A fluorine-containing resin composition and use thereof
By blending fluorinated resin with polysiloxane microspheres, copper clad laminates with low dielectric constant and low density are prepared, solving the problem of difficulty in balancing dielectric properties and density in existing technologies, and realizing the preparation of high-performance copper clad laminates.
Patent Information
- Application Number
- CN202510587907.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to fabricate copper-clad laminates with low dielectric constant, low coefficient of thermal expansion, and low density, and traditional fillers often lead to poor interfacial bonding and high fabrication costs.
Fluoropolymer-based copper-clad laminates were prepared by blending polysiloxane microspheres with fluorinated resin, followed by coating, sintering, copper plating, and high-temperature pressing. The particle size and density of the polysiloxane microspheres were controlled to optimize the dielectric properties and density.
The prepared copper-clad laminate has a dielectric constant as low as 2.30-2.35, a dielectric loss of less than 0.003, and a density as low as 1.56-1.58 g/cm3 at a frequency of 10 GHz, meeting the needs of high-performance and weight-sensitive fields.
Smart Images

Figure BDA0005392320990000111
Abstract
Description
Technical Field
[0001] This invention belongs to the field of laminate technology and relates to a fluoropolymer composition and its application, specifically to a low dielectric, high filler, low density, and high reliability fluoropolymer composition and its application. Background Technology
[0002] Copper clad laminates are a core component of modern military electronic components and 5G communication technology. With the continuous upgrading and iteration of high-end devices, high-quality, multi-layered precision design of signals during transmission has become an inevitable trend in the future development of electronic circuits. Traditional low dielectric loss and low thermal expansion coefficient copper clad laminates use thermosetting resin with inorganic fillers or thermoplastic resin with glass microspheres to reduce dielectric constant, loss and thermal expansion coefficient. However, the addition of inorganic fillers will reduce dielectric performance, and glass microspheres are prone to floating during the preparation of adhesive solution, resulting in uneven material mixing.
[0003] CN112480579A discloses a method for preparing a PTFE-based circuit board with low dielectric constant, low loss, and low coefficient of thermal expansion. This material has excellent dielectric properties, but its coefficient of thermal expansion (70ppm / ℃) is relatively high. Furthermore, the method involves preparing a composite material by blending short glass fibers, hollow glass microspheres, polytetrafluoroethylene (PTFE) resin, and anhydrous ethanol. This method cannot avoid the problem of hollow glass microspheres floating in the resin solution, resulting in uneven distribution of material components. In addition, the preparation cost is high and it is not conducive to continuous large-scale production.
[0004] CN104650574A discloses a polyphenylene ether copper-clad laminate composition, which uses polyphenylene ether in combination with silicone resin, but the laminate prepared by it has a D k >3.0, difficult to meet low D requirements k The demand.
[0005] With the development of high-frequency electronic devices such as 5G communication and AI servers, the dielectric properties (low dielectric constant D) of printed circuit board (PCB) substrates are becoming increasingly important. k Low dielectric loss D f With the increasing demand for lightweight materials and materials, PTFE is favored due to its excellent dielectric properties (D...). k ≈2.1, D f <5×10 -4 While the dielectric constant and thermal stability of hollow glass microspheres have received widespread attention, their processing is difficult and costly, and traditional fillers (such as hollow glass microspheres) are prone to causing poor interfacial bonding and reduced mechanical strength. In existing technologies, although hollow glass microsphere / PTFE composite materials can reduce the dielectric constant, hollow glass microspheres are prone to cracking under high-speed stirring or high pressure on the plate, which can easily lead to pore defects.
[0006] Therefore, it is desirable in the art to develop a resin composition for use in the preparation of laminates, such that the laminates have excellent dielectric properties, low coefficient of thermal expansion, low density, and do not exhibit defects such as poor interfacial bonding. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the present invention aims to provide a fluoropolymer composition and its applications, specifically relating to a low-dielectric, high-filling, low-density, and high-reliability fluoropolymer composition and its applications. This invention introduces low-dielectric-constant polysiloxane microspheres into a fluoropolymer composition, blends them with the fluoropolymer, and then processes the mixture through coating, sintering, copper plating, and high-temperature pressing. The resulting fluoropolymer-based copper-clad laminate exhibits high D-values at 10 GHz. k As low as 2.30-2.35, D f Below 0.003, density as low as 1.56-1.58 g / cm³. 3 It can be applied to high-performance and circuit weight-sensitive fields.
