A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating and its preparation method
By growing carbon nanotubes in situ on three-dimensional graphene to form multidimensional composite nano-carbon materials, the problems of difficult carbon material dispersion and weak interface in traditional zinc-rich epoxy coatings are solved, and the long-term protection and self-healing performance of the coating are synergistically improved.
Patent Information
- Application Number
- CN202611491757.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional zinc-rich epoxy coatings suffer from difficulties in dispersing carbon materials, weak interfaces, and unstable conductive networks, resulting in limited improvement in corrosion resistance.
A multidimensional graphene-grafted carbon nanotube modified epoxy anti-corrosion coating is used. By growing carbon nanotubes in situ on three-dimensional graphene, a multidimensional composite nano-carbon material is formed. Combined with zinc powder, epoxy resin and curing agent, a stable three-dimensional conductive network is constructed.
It significantly improves zinc powder utilization, enhances the cathodic protection function and physical shielding performance of the coating, achieves long-term corrosion protection and self-healing performance, and reduces the corrosion current density of the coating by several orders of magnitude, making it suitable for harsh corrosive environments.
Smart Images

Figure CN123063036A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of anti-corrosion coating technology, specifically to a multidimensional graphene-grafted carbon nanotube modified epoxy anti-corrosion coating and its preparation method. Background Technology
[0002] Traditional zinc-rich epoxy coatings rely on high zinc powder content (typically >80 wt%) for cathodic protection, but this results in low zinc powder utilization, easy coating cracking, and a heavy environmental burden. To reduce zinc usage, researchers have attempted to introduce carbon materials (such as graphene and carbon nanotubes) to improve coating conductivity and zinc powder utilization. However, two-dimensional graphene sheets are prone to agglomeration and are difficult to disperse in resin; one-dimensional carbon nanotubes also suffer from poor dispersibility and weak interfacial bonding with the resin matrix. Single-dimensional carbon materials are insufficient to construct a stable and efficient three-dimensional conductive network in the coating, thus offering limited improvement in corrosion resistance. Therefore, a new type of anti-corrosion coating is urgently needed. Summary of the Invention
[0003] To address the aforementioned technical problems, the present invention aims to provide a multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating and its preparation method, thereby solving the problems of difficult dispersion of carbon materials, weak interfaces, and unstable conductive networks in existing anticorrosive coatings.
[0004] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: a multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating is provided, comprising the following components by weight: 30-60 parts epoxy resin, 25-45 parts zinc powder, 0.02-0.5 parts multidimensional graphene-grafted carbon nanotubes, 15-30 parts curing agent, and 20-40 parts organic solvent; wherein, the multidimensional graphene-grafted carbon nanotubes are carbon nanotubes grown in situ on three-dimensional graphene.
[0005] Based on the above technical solution, the present invention can be further improved as follows: Furthermore, the anti-corrosion coating comprises the following components by weight: 30-60 parts epoxy resin, 25-45 parts zinc powder, 0.02-0.2 parts multidimensional graphene-grafted carbon nanotubes, 15-30 parts curing agent, and 20-40 parts organic solvent; wherein the multidimensional graphene-grafted carbon nanotubes are carbon nanotubes grown in situ on three-dimensional graphene.
[0006] Furthermore, the anti-corrosion coating comprises the following components in parts by weight: 30 parts epoxy resin, 35 parts zinc powder, 0.1 parts multidimensional graphene-grafted carbon nanotubes, 15 parts curing agent, and 20 parts organic solvent; wherein the multidimensional graphene-grafted carbon nanotubes are carbon nanotubes grown in situ on three-dimensional graphene.
[0007] Furthermore, the zinc powder is flake-shaped zinc powder with a particle size of 5-10 μm.
[0008] Furthermore, multidimensional graphene-grafted carbon nanotubes account for 0.1 wt% of the total of the remaining components.
[0009] Furthermore, multidimensional graphene-grafted carbon nanotubes were prepared by the following method: S1: Polyurethane sponge is impregnated in an ethanol dispersion of graphene oxide, dried to obtain a precursor, and then burned in an ethanol flame to obtain three-dimensional thermally reduced graphene oxide. S2: The three-dimensional thermally reduced graphene oxide obtained in step S1 is immersed in an ethanol solution of nickel salt and then burned in an ethanol flame to obtain multi-dimensional graphene-grafted carbon nanotubes.
