A Highly Dispersed Inorganic Nanoparticle System, Its Preparation Method and Application
By constructing a three-dimensional permeation network structure using cellulose nanocrystals and utilizing the steric hindrance effect of hydrogen bonds, the problems of aggregation, interfacial compatibility, and sedimentation of inorganic nanoparticles in aqueous systems were solved, achieving stable dispersion and performance improvement of inorganic nanoparticles in functional coatings on engineered wood panels.
Patent Information
- Application Number
- CN202611553749.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, inorganic nanoparticles are prone to aggregation in aqueous systems, have poor interfacial compatibility with organic resin matrices, and are prone to migration and sedimentation in coatings, resulting in unstable dispersibility and performance of functional coatings on the surface of engineered wood panels.
Cellulose nanocrystals (CNC) were used as dispersants to construct a highly dispersed inorganic nanoparticle system through hydrogen bond steric hindrance, three-dimensional network spatial isolation, and bridging molecular interface enhancement mechanisms. This system formed a three-dimensional permeation network structure, which inhibited aggregation, improved interfacial compatibility, and prevented sedimentation.
This method achieves long-term stable dispersion of inorganic nanoparticles in an aqueous system, improves the superhydrophobicity and wear resistance of the coating, and ensures the uniformity and reliability of the functional coating on the surface of the engineered wood panel.
Smart Images

Figure CN123063005A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nanocomposite materials and wood-based panels, and particularly to a highly dispersed inorganic nanoparticle system, its preparation method, and its application. Background Technology
[0002] Engineered wood products (including particleboard, fiberboard, plywood, etc.) are the main substrates for interior decoration and furniture manufacturing, and their surface properties directly determine the service life and functional quality of the end products. With the upgrading of consumption and the promotion of green home concepts, the market has placed demands on engineered wood surfaces for multi-dimensional synergistic functions such as superhydrophobic self-cleaning, wear and scratch resistance, formaldehyde removal, and flame retardancy. Among numerous surface modification technologies, inorganic nanoparticles (such as nano-SiO2, nano-TiO2, etc.) are widely recognized as ideal functional fillers for constructing functional coatings for engineered wood products due to their high specific surface area, high surface activity, and excellent functional properties. However, existing technologies face the following three core bottlenecks in practical industrial applications: First: Irreversible aggregation of inorganic nanoparticles in aqueous systems. Inorganic nanoparticles such as nano-SiO2 and nano-TiO2 possess extremely high specific surface areas (typically >200 m²). 2 The inorganic nanoparticles ( / g) contain numerous highly reactive hydroxyl (-OH) sites on their surface. In aqueous dispersion media, these highly reactive surface hydroxyl groups readily aggregate irreversibly through hydrogen bonding and van der Waals forces, forming secondary aggregates with particle sizes ranging from hundreds of nanometers to micrometers. Once aggregation occurs, the inorganic nanoparticles lose their unique nanoscale effects—including small size effects, surface effects, and quantum size effects—preventing them from performing their intended functional enhancement role in coatings. While commonly used physical methods such as ultrasonic dispersion and high-speed shear dispersion can break up secondary aggregates in a short time, the dispersion system is thermodynamically unstable and rapidly re-aggregates after standing, failing to meet the requirements for long-term storage stability and uniform application of coatings in industrial production.
[0003] Second, the interfacial compatibility between inorganic nanoparticles and organic resin matrices is poor. Coatings on engineered wood panels typically use organic polymer resins (such as waterborne polyurethane, acrylic resin, melamine-formaldehyde resin, etc.) as the film-forming matrix. Inorganic nanoparticles are hydrophilic, while organic resin matrices are hydrophobic or have intermediate polarity, resulting in significant differences in chemical polarity and surface energy. This polarity difference leads to microphase separation of inorganic nanoparticles within the resin matrix—inorganic nanoparticles tend to aggregate inside the coating, forming "island structures," or settle towards the coating-substrate interface, causing uneven coating composition. Microphase separation not only weakens the enhancing effect of nanoparticles on the mechanical and functional properties of the coating but may also introduce interfacial defects, reducing the coating's adhesion, density, and weather resistance. While commonly used surface modification methods using silane coupling agents (such as KH-550 and KH-560) can improve interfacial compatibility to some extent, the grafting efficiency of silane coupling agents on the surface of inorganic nanoparticles is limited, and the modification process involves organic solvents, which contradicts the current industrial development trends of green manufacturing and low VOC emissions.
[0004] Third: Migration and sedimentation of modified nanoparticles in the coating. Although surface modification methods improve the dispersibility and compatibility of inorganic nanoparticles to some extent, during the coating curing process, due to density differences (nano SiO2 density is approximately 2.2 g / cm³), sedimentation still occurs. 3 The density of nano-TiO2 is approximately 4.0 g / cm³. 3 Its density is much greater than that of water-based resins, which is approximately 1.0 g / cm³. 3 Due to the hydrodynamic effects of the resin matrix during curing and shrinkage, inorganic nanoparticles will still migrate and settle towards the bottom of the coating. This settling behavior leads to a gradient distribution of the functional layer along the coating thickness direction—insufficient concentration of inorganic nanoparticles in the surface functional layer and excessive concentration in the bottom layer, resulting in a significant decrease in key indicators such as superhydrophobicity and wear resistance. Furthermore, settling also causes functional inhomogeneity in different areas of the coating, resulting in a "weakest link effect," which severely restricts the overall service reliability of the functional coating of engineered wood panels.
[0005] To address the aforementioned three major technical challenges, researchers both domestically and internationally have conducted extensive work. For example, Chinese patent CN105670514A discloses a method for modifying waterborne wood coatings with nanocellulose hybrid inorganic nanoparticles. This method uses nanocellulose as a carrier to load and hybridize inorganic nanoparticles onto the cellulose surface. The dispersion mechanism relies on the high specific surface area of nanocellulose to support the inorganic nanoparticles. However, it neither constructs a three-dimensional network space throughout the system to achieve isolated dispersion of the inorganic nanoparticles nor utilizes cellulose as a bridging molecule to improve the interfacial compatibility between the inorganic nanoparticles and the organic resin matrix. Therefore, it fails to simultaneously solve the three major technical problems of agglomeration, interface, and sedimentation. Chinese patent CN108117068A discloses a method for preparing a graphene / nanocrystalline cellulose aqueous dispersion. This method uses nanocrystalline cellulose to improve the aqueous dispersion of graphene (a two-dimensional carbon material) through electrostatic interactions and steric hindrance. The dispersion target and mechanism differ from inorganic oxide systems, and similarly, it does not involve a three-dimensional network structure or bridging molecule interface enhancement. While existing literature reports methods such as Pickering emulsion and in-situ generation have improved the dispersion of inorganic nanoparticles to some extent, they are complex and costly, and cannot meet the requirements of large-scale continuous production in the wood-based panel industry.
