Sublimation transfer film, its preparation process, and coating slurry

By using a coating slurry composed of polyvinyl alcohol and nanofillers in the thermal sublimation transfer film to form a borate ester crosslinking structure, the problems of pattern distortion and edge blurring on 3D curved surfaces of the thermal sublimation paper coating are solved, achieving a transfer effect with high rigidity and high thermal stability.

CN123063014APending Publication Date: 2026-11-10QINGYI (FUJIAN) HEAT TRANSFER SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611280352.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-22
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

When existing thermal sublimation paper coatings are made of polyvinyl alcohol as the film material, they are mostly designed for flat transfer printing. When used on rigid 3D curved surfaces, the substrate is prone to stretching or wrinkling during vacuum forming, which causes the coating and ink layer to deform, resulting in phenomena such as pattern distortion and blurred edges.

Method used

A coating slurry containing polyvinyl alcohol, nanofillers, crosslinking agents, catalysts, viscosity modifiers, leveling agents, and defoamers is used to improve the rigidity and thermal stability of the film and reduce the pattern deformation rate by forming a borate ester crosslinking structure and nanofiller composite regulation.

Benefits of technology

It significantly improves the fidelity and aesthetics of graphic reproduction, reduces the distortion rate of the transferred pattern, and enhances the clarity and beauty of the pattern.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The thermal sublimation transfer film, its preparation process, and coating slurry belong to the field of thermal transfer technology. It includes a substrate and a coating on the substrate surface. The coating uses the coating slurry of the thermal sublimation transfer film. Polyvinyl alcohol (PVA) molecular chains contain a large number of hydroxyl groups. Boron atoms in borate ester compounds can coordinate with hydroxyl groups to form a borate ester crosslinking structure, connecting linear PVA molecular chains into a three-dimensional network structure. This significantly improves the rigidity, strength, and thermal stability of the film. Furthermore, through the composite regulation of deformation using nanofillers, the deformation rate of the transferred pattern is reduced, significantly improving the graphic fidelity and aesthetics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a thermal sublimation transfer film, its preparation process, and coating paste, belonging to the field of thermal transfer technology. Background Technology

[0002] Dye sublimation transfer technology is widely used in the field of personalized customization due to its advantages such as bright colors and strong adhesion. In the transfer of 3D curved products (such as mobile phone cases), a film with a pattern is wrapped on the surface of the substrate through vacuum forming process to achieve three-dimensional transfer of multiple curved surfaces.

[0003] Existing thermal sublimation paper coatings, which use polyvinyl alcohol as the film material, are mostly designed for flat transfer printing. When used on 3D curved surfaces of rigid substrates, the substrate is prone to stretching or wrinkling during vacuum forming, causing the coating and ink layer to deform accordingly, resulting in phenomena such as pattern distortion and blurred edges. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the present invention aims to provide a thermal sublimation transfer film, its preparation process, and coating slurry. This addresses the problem that existing thermal sublimation paper coatings, made of polyvinyl alcohol, are primarily designed for planar transfers. When used on rigid 3D curved surfaces, the substrate is prone to stretching or wrinkling during vacuum forming, causing deformation of the coating and ink layer, resulting in distorted patterns and blurred edges.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solution: a coating paste for a thermal sublimation transfer film, comprising the following parts by weight: 6-10 parts of polyvinyl alcohol; 70-90 parts deionized water; 1-3 parts of nanofiller; Dispersant 0.05-0.3 parts; Crosslinking agent 0.5-4 parts; Catalyst 0.05-0.4 parts; 3-6 parts viscosity modifier; Leveling agent 0.1-1 part; 0.2-0.8 parts of defoamer.

[0006] Furthermore, the substrate is amorphous polyethylene terephthalate or ethylene glycol-modified polyethylene terephthalate.

[0007] Furthermore, the nanofiller is one or more of nano-silica, nano-calcium carbonate, and nano-cellulose.

[0008] Furthermore, the dispersant is polyvinylpyrrolidone.

[0009] Furthermore, the crosslinking agent is one or more of phenylborane pinacol ester, methacrylate borate ester, and trimethoxyboronate ester.