[0008] To achieve this objective, the present invention adopts the following technical solution:
[0009] In a first aspect, the present invention provides a fluorinated resin composition, wherein the fluorinated resin composition comprises, by weight parts, the following components:
[0010] 30-70 parts of fluorinated resin;
[0011] 30-70 parts of polysiloxane microspheres;
[0012] The median particle size (D50) of the polysiloxane microspheres is 1–10 μm, for example, it can be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, or 9 μm, as well as specific values between the above values. For space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range. The density is 1.33–1.38 g / cm³. 3 For example, it can be 1.34 g / cm³. 3 1.35g / cm 3 1.36 g / cm 3 Or 1.37g / cm 3 As well as the specific point values between the above point values, due to space limitations and for the sake of brevity, this invention will not exhaustively list the specific point values included in the range.
[0013] The fluorinated resin composition provided by the present invention contains a specific amount of fluorinated resin and polysiloxane microspheres, and the particle size and density of the polysiloxane microspheres are limited, so that the copper clad laminate prepared from the fluorinated resin composition has a lower dielectric constant, dielectric loss and lower density, while taking into account the appearance of the dielectric layer, and can fully meet the performance requirements of low dielectric and low density copper clad laminate.
[0014] Compared to using silica as a filler, this invention introduces polysiloxane microspheres as a filler into the fluorinated resin composition. When this fluorinated resin composition is used to prepare copper-clad laminates, the density of the copper-clad laminate will not be too high after sintering.
[0015] If the particle size of polysiloxane microspheres is too large, it will lead to D k Larger particle sizes lead to increased density and poor film-forming processability; smaller particle sizes can cause adhesive agglomeration and reduced loss.
[0016] In this invention, the amount of fluorinated resin in the fluorinated resin composition, based on parts by weight, can be, for example, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts, 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, 62 parts, 64 parts, 66 parts, or 68 parts, as well as specific values between the above-mentioned values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range.
[0017] In this invention, the amount of polysiloxane microspheres in the fluorinated resin composition, based on parts by weight, can be, for example, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts, 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, 62 parts, 64 parts, 66 parts, or 68 parts, as well as specific values between the above-mentioned values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range.
[0018] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The purpose and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.
[0019] Preferably, the median particle size of the polysiloxane microspheres is 1–5 μm.
[0020] In this invention, the particle size was obtained using an MS3000 Malvern laser particle size analyzer.
[0021] Preferably, the weight loss rate of the polysiloxane microspheres at 500°C is <20%, for example, it can be 18%, 16%, 15%, 14%, 12%, or 10%, etc. In this invention, the weight loss rate of the polysiloxane microspheres is tested by thermogravimetric analysis (TGA).
[0022] Preferably, based on the total weight of the fluorinated resin and polysiloxane microspheres as 100%, the weight percentage of the polysiloxane microspheres is 50% to 70%, for example, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, or 68%, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0023] Preferably, the polysiloxane microspheres are prepared by the following method:
[0024] The silane compound and water were mixed, a pH adjuster was added, then an alkaline reagent was added, the mixture was stirred, and post-treated to obtain the polysiloxane microspheres.
[0025] Preferably, the silane compound includes methyltrimethoxysilane.
[0026] Preferably, the pH adjuster includes acetic acid.
[0027] Preferably, the amount of pH adjuster added is such that the pH value of the system is 4.5 to 5, for example, 4.6, 4.7, 4.8 or 4.9, and specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0028] Preferably, the alkaline reagent includes ammonia.
[0029] Preferably, the stirring time is 5 to 15 seconds, for example, it can be 6 seconds, 7 seconds, 8 seconds, 9 seconds, 10 seconds, 11 seconds, 12 seconds, 13 seconds or 14 seconds, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0030] Preferably, the post-processing includes filtration and drying after settling.
[0031] Preferably, the settling time is 0.5 to 2 hours, for example, it can be 0.6 hours, 0.8 hours, 1 hour, 1.2 hours, 1.4 hours, 1.5 hours, 1.6 hours or 1.8 hours, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0032] Preferably, the drying temperature is 100-120°C, for example, 102°C, 105°C, 108°C, 110°C, 112°C, 114°C, 116°C or 118°C, and specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0033] In this invention, during the preparation of polysiloxane microspheres, the polysiloxane microspheres are obtained after drying without high-temperature calcination. High-temperature calcination would cause weight loss, converting the polysiloxane into inorganic silica. Using a fluorinated resin composition containing this silica in the preparation of a laminate would result in increased board density. k If the dielectric constant is increased, it will not meet the requirements for low dielectric constant.