[0006] In summary, Chinese patent CN105670514A relies on the high specific surface area of nanocellulose to achieve physical load-bearing, while Chinese patent CN108117068A disperses two-dimensional carbon materials. Neither of these solutions simultaneously addresses the issues of interfacial compatibility and anti-settling. Therefore, there is an urgent need to develop a green, low-cost inorganic nanoparticle high-dispersion system that combines efficient dispersion control, enhanced interfacial compatibility, and anti-settling stability, and to successfully apply it to the industrial manufacturing of functional coatings for engineered wood panels. Summary of the Invention
[0007] In view of this, the present invention provides a highly dispersed inorganic nanoparticle system, its preparation method and application. The highly dispersed inorganic nanoparticle system provided by the present invention, through the regulation of good dispersion of inorganic nanoparticles by cellulose nanocrystals (CNC), can be used for industrial-scale production.
[0008] This invention provides a method for preparing a highly dispersed inorganic nanoparticle system, comprising the following steps: (1) Mix CNC and water to obtain a CNC dispersion; (2) Mix the CNC dispersion and inorganic nanoparticles, shear and sonicate, adjust the pH value to 7~10, and age to obtain a highly dispersed inorganic nanoparticle system.
[0009] Preferably, the CNC surface has a sulfonate group content of 0.5~1.5 mmol / g and a surface hydroxyl number density of 3~5 per nm. 2 The length is 100~500nm, the diameter is 5~20nm, and the aspect ratio is 5~100:1.
[0010] Preferably, in step (1), the mixing is carried out under temperature control conditions, and the temperature control temperature does not exceed 30°C; the mixing method is pulsed ultrasonic dispersion; the power of pulsed ultrasonic dispersion is 400~1200W, the frequency is 20~25kHz, the duty cycle is 1:1~1:3; the mixing time is 10~30 minutes.
[0011] Preferably, the concentration of CNC in the CNC dispersion is 1~10 mg / mL.
[0012] Preferably, the inorganic nanoparticles include one or more of nano-SiO2, nano-TiO2, nano-Al2O3 and nano-ZnO; the original particle size of the inorganic nanoparticles is 5~50nm.
[0013] Preferably, the mass ratio of CNC to inorganic nanoparticles is 0.5~10:100.
[0014] Preferably, the shearing ultrasound includes sequential shearing and ultrasound; the shearing speed is 8000~15000rpm, and the time is 5~15 minutes; the ultrasound power is 200~600W, the mode is pulse ultrasound, the working mode is 2s working followed by 3s interval, and the time is 10~30 minutes; the ultrasound is performed under temperature control, and the temperature control temperature does not exceed 30℃.
[0015] This invention also provides a highly dispersed inorganic nanoparticle system, prepared using the method described above. The system comprises CNC, inorganic nanoparticles, and water. The CNC forms a hydrogen-bonded steric hindrance layer on the surface of the inorganic nanoparticles and constructs a three-dimensional permeation network structure in an aqueous medium. The pore size of the three-dimensional permeation network structure is 50-200 nm, and the inorganic nanoparticles are isolated and dispersed within the pore units of the three-dimensional permeation network structure. The zeta potential of the highly dispersed inorganic nanoparticle system is -30 to -50 mV, measured at pH 7-10.
[0016] This invention also provides the application of the above-described inorganic nanoparticle highly dispersed system in the field of surface modification of engineered wood panels.
[0017] Preferably, the application method includes the following steps: mixing an inorganic nanoparticle highly dispersed system with an aqueous resin and additives to obtain a functional composite coating, then coating the functional composite coating onto the surface of a wood-based panel substrate and curing it to obtain a functional composite coating layer.
[0018] Compared with the prior art, the present invention has achieved the following beneficial effects: This invention uses naturally sourced, renewable, and biodegradable CNC as a green dispersant to construct a highly dispersed system of inorganic nanoparticles (SiO2, TiO2, Al2O3, ZnO, and other nano-oxide particles). The highly dispersed system of inorganic nanoparticles of this invention is then combined with an organic resin matrix for use as a superhydrophobic and wear-resistant composite coating on the surface of engineered wood panels.
[0019] This invention utilizes the unique rod-shaped nanostructure of CNC (length 100~500nm, diameter 5~20nm, aspect ratio 5:1~100:1) and abundant hydroxyl groups on the surface (surface hydroxyl number density of approximately 3~5 / nm). 2 The chemical properties of inorganic nanoparticles are synergistically regulated by hydrogen bond steric hindrance, three-dimensional network spatial isolation, and bridging molecular interfaces, forming multi-level interfacial bonds that range from strong to weak and span inorganic and organic phases. This effectively solves the technical problems of easy aggregation of inorganic nanoparticles in aqueous systems, poor interfacial compatibility with organic resin matrices, and easy migration and sedimentation during coating curing. Specifically, the mechanism of this invention (e.g.) Figure 1 and Figure 3 As shown below: Mechanism 1: Hydrogen bond-induced steric hindrance effect – inhibiting aggregation. The CNC surface contains a large number of primary hydroxyl groups (C6-OH) and secondary hydroxyl groups (C2-OH, C3-OH), with a hydroxyl number density as high as 3~5 per nm. 2 In aqueous systems with a pH of 7–10, these surface hydroxyl groups can form multiple intermolecular hydrogen bonds (OH···O bond energy approximately 12–30 kJ / mol) with the silanol groups (Si-OH) on the surface of inorganic nanoparticles (nano SiO2) and the titanium hydroxyl groups (Ti-OH) on the surface of nano TiO2. After CNCs are anchored to the surface of inorganic nanoparticles through hydrogen bonding, their rigid rod-like structures extend outward, forming a steric hindrance layer with a thickness of approximately 5–20 nm around the inorganic nanoparticles. According to the DLVO (Derjaguin-Landau-Verwey-Overbeek) colloidal stability theory, this steric hindrance layer effectively increases the minimum approach distance between inorganic nanoparticles, extending the van der Waals gravitational potential energy decay distance from <1 nm without CNCs to approximately 10–20 nm. This transforms the total interaction potential energy between inorganic nanoparticles from a net attractive force to a net repulsive force, effectively inhibiting the irreversible aggregation of inorganic nanoparticles. In addition, the small amount of sulfonate groups remaining on the CNC surface (from the sulfuric acid hydrolysis preparation process) provides an additional contribution to electrostatic repulsion, forming a synergistic dispersion mechanism with the steric hindrance effect (e.g. Figure 1 and Figure 3As shown, the multiple hydrogen bond network between C2-OH, C3-OH, and C6-OH on the CNC glucose ring and Si-OH on the SiO2 surface is displayed at the molecular scale, as well as the interfacial structure of CNC as a bridge molecule connecting nanoparticles and organic resin matrix.