[0010] Furthermore, the catalyst is one or more of acetic acid, citric acid, dilute hydrochloric acid, and potassium persulfate.

[0011] Furthermore, the viscosity modifier is N-methylpyrrolidone.

[0012] Furthermore, the leveling agent is one or more of polyether-modified acrylate, polyether-modified polydimethylsiloxane, and acrylate-methacrylate.

[0013] A thermal sublimation transfer film includes a substrate and a coating on the surface of the substrate, wherein the coating is made using the coating paste of the thermal sublimation transfer film.

[0014] A process for preparing the aforementioned thermal sublimation transfer film includes the following steps: Step S1: Take polyvinyl alcohol and deionized water and stir under heating until the polyvinyl alcohol is completely dissolved. Cool, then add a catalyst and adjust the pH of the solution to 3-6. Then add a crosslinking agent, heat and stir to allow it to react fully and obtain a mixed solution. Step S2: Mix the nanofiller with the dispersant and deionized water to obtain a nanofiller slurry; Step S3: Slowly add the nanofiller slurry from step S2 to the mixed solution from step S1, stir and mix, and then add a viscosity modifier to adjust the viscosity to 2000-3000 mPa·s. Step S4: Add leveling agent and defoamer, and continue stirring until uniform to obtain coating slurry; Step S5: Apply the coating paste from step S4 onto the substrate and dry it to obtain a thermal sublimation transfer film.

[0015] The beneficial effects of this invention are: the polyvinyl alcohol molecular chain contains a large number of hydroxyl groups, and the boron atoms in the borate ester compound can undergo coordination reaction with the hydroxyl groups to form a borate ester cross-linked structure, which connects the linear polyvinyl alcohol molecular chain into a three-dimensional network structure, thereby significantly improving the rigidity, strength and thermal stability of the film. Furthermore, when the deformation is controlled by the composite of nanofillers, the deformation rate of the transferred pattern is reduced, and the graphic reproduction and aesthetics are significantly improved. Detailed Implementation

[0016] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.

[0017] This invention provides a thermal sublimation transfer film, its preparation process, and a coating slurry technical solution: The coating slurry for the thermal sublimation transfer film comprises the following parts by weight: 6-10 parts of polyvinyl alcohol; 70-90 parts deionized water; 1-3 parts of nanofiller; Dispersant 0.05-0.3 parts; Crosslinking agent 0.5-4 parts; Catalyst 0.05-0.4 parts; 3-6 parts viscosity modifier; Leveling agent 0.1-1 part; 0.2-0.8 parts of defoamer.

[0018] According to some embodiments of this application, optionally, the substrate is amorphous polyethylene terephthalate or ethylene glycol-modified polyethylene terephthalate, and the substrate thickness is 0.2-0.3 mm.

[0019] According to some embodiments of this application, optionally, the nanofiller is one or more of nano-silica, nano-calcium carbonate, and nano-cellulose, and the particle size of the nanofiller is 20-100 nm.

[0020] According to some embodiments of this application, optionally, the dispersant is polyvinylpyrrolidone.

[0021] According to some embodiments of this application, optionally, the crosslinking agent is one or more of phenylborane ester, borate methacrylate, and trimethoxyborane ester.

[0022] According to some embodiments of this application, optionally, the catalyst is one or more of acetic acid, citric acid, dilute hydrochloric acid, and potassium persulfate.

[0023] According to some embodiments of this application, optionally, the viscosity modifier is N-methylpyrrolidone.

[0024] According to some embodiments of this application, optionally, the leveling agent is one or more of polyether-modified acrylate, polyether-modified polydimethylsiloxane, and acrylate-methacrylate.

[0025] According to some embodiments of this application, optionally, the defoamer is one or more of polyethylene glycol-polypropylene glycol block copolymer and methacrylate-styrene copolymer.

[0026] A thermal sublimation transfer film includes a substrate and a coating on the surface of the substrate, wherein the coating is made using the coating paste of the thermal sublimation transfer film.