[0034] In this invention, the polysiloxane microspheres can also be purchased through commercial channels.
[0035] Preferably, the fluorinated resin includes any one or a combination of at least two of the following: polytetrafluoroethylene, polytetrafluoroethylene-fluoropropyl perfluorovinyl ether copolymer, polytetrafluoroethylene propylene, polytetrafluoroethylene-perfluoroalkoxy perfluorovinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, polychlorotrifluoroethylene, ethylene-chlorotrifluoroethylene copolymer and their derivatives.
[0036] More preferably, the fluorinated resin comprises a combination of polytetrafluoroethylene and polytetrafluoroethylene-fluoropropyl perfluorovinyl ether copolymer, which gives the fluorinated resin composition excellent adhesion properties and can improve the peel strength and adhesion stability of the copper clad laminate containing it.
[0037] Preferably, the fluorinated resin composition further includes a thickener.
[0038] Preferably, the thickener comprises any one or a combination of at least two of polyoxyethylene distyrene phenyl ether, sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether, sodium dodecyl sulfate, and polydimethylsilane.
[0039] Preferably, the fluoropolymer composition further includes other additives that are motivated to be added in the art, such as leveling agents, surfactants, etc.
[0040] Solvents may also be added to the above-mentioned fluorinated resin compositions. The amount of solvent added is selected by those skilled in the art based on experience and process requirements, so that the fluorinated resin composition reaches a suitable viscosity for use, facilitating the coating of the fluorinated resin composition and the preparation of resin films, etc. Subsequently, in the drying stage, the solvent in the fluorinated resin composition will partially or completely evaporate.
[0041] Water is specified as the solvent in this invention.
[0042] In a second aspect, the present invention provides a resin film, the material of which includes the fluorinated resin composition as described in the first aspect.
[0043] Preferably, the resin film is prepared by coating the fluorinated resin composition onto a release material and then drying and / or sintering it.
[0044] Preferably, the drying temperature is 50 to 200°C, for example, it can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or 190°C, as well as specific values between the above-mentioned values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0045] Preferably, the drying time is 10 to 120 minutes, for example, it can be 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes or 110 minutes, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0046] Preferably, the sintering temperature is 200–400°C, for example, it can be 210°C, 230°C, 250°C, 270°C, 290°C, 300°C, 310°C, 330°C, 350°C, 370°C or 390°C, as well as specific values between the above-mentioned values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0047] Preferably, the sintering time is 0.1 to 10 hours, for example, it can be 0.2 hours, 0.25 hours, 0.5 hours, 0.75 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 7 hours, 8 hours, or 9 hours, as well as specific values between the above values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range.
[0048] Thirdly, the present invention provides a prepreg comprising a reinforcing material and a fluoropolymer composition as described in the first aspect, which is attached to the reinforcing material by impregnation, drying and / or sintering.
[0049] Preferably, the reinforcing material includes glass fiber cloth, quartz fiber cloth, quartz-glass fiber blended cloth, or non-woven cloth, etc.
[0050] Preferably, the drying temperature is 50 to 200°C, for example, it can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or 190°C, as well as specific values between the above-mentioned values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0051] Preferably, the drying time is 5 to 120 minutes, for example, it can be 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes or 110 minutes, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0052] Preferably, the sintering temperature is 200–400°C, for example, it can be 210°C, 230°C, 250°C, 270°C, 290°C, 300°C, 310°C, 330°C, 350°C, 370°C or 390°C, as well as specific values between the above-mentioned values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0053] Preferably, the sintering time is 0.1 to 12 hours, for example, it can be 0.2 hours, 0.25 hours, 0.5 hours, 0.75 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours or 11 hours, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0054] Fourthly, the present invention provides a metal foil-coated laminate, the metal foil-coated laminate comprising one or at least two laminated resin films as described in the second aspect, and metal foils located on one or both sides of the laminated resin films; or,
[0055] The metal foil laminate includes one or at least two stacked prepregs as described in the third aspect, and metal foils located on one or both sides of the stacked prepregs.
[0056] Preferably, the metal foil includes copper foil.
[0057] Preferably, the metal foil-coated laminate is prepared by the following method:
[0058] A laminated structure comprising at least one resin film and / or at least one prepreg is provided, wherein a metal foil is covered on one or both sides of the laminated structure and laminated to obtain the metal foil-coated laminate.