[0020] Mechanism 2: Spatial Isolation and Multidimensional Dispersion through a Three-Dimensional Network of Rod-like Nanostructures. CNC (Cyclic Nucleated Nanoparticles) possess unique rod-like nanomorphological characteristics: length (L) of 100–500 nm, cross-sectional diameter (D) of 5–20 nm, and aspect ratio (L / D) of 5:1–100:1. When the CNC dosage reaches the critical percolation concentration (approximately 0.5–1.0 wt%), these high aspect ratio rigid nanorods self-assemble in an aqueous medium through physical entanglement and hydrogen bonding, forming a three-dimensional percolation network structure that permeates the entire system. The characteristic pore size of this three-dimensional percolation network structure is approximately 50–200 nm, which precisely matches the particle size of inorganic nanoparticles (5–50 nm). Inorganic nanoparticles are "trapped" within the individual pore units of the three-dimensional percolation network structure, with each pore unit accommodating only 1–3 inorganic nanoparticles, thus achieving uniform isolation and dispersion of inorganic nanoparticles in three-dimensional space—the "spatial confinement dispersion" mechanism. This three-dimensional percolation network structure exhibits excellent mechanical stability. Even during storage shearing, transportation vibration, or coating processes, the three-dimensional percolation network structure remains intact, continuously preventing the re-aggregation of inorganic nanoparticles. More importantly, the three-dimensional percolation network structure does not collapse during coating curing, effectively inhibiting the sedimentation and migration of inorganic nanoparticles driven by resin shrinkage (e.g., Figure 1 and Figure 3 (As shown). It should be noted that the 50~200nm mentioned above are the characteristic pore sizes of the three-dimensional permeation network structure. These sizes were obtained by observation and statistics using a scanning electron microscope (SEM) after freeze-drying. The actual pore sizes fluctuate within this range depending on the CNC dosage and the particle size of the inorganic nanoparticles, and always match the original particle size (5~50nm) of the inorganic nanoparticles, thereby achieving effective trapping and isolation of the inorganic nanoparticles by the pores.
[0021] Mechanism 3: Bridge Molecular Interface Enhancement Effect (Short-range van der Waals forces, hydrophobic interactions, dipole interactions, physical cross-linking) – Enhancing Compatibility. The CNC molecular structure contains a large number of hydrophilic hydroxyl groups (affinity with the inorganic nanoparticle surface) and hydrophobic glucose ring planes (affinity with the hydrocarbon backbone of the organic resin matrix). This unique "amphiphilic" molecular structure endows CNC with excellent interfacial compatibility control capabilities. In the CNC-controlled inorganic nanoparticle-resin composite system, the CNC molecule plays the role of a "molecular bridge": one end is firmly anchored to the inorganic nanoparticle surface through multiple hydrogen bonds, while the other end undergoes physical cross-linking with the molecular chain segments of the organic resin matrix through intermolecular van der Waals forces, hydrophobic interactions, and possible hydrogen bonding. This bridging effect transforms the weak physical interface between the inorganic nanoparticles and the resin matrix into a quasi-chemically bonded strong interface, significantly improving interfacial shear strength and stress transfer efficiency. Dynamic mechanical analysis (DMA) results show that after introducing CNC control, the storage modulus (E') of the composite coating is above the glass transition temperature (T). g The decrease in crosslinking density at +30℃ narrowed from -72% without CNC to -38%, confirming a significant improvement in interfacial crosslinking density (see Test Example 3 for relevant test data).
[0022] The inorganic nanoparticle high dispersion system provided by this invention can maintain uniform dispersion after 90 days of sealed storage at room temperature. The water contact angle of the formed functional composite coating can reach more than 150°, and the wear resistance is improved compared with pure resin coating (Taibo wear loss is reduced by more than 50% compared with pure resin coating). It takes into account the long-term storage stability of the dispersion system, the interfacial compatibility with the organic resin matrix, and the anti-settling ability during the coating curing process, and provides a systematic technical solution for the large-scale industrial manufacturing of multifunctional composite coatings on the surface of artificial boards. Attached Figure Description
[0023] To more clearly illustrate the technical solutions of this invention, the accompanying drawings used in the embodiments of this invention or in the prior art are briefly described below. For those skilled in the art, other drawings can be derived from the following drawings without creative effort, and all such drawings are within the protection scope of this invention.
[0024] Figure 1 This is a schematic diagram of the three-dimensional network spatial isolation and steric hindrance effect mechanism of the highly dispersed inorganic nanoparticle system controlled by CNC in this invention; wherein, (a) is the irreversible aggregation state of inorganic nanoparticles without CNC control, and (b) is the uniform dispersion state of inorganic nanoparticles under the triple synergistic control of CNC. Figure 2 A schematic diagram of the multi-layer structure of a functional composite coating applied to the surface of a wood-based panel; Figure 3 A schematic diagram of the multiple hydrogen bonds and the interface enhancement mechanism of "bridge molecules" between the hydroxyl groups on the CNC surface and the silanol groups on the surface of inorganic nanoparticles (SiO2); Figure 4 The relationship between the storage particle size and the water contact angle of the functional composite coating in the inorganic nanoparticle highly dispersed system under different CNC dosages is shown in the figure. Detailed Implementation
[0025] This invention provides a method for preparing a highly dispersed inorganic nanoparticle system, comprising the following steps: (1) Mix CNC and water to obtain a CNC dispersion; (2) Mix the CNC dispersion and inorganic nanoparticles, shear and sonicate, adjust the pH value to 7~10, and age to obtain a highly dispersed inorganic nanoparticle system.
[0026] This invention involves mixing CNC with water (referred to as the first mixture) to obtain a CNC dispersion. In this invention, the CNC is prepared by sulfuric acid hydrolysis; the surface sulfonate group content of the CNC can be 0.5~1.5 mmol / g, and the surface hydroxyl number density can be 3~5 per nm. 2 The length can be 100~500nm, specifically 300nm; the diameter can be 5~20nm, specifically 10nm or 15nm; and the aspect ratio can be 5~100:1, specifically 10~50:1.
[0027] In specific embodiments of the present invention, the CNC can be a commercially available CNC or a self-made CNC; the commercially available CNC can be an FPInnovations CNC or a CelluForce FPLCC. Commercially available CNC products in the art can be used in the present invention.
[0028] In this invention, the water can be deionized water.
[0029] In this invention, the first mixing can be carried out under temperature control; the temperature can not exceed 30°C, specifically 25°C, 20°C or 15°C; the temperature control method can be an ice bath.
[0030] In this invention, the first mixing method can be pulsed ultrasonic dispersion; the power of pulsed ultrasonic dispersion can be 400~1200W, specifically 400W or 600W, the frequency can be 20~25kHz, specifically 20kHz, the duty cycle can be 1:1~1:3, specifically 2s of operation followed by a 3s interval; the device for the first mixing can include an ultrasonic cell disruptor, the probe diameter can be 6mm; the time for the first mixing can be 10~30 minutes, specifically 20 minutes.
[0031] The present invention employs the above-mentioned frequency, which can effectively disperse CNC, and the corresponding cavitation energy can interrupt the agglomeration of CNC dry powder without causing damage to the CNC crystal structure; employing the above-mentioned duty cycle can ensure effective cavitation time while avoiding local overheating and degradation of CNC caused by continuous ultrasound; employing the above-mentioned power can balance the deagglomeration efficiency of CNC and the integrity of CNC crystal structure.
