A passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment and its construction method

By using a composite structure consisting of a substrate bonding layer, a spectral functional layer, and a surface protective layer, the adhesion and weather resistance issues of passive radiation cooling coatings on outdoor high-temperature equipment are solved, achieving efficient and low-energy all-weather cooling effects. It is adaptable to various substrate materials and environments, improving the stability and application range of the coating.

CN123063016APending Publication Date: 2026-11-10FUJIAN ZHANGPING XINCHUANG ROBOT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611272945.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing passive radiation cooling coatings have poor adhesion and insufficient weather resistance on outdoor high-temperature equipment, poor mass production stability, and traditional cooling methods are energy-intensive or cause substrate corrosion. Glass insulation products cannot achieve both light transmittance and cooling effect.

Method used

It adopts a three-layer composite structure consisting of a substrate bonding layer, a spectral functional layer, and a surface protective layer. Each layer is responsible for interface bonding, spectral modulation, and weather protection, respectively. The coating design has standardized raw material ratios and preparation processes, adapting to various substrates and environments, and achieving high reflectivity and high infrared emissivity.

Benefits of technology

It improves the durability and cooling effect of the coating, reduces energy consumption, broadens the application scenarios, adapts to a variety of substrate materials, and is easy to apply, meeting the needs of industrial energy conservation and dual-carbon development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063016A_ABST
    Figure CN123063016A_ABST
Patent Text Reader

Abstract

This invention relates to the field of passive radiation cooling materials and industrial protective coating technology. It discloses a passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment, comprising a substrate bonding layer, a spectral functional layer, and a surface protective layer stacked sequentially. The dry film thickness of the substrate bonding layer is 10 μm to 25 μm, the dry film thickness of the spectral functional layer is 20 μm to 80 μm, and the dry film thickness of the surface protective layer is 10 μm to 25 μm. This invention features a three-layer functionally decoupled coating system that works collaboratively to solve the problems of performance imbalance, poor adhesion, and easy aging, chalking, and degradation associated with single-layer coatings. The spectral functional layer formulation and preparation process are standardized, allowing for stable mass production via both water-based and solvent-based routes. Customized film thickness and light transmittance parameters based on the substrate provide a wide range of applications. The curing method is flexible and the application is convenient, enabling passive, zero-energy cooling and energy conservation. The protective layer can be modified to be flame-retardant and insulating. The rigid substrate-specific route distinguishes it from fabric-based products, highlighting its significant industrialization value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of passive radiation cooling materials and industrial protective coating technology, specifically a passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment and its construction method. Background Technology

[0002] Equipment such as air conditioner outdoor units, vehicles, outdoor communication cabinets, energy storage battery compartments, box-type transformers, and chemical storage tanks are used outdoors for extended periods. Under strong sunlight in summer, the surface temperature can reach 60℃~75℃. Sustained high temperatures accelerate the aging of electronic components, increase the risk of thermal runaway, significantly increase cooling energy consumption, and accelerate the corrosion and aging of metal substrates and coatings.

[0003] Currently, the industry mainly uses methods such as awnings, active cooling fans, traditional thermal insulation coatings, and spraying for cooling and protection. Awnings require a large area and have high overall costs, making them unsuitable for most industrial scenarios; active cooling devices such as fans consume continuous power and have high failure rates and short lifespans under complex outdoor conditions such as wind, sand, rain, and salt spray; traditional thermal insulation coatings have low solar spectral reflectivity and infrared emissivity, resulting in limited cooling effects and significant performance degradation over long-term use; spraying methods consume large amounts of water and are prone to corroding the substrate. Passive radiative cooling technology achieves high solar reflectivity and high infrared emissivity through spectral modulation, enabling all-weather, zero-energy passive cooling, and represents a highly promising direction for green temperature control technology.