[0010] Furthermore, in step S1, the concentration of the ethanol dispersion of graphene oxide is 2 mg / mL.
[0011] Furthermore, in step S1, the flame temperature during combustion is 500-600℃, and the time is 1 min.
[0012] Furthermore, in step S1, the pore size of the three-dimensionally reduced graphene oxide is 100-500 μm.
[0013] Furthermore, in step S2, the concentration of the nickel salt ethanol solution is 0.2 mol / L.
[0014] Furthermore, in step S2, the nickel salt is nickel chloride.
[0015] Furthermore, in step S2, the flame temperature during combustion is 500-600℃, and the time is 10 min.
[0016] Furthermore, in step S2, the mass ratio of three-dimensional thermally reduced graphene oxide to carbon nanotubes in the multidimensional graphene-grafted carbon nanotubes is 1:3.
[0017] Furthermore, the curing agent is a polyamide-based epoxy resin curing agent.
[0018] Furthermore, the organic solvent is a mixture of xylene and n-butanol in a mass ratio of 7:3.
[0019] This invention also provides a method for preparing the above-mentioned multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosion coating, comprising the following steps: Multidimensional graphene-grafted carbon nanotubes were dispersed in an organic solvent, zinc powder and epoxy resin were added, and the mixture was stirred evenly. Then, a curing agent was added, and the mixture was stirred evenly again to prepare a multidimensional graphene-grafted carbon nanotube modified epoxy anti-corrosion coating.
[0020] The present invention also provides the application of the above-mentioned multidimensional graphene-grafted carbon nanotube modified epoxy anti-corrosion coating in anti-corrosion coatings for civil engineering steel structures, ships, marine engineering or chemical equipment.
[0021] The present invention has the following beneficial effects: 1. The application of multidimensional composite carbon nanomaterials formed by in-situ growth of carbon nanotubes on the surface of three-dimensional graphene in the field of anti-corrosion coatings, especially their synergistic enhancement of the anti-corrosion and self-healing properties of zinc-rich epoxy coatings in heavy-duty anti-corrosion applications, has not yet been reported in research. The flame method, as a simple and low-cost material preparation method, has been proven to be suitable for in-situ growth of carbon nanotubes on carbon materials (such as carbon fibers). This invention creatively introduces a specific structured multidimensional composite carbon nanomaterial (3DRGO-fCNT) prepared by the flame method into a zinc-rich epoxy system, solving the problems of difficult dispersion, weak interface, and unstable conductive network of traditional carbon materials, achieving a synergistic leap in the long-term protective and self-healing properties of the coating.
[0022] 2. The anti-corrosion coating of this invention uses three-dimensional graphene as a carrier. Carbon nanotubes are grown in situ using a flame method to form multi-dimensional graphene-grafted carbon nanotubes that directly combine three-dimensional and one-dimensional elements. These multi-dimensional graphene-grafted carbon nanotubes are then composited with zinc powder, epoxy resin, and a curing agent to prepare the anti-corrosion coating. This composite carbon material constructs a three-dimensional conductive network in the zinc-rich epoxy coating system, significantly improving the utilization rate of zinc powder and enhancing the cathodic protection function and physical shielding performance of the coating. The coating system of this invention achieves excellent anti-corrosion effects with extremely low amounts of nano-carbon materials, making it suitable for harsh corrosive environments.
[0023] 3. The anti-corrosion coating of the present invention only requires the addition of 0.1 wt% graphene-grafted carbon nanotubes, which can greatly reduce the corrosion current density of the coating, even by up to 6 orders of magnitude compared with zinc-rich epoxy coatings without nano-carbon material modification.
[0024] 4. The anti-corrosion coating of the present invention has a stable structure and maintains long-term protective performance during long-term immersion. After the coating is scratched, the activated zinc powder in the coating can preferentially corrode and form a zinc corrosion product film at the scratch, covering the exposed metal substrate, delaying its further corrosion, and exhibiting stronger self-healing properties.
[0025] 5. Unlike the direct mixing of carbon nanotubes and multidimensional graphene in coatings, the multidimensional graphene-grafted carbon nanotubes proposed in this invention, due to the direct growth and bonding of carbon nanotubes and graphene, can improve the uniform dispersion of carbon nanotubes and multidimensional graphene in the zinc-rich epoxy anticorrosive coating modified with it, and efficiently establish a nano-carbon network, thereby significantly improving the long-term anticorrosive and self-healing performance of the coating with extremely low dosage.