[0032] In this invention, the concentration of CNC in the CNC dispersion can be 1~10 mg / mL, specifically 5 mg / mL.
[0033] After obtaining the CNC dispersion, the present invention mixes the CNC dispersion and inorganic nanoparticles under stirring conditions (referred to as the second mixture), performs shearing and ultrasonication, adjusts the pH value to 7-10, and ages the mixture to obtain a highly dispersed inorganic nanoparticle system. In the present invention, the inorganic nanoparticles may include one or more of nano-SiO2, nano-TiO2, nano-Al2O3, and nano-ZnO; the original particle size of the inorganic nanoparticles may be 5-50 nm, specifically 10-30 nm.
[0034] Furthermore, when the aspect ratio of CNC is in the range of 10 to 50:1, the original particle size of inorganic nanoparticles is on the same order of magnitude as the diameter of CNC (i.e., 10 to 30 nm). CNC can form a proportional coating on the surface of inorganic nanoparticles, and the size of the three-dimensional network nodes matches the network span, thereby obtaining the maximum contact angle, wear resistance, and anti-migration gain. If the original particle size of inorganic nanoparticles is too small (<10 nm), the specific surface energy is high, and the CNC coating layer is relatively thin, the long-range van der Waals attraction cannot be completely shielded, which will instead exacerbate the secondary aggregation of particles. If the original particle size of inorganic nanoparticles is too large (>30 nm), the specific surface energy is low, the interaction area with CNC is insufficient, the bridging density decreases, and the three-dimensional percolation network structure is difficult to construct completely.
[0035] In this invention, the mass ratio of CNC to inorganic nanoparticles can be 0.5~10:100, specifically 1.5:100, 2:100, 3:100, 5:100, 7:100, or 9:100. When the mass ratio is 0.5~2:100, CNC mainly inhibits particle aggregation through the synergistic effect of electrostatic repulsion and hydrogen bond anchoring provided by surface sulfonate groups, making it suitable for inorganic nanoparticles with small primary particle size and high surface hydroxyl density. When the mass ratio is 5~10:100, the amount of CNC used is higher than the critical percolation concentration, which can form a complete and interconnected three-dimensional percolation network in aqueous media, making the spatial isolation effect dominant, suitable for dispersion systems with high solid content or requiring long-term storage.
[0036] In this invention, the specific surface area of nano-SiO2 can be 150~350m². 2 / g; The mass ratio of CNC and nano SiO2 can be 1~10:100, specifically 3:100, 5:100, 7:100 or 9:100.
[0037] In this invention, the nano-TiO2 can be anatase TiO2; the specific surface area of the nano-TiO2 can be 30~100m². 2 / g; the mass ratio of CNC and nano TiO2 can be 1.5~4:100, specifically 2:100, 2.5:100, 3:100 or 3.5:100.
[0038] In this invention, the crystal form of nano-Al2O3 can be α-phase or γ-phase; the specific surface area of nano-Al2O3 can be 20~80m². 2 / g; The mass ratio of CNC and nano Al2O3 can be 2~5:100, specifically 3:100 or 4:100.
[0039] In this invention, the specific surface area of nano-ZnO can be 40~100 m². 2 / g; The mass ratio of CNC and nano ZnO can be 2~5:100, specifically 3:100 or 4:100.
[0040] In this invention, the stirring speed can be 50~400 rpm, specifically 100 rpm or 200 rpm. Using the above-mentioned speed ensures uniform wetting and dispersion of inorganic nanoparticles without causing excessive shear degradation of the CNC dispersion.
[0041] In this invention, the second mixing can be stirring, with a stirring speed of 50-400 rpm, specifically 100 rpm or 200 rpm; the second mixing time can be 10-20 minutes, specifically 15 minutes. This invention obtains a CNC-inorganic nanoparticle premixed suspension through the second mixing.
[0042] In this invention, shearing ultrasound can include sequential shearing and ultrasound; the shearing rotation speed can be 8000~15000 rpm, specifically 12000 rpm, and the time can be 5~15 minutes, specifically 10 minutes; the ultrasound power can be 200~600W, specifically 300W, 400W, or 500W, and the mode can be pulsed ultrasound, with a working mode of 2 seconds followed by a 3-second interval, and the time can be 10~30 minutes, specifically 20 minutes; the ultrasound can be performed under temperature control, and the temperature can not exceed 30℃, specifically 25℃, 20℃, or 15℃; the temperature control method can be an ice bath. This invention, through the above-mentioned shearing and ultrasound, synergistically disperses inorganic nanoparticles.
[0043] In this invention, the pH value is adjusted to 7-10, specifically 8 or 9; the reagent used to adjust the pH value can be NaOH solution or KOH solution; the concentration of NaOH solution or KOH solution can be 0.05-0.2 mol / L, specifically 0.1 mol / L or 0.15 mol / L.
[0044] In this invention, the aging temperature can be 15~35℃, specifically 20℃, 25℃, or 30℃, and the time can be 2~6 hours, specifically 3 hours, 4 hours, or 5 hours; aging can be carried out under static conditions. By using the above-mentioned aging temperature and time, this invention allows the hydrogen bond anchoring of CNC on the surface of inorganic nanoparticles to tend towards equilibrium and promotes the full relaxation and shaping of the three-dimensional permeation network structure, thereby obtaining a stable dispersion state.
[0045] This invention also provides a highly dispersed inorganic nanoparticle system, prepared using the method described above. The system comprises CNC, inorganic nanoparticles, and water. The CNC forms a hydrogen-bonded steric hindrance layer on the surface of the inorganic nanoparticles and constructs a three-dimensional permeable network structure in an aqueous medium. The pore size of the three-dimensional permeable network structure is 50–200 nm (matching the original particle size of the inorganic nanoparticles; the pore size was obtained by scanning electron microscopy after freeze-drying). The inorganic nanoparticles are isolated and dispersed within the pore units of the three-dimensional permeable network structure. The zeta potential of the highly dispersed inorganic nanoparticle system is -30 to -50 mV, measured at pH 7–10.
[0046] In this invention, a single mesh unit of the three-dimensional permeation network structure can accommodate 1 to 3 inorganic nanoparticles.
[0047] This invention also provides the application of the above-described inorganic nanoparticle highly dispersed system in the field of surface modification of engineered wood panels.
[0048] In this invention, the method may include the following steps: mixing an inorganic nanoparticle highly dispersed system with an aqueous resin and additives (referred to as the third mixture) to obtain a functional composite coating, then coating the functional composite coating onto the surface of a wood-based panel substrate and curing it to obtain a functional composite coating layer.
[0049] In this invention, the mass ratio of inorganic nanoparticles to resin in the aqueous resin solution in the inorganic nanoparticle high dispersion system can be 0.5~5:100, specifically 1:100, 2:100, 3:100 or 4:100; the solid content of the aqueous resin solution can be 30~40wt%, specifically 35wt.