[0004] Existing radiation cooling coating products still have significant drawbacks: some products are only single-layer coatings with insufficient adhesion and weather resistance, making them prone to cracking, chalking, and peeling after long-term outdoor use; most products lack standardized formulation systems, resulting in poor powder particle size control and poor mass production stability; and some coatings have stringent curing conditions, making them difficult to adapt to diverse industrial coating scenarios. Furthermore, automotive and architectural windows are the main sources of heat gain indoors and in vehicles, and traditional heat insulation films and low-emissivity glass have limited cooling effects. Existing radiation cooling coatings struggle to balance light transmittance and durability on glass substrates. Therefore, we propose a passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment and its application method to address these issues. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a passive radiation cooling composite coating system for outdoor high-temperature equipment in multiple scenarios and its construction method. It solves the problems of poor adhesion, rapid weathering degradation, lack of unified standards for mass production, and limited scenario adaptability of existing single-layer radiation cooling coatings. Traditional sunshade, fan, and spray cooling solutions are energy-intensive, occupy space, or corrode the substrate. Glass insulation products cannot simultaneously achieve both lighting and long-term cooling.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solution: a passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment, comprising a substrate bonding layer, a spectral functional layer and a surface protective layer stacked sequentially;

[0007] The dry film thickness of the substrate bonding layer is 10 μm to 25 μm, the dry film thickness of the spectral functional layer is 20 μm to 80 μm, and the dry film thickness of the surface protective layer is 10 μm to 25 μm.

[0008] The spectral functional layer is prepared from raw materials comprising the following mass fractions:

[0009] The mixture consists of 20-45 parts of spectrally modulating powder, 30-55 parts of film-forming resin, 2-6 parts of dispersant, 1-4 parts of leveling agent, 1-5 parts of weather-resistant agent, 0.5-2 parts of defoamer, and the remainder is a dispersion medium.

[0010] The particle size of the spectrally modulated powder is 200 nm to 800 nm;

[0011] After the composite coating system is formed, its overall coating has an average reflectivity of ≥90% for sunlight in the 0.3 μm to 2.5 μm band and an emissivity of ≥90% for infrared light in the 8 μm to 13 μm band; after 3000 h of artificial ultraviolet accelerated aging, its total attenuation rate of spectral cooling performance is ≤6%.

[0012] This invention provides a method for preparing a spectral functional layer coating in a composite coating system, comprising the following steps:

[0013] S1. Mix the dispersion medium, dispersant and defoamer in the specified proportions evenly, then add the specified proportions of spectral control powder, and mix with high-speed stirring and sand milling for 15-30 minutes to obtain powder slurry;

[0014] S2. Add the film-forming resin, leveling agent and weather-resistant agent in the specified proportions to the powder slurry, and mix them by stirring to obtain a mixture.

[0015] S3. Filter the mixture to remove impurities and agglomerates, thus obtaining the spectral functional layer coating.

[0016] This invention provides a method for applying a composite coating system, comprising the following steps:

[0017] S11. Pre-treat the surface of the rigid substrate to make it clean and dry;

[0018] S12. A substrate bonding layer, a spectral functional layer and a surface protective layer are sequentially coated on the surface of the rigid substrate, and surface drying treatment is performed after each coating.

[0019] S13. Curing treatment is performed on the completed coating to form a continuous and dense composite coating film.

[0020] Beneficial effects

[0021] This invention provides a passive radiation cooling composite coating system for outdoor high-temperature equipment in multiple scenarios and its construction method. Compared with the prior art, it has the following advantages:

[0022] This passive radiation cooling composite coating system and its construction method for multi-scenario outdoor high-temperature equipment adopts a three-layer functionally decoupled composite structure consisting of a substrate bonding layer, a spectral functional layer, and a surface protective layer. Each layer performs its own function and complements each other's performance, overcoming the shortcomings of existing single-layer radiation cooling coatings that have to simultaneously assume multiple functions such as adhesion, cooling, and weather resistance, making it difficult to balance performance. The substrate bonding layer specifically addresses the problem of insufficient adhesion at interfaces with different rigid substrates, while the surface protective layer provides long-term protection against ultraviolet rays, salt spray, and rainwater erosion. Combined with the core spectral functional layer, it achieves high solar reflectance and infrared radiation heat dissipation. The entire coating does not crack, blister, or peel off after high and low temperature cycling and long-term ultraviolet aging, significantly improving outdoor service durability and fundamentally solving the pain points of traditional coatings such as easy chalking and rapid degradation of cooling performance.