[0026] 6. The process of this invention is simple and low-cost. The core filler is prepared by flame method, which is simple in equipment, open in environment, and low in energy consumption, which is conducive to large-scale production. At the same time, the preparation process of the final anti-corrosion coating is compatible with traditional epoxy coatings. Attached Figure Description
[0027] Figure 1 The image shows a SEM image of the 3DRGO-fCNT obtained in Example 1. Figure 2 The image shows the potentiodynamic polarization curves of the coatings in Example 2 and Comparative Examples 1-3 after immersion in NaCl solution. Detailed Implementation
[0028] The principles and features of the present invention are described below with reference to the accompanying drawings. The examples given are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer should be followed. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0029] Example 1: A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating comprises the following components by weight: 30 parts epoxy resin, 35 parts zinc powder, 0.02 parts multidimensional graphene-grafted carbon nanotubes, 15 parts curing agent, and 20 parts organic solvent.
[0030] A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating, the preparation method of which includes the following steps: (1) A piece of cleaned and dried polyurethane sponge (PU, about 2×2×1 cm) was immersed in an ethanol dispersion of graphene oxide (2 mg / mL). The sponge was repeatedly squeezed to ensure full immersion. After being removed, it was dried in an oven at 60°C for 12 h to obtain the precursor. Then, it was held with tweezers and burned in an ethanol flame at a temperature of 550°C for 1 min until the PU template was completely burned and decomposed to obtain self-supporting porous three-dimensional thermally reduced graphene oxide (3DRGO). (2) The three-dimensional thermally reduced graphene oxide obtained in step (1) was immersed in an ethanol solution (0.2 mol / L) of nickel salt catalyst (nickel chloride hexahydrate). After a short while, it was taken out and the solution was saturated with the catalyst. Then it was placed on a stainless steel mesh and burned in an ethanol flame at a flame temperature of 550°C for 10 min to obtain multi-dimensional graphene-grafted carbon nanotubes (denoted as 3DRGO-fCNT). (3) Add 0.002 g of multidimensional graphene-grafted carbon nanotubes to an organic solvent (a mixture of 1.4 g xylene and 0.6 g n-butanol), and ultrasonically disperse in an ultrasonic cleaner for 30 min until a uniform and stable dispersion is formed. Add 3.5 g of zinc powder (flake-shaped zinc powder with a particle size of 5-10 μm) and 3 g of epoxy resin, and stir vigorously on a magnetic stirrer for 2 h to ensure that all components are fully mixed. Then add 1.5 g of curing agent (polyamide 651), and continue stirring for 10 min to obtain multidimensional graphene-grafted carbon nanotube modified epoxy anti-corrosion coating.
[0031] The prepared anti-corrosion coating was applied to a Q235 steel substrate (30×40×1.5 mm) that had been sandblasted and ultrasonically cleaned with acetone using a coating applicator. The substrate was then placed in an oven at 60°C for 24 hours to cure, forming a coating with a dry film thickness of approximately 150±10 μm, denoted as 0.02wt%3DRGO-fCNT / EP / Zn.
[0032] Example 2: A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating comprises the following components in parts by weight: 30 parts epoxy resin, 35 parts zinc powder, 0.1 parts multidimensional graphene-grafted carbon nanotube, 15 parts curing agent, and 20 parts organic solvent.
[0033] A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating, the preparation method of which includes the following steps: Add 0.01 g of 3DRGO-fCNT, and the rest is the same as in Example 1.
[0034] The resulting coating was denoted as 0.1wt%3DRGO-fCNT / EP / Zn, and the rest was the same as in Example 1.
[0035] Example 3: A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating comprises the following components by weight: 30 parts epoxy resin, 35 parts zinc powder, 0.2 parts multidimensional graphene-grafted carbon nanotubes, 15 parts curing agent, and 20 parts organic solvent.
[0036] A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating, the preparation method of which includes the following steps: Add 0.02g of 3DRGO-fCNT, and the rest is the same as in Example 1.
[0037] The resulting coating was denoted as 0.2wt%3DRGO-fCNT / EP / Zn, and the rest was the same as in Example 1.