[0027] A process for preparing the aforementioned thermal sublimation transfer film includes the following steps: Step S1: Take polyvinyl alcohol and deionized water and stir under heating until the polyvinyl alcohol is completely dissolved. Cool, then add a catalyst and adjust the pH of the solution to 3-6. Then add a crosslinking agent, heat and stir to allow it to react fully and obtain a mixed solution. Step S2: Mix the nanofiller with the dispersant and deionized water to obtain a nanofiller slurry; Step S3: Slowly add the nanofiller slurry from step S2 to the mixed solution from step S1, stir and mix, and then add a viscosity modifier to adjust the viscosity to 2000-3000 mPa·s. Step S4: Add leveling agent and defoamer, and continue stirring until uniform to obtain coating slurry; Step S5: Apply the coating paste from step S4 onto the substrate and dry it to obtain a thermal sublimation transfer film.

[0028] Polyvinyl alcohol (PVA) molecules contain a large number of hydroxyl groups. Boron atoms in borate esters can coordinate with hydroxyl groups to form a borate ester crosslinking structure, which connects linear PVA molecules into a three-dimensional network structure. This significantly improves the rigidity, strength, and thermal stability of the film. Furthermore, when deformation is controlled by the composite of nanofillers, the deformation rate of the transferred pattern is reduced, significantly improving the fidelity and aesthetics of the pattern. Example 1

[0029] For the sake of brevity, the parts that are the same as those in other embodiments will not be described again. The main focus here is on the structure that differs from other embodiments of the present invention. The substrate is polyethylene terephthalate. In the specific preparation of the coating, the material composition by weight is as follows: 8 parts polyvinyl alcohol; 90 parts deionized water; 2 parts nanofiller; 0.2 parts polyvinylpyrrolidone; 2 parts crosslinking agent; 0.2 parts catalyst; 4 parts N-methylpyrrolidone; 0.5 parts leveling agent; and 0.5 parts defoamer.

[0030] The polyethylene terephthalate has a thickness of 0.2 mm; the nanofiller is nano-silica with a particle size of 20 nm; the crosslinking agent is pinacol phenylborate; the catalyst is dilute hydrochloric acid with a concentration of 10%; the leveling agent is acrylate-methacrylate; and the defoamer is methacrylate-styrene copolymer.

[0031] A process for preparing the aforementioned thermal sublimation transfer film includes the following steps: Step S1: Take two preparation containers. First, put 70 parts of deionized water and 8 parts of polyvinyl alcohol into the reaction vessel and heat it to 87°C. Then, pour the mixture into one of the preparation containers and stir for 3 hours until the polyvinyl alcohol is completely dissolved. Cool it to room temperature, then add 0.2 parts of 10% dilute hydrochloric acid to adjust the pH of the solution to about 4. Then, slowly add 2 parts of pinacol phenylboronic acid ester. Heat the mixture to 40°C and stir for 2 hours to allow it to react fully. Cool it to room temperature to obtain the mixed solution. Step S2: In another preparation container, mix 2 parts of nano silica with the dispersant polyvinylpyrrolidone, add the remaining deionized water, and stir at 1400 rpm for 60 minutes to disperse the nano silica and obtain nano silica slurry. Step S3: Slowly add the dispersed nano-silica slurry to the mixed solution in step S1, and stir at a stirring speed of 1300 rpm for 1 hour to ensure that the two are fully mixed. Then add 4 parts of N-methylpyrrolidone to adjust the viscosity of the solution to about 2500 mPa·s. Step S4: Add 0.5 parts of acrylate-methacrylate and 0.5 parts of methacrylate-styrene copolymer in sequence, and stir continuously at 500 rpm for 60 minutes until uniform to obtain the coating slurry; Step S5: Apply the coating slurry from step S4 onto the substrate with a coating amount of 80 g / m² and a drying temperature of 70°C to obtain a thermal sublimation transfer film that can be used on rigid substrates. Example 2

[0032] For the sake of brevity, the parts that are the same as those in other embodiments will not be repeated. The main focus here is on the structure that differs from other embodiments of the present invention. The substrate is ethylene glycol modified polyethylene terephthalate. In the specific preparation of the coating, the material composition by weight is as follows: 7 parts polyvinyl alcohol; 70 parts deionized water; 1.5 parts nanofiller; 0.15 parts dispersant; 2 parts crosslinking agent; 0.12 parts catalyst; 2 parts N-methylpyrrolidone; 0.5 parts leveling agent; and 0.4 parts defoamer.