[0023] Standardized raw material ratio ranges and defined particle size windows for spectral control are established for the spectral functional layer. A complete standardized preparation process, including sand milling and dispersion, mixing, filtration, and filling, is implemented. Two mature product routes—water-based and solvent-based—are established. Existing conventional coating production lines can achieve stable mass production without modification. Batch-to-batch fluctuations in spectral reflectance and infrared emission performance are controllable, solving industry problems such as lack of unified formula control, missing powder dispersion processes, and poor mass production quality stability found in similar products on the market. Furthermore, film thickness and visible light transmittance are designed differently for glass and metal substrates, making it suitable for automotive glass, architectural glass, industrial metal equipment, and concrete components, significantly expanding the application scenarios of passive radiation cooling coatings.

[0024] The coating boasts strong compatibility with various construction processes and a wide curing window. It can air dry at room temperature (5℃~35℃) to meet the needs of outdoor on-site renovation and repair, or it can be cured at low temperatures (40℃~150℃) to adapt to prefabrication on factory production lines. It can be applied using common coating methods such as spraying, brushing, and roller coating, without requiring customized equipment, making it easy to apply and readily available. The coating achieves all-weather, passive, zero-energy cooling through spectral modulation, eliminating the need for fans, refrigeration units, or other power-consuming equipment. It does not require space for shading facilities and avoids the water consumption and substrate corrosion risks associated with spraying processes. This significantly reduces the cooling energy consumption of various outdoor high-temperature equipment, aligning with industrial energy conservation and dual-carbon development requirements.

[0025] The surface protective layer can be compounded with flame-retardant and insulating functional components as needed, giving the coating fireproof and insulating properties while retaining the core performance of radiative cooling. It is suitable for high-safety-level and harsh working conditions such as energy storage battery compartments, box transformers, and chemical storage tanks. The overall technical route is aimed at rigid substrates such as metal, glass, and concrete, forming a clear technical distinction from flexible fabric-based radiative cooling materials that are prone to powdering and failure after washing. There is no conflict in application scenarios, the added value of the product is stronger and more commercially adaptable, and it has good prospects for industrialization and promotion. Attached Figure Description

[0026] Figure 1 This diagram illustrates a method for preparing a spectral functional layer coating in a composite coating system according to the present invention.

[0027] Figure 2 This is a diagram illustrating a construction method for a composite coating system according to the present invention. Detailed Implementation

[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] like Figure 1-2 As shown:

[0030] A passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment includes:

[0031] The substrate bonding layer, spectral functional layer, and surface protective layer are stacked sequentially from the inside out. These three layers are invariably linked and cannot be omitted, and the dry film thickness of each layer has clearly defined technical boundaries. The substrate bonding layer, with a dry film thickness controlled between 10μm and 25μm, primarily functions to seal the substrate interface and facilitate interlayer transition bonding, addressing the common industry problem of insufficient adhesion between different substrate materials and the upper coating layer at the interface level. The spectral functional layer, with a dry film thickness controlled between 20μm and 80μm, is the core functional layer for achieving passive cooling in this invention. It relies on internally spectrally modulated powders to simultaneously achieve high solar reflectivity and high infrared long-wave emission, thereby achieving passive radiative heat dissipation. The surface protective layer, also with a dry film thickness of 10μm to 25μm, serves as the outermost weather-resistant protective layer, isolating it from ultraviolet rays, rain, sandstorms, salt spray, and various corrosive media, continuously protecting the inner spectral functional layer and extending the overall outdoor service life of the coating system.

[0032] The applicable rigid substrates cover a wide range of commonly used rigid components in industry, including but not limited to carbon steel / aluminum alloy metal sheets, tempered / laminated glass for passenger vehicles, float / insulating / curtain wall glass for buildings, concrete walls, rigid engineering plastics, industrial equipment housings, ceramics, and stone.

[0033] After the coating has cured and formed, it must meet a full set of quantitative performance indicators, and all testing operations shall be carried out in accordance with the current national standards for coatings. The first is the core indicator of spectral cooling. The overall coating has an average reflectivity of ≥90% for the entire wavelength range of sunlight from 0.3μm to 2.5μm, and an infrared long-wave emissivity of ≥90% for the atmospheric transparency window from 8μm to 13μm. Based on this spectral characteristic, the coating can reflect most of the solar radiation heat during the day and continuously conduct and accumulate heat into space day and night, achieving passive cooling without the need for external energy.

[0034] The second aspect is the adhesive mechanical properties. The adhesion between the coating and the rigid substrate is tested using the cross-cut adhesion test and is ≥ Grade 1. There is no peeling or complete detachment of the film.