[0038] Comparative Example 1: An epoxy anti-corrosion coating is prepared by the following steps: Carbon nanotubes without multidimensional graphene grafted into them served as a blank control group, and the rest were the same as in Example 1.
[0039] The resulting coating is denoted as Neat EP / Zn.
[0040] Comparative Example 2: An epoxy anti-corrosion coating comprises the following components in parts by weight: 30 parts epoxy resin, 35 parts zinc powder, 0.1 parts 3DRGO, 15 parts curing agent, and 20 parts organic solvent.
[0041] An epoxy anti-corrosion coating is prepared by the following steps: Replace the multidimensional graphene-grafted carbon nanotubes with 0.01g of 3DRGO, and the rest is the same as in Example 1.
[0042] The resulting coating was denoted as 0.1 wt% 3DRGO / EP / Zn.
[0043] Comparative Example 3: An epoxy anti-corrosion coating comprises the following components in parts by weight: 30 parts epoxy resin, 35 parts zinc powder, 0.1 parts 3DRGO and commercial multi-walled carbon nanotubes, 15 parts curing agent, and 20 parts organic solvent.
[0044] An epoxy anti-corrosion coating is prepared by the following steps: The multidimensional graphene-grafted carbon nanotubes were replaced with a mixed filler of 0.01 g of 3DRGO and commercial multi-walled carbon nanotubes (outer diameter 50 nm) in a mass ratio of 3:1, and the rest was the same as in Example 1.
[0045] The resulting coating was denoted as 0.1 wt% 3DRGO-aCNT / EP / Zn.
[0046] Test case I. The 3DRGO-fCNTs prepared in Example 1 were subjected to SEM detection, and the results are shown in [the table below]. Figure 1 ( Figure 1 (b) is an enlarged view of (a).
[0047] Depend on Figure 1 As can be seen, Example 1 successfully vertically grew a large number of uniformly distributed carbon nanotubes on the graphene surface of 3DRGO, and the generated fCNTs had an average diameter of about 65 nm and a length of about 1-2 μm. The 3DRGO particles have obvious lamellar structure, while the fCNTs grown in situ by flame method have obvious one-dimensional structure.
[0048] II. The corrosion performance of the coatings prepared in Examples 1-3 and Comparative Examples 1-3 was tested. The specific testing methods were as follows: electrochemical impedance spectroscopy (EIS) and potentiodynamic polarization curves were used to test the corrosion performance of the coatings. The specific equipment was a CHI660E electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd.). A typical three-electrode system was used, with a saturated calomel electrode as the reference electrode, a platinum sheet electrode as the auxiliary electrode, and the metal anti-corrosion coating as the working electrode. The test area was 1 cm². 2 The corrosion resistance of the coating was tested in a 3.5 wt% NaCl solution. The specific test results are shown in Table 1.
[0049] Table 1: Test results of EIS and potentiodynamic polarization curves of anticorrosive coatings
[0050] As shown in Table 1, compared to Comparative Example 1 (without added carbon nanotubes), all coatings with added carbon nanotubes exhibited significantly improved corrosion resistance. Among the three examples, the anti-corrosion coating of Example 2 showed the best corrosion resistance, indicating that the optimal content of the 3DRGO-fCNT carbon nanotubes in the coating was 0.1 wt%. With the same content but different types of carbon nanotubes, the anti-corrosion coating of Example 2, compared to Comparative Example 2, had a higher low-frequency impedance modulus, polarization resistance, and lower corrosion current. This suggests that growing fCNTs on multidimensional graphene can further improve the corrosion resistance of the coating compared to single multidimensional graphene. More importantly, compared to Comparative Example 3, although the content of three-dimensional graphene and carbon nanotubes in the two coatings remained consistent, the corrosion resistance of Example 2 was significantly stronger than that of Comparative Example 3. This demonstrates that the in-situ growth of carbon nanotubes grafted with multidimensional graphene proposed in this invention has an irreplaceable synergistic enhancement effect on zinc-rich epoxy anti-corrosion coatings, meaning that the anti-corrosion coating prepared using the method described in this application has superior corrosion resistance.