[0050] In this invention, the waterborne resin may include one or more of waterborne polyurethane resin, waterborne acrylic resin, and melamine-formaldehyde resin.
[0051] In this invention, the additives may include defoamers, leveling agents, and thickeners; the defoamer may be BYK-024 defoamer; the amount of defoamer may be 0.1~0.5wt% (based on 100wt% of the functional composite coating), specifically 0.3wt%; the leveling agent may be BYK-333 leveling agent; the amount of leveling agent may be 0.2~1wt% (based on 100wt% of the functional composite coating), specifically 0.5wt% or 0.8wt%; the thickener may be RM-8W thickener; the amount of thickener may be 0.1~0.5wt% (based on 100wt% of the functional composite coating), specifically 0.3wt%.
[0052] In this invention, the third mixing can be stirring; the stirring speed can be 500~1000 rpm, specifically 800 rpm; the third mixing time can be 15~30 minutes, specifically 20 minutes.
[0053] In this invention, the substrate material of the engineered wood panel can be particleboard, blockboard, fiberboard or plywood.
[0054] In this invention, the artificial board substrate can be pretreated before use; the pretreatment can be surface sanding followed by blowing off surface dust; the surface sanding can be done with 240-mesh sandpaper; the surface dust can be blown off with compressed air.
[0055] In this invention, the coating method can be spraying, roller coating or curtain coating; the thickness of the coated wet film can be 50~200μm, specifically 100μm.
[0056] In this invention, the process may include applying a primer before coating; the primer may be a conventional industrial sealing primer.
[0057] In this invention, curing can be heat curing, room temperature curing, or a combination of both. Heat curing can be performed at a temperature of 60-120°C, specifically 80°C or 100°C, for a time of 10-60 minutes, specifically 30 minutes or 45 minutes. Room temperature curing can be performed for 24-48 hours, specifically 36 hours. Combination curing can include sequential room temperature curing and high temperature curing. Room temperature curing can be performed at room temperature for 10-30 minutes; high temperature curing can be performed at a temperature of 80-100°C, specifically 90°C, for 20-40 minutes, specifically 30 minutes. During the curing process, CNC forms a physical cross-linking structure with the water-based resin matrix in the functional composite coating.
[0058] In this invention, the functional composite coating can be a superhydrophobic functional layer or a surface wear-resistant functional layer. When the functional composite coating is a superhydrophobic functional layer, the inorganic nanoparticles are uniformly dispersed in the thickness direction of the functional composite coating, and the surface density variation coefficient of the inorganic nanoparticles is ≤15% (the surface density variation coefficient is obtained by performing scanning electron microscopy-energy dispersive spectroscopy surface scanning analysis on the cross-section of the functional composite coating, statistically analyzing the surface density of the characteristic elements of the inorganic nanoparticles in 5 random fields of view, and calculating the variation coefficient). When the functional composite coating is a surface wear-resistant functional layer, the mass percentage of inorganic nanoparticles in the functional composite coating is 0.5~5.0wt%, and the original particle size of the inorganic nanoparticles is 10~30nm.
[0059] In this invention, the functional composite coating can also be a multifunctional composite coating that combines superhydrophobicity, wear resistance, and weather resistance. In this case, the waterborne resin can be a mixture of waterborne polyurethane and waterborne acrylic resin, and the mass ratio of waterborne polyurethane to waterborne acrylic resin can be 1:0.5~2, specifically 1:1 or 1:1.5.
[0060] To further illustrate the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings and embodiments. Unless otherwise specified, specific conditions in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments used without specified manufacturers are all commercially available conventional products.
[0061] In a specific embodiment of the present invention, the self-made CNC is prepared as follows: bleached sulfate eucalyptus pulp board is taken and hydrolyzed for 60 minutes under the conditions of 65wt% sulfuric acid, 65℃, and mechanical stirring in a water bath. The reaction is terminated by dilution by 10 times, centrifuged (5000rpm, 10 minutes), dialyzed (molecular weight cutoff 12000Da, deionized water is replaced until the pH value is constant), ultrasonically dispersed (1000W, 20kHz, duty cycle 1:1, 15 minutes), and freeze-dried to obtain self-made CNC dry powder.
[0062] Test results showed that the sulfate group content of the self-made CNC was 0.78 mmol / g (conductivity titration method), the aspect ratio was about 25:1 (TEM statistical average), the zeta potential was -48 mV (pH value was 8.5), the DLS hydrated particle size was 38±5 nm, and the PDI was 0.1.
[0063] Example 1: Preparation of a highly dispersed system of inorganic nanoparticles (SiO2): (1) Preparation of CNC dispersion: Take 100 mg of CNC dry powder prepared according to the above method, add it to 100 mL of deionized water, and disperse it in an ultrasonic cell disruptor (power 400 W, frequency 20 kHz, probe diameter 6 mm) for 15 minutes (2 s working / 3 s intermittent) under ice bath conditions to obtain a CNC dispersion with a concentration of 1 mg / mL. During the ultrasonic process, the temperature of the CNC dispersion is monitored in real time with a thermocouple and the temperature is controlled not to exceed 25℃.
[0064] (2) Pre-dispersion of nano-SiO2: Under magnetic stirring (200 rpm), 1.0 g of nano-SiO2 powder (original particle size 15±5 nm, specific surface area 250±30 m²) was pre-dispersed. 2 / g, hydrophilic gas phase method) added in 3 batches (to avoid local concentration surge leading to uneven CNC coating) to the CNC dispersion obtained in step (1), and continued stirring for 15 minutes to obtain CNC-nano SiO2 premixed suspension. The amount of CNC used is 10.0wt% of the mass of nano SiO2.
[0065] (3) Co-dispersion: The CNC-nano SiO2 pre-suspension obtained in step (2) was transferred to a high-speed shear homogenizer and sheared and dispersed at 12,000 rpm for 10 minutes to deaggregate the inorganic nanoparticles to the original particle size level under CNC coating; then the dispersion was transferred to an ultrasonic cell disruptor and pulsed ultrasonic treatment at 400W power for 20 minutes (2s working / 3s intermittent), and the temperature was controlled by an ice bath during the ultrasonic treatment to obtain the dispersion.
[0066] (4) pH adjustment: Use 0.1 mol / L NaOH solution to adjust the pH of the dispersion obtained in step (3) to 8.5 ± 0.2. At this time, the zeta potential of the dispersion is measured to be -42 mV.
[0067] (5) Aging: The dispersion obtained in step (4) was aged at room temperature (25±2℃) for 4 hours to obtain a highly dispersed inorganic nanoparticle system (denoted as CNC-SiO2).