[0035] Thirdly, the coating exhibits excellent temperature cycling performance. After undergoing 50 cycles of alternating high and low temperatures from -20℃ to 70℃, it shows no defects such as cracking, blistering, pinholes, or peeling.

[0036] Fourthly, regarding UV aging resistance and durability, a 3000-hour accelerated UV aging test was conducted according to GB / T1865 standard. After aging, the total attenuation rate of spectral cooling performance was ≤6%, ensuring stable cooling effect during long-term outdoor use. Fifthly, regarding appearance indicators, the cured coating surface is continuous and smooth, without pinholes, bubbles, through cracks, or other appearance defects.

[0037] For two types of rigid substrates, glass and metal-concrete composites, this invention sets differentiated total film thickness and visible light transmittance parameters to balance lighting requirements with cooling and corrosion resistance. For rigid glass substrates such as automotive tempered / laminated glass and architectural window / curtain wall glass, the total dry film thickness of the coating is uniformly controlled between 30μm and 80μm, with a matching transparent spectral powder formula to simultaneously achieve lighting and cooling. Specifically, the visible light transmittance of automotive glass is ≥70%, which meets the national standard GB9656-2021 for motor vehicle safety glass, while the visible light transmittance of architectural glass and curtain wall glass is ≥60%, meeting the daily lighting needs of buildings.

[0038] For non-transparent substrates such as metals, aluminum alloy skins, vehicle electrophoretic paint surfaces, concrete, and hard plastics, the overall dry film thickness of the coating is set to 60μm~150μm. By thickening the film layer, the amount of spectral powder filling is increased, enhancing the overall cooling, corrosion resistance, and wear resistance performance, with no visible light transmission requirement.

[0039] The spectral functional layer is the core structure of the entire system for achieving radiative cooling. The proportions of each component are designed using a standardized range, with a total mass of 100 parts. The specific proportions are: 20-45 parts spectral control powder, 30-55 parts film-forming resin, 2-6 parts dispersant, 1-4 parts leveling agent, 1-5 parts weather-resistant agent, and 0.5-2 parts defoamer. The remaining parts are made up to 100 parts by the dispersion medium. The detailed parameters, selection, and functions of each component are defined as follows:

[0040] One type is the spectrally modulated powder, with its particle size strictly controlled within the range of 200nm to 800nm. It also possesses dual spectral characteristics of high solar reflectance (0.3–2.5μm) and high infrared emission (8–13μm). If the powder particle size is below 200nm, it is prone to agglomeration, which greatly increases the difficulty of coating dispersion and processing. If the powder particle size is above 800nm, it will directly cause a decrease in the light transmittance of the coating, surface roughness, and attenuation of spectral reflectance.

[0041] Secondly, the film-forming resin can be selected from single resins or multiple resins such as acrylic resin, polyurethane resin, silicone resin, and epoxy resin, or used in combination. Different resins are suitable for corresponding working conditions: acrylic resin is suitable for water-based general industrial scenarios; polyurethane resin is wear-resistant and wind and sand resistant, and is suitable for rail transportation and automotive fields; silicone resin has excellent UV resistance and light transmittance, and is suitable for glass systems; epoxy resin has outstanding corrosion resistance and is suitable for energy storage and highly corrosive chemical working conditions. The resin as a whole is used to construct a continuous and dense film skeleton, ensuring the flexibility of the coating and the adhesion of the interface.

[0042] The third is the dispersant, which reduces the surface tension of the powder, inhibits the agglomeration and precipitation of the spectrally regulated powder, and improves the storage stability of the coating.

[0043] The fourth is a leveling agent, which is used to improve the leveling effect of the coating film, eliminate pinholes and orange peel defects, and ensure a smooth and continuous coating.

[0044] Fifthly, there are weather-resistant additives, which use a compound system of ultraviolet absorbers and light stabilizers to inhibit resin yellowing and powder aging, and reduce the rate of spectral performance decay during long-term use of the coating.

[0045] The sixth is the defoamer, which eliminates tiny air bubbles generated during the pulping and coating processes, thus preventing pinhole defects in the coating from the source.

[0046] The seventh component is the dispersion medium, which is divided into two major systems: aqueous and solvent-based. The aqueous system uses deionized water, while the solvent-based system uses alcohol solvents or ester solvents, either alone or in combination. The appropriate type can be flexibly selected according to the environmental protection control requirements of the project site.