[0033] The polyethylene terephthalate has a thickness of 0.2 mm; the nanofiller is nano-silica with a particle size of 20 nm; the crosslinking agent is borate methacrylate; the catalyst is potassium persulfate; the leveling agent is polyether-modified acrylate; and the defoamer is polyethylene glycol-polypropylene glycol block copolymer.

[0034] A process for preparing the aforementioned thermal sublimation transfer film includes the following steps: Step S1: Take two preparation containers. First, put 55 parts of deionized water and 7 parts of polyvinyl alcohol into the reaction vessel and heat it to 85°C. Then, pour the mixture into one of the preparation containers and stir for 3 hours until the polyvinyl alcohol is completely dissolved. Cool to room temperature, then add 0.12 parts of potassium persulfate and slowly add 2 parts of pinacol phenylboronic acid ester. Heat the mixture to 50°C and stir for 2 hours to allow it to react fully. Cool to room temperature to obtain a mixed solution. Step S2: In another preparation container, 1.5 parts of nano silica are mixed with the dispersant polyvinylpyrrolidone, the remaining deionized water is added, and the mixture is stirred at 1500 rpm for 60 minutes to disperse the nano silica and obtain nano silica slurry. Step S3: Slowly add the dispersed nano-silica slurry to the mixed solution in step S1, and stir at a stirring speed of 1300 rpm for 1 hour to ensure thorough mixing; then add 2 parts of N-methylpyrrolidone to adjust the viscosity of the solution to about 2600 mPa·s. In step S4, 0.5 parts of polyether-modified acrylate and 0.5 parts of polyethylene glycol-polypropylene glycol block copolymer are added sequentially, and the mixture is stirred continuously at 500 rpm for 60 minutes until homogeneous to obtain the coating slurry. Step S5: Apply the coating slurry from step S4 onto the substrate with a coating amount of 82 g / m² and a drying temperature of 70°C to obtain a thermal sublimation transfer film that can be used on rigid substrates. Example 3

[0035] For the sake of brevity, the parts that are the same as those in other embodiments will not be repeated. The main focus here is on the structure that differs from other embodiments of the present invention. The substrate is polyethylene terephthalate. In the specific preparation of the coating, the material composition by weight is: 9 parts polyvinyl alcohol; 90 parts deionized water; 2 parts nanofiller; 0.2 parts dispersant; 2 parts crosslinking agent; 0.2 parts catalyst; 5 parts N-methylpyrrolidone; 0.6 parts leveling agent; and 0.5 parts defoamer. The polyethylene terephthalate has a thickness of 0.2 mm; the nanofiller is nano-silica with a particle size of 20 nm; the crosslinking agent is trimethoxyboronic acid ester; the catalyst is acetic acid; the leveling agent is polyether-modified acrylate; and the defoamer is polyethylene glycol-polypropylene glycol block copolymer.

[0036] A process for preparing the aforementioned thermal sublimation transfer film includes the following steps: Step S1: Take two preparation containers. First, put 70 parts of deionized water and 9 parts of polyvinyl alcohol into the reaction vessel and heat it to 85°C. Then, pour the mixture into one of the preparation containers and stir for 3 hours until the polyvinyl alcohol is completely dissolved. Cool to room temperature, then add 0.2 parts of acetic acid and slowly add 2 parts of trimethoxyboronic acid ester. Heat the mixture to 50°C and stir for 2 hours to allow it to react fully. Cool to room temperature to obtain a mixed solution. Step S2: In another preparation container, mix 2 parts of nano silica with the dispersant polyvinylpyrrolidone, add the remaining deionized water, and stir at 1500 rpm for 60 minutes to disperse the nano silica and obtain nano silica slurry. Step S3: Slowly add the dispersed nano-silica slurry to the mixed solution in step S1, and stir at a stirring speed of 1300 rpm for 1 hour to ensure thorough mixing; then add 5 parts of N-methylpyrrolidone to adjust the viscosity of the solution to about 2600 mPa·s. In step S4, 0.6 parts of polyether-modified acrylate and 0.5 parts of polyethylene glycol-polypropylene glycol block copolymer are added sequentially, and the mixture is stirred continuously at 500 rpm for 60 minutes until homogeneous to obtain the coating slurry. Step S5: Apply the coating slurry from step S4 onto the substrate with a coating amount of 82 g / m² and a drying temperature of 70°C to obtain a thermal sublimation transfer film that can be used on rigid substrates.

