, reinforcing filler additives, vulcanization activators and plasticizers, and mix for 180-240 seconds; control the temperature at 150-160℃, and discharge the glue to obtain a first-stage premixed rubber; S2. After cooling a section of premixed rubber, put it back into the internal mixer, add vulcanizing agent, accelerator, functional additive and micro-foaming agent, mix for 60-90 seconds and discharge in the range of 80-90℃ to obtain the final rubber. Place the final rubber in a mold and vulcanize it at 165-175℃ for 20-35 minutes. After vulcanization, cool it to obtain the micro-foamed automotive rubber sealing strip.