[0047] The substrate bonding layer is matched with a special primer system based on the substrate material to achieve targeted interface treatment. For metal substrates, an industrial anti-rust primer is used to pre-seal the micropores on the metal surface and block the penetration of rust media; for low surface energy substrates such as glass and hard plastics, a special silane interface activation primer is used to effectively improve the adhesion between the coating and the smooth substrate.

[0048] The surface protective layer can be compounded with functional components according to the actual operating conditions of the equipment to expand the coating's flame retardant, insulation, and additional safety performance. The flame retardant modification scheme involves adding aluminum hydroxide and melamine flame retardant components, suitable for scenarios with high fire resistance requirements such as energy storage battery compartments and power equipment. The insulation modification scheme involves adding phosphate ester additives to improve the coating's insulation resistance, suitable for power equipment such as box-type transformers and outdoor power cabinets. The basic function of the surface protective layer is to isolate rainwater, salt spray, and ultraviolet rays, preventing the spectral functional layer from being directly exposed to the outdoor environment and undergoing aging and deterioration.

[0049] The spectral functional layer coating adopts a standardized three-step preparation process, with strict control of parameters in each process to ensure uniform dispersion and stable performance of the finished coating.

[0050] S1. Add the dispersion medium, dispersant, and defoamer according to the formula ratio, and stir at low speed for 5-10 minutes to achieve initial mixing of the materials; add all the spectral control powder at one time, premix it by high-speed stirring, and then add zirconia beads as the grinding medium for sand milling treatment. The sand milling time is controlled at 15-30 minutes to fully disperse the powder agglomerates and obtain a stable powder slurry that is uniformly dispersed and does not settle during long-term storage; if the sand milling time is less than 15 minutes, the powder will not be completely dispersed, and if it exceeds 30 minutes, the original particle size of the powder will be broken, resulting in a decrease in spectral cooling performance;

[0051] S2. Add all film-forming resin, leveling agent, and weather-resistant agent to the sand-milled powder slurry, and stir at medium speed for 30-60 minutes to achieve uniform mixing of resin, various additives, and powder slurry at the molecular level. If the stirring time is less than 30 minutes, the additives will be unevenly dispersed, and if it exceeds 60 minutes, a large number of micro bubbles will be continuously introduced, increasing the burden on the subsequent defoaming process.

[0052] S3. The mixture is filtered using an industrial filter screen to remove large, undispersed agglomerates and production impurities. After the viscosity, solid content, and powder dispersion fineness of the coating are all tested and found to meet the standards, it is sealed and filled to obtain the finished spectral functional layer coating, which can be stored in a sealed container for long-term use.

[0053] The entire composite coating adopts a layered construction process, which is divided into three core steps: substrate pretreatment, layered coating, and overall curing.

[0054] S11. Targeted pretreatment of rigid substrates: This step is crucial for ensuring coating adhesion. After all substrates have been treated, the surface must be clean, dry, and free of oil, dust, and rust residue. Metal substrates are derusted by sandblasting or grinding, and surface oil is removed with a degreasing agent, followed by dust removal by blowing. Concrete substrates are ground to remove surface laitance and dust, and then coated with a special alkali-resistant sealing primer to prevent alkali leaching from the concrete from damaging the film. Rigid plastic substrates are treated with flame surface activation or a special adhesion-enhancing primer, depending on their surface tension. Glass substrates are thoroughly cleaned with a special cleaning agent, rinsed with pure water, and then air-dried. For standard applications, a silane coupling agent is applied for surface activation. For high-end optical and high-durability applications, plasma surface treatment can be added to further enhance the adhesion between the coating and the glass substrate.

[0055] S12. Construction must strictly follow the order of substrate bonding layer → spectral functional layer → surface protective layer. The coating order cannot be changed, and no layer can be omitted. After each layer is applied, allow it to dry at room temperature for 5-20 minutes until the coating is no longer tacky to the touch before applying the next layer. Industry-standard spraying, brushing, and roller coating methods are all acceptable. For large storage tanks and building curtain walls, roller coating or large-area air spraying is preferred. For irregularly shaped equipment, small components, and repairs of damaged edges and corners, brushing or small-scale low-pressure spraying is used.