[0059] Preferably, the lamination temperature is 200–400°C, for example, 220°C, 250°C, 280°C, 300°C, 320°C, 350°C, or 380°C, as well as specific values between these ranges. For space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range. The lamination pressure is 300–500 PSI, for example, 320 PSI, 350 PSI, 380 PSI, 400 PSI, 420 PSI, etc. 0 PSI, 450 PSI, or 480 PSI, and specific point values between the above values, are not exhaustively listed in this invention due to space limitations and for the sake of brevity. The lamination time is 0.2 to 12 hours, for example, it can be 0.5 hours, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 8 hours, or 10 hours, and specific point values between the above values, are not exhaustively listed in this invention due to space limitations and for the sake of brevity.
[0060] Fifthly, the present invention provides a printed circuit board, the printed circuit board comprising at least one of the resin film as described in the second aspect, the prepreg as described in the third aspect, and the metal foil laminate as described in the fourth aspect.
[0061] Preferably, the substrate of the printed circuit board is a high-frequency substrate.
[0062] In this invention, the high-frequency substrate refers to a special circuit board with a high radio frequency, specifically defined as a substrate with a frequency of 1 GHz or higher.
[0063] Compared with the prior art, the present invention has at least the following beneficial effects:
[0064] (1) The fluorinated resin composition provided by the present invention contains a specific amount of fluorinated resin and polysiloxane microspheres, and limits the particle size and density of the polysiloxane microspheres, so that the copper clad laminate prepared by the fluorinated resin composition has a lower dielectric constant, dielectric loss and lower density, while taking into account the appearance of the dielectric layer, and can fully meet the performance requirements of low dielectric and low density copper clad laminate.
[0065] (2) This invention designs and optimizes the components of the fluorinated resin composition to achieve a dielectric constant of ≤2.35 for the copper-clad laminate containing the fluorinated resin composition, within the range of 2.2-2.35; simultaneously, the overall resin density of the fluorinated resin-based copper-clad laminate (substrate after removing copper foil) is ≤1.58, within the range of 1.56-1.58 g / cm³. 3 Between these values, it is significantly lower than the 2.0g / cm³ of other boards. 3 With its low density, low dielectric and lightweight characteristics, it can be applied to high-performance and weight-sensitive circuit applications. Detailed Implementation
[0066] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0067] The sources of some components in the embodiments and comparative examples of this invention are as follows:
[0068] (1) Fluorine-containing resin
[0069] Polytetrafluoroethylene (PTFE) emulsion: Daikin Industries, Japan, D210C;
[0070] Polytetrafluoroethylene-perfluoroalkoxyperfluorovinyl ether copolymer emulsion: Sichuan Chenguang, PFA-E50;
[0071] It should be noted that in the following specific embodiments of the present invention, the mass percentage of fluorinated resin in the fluorinated resin composition is based on the solids content of the fluorinated resin emulsion, and does not include solvents in the emulsion.
[0072] (2) Thickener
[0073] Polyoxyethylene distyrene phenyl ether, purchased from Kao Corporation's EMULGEN A-60.
[0074] (3) Polysiloxane microspheres
[0075] Polysiloxane microspheres A1: D50: 1μm, grade: EQK10, density: 1.33g / cm³ 3 Manufacturer: Zhejiang Sanshiji;
[0076] Polysiloxane microspheres A2, D50: 3μm, grade: EQK30, density: 1.34g / cm³ 3 Manufacturer: Zhejiang Sanshiji;
[0077] Polysiloxane microspheres A3: D50: 5μm, grade: EQK50, density: 1.35g / cm³ 3 Manufacturer: Zhejiang Sanshiji;
[0078] Polysiloxane microspheres A4: D50: 6μm, grade: EQK60, density 1.36g / cm³ 3 Manufacturer: Zhejiang Sanshiji;
[0079] Spherical silica B1: D50: 3μm, grade: DQ1030, density 2.1g / cm³ 3 Manufacturer: Jiangsu Lianrui;
[0080] Polysiloxane microspheres B2: D50: 11μm, density: 1.45g / cm³ 3 Brand: KMP-601, Manufacturer: Shin-Etsu (Japan);
[0081] Polysiloxane microspheres B3: D50: 0.5μm, density: 1.21g / cm³ 3 Brand: KMP-605, Manufacturer: Shin-Etsu (Japan);
[0082] Polysiloxane microspheres B4: D50: 3μm, density 1.5g / cm³ 3 Samples from the Zhejiang San Shi Ji Laboratory.
[0083] Example 1
[0084] A fluorinated resin composition, wherein the specific components and amounts (parts by weight) of the fluorinated resin composition are shown in Table 1.