[0068] (6) Performance Characterization: Dynamic light scattering (DLS) analysis showed that the average hydrated particle size of the nano-SiO2 in the inorganic nanoparticle highly dispersed system prepared in this embodiment was 38±5 nm (n=3, original particle size 15 nm), and the polydispersity index (PDI) was 0.12±0.03. After 90 days of sealed storage at room temperature, DLS analysis showed that the average hydrated particle size was 42±6 nm, and the PDI was 0.15±0.04. No visible sedimentation or stratification was observed, confirming the long-term storage stability of the inorganic nanoparticle highly dispersed system. In this embodiment, the CNC dosage was 10.0 wt% of the nano-SiO2 mass, demonstrating a denser three-dimensional network and better dispersion stability under high CNC dosage.
[0069] Example 2: Preparation of a highly dispersed system of inorganic nanoparticles (TiO2): (1) The preparation method of this embodiment is the same as that of Example 1, except that: nano-SiO2 is replaced with nano-TiO2 (anatase type, primary particle size 25±5nm, specific surface area 50±10m²). 2 / g), the amount of CNC is adjusted to 3.0wt% of the mass of nano TiO2 (that is, the mass ratio of CNC to nano TiO2 is 3:100).
[0070] (2) Performance characterization: DLS measurements showed that the average hydrated particle size of the nano-TiO2 in the inorganic nanoparticle high dispersion system prepared in this embodiment was 55±8 nm (n=3, original particle size 25 nm), and the PDI was 0.18±0.04. After 90 days of sealed storage at room temperature, the average hydrated particle size was 60±9 nm, and the PDI was 0.20±0.05, indicating good dispersion stability.
[0071] Example 3: Preparation of a highly dispersed system of inorganic nanoparticles (Al2O3): (1) The preparation method of this embodiment is the same as that of Example 1, except that: nano SiO2 is replaced with nano Al2O3 (α phase, primary particle size 30±10nm, specific surface area 40±10m²). 2 / g), the CNC dosage was adjusted to 4.0wt% of the mass of nano Al2O3. The pH of the dispersion system was adjusted to 9.0±0.2.
[0072] (2) Performance characterization: DLS measurements showed that the average hydrated particle size of Al2O3 nanoparticles in the highly dispersed inorganic nanoparticle system prepared in this embodiment was 68±10 nm (n=3, original particle size 30 nm), and the PDI was 0.20±0.05. After 90 days of sealed storage at room temperature, the average hydrated particle size was 75±12 nm, and the PDI was 0.23±0.06.
[0073] Example 4: Preparation of a highly dispersed system of inorganic nanoparticles (ZnO): (1) The preparation method of this embodiment is the same as that of Example 1, except that: nano-SiO2 is replaced with nano-ZnO (native particle size 20±5nm, specific surface area 60±10m²). 2 / g), the CNC dosage was adjusted to 3.5wt% of the nano ZnO mass. The pH of the dispersion system was adjusted to 9.5±0.2.
[0074] (2) Performance characterization: DLS measurements showed that the average hydrated particle size of the ZnO nanoparticles in the highly dispersed inorganic nanoparticle system prepared in this embodiment was 48±7 nm (n=3, original particle size 20 nm), and the PDI was 0.16±0.04. After 90 days of sealed storage at room temperature, the average hydrated particle size was 52±8 nm, and the PDI was 0.18±0.05.
[0075] Example 5: Application of superhydrophobic composite coating on the surface of engineered wood panels: (1) Coating preparation: Take 50g of the inorganic nanoparticle high dispersion system prepared in Example 1 and mix it with 100g of waterborne polyurethane resin (solid content 35wt%, pH value 8.0). The mass of nano SiO2 accounts for 1.4wt% of the resin solids in the waterborne resin. Add 0.2g of defoamer (BYK-024), 0.5g of leveling agent (BYK-333), and 0.3g of thickener (RM-8W). Stir at 800rpm for 20 minutes to mix evenly to obtain a superhydrophobic functional composite coating.
[0076] (2) Substrate pretreatment: Select commercially available E1 grade particleboard (300mm×300mm×18mm), sand the surface with 240 mesh sander belt, and blow away surface dust with compressed air.
[0077] (3) Spray the primer layer, using industrial conventional sealing primer.
[0078] (4) Coating and curing: The superhydrophobic functional composite coating was uniformly sprayed onto the particleboard surface using air spraying, with the wet film thickness controlled at 120±20μm. After surface drying at room temperature for 20 minutes, it was transferred to a forced-air drying oven and heated and cured at 100℃ for 30 minutes. After curing, it was cooled to room temperature to obtain the superhydrophobic functional composite coating.
[0079] (5) Structural characterization: Figure 2 A schematic cross-sectional view of the multi-layer structure of the functional composite coating applied to the surface of a wood-based panel is shown. From bottom to top, the figure displays a four-layer gradient structure: the wood-based panel, a base coat, a CNC-inorganic nanoparticle composite functional layer, and a superhydrophobic protective layer. The base coat is a conventional sealing primer layer, optional in industrial coating depending on the substrate. The CNC-nanoparticle composite functional layer is the main functional layer of the functional composite coating of this invention. The superhydrophobic protective layer is a surface functional area formed by the moderate enrichment of inorganic nanoparticles on the coating surface during the curing process of the functional composite coating. The surface of the superhydrophobic protective layer has micro-nano rough protrusions (protrusion height 0.08~0.25 μm) to construct a lotus leaf-like micro-rough structure, achieving the superhydrophobic effect.
[0080] (6) Performance characterization (n=3): Water contact angle (CA) of the coating surface: 158.3±2.5° (superhydrophobic grade); roll-off angle (SA): 6.5±1.5°. In 100 consecutive water contact angle measurements, CA remained above 155°.
[0081] Taber abrasion test (GB / T 17657-2022, CS-10 grinding wheel, 500g load, 500 rpm): mass loss is 12.3±1.5mg; under the same conditions, the mass loss of pure water-based polyurethane coating is 28.7±2.1mg, and the abrasion resistance is improved by about 57%.
[0082] Cross-cut adhesion test (GB / T 9286-2021): Grade 0, no coating peeling.
[0083] Pencil hardness (GB / T 6739-2022): 4H.
[0084] Ultraviolet aging test (QUV, 340nm, 0.89W / m) 2 (60℃, 1000 hours): Coating color difference ΔE=2.8±0.4, no obvious yellowing, excellent weather resistance.
[0085] Water resistance: After immersion in deionized water at 25℃ for 48 hours, the coating showed no blistering, peeling, or discoloration.
[0086] Example 6: Application of surface wear-resistant composite coating on the surface of engineered wood panels: (1) The preparation method of this embodiment is the same as that of Example 5, except that the inorganic nanoparticle high dispersion system prepared in Example 1 is replaced with the inorganic nanoparticle high dispersion system prepared in Example 2, and the nano TiO2 accounts for 3.0 wt% of the resin solids in the waterborne resin. The waterborne resin is waterborne acrylic resin (solid content 40 wt%).
[0087] (2) Performance characterization (n=3): Water contact angle (CA) of the coating surface: 148.7±3.0°, which is close to the superhydrophobic level.
[0088] Taber abrasion test (GB / T 17657-2022, CS-10 grinding wheel, 500g load, 500 rpm): mass loss is 8.7±1.2mg, indicating excellent abrasion resistance.