[0056] S13. After all three coating layers are applied, choose one of two curing modes. The first is room temperature air drying, suitable for ambient temperatures of 5℃~35℃, curing naturally with a total curing time of 10~60 minutes, suitable for outdoor on-site renovation without baking equipment; the second is low-temperature baking curing, with oven temperature controlled at 40℃~150℃, baking time of 10~60 minutes, suitable for pre-fabricated coating on factory production lines, with faster curing speed and higher film density. After curing, a three-layer integrated continuous dense functional coating film is formed.

[0057] Example 1: Water-based universal coating system (air conditioner outdoor unit, concrete building substrate)

[0058] Suitable for: ordinary industrial air conditioner outdoor units, outdoor equipment casings, concrete walls, all-water-based environmentally friendly formula.

[0059] Spectral functional layer formulation: 32 parts spectral control powder, 42 parts acrylic resin, 4 parts dispersant, 2 parts leveling agent, 3 parts weathering agent, 1 part defoamer, and deionized water to make up to 100 parts; the particle size of the spectral control powder is controlled at 200nm~600nm.

[0060] Coating preparation: Deionized water, dispersant, and defoamer are mixed at low speed, then powder is added and stirred at high speed and milled with zirconia beads for 22 minutes to form a slurry; acrylic resin and additives are added and stirred at medium speed for 40 minutes, then filtered and filled through a 200-mesh filter.

[0061] Overall construction: Remove rust and oil from the metal substrate, apply alkali-resistant primer to the concrete; apply in layers by roller coating, and allow to cure naturally at room temperature (30℃).

[0062] Performance testing: Solar full-spectrum reflectance 89.1%, 8-13μm infrared emissivity 88.6%; adhesion grade 0; no cracking or blistering after 50 cycles of high and low temperatures from -20 to 70℃; 3000h ultraviolet aging spectral performance degradation of 4.8%; actual outdoor exposure to sunlight resulted in a substrate temperature drop of 7-12℃, and all indicators met the standards.

[0063] Example 2: Solvent-based wear-resistant system (passenger vehicles, rail transportation, outdoor metal sheets)

[0064] Suitable for: automotive bodies, rail vehicle exteriors, outdoor steel structure panels, solvent-based high wear-resistant formula.

[0065] Spectral functional layer formulation: 38 parts spectral control powder, 36 parts polyurethane resin, 5 parts dispersant, 3 parts leveling agent, 4 parts weathering agent, 1.2 parts defoamer, and ester solvent to make up to 100 parts; powder particle size 150nm~500nm.

[0066] Preparation process: Same as in Example 1, sand milling for 20 min, and medium-speed stirring for 45 min.

[0067] Construction process: Metal grinding and cleaning, high-pressure air spraying for layered coating, low-temperature baking and curing at 80℃ for 30 minutes.

[0068] Performance: Spectral reflectance 89.3%, infrared emissivity 88.8%, resistant to wind and sand erosion, resistant to high and low temperatures, and does not easily powder or fall off after long-term outdoor use.

[0069] Example 3: High-transparency automotive glass system (tempered / laminated automotive glass)

[0070] Suitable for: front and rear windshields and side windows of automobiles; the high light transmittance formula meets national standards for motor vehicles.

[0071] Spectral functional layer formulation: 35 parts spectral control powder, 41 parts silicone resin, 3 parts dispersant, 2 parts leveling agent, 4 parts weathering agent, 0.9 parts defoamer, and mixed alcohol ester solvent to make up to 100 parts; powder particle size 120nm~450nm.

[0072] Preparation: Standard sand milling and stirring process, fine filter screen to avoid optical defects.

[0073] Application: Degrease and clean the glass, activate with silane coupling agent; apply thin-layer spray, total dry film thickness 45μm, bake and cure at 45℃ for 25min.

[0074] Performance: Visible light transmittance is 73%, which meets GB9656-2021; spectral indicators meet the standards, with no optical distortion and no fogging; UV aging decay is 5.1% after 3000 hours, and there is no wear and transmittance loss due to high-speed wind and sand erosion.

[0075] Example 4: Dedicated System for Architectural Curtain Wall Glass (Insulated and Float Glass)

[0076] Suitable scenarios: office buildings, factory buildings, window glass, exterior curtain walls, and large-scale engineering construction.