[0085] A fluoropolymer resin membrane is prepared by the following method:
[0086] According to the formulation in Table 1, the fluoropolymer emulsion was mixed with polysiloxane microspheres. A thickener was added while stirring until the viscosity of the adhesive was 280 mPa·s. The mixture was stirred at high speed for 2 hours to obtain an adhesive solution. According to the film thickness requirements shown in Table 1, the above adhesive solution was coated onto the surface of the release material (polyimide film, PI film) using a coating machine to obtain a coated PI film. The coated PI film was placed in a vacuum oven at 100°C and baked for 1 hour to remove moisture. It was then baked at 260°C for 1 hour to remove the additives (thickener). Finally, it was sintered at 350°C for 10 minutes. After cooling, the resin layer was peeled off from the PI film to obtain a fluoropolymer film of a specific thickness with uniform thickness and good appearance.
[0087] A fluorinated resin-based copper clad laminate includes a dielectric layer and copper foils (1 oz) disposed on both sides of the dielectric layer, wherein the dielectric layer is composed of the aforementioned fluorinated resin film.
[0088] The preparation method of the fluorinated resin-based copper clad laminate includes: stacking two fluorinated resin films with a size of 320mm×380mm, covering the top and bottom surfaces of the stacked resin films with 1oz thick copper foil, laminating, applying a pressure of 7MPa, a maximum temperature of 390℃, and a holding time of 60min to obtain the fluorinated resin-based copper clad laminate.
[0089] Examples 2-7, Comparative Examples 1-4
[0090] A fluorinated resin composition and a fluorinated resin film and a fluorinated resin-based copper clad laminate containing the same are different from those in Example 1 in that the formulation of the fluorinated resin composition is different, as shown in Tables 1 and 2; wherein, the amount of each component is in "parts".
[0091] Table 1
[0092]
[0093] Table 2
[0094] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Fluorine-containing resin film thickness (μm) 100 100 100 100 PTFE 28 28 28 28 PFA 2 2 2 2 B1 70 B2 70 B3 70 B4 70
[0095] The following performance tests were performed on the fluorinated resin-based copper-clad laminates provided in the above embodiments and comparative examples:
[0096] (1) Dielectric constant D k and dielectric loss D f The SPDR (Split Post Dielectric Resonator) method was used for testing under A-state conditions at a frequency of 10 GHz.
[0097] (2) Density of dielectric layer of fluorinated resin-based copper clad laminate: The density was tested using the water displacement method and an electronic balance.
[0098] (3) Coefficient of thermal expansion (CTE): Tested using IPC-TM-650 2.4.24 method;
[0099] The performance test results are shown in Table 3.
[0100] Table 3
[0101] <![CDATA[Dielectric constant D k > <![CDATA[Dielectric loss D f > <![CDATA[Dielectric layer density g / cm 3 > Z-axis thermal expansion coefficient (ppm) Example 1 2.35 0.0028 1.56 40 Example 2 2.30 0.0025 1.57 38 Example 3 2.30 0.0024 1.58 39 Example 4 2.34 0.0028 1.58 41 Example 5 2.31 0.0023 1.59 42 Example 6 2.30 0.0020 1.60 44 Example 7 2.34 0.0028 1.56 35 Comparative Example 1 2.80 0.0028 2.10 25 Comparative Example 2 2.45 0.0042 1.65 45 Comparative Example 3 2.43 0.0062 1.48 55 Comparative Example 4 2.46 0.0028 1.68 44
[0102] As can be seen from Table 3, the fluorinated resin films (i.e., dielectric layers) prepared from the fluorinated resin compositions provided in the embodiments of the present invention all have low densities (1.56–1.60 g / cm³). 3 The fluorinated resin-based copper clad laminates made from it have low dielectric constant (2.30-2.35) and dielectric loss (0.0024-0.0028), and low coefficient of thermal expansion (≤44ppm).
[0103] Compared to Examples 1-4, Comparative Example 1 used spherical silica as a filler, resulting in a copper-clad laminate with a D-value of [missing information - likely a specific value]. k The density of the dielectric layer increases significantly.
[0104] Compared to Examples 1-4, the polysiloxane microspheres used in Comparative Example 2 had a particle size >10 μm and an excessively high density, resulting in a lower D-value for the fluorinated resin-based copper-clad laminate. k D f The density of both the dielectric layer and the dielectric layer increases.