[0037] Comparative Example 1 For the sake of brevity, the parts that are the same as in Example 1 will not be repeated. The main focus here is on the structure that is different from that in Example 1, where the crosslinking agent is tripropylene glycol diacrylate.

[0038] Test methods for thermal sublimation transfer films Comparing the formulations without crosslinking agent, with a non-crosslinking agent of the present invention, and with a crosslinking agent of the present invention, lines of 1 pound, 2 pounds, and 3 pounds were printed on the three coatings respectively. The ratio of the difference in actual line width before and after transfer to the line width before transfer is the deformation rate of the pattern. The calculation formula is: ; In the formula: D represents the pattern transfer deformation rate; This refers to the line width on the substrate after transfer. This represents the actual line width on the coating surface before transfer. The comparison data before and after the coating formulation improvement are shown in Table 1 below. According to the test calculation, the deformation rate is greatly reduced after the coating improvement, and there is almost no change based on visual observation. Table 1

[0039] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered illustrative and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No markings in the claims should be construed as limiting the scope of the claims.

[0040] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A coating paste for a thermal sublimation transfer film, characterized in that, Includes the following weight parts: 6-10 parts of polyvinyl alcohol; 70-90 parts deionized water; 1-3 parts of nanofiller; Dispersant 0.05-0.3 parts; Crosslinking agent 0.5-4 parts; Catalyst 0.05-0.4 parts; 3-6 parts viscosity modifier; Leveling agent 0.1-1 part; 0.2-0.8 parts of defoamer.

2. The coating paste for the thermal sublimation transfer film according to claim 1, characterized in that: The nanofiller is one or more of nano-silica, nano-calcium carbonate, and nano-cellulose.

3. The coating paste for the thermal sublimation transfer film according to claim 1, characterized in that: The dispersant is polyvinylpyrrolidone.

4. The coating paste for the thermal sublimation transfer film according to claim 1, characterized in that: The crosslinking agent is one or more of phenylborane pinacol ester, methacrylate borate ester, and trimethoxyboronate.

5. The coating paste for the thermal sublimation transfer film according to claim 1, characterized in that: The catalyst is one or more of acetic acid, citric acid, dilute hydrochloric acid, and potassium persulfate.

6. The coating paste for the thermal sublimation transfer film according to claim 1, characterized in that: The viscosity modifier is N-methylpyrrolidone.

7. The coating paste for the thermal sublimation transfer film according to claim 1, characterized in that: The leveling agent is one or more of polyether-modified acrylate, polyether-modified polydimethylsiloxane, and acrylate-methacrylate.

8. A thermal sublimation transfer film, characterized in that: It includes a substrate and a coating on the surface of the substrate, said coating being a coating paste of a thermal sublimation transfer film as described in any one of claims 1 to 7.

9. The thermal sublimation transfer film according to claim 8, characterized in that: The substrate is amorphous polyethylene terephthalate or ethylene glycol-modified polyethylene terephthalate.

10. A process for preparing a thermal sublimation transfer film as described in claim 8, characterized in that, Includes the following steps: Step S1: Take polyvinyl alcohol and deionized water and stir under heating until the polyvinyl alcohol is completely dissolved. Cool, then add a catalyst and adjust the pH of the solution to 3-6. Then add a crosslinking agent, heat and stir to allow it to react fully and obtain a mixed solution. Step S2: Mix the nanofiller with the dispersant and deionized water to obtain a nanofiller slurry; Step S3: Slowly add the nanofiller slurry from step S2 to the mixed solution from step S1, stir and mix, and then add a viscosity modifier to adjust the viscosity to 2000-3000 mPa·s. Step S4: Add leveling agent and defoamer, and continue stirring until uniform to obtain coating slurry; Step S5: Apply the coating paste from step S4 onto the substrate and dry it to obtain a thermal sublimation transfer film.