[0077] Spectral functional layer formulation: 40 parts spectral control powder, 39 parts organosilicon modified resin, 3.5 parts dispersant, 2.5 parts leveling agent, 4.5 parts weather-resistant agent, 0.8 parts defoamer, and mixed solvent to make up to 100 parts; powder particle size 180nm~550nm.

[0078] Application: Glass silane activation, roller coating, total dry film thickness 50μm, cured at 45℃.

[0079] Performance: 65% visible light transmittance, meeting building lighting requirements; resistant to rain and atmospheric aging, suitable for large-area mass coating of exterior facades.

[0080] Example 5: Special Flame-Retardant Insulation System (Energy Storage Cabin, Transformer Box, Chemical Storage Tank)

[0081] Suitable for: Highly corrosive and high-safety-level industrial equipment, with coatings that also provide flame retardant and insulating properties.

[0082] Spectral functional layer formulation: 36 parts spectral control powder, 38 parts epoxy modified resin, 4 parts dispersant, 3 parts leveling agent, 4 parts weathering agent, 1 part defoamer, and mixed solvent to make up to 100 parts; powder particle size 160nm~520nm.

[0083] Application: High-pressure spraying, baking and curing at 60℃ for 35 minutes; the surface protective layer contains aluminum hydroxide flame retardant and phosphate ester insulation additives.

[0084] Performance: Meets all spectral, mechanical, and weather resistance standards; possesses excellent insulation, flame retardancy, and resistance to chemical penetration; suitable for harsh working conditions in power, energy storage, and chemical industries.

[0085] Example 1 (general industrial coating) and Example 3 (automotive transparent coating) were selected and compared with ordinary single-layer radiative cooling coatings and high-end automotive heat insulation films in Hainan from June to August, under strong sunlight and high temperature. All tests were carried out in accordance with national standards. The measured data are as follows:

[0086]

[0087] The comparative data clearly show that the three-layer composite coating system of this invention is superior to existing single-layer radiation cooling coatings and traditional glass heat insulation films in terms of cooling range, initial spectral cooling performance, and long-term aging resistance.

[0088] This solution employs a three-layer decoupled composite structure consisting of a substrate bonding layer, a spectral functional layer, and a surface protective layer. Each layer performs its specific function, with synergistic and complementary performance, overcoming the shortcomings of existing single-layer radiation cooling coatings that struggle to balance multiple functions such as adhesion, cooling, and weather resistance. The substrate bonding layer specifically addresses the issue of insufficient adhesion at interfaces with different rigid substrates, while the surface protective layer provides long-term protection against UV, salt spray, and rain erosion. Combined with the core spectral functional layer, it achieves high solar reflectance and infrared radiation heat dissipation. The entire coating system remains crack-free, blister-free, and resistant to peeling even after high and low temperature cycling and prolonged UV aging, significantly improving its outdoor service durability and fundamentally addressing the pain points of traditional coatings, such as easy chalking and rapid degradation of cooling performance.

[0089] Standardized raw material ratio ranges and defined particle size windows for spectral control are established for the spectral functional layer. A complete standardized preparation process, including sand milling and dispersion, mixing, filtration, and filling, is implemented. Two mature product routes—water-based and solvent-based—are established. Existing conventional coating production lines can achieve stable mass production without modification. Batch-to-batch fluctuations in spectral reflectance and infrared emission performance are controllable, solving industry problems such as lack of unified formula control, missing powder dispersion processes, and poor mass production quality stability found in similar products on the market. Furthermore, film thickness and visible light transmittance are designed differently for glass and metal substrates, making it suitable for automotive glass, architectural glass, industrial metal equipment, and concrete components, significantly expanding the application scenarios of passive radiation cooling coatings.

[0090] The coating boasts strong compatibility with various construction processes and a wide curing window. It can air dry at room temperature (5℃~35℃) to meet the needs of outdoor on-site renovation and repair, or it can be cured at low temperatures (40℃~150℃) to adapt to prefabrication on factory production lines. It can be applied using common coating methods such as spraying, brushing, and roller coating, without requiring customized equipment, making it easy to apply and readily available. The coating achieves all-weather, passive, zero-energy cooling through spectral modulation, eliminating the need for fans, refrigeration units, or other power-consuming equipment. It does not require space for shading facilities and avoids the water consumption and substrate corrosion risks associated with spraying processes. This significantly reduces the cooling energy consumption of various outdoor high-temperature equipment, aligning with industrial energy conservation and dual-carbon development requirements.