[0105] Compared to Examples 1-4, the polysiloxane microspheres used in Comparative Example 3 had too small a particle size and too low a density, which led to agglomeration and incomplete dispersion of the polysiloxane microspheres, resulting in deterioration of the dielectric properties of the prepared fluorinated resin-based copper-clad laminate. k D f The coefficients of thermal expansion along both the Z and Z axes increase.
[0106] Compared to Example 2, the density of the polysiloxane microspheres used in Comparative Example 4, with the same particle size, was too high, resulting in a lower D-value for the fluorinated resin-based copper-clad laminate. k The density of both the medium layer and the Z-axis thermal expansion coefficient increases.
[0107] The applicant declares that the present invention is illustrated by the above embodiments to demonstrate the fluoropolymer composition and its application, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A fluorinated resin composition, characterized in that, The fluororesin composition comprises the following components in parts by weight: 30-70 parts of fluorinated resin; 30-70 parts of polysiloxane microspheres; The median particle size of the polysiloxane microspheres is 1–10 μm, and the density is 1.33–1.38 g / cm³. 3 .
2. The fluorinated resin composition according to claim 1, characterized in that, The median particle size of the polysiloxane microspheres is 1–5 μm; Preferably, the polysiloxane microspheres have a weight loss rate of <20% at 500°C.
3. The fluorinated resin composition according to claim 1 or 2, characterized in that, Based on the total weight of fluorinated resin and polysiloxane microspheres as 100%, the weight percentage of the polysiloxane microspheres is 50% to 70%.
4. The fluorinated resin composition according to any one of claims 1-3, characterized in that, The polysiloxane microspheres were prepared by the following method: The silane compound and water were mixed, a pH adjuster was added, then an alkaline reagent was added, the mixture was stirred, and post-treated to obtain the polysiloxane microspheres. Preferably, the silane compound includes methyltrimethoxysilane; Preferably, the pH adjuster includes acetic acid; Preferably, the amount of pH adjuster added is such that the pH value of the system is 4.5 to 5; Preferably, the alkaline reagent includes ammonia. Preferably, the stirring time is 5 to 15 seconds; Preferably, the post-processing includes filtration and drying after settling. Preferably, the settling time is 0.5 to 2 hours; Preferably, the drying temperature is 100–120°C.
5. The fluorinated resin composition according to any one of claims 1-4, characterized in that, The fluorinated resin includes any one or a combination of at least two of the following: polytetrafluoroethylene, polytetrafluoroethylene-fluoropropyl perfluorovinyl ether copolymer, perfluoroethylene propylene, polytetrafluoroethylene-perfluoroalkoxy perfluorovinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, polychlorotrifluoroethylene, ethylene-chlorotrifluoroethylene copolymer and their derivatives.
6. The fluorinated resin composition according to any one of claims 1-5, characterized in that, The fluororesin composition also includes a thickener; Preferably, the thickener comprises any one or a combination of at least two of polyoxyethylene distyrene phenyl ether, sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether, sodium dodecyl sulfate, and polydimethylsilane.
7. A resin film, characterized in that, The resin film is made of a fluorinated resin composition as described in any one of claims 1-6; Preferably, the resin film is obtained by coating the fluorinated resin composition onto a release material and then drying and / or sintering it; Preferably, the drying temperature is 50–200°C; Preferably, the drying time is 10–120 min; Preferably, the sintering temperature is 200–400°C; Preferably, the sintering time is 0.1 to 10 hours.
8. A prepreg, characterized in that, The prepreg includes a reinforcing material and a fluoropolymer composition as described in any one of claims 1-6, which is attached to the reinforcing material by impregnation, drying and / or sintering. Preferably, the drying temperature is 50–200°C; Preferably, the drying time is 5 to 120 minutes; Preferably, the sintering temperature is 200–400°C; Preferably, the sintering time is 0.1 to 12 hours.
9. A metal foil-coated laminate, characterized in that, The metal foil laminate comprises one or at least two laminated resin films as described in claim 7, and metal foils located on one or both sides of the laminated resin films; or, The metal foil laminate comprises one or at least two stacked prepregs as described in claim 8, and metal foils located on one or both sides of the stacked prepregs.
10. A printed circuit board, characterized in that, The printed circuit board includes at least one of the resin film as described in claim 7, the prepreg as described in claim 8, and the metal foil laminate as described in claim 9.
Citation Information
Patent Citations
Polyphenyl ether copper-clad laminate composition
CN104650574A
PTFE-based circuit substrate with low dielectric constant, low loss and low thermal expansion coefficient and preparation method thereof
CN112480579A