[0089] Pencil hardness: 5H.
[0090] Ultraviolet aging test (QUV, 340nm, 0.89W / m) 2 (60℃, 1000 hours): Coating color difference ΔE=3.2±0.5, no obvious yellowing, excellent weather resistance.
[0091] Example 7: Preparation of a highly dispersed system of inorganic nanoparticles (SiO2): (1) The preparation method of this embodiment is the same as that of Example 1, except that the amount of CNC used is 3.0wt% of the mass of nano SiO2 (i.e., 30mg of CNC dry powder).
[0092] (2) Performance characterization: DLS analysis showed that the average hydrated particle size of nano-SiO2 in the inorganic nanoparticle high dispersion system prepared in this embodiment was 40±6 nm (n=3, original particle size 15 nm), and the polydispersity index (PDI) was 0.15±0.04. After 90 days of sealed storage at room temperature, DLS analysis showed that the average hydrated particle size was 46±7 nm, the PDI was 0.19±0.05, and there was no visible sedimentation or stratification. After preparing a functional composite coating using the inorganic nanoparticle high dispersion system of this embodiment according to the coating process of Example 5, the water contact angle of the functional composite coating was measured to be 153.2±3.1°, and the mass loss in the Taber abrasion test (GB / T 17657-2022, CS-10 grinding wheel, 500g load, 500 rpm) was 14.8±1.8 mg. The above results demonstrate that even at a low to medium CNC dosage of 3.0 wt%, the three-dimensional permeation network constructed in this invention can still effectively achieve spatial isolation and dispersion of inorganic nanoparticles. The dispersion system maintains long-term storage stability for more than 90 days, and the functional composite coating exhibits both excellent superhydrophobicity and wear resistance. The relationship between CNC dosage and performance is as follows: Figure 4 As shown.
[0093] Comparative Example 1: The preparation method of this comparative example is the same as that of Example 1, except that: no CNC is added, 1.0g of nano SiO2 powder is directly added to 100mL of deionized water, and the same high-speed shearing and ultrasonic treatment as in Example 1 are performed in sequence, and the same pH value is adjusted and aged to obtain a nano SiO2 aqueous dispersion without CNC.
[0094] Comparative Example 2: The preparation method of this comparative example is the same as that of comparative example 1, except that: the nano-SiO2 is modified with silane coupling agent KH-560 in the nano-SiO2 aqueous dispersion (the amount of KH-560 is 5wt% of the mass of nano-SiO2).
[0095] Comparative Example 3: The preparation method of this comparative example is the same as that of comparative example 1, except that sodium polyacrylate (PAAS) is used to disperse the nano-SiO2 in the nano-SiO2 aqueous dispersion (the amount of PAAS is 3wt% of the mass of nano-SiO2).
[0096] Test Example 1: Dispersion Stability and Coating Performance The dispersion stability of the inorganic nanoparticle highly dispersed systems prepared in Example 1 and Comparative Examples 1-3 was tested (n=3), and the results are shown in Table 1.
[0097] Table 1. Dispersion stability test results of Example 1 and Comparative Examples 1-3:
[0098] As can be seen from Table 1, the inorganic nanoparticle high dispersion system prepared by the present invention has better dispersion uniformity and dispersion stability, and can maintain a stable dispersion state for a long time.
[0099] Test Example 2: The performance of the functional composite coatings of Examples 5 and 6 and the pure resin (PU) coatings was compared (n=3), with comparative examples 1-3 used as controls to compare the water contact angles. The results are shown in Table 2 and... Figure 4 As shown.
[0100] Table 2 Surface properties of Examples 5-6 and pure resin coatings:
[0101] According to Tables 1 and 2, and Figure 4 It can be seen that after introducing a CNC-controlled inorganic nanoparticle high dispersion system, the functional composite coating has achieved significant improvements in key indicators such as superhydrophobicity (CA can reach more than 150°), wear resistance (wear loss is reduced by more than 50%), hardness and weather resistance, and is significantly better than the pure resin coating without inorganic nanoparticles.
[0102] Test Example 3: Crosslinking density and dynamic mechanical properties of coating interface: Dynamic mechanical analysis (DMA, heating rate of 5℃ / min, frequency of 1Hz, temperature range of -20~120℃) was performed on the functional composite coating and pure water polyurethane coating prepared in Example 5 (n=3).
[0103] Test results show that above the glass transition temperature (T g In the +30℃ range, the storage modulus (E') of the pure water-based polyurethane coating decreased by -72%, while the storage modulus of the functional composite coating in Example 5 decreased by -38%. The difference between the two indicates that after the introduction of CNC regulation, CNC formed physical cross-links between inorganic nanoparticles and resin matrix through the action of "bridge molecules". The interfacial cross-linking density of the functional composite coating was significantly improved, which is consistent with the analysis of the aforementioned mechanism three.
[0104] As can be seen from the above embodiments, the present invention has achieved the following beneficial effects: (1) Triple synergistic dispersion mechanism: This invention proposes and realizes for the first time a triple synergistic dispersion mechanism using CNC as a multifunctional dispersion regulator—hydrogen bond steric hindrance effect (mechanism 1), three-dimensional network spatial isolation (mechanism 2), and bridging molecular interface enhancement (mechanism 3). The three mechanisms work together and complement each other, effectively solving the three key technical problems of easy aggregation of inorganic nanoparticles in aqueous systems, poor interfacial compatibility with organic resin matrix, and easy sedimentation during coating curing, thus realizing the whole-chain regulation of "dispersion-compatibility-stability".
[0105] (2) Green and environmentally friendly: CNC is derived from natural cellulose (such as wood, cotton, linen, straw, etc.), which has the outstanding advantages of being renewable, biodegradable, and non-toxic. The entire preparation process uses water as the only dispersion medium and does not use any organic solvents or toxic and harmful chemicals, which fully conforms to the industrial development trend of green manufacturing and sustainable development.
[0106] (3) Excellent long-term storage stability: The inorganic nanoparticle high dispersion system can maintain a uniform dispersion state for more than 90 days under sealed storage conditions at room temperature, with no visible sedimentation or stratification, which is far superior to the system obtained by traditional ultrasonic or high-speed shear dispersion methods (which usually result in significant sedimentation within 24 hours). This excellent storage stability provides a reliable material guarantee for the industrial continuous coating production of wood-based panels.
[0107] (4) Significantly improved coating performance: The functional composite coating prepared by this invention has a surface water contact angle of over 150° (superhydrophobic or near-superhydrophobic). The mass loss of the coating in the Taber abrasion test (GB / T 17657-2022, CS-10 grinding wheel, 500g load) is reduced by more than 50% compared with the pure resin coating without inorganic nanoparticles. At the same time, the adhesion between the functional composite coating and the substrate (cross-cut test) reaches level 0-1, and the pencil hardness reaches 4H-5H.