[0091] The surface protective layer can be compounded with flame-retardant and insulating functional components as needed, giving the coating fireproof and insulating properties while retaining the core performance of radiative cooling. It is suitable for high-safety-level and harsh working conditions such as energy storage battery compartments, box transformers, and chemical storage tanks. The overall technical route is aimed at rigid substrates such as metal, glass, and concrete, forming a clear technical distinction from flexible fabric-based radiative cooling materials that are prone to powdering and failure after washing. There is no conflict in application scenarios, the added value of the product is stronger and more commercially adaptable, and it has good prospects for industrialization and promotion.

[0092] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment, characterized in that: It includes a substrate bonding layer, a spectral functional layer and a surface protective layer that are stacked sequentially; The dry film thickness of the substrate bonding layer is 10 μm to 25 μm, the dry film thickness of the spectral functional layer is 20 μm to 80 μm, and the dry film thickness of the surface protective layer is 10 μm to 25 μm. The spectral functional layer is prepared from raw materials comprising the following mass fractions: The mixture consists of 20-45 parts of spectrally modulating powder, 30-55 parts of film-forming resin, 2-6 parts of dispersant, 1-4 parts of leveling agent, 1-5 parts of weather-resistant agent, 0.5-2 parts of defoamer, and the remainder is a dispersion medium. The particle size of the spectrally modulated powder is 200 nm to 800 nm; After the composite coating system is formed, its overall coating has an average reflectivity of ≥90% for sunlight in the 0.3 μm to 2.5 μm band and an emissivity of ≥90% for infrared light in the 8 μm to 13 μm band; after 3000 h of artificial ultraviolet accelerated aging, its total attenuation rate of spectral cooling performance is ≤6%.

2. The passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment according to claim 1, characterized in that: The film-forming resin is selected from one or more of acrylic resin, polyurethane resin, silicone resin, and epoxy resin; and / or the dispersion medium is selected from one or more of deionized water, alcohol solvents, and ester solvents.

3. The passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment according to claim 1, characterized in that: The substrate bonding layer is an anti-rust primer or an interface-activating primer suitable for glass or rigid plastics.

4. The passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment according to claim 1, characterized in that: When the composite coating system is applied to a glass substrate, its total dry film thickness is 30 μm to 80 μm; when applied to automotive glass, its visible light transmittance is ≥70%; when applied to architectural glass, its visible light transmittance is ≥60%.

5. The passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment according to claim 1, characterized in that: When the composite coating system is applied to a metal substrate or a composite material paint substrate, its total dry film thickness is 60 μm to 150 μm.

6. The passive radiation cooling composite coating system for multi-scenario outdoor high-temperature equipment according to claim 1, characterized in that: The surface protective layer also contains flame-retardant components and / or insulating components; the flame-retardant components include aluminum hydroxide and / or melamine; the insulating components include phosphate ester additives.

7. A method for preparing a spectral functional layer coating in a composite coating system as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Mix the dispersion medium, dispersant and defoamer in the specified proportions evenly, then add the specified proportions of spectral control powder, and then mix and grind at high speed for 15-30 minutes to obtain the powder slurry. S2. Add the film-forming resin, leveling agent and weather-resistant agent in the specified proportions to the powder slurry, and mix them by stirring to obtain a mixture. S3. Filter the mixture to remove impurities and agglomerates, thus obtaining the spectral functional layer coating.

8. The preparation method according to claim 7, characterized in that, In step S01, the grinding medium is zirconium oxide beads; In step S2, the stirring time is 30–60 min; In step S3, a filter screen is used for filtration.

9. A method for applying a composite coating system as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S11. Pre-treat the surface of the rigid substrate to make it clean and dry; S12. A substrate bonding layer, a spectral functional layer and a surface protective layer are sequentially coated on the surface of the rigid substrate, and surface drying treatment is performed after each coating. S13. Curing treatment is performed on the completed coating to form a continuous and dense composite coating film.

10. The construction method according to claim 9, characterized in that, In step S11, when the rigid substrate is glass, a silane coupling agent is used for surface activation treatment. In step S13, the curing method is to air dry at room temperature under conditions of 5℃~35℃, or to bake and cure at low temperature under conditions of 40℃~150℃, and the curing time is 10~60 min. The layered coating method is selected from any one of spraying, brushing, or roller coating.