[0051] III. The coatings obtained in Example 2 and Comparative Examples 1-3 were subjected to electrochemical corrosion reaction detection. The specific detection method was as follows: the coating samples prepared in Example 2 and Comparative Examples 1-3 were immersed in 3.5 wt% NaCl solution for 300 h. The potentiodynamic polarization curves are shown in the figure. Figure 2 The corresponding parameters of the obtained electrochemical corrosion reaction are shown in Table 2.
[0052] Table 2. Test results of the potentiodynamic polarization curves of the anti-corrosion coating.
[0053] As shown in Table 2, the coating obtained in Example 2 exhibits the highest polarization resistance and the lowest corrosion current after prolonged immersion in a 3.5 wt% NaCl solution, with a corrosion current density as low as 2.93 × 10⁻⁶. -9 A·cm -2 The corrosion resistance was reduced by nearly four orders of magnitude compared to the coating in Comparative Example 1, indicating that the coating with added 3DRGO-fCNT has superior long-term corrosion protection. Furthermore, its performance is far better than that of the samples obtained in Comparative Examples 2 and 3.
[0054] V. Visually inspect the appearance and color of the anti-corrosion coatings in Examples 1-3 and Comparative Examples 1-3. Test the pencil hardness of the anti-corrosion coatings according to the method in GB / T6739-2006 "Determination of Hardness of Paint Film by Pencil Method". Test the salt water resistance of the coatings in 3.5% NaCl for 30 days according to the method in GB1763-79 "Determination of Chemical Resistance of Paint Film". The specific test results are shown in Table 3.
[0055] Table 3: Tests for the appearance, pencil hardness, and salt water resistance of anti-corrosion coatings
[0056] As shown in Table 3, the appearance, pencil hardness, and salt water resistance of the anti-corrosion coating prepared by this invention all meet the requirements of national standards.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating, characterized in that, It comprises the following components by weight: 30-60 parts epoxy resin, 25-45 parts zinc powder, 0.02-0.5 parts multidimensional graphene-grafted carbon nanotubes, 15-30 parts curing agent, and 20-40 parts organic solvent; wherein the multidimensional graphene-grafted carbon nanotubes are carbon nanotubes grown in situ on three-dimensional graphene.
2. The multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating according to claim 1, characterized in that, The product comprises the following components by weight: 30 parts epoxy resin, 35 parts zinc powder, 0.02 parts multidimensional graphene-grafted carbon nanotubes, 15 parts curing agent, and 20 parts organic solvent; wherein the multidimensional graphene-grafted carbon nanotubes are carbon nanotubes grown in situ on three-dimensional graphene.
3. The multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosion coating according to claim 1 or 2, characterized in that, The zinc powder is in the form of flakes, with a particle size of 5-10 μm.
4. The multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosion coating according to claim 1 or 2, characterized in that, Multidimensional graphene-grafted carbon nanotubes were prepared by the following method: S1: Polyurethane sponge is impregnated in an ethanol dispersion of graphene oxide, dried to obtain a precursor, and then burned in an ethanol flame to obtain three-dimensional thermally reduced graphene oxide. S2: The three-dimensional thermally reduced graphene oxide obtained in step S1 is immersed in an ethanol solution of nickel salt and then burned in an ethanol flame to obtain multi-dimensional graphene-grafted carbon nanotubes.
5. The multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating according to claim 4, characterized in that, In step S1, the concentration of the ethanol dispersion of graphene oxide is 2 mg / mL.
6. The multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating according to claim 4, characterized in that, In step S2, the nickel salt is nickel chloride.
7. The multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating according to claim 1 or 2, characterized in that, The curing agent is a polyamide-based epoxy resin curing agent.
8. The multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating according to claim 1 or 2, characterized in that, The organic solvent is a mixture of xylene and n-butanol in a mass ratio of 7:
3.
9. The method for preparing the multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosive coating according to any one of claims 1-8, characterized in that, Includes the following steps: Multidimensional graphene-grafted carbon nanotubes were dispersed in an organic solvent, zinc powder and epoxy resin were added, and the mixture was stirred evenly. Then, a curing agent was added, and the mixture was stirred evenly again to prepare a multidimensional graphene-grafted carbon nanotube modified epoxy anti-corrosion coating.
10. The application of the multidimensional graphene-grafted carbon nanotube modified epoxy anticorrosion coating according to any one of claims 1-8 in anticorrosion coatings for civil engineering steel structures, ships, marine engineering or chemical equipment.