[0108] (5) Wide applicability: The inorganic nanoparticle high dispersion system provided by the present invention is applicable to a variety of inorganic nanoparticles, a variety of water-based resin matrices (polyurethane, acrylic, melamine-formaldehyde resin, etc.) and a variety of artificial board substrates (particleboard, fiberboard, plywood, etc.), and has good versatility and scalability.
[0109] (6) Simple process and low cost: The entire preparation process only requires conventional ultrasonic dispersion and high-speed shearing equipment. The operation steps are simple and the process conditions are mild (room temperature ~ 120℃). No special equipment or extreme conditions are required. It is particularly suitable for direct grafting and upgrading of existing production lines in the wood-based panel industry, and has significant technical and economic advantages.
[0110] Currently, the common approach to addressing the aggregation problem of inorganic nanoparticles in aqueous systems involves selecting a single-mechanism dispersion method—either covalently modifying the surface of inorganic nanoparticles through chemical coupling (such as silane coupling agents) or increasing the repulsion energy between inorganic nanoparticles through electrostatic repulsion (such as polyelectrolyte dispersants). However, this approach struggles to simultaneously address the requirements of dispersion stability, interfacial compatibility, and resistance to migration and sedimentation. Furthermore, reports on using CNC—traditionally considered a biomass nanomaterial that reinforces fillers or creates pores—as a multifunctional dispersion regulator are rare. This invention utilizes CNC simultaneously as a steric hindrance agent, a three-dimensional network builder, and an interfacial bridging agent, providing a new approach to solving the aforementioned problems. (a) In common knowledge, CNCs typically function as mechanical reinforcing phases or pore-forming templates in composite materials, and their concept as a "multifunctional dispersant" has not been reported prior to this invention. This invention utilizes the rod-like morphology and surface hydroxyl groups of CNCs to simultaneously achieve the triple functions of dispersion, stabilization, and interfacial reinforcement in the same system.
[0111] (b) This invention uses CNC as a dispersing agent and unexpectedly discovered that CNC can form a sufficiently dense hydrogen bond anchoring layer (5-20 nm thick steric hindrance layer) on the surface of inorganic nanoparticles, while simultaneously self-assembling in aqueous media to form a permeation network (50-200 nm pore size) that runs through the system, and continues to exert a bridging effect after the functional composite coating has cured. The synergistic operation of these three mechanisms depends on the precise matching of multiple parameters such as CNC dosage, nanoparticle type, particle size, and pH conditions, and cannot be obtained through simple trial and error.
[0112] (c) The test data (Tables 1 and 2) objectively demonstrate that the technical effect produced by the synergistic operation of the three mechanisms of this invention significantly surpasses any single-mechanism dispersion scheme. Comparative Example 2 (silane coupling agent method, single chemical coupling mechanism) and Comparative Example 3 (sodium polyacrylate method, single electrostatic / steric hindrance mechanism) showed a significant increase in particle size after 7 days (Comparative Example 2 reached 120±25nm, Comparative Example 3 reached 95±18nm), and both showed obvious sedimentation after 90 days, far inferior to this invention (uniform dispersion after ≥90 days). The above test data indicate that the beneficial effects of this invention depend on the combined effect of the above mechanisms, rather than being contributed by a single known mechanism, strongly demonstrating the synergistic effect among the three mechanisms.
[0113] The embodiments of the present invention have been described above; however, these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. All other embodiments obtained by those skilled in the art based on the above embodiments of the present invention without inventive effort are within the protection scope of the present invention.
Claims
1. A method for preparing a highly dispersed inorganic nanoparticle system, characterized in that, Includes the following steps: (1) Mix cellulose nanocrystals with water to obtain a cellulose nanocrystal dispersion; (2) The cellulose nanocrystal dispersion and inorganic nanoparticles were mixed, sheared and sonicated, the pH value was adjusted to 7-10, and aged to obtain a highly dispersed inorganic nanoparticle system. The surface sulfonate group content of cellulose nanocrystals is 0.5~1.5 mmol / g, and the surface hydroxyl number density is 3~5 / nm. 2 The length is 100~500nm, the diameter is 5~20nm, and the aspect ratio is 5~100:
1.
2. The method for preparing the highly dispersed inorganic nanoparticle system according to claim 1, characterized in that, In step (1), the mixing is carried out under temperature control, and the temperature does not exceed 30°C; the mixing method is pulsed ultrasonic dispersion; the power of pulsed ultrasonic dispersion is 400~1200W, the frequency is 20~25kHz, the duty cycle is 1:1~1:3; the mixing time is 10~30 minutes.
3. The method for preparing the highly dispersed inorganic nanoparticle system according to claim 1, characterized in that, The concentration of cellulose nanocrystals in the cellulose nanocrystal dispersion is 1~10 mg / mL.
4. The method for preparing the highly dispersed inorganic nanoparticle system according to claim 1, characterized in that, Inorganic nanoparticles include one or more of nano-SiO2, nano-TiO2, nano-Al2O3, and nano-ZnO; the original particle size of inorganic nanoparticles is 5~50nm.
5. The method for preparing the highly dispersed inorganic nanoparticle system according to claim 1, characterized in that, The mass ratio of cellulose nanocrystals to inorganic nanoparticles is 0.5~10:
100.
6. The method for preparing the highly dispersed inorganic nanoparticle system according to claim 1, characterized in that, Shearing ultrasound involves sequential shearing and ultrasound; the shearing speed is 8000~15000rpm, and the time is 5~15 minutes; the ultrasound power is 200~600W, the mode is pulse ultrasound, the working mode is 2s working followed by 3s interval, and the time is 10~30 minutes; the ultrasound is performed under temperature control, and the temperature control temperature does not exceed 30℃.
7. A highly dispersed inorganic nanoparticle system, characterized in that, The preparation method described in any one of claims 1 to 6 is used to prepare the product, which comprises cellulose nanocrystals, inorganic nanoparticles, and water. The cellulose nanocrystals form a steric hindrance layer anchored by hydrogen bonds on the surface of the inorganic nanoparticles and construct a three-dimensional permeable network structure in an aqueous medium. The pore size of the three-dimensional permeable network structure is 50 to 200 nm, and the inorganic nanoparticles are isolated and dispersed in the pore units of the three-dimensional permeable network structure. The zeta potential of the highly dispersed inorganic nanoparticle system is -30 to -50 mV when measured at a pH of 7 to 10.
8. The application of a highly dispersed inorganic nanoparticle system in the field of surface modification of engineered wood panels, characterized in that, The inorganic nanoparticle highly dispersed system is the inorganic nanoparticle highly dispersed system as described in claim 7.
9. The application according to claim 8, characterized in that, The application method includes the following steps: mixing an inorganic nanoparticle highly dispersed system with an aqueous resin and additives to obtain a functional composite coating; then coating the functional composite coating onto the surface of a wood-based panel substrate and curing it to obtain a functional composite coating layer.
Citation Information
Patent Citations
Method for modifying waterborne wood coating by nano-crystalline cellulose hybridizing inorganic nanoparticles
CN105670514A
Preparation method of graphene / nanocrystalline cellulose water-phase dispersion solution