A binder for silicon-carbon / graphite composite negative electrodes, its preparation method and application.
The amphiphilic binder prepared by emulsion copolymerization and controlled free radical polymerization solves the interfacial compatibility and mechanical stability problems of silicon-carbon composite anode materials, achieving high stability and efficient adhesion, and improving the cycle performance and mechanical properties of lithium-ion batteries.
Patent Information
- Application Number
- CN202611351025.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-10
AI Technical Summary
Existing binders for silicon-carbon composite anode materials in lithium-ion batteries have shortcomings in terms of interfacial compatibility and mechanical stability, leading to electrode failure during cycling. They cannot simultaneously achieve good adhesion of silicon and graphite and suppress the volume expansion of silicon.
Hydrophobic component A and strongly hydrophilic component B were prepared by emulsion copolymerization and controlled free radical polymerization. Natural polyphenol compounds were used as supramolecular crosslinking agents C to form an amphiphilic binder with strong cohesive force, thereby achieving stable interfacial compatibility and mechanical properties between silicon and graphite.
The binder system achieves high stability during electrode cycling, with an elongation at break of at least 210%, stable cycling for more than 550 cycles, capacity retention of 80%, and average coulombic efficiency of >99%. Furthermore, the preparation process is simple and the raw material cost is low.
Smart Images

Figure CN123063104A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery anode binders, specifically relating to a binder for silicon-carbon / graphite composite anodes, its preparation method, and its application. Background Technology
[0002] To achieve high energy density in lithium-ion batteries and overcome the large volume expansion and low conductivity of pure silicon binders, silicon-graphite composites are a promising anode material for lithium-ion batteries, synergistically combining the high capacity of silicon with the high conductivity of graphite. However, the interaction between hydrophilic silicon binders and hydrophobic graphite binders is hampered by interfacial incompatibility and mechanical instability. Hydrophilic polar binders suitable for silicon materials perform poorly in hydrophobic graphite-dominated SiC composites; while hydrophobic nonpolar binders suitable for graphite materials cannot effectively suppress the volume expansion of silicon.
[0003] For example, CN119220209A discloses a multi-component three-dimensional network binder rich in hydroxyl, amino, and epoxy groups for silicon-carbon anodes. This hydrophilic binder, rich in polar groups, is not suitable for hydrophobic graphite materials. CN117777891A discloses a styrene-butadiene latex binder with different glass transition temperatures for silicon-carbon anodes. This non-polar latex binder lacks polar groups that can form strong covalent bonds with the silicon material surface, resulting in poor performance in suppressing silicon expansion. None of the above solutions have achieved amphiphilic interfacial adhesion that simultaneously exhibits good affinity for both silicon and graphite materials.
[0004] Currently, a common strategy to address the aforementioned problems is to physically blend polar binders with non-polar binders. For example, CN116230849A discloses a PAA-CMC-SBR composite binder for use in silicon-carbon anodes. While this method can achieve effective adhesion to both hydrophilic silicon and hydrophobic graphite, the thermodynamic incompatibility between the highly polar PAA and the non-polar SBR leads to phase separation during electrode cycling, resulting in electrode failure.
[0005] Therefore, binders suitable for SiC composites must not only have both hydrophilic polar groups and hydrophobic structures, but more importantly, they must have strong and continuous interchain interactions to maintain stable interfacial chemical and mechanical structural integrity during long-term cycling. Summary of the Invention
[0006] The purpose of this invention is to provide a binder for silicon-carbon / graphite composite negative electrodes, its preparation method, and its application. The prepared binder achieves strong adhesion to both silicon and graphite simultaneously, and its application in lithium batteries enables the binder system to maintain high stability during electrode cycling.
[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A method for preparing a binder for silicon-carbon / graphite composite negative electrodes includes the following steps: (1) Preparation of component A by emulsion copolymerization: at least two of the functional monomer, hard monomer and soft monomer are emulsion copolymerized to obtain component A; wherein the functional monomer and soft monomer are both selected from acrylate monomers, and the hard monomer is selected from acrylate monomers and / or styrene; (2) Preparation of component B by controlled free radical polymerization: component B is obtained by controlled free radical polymerization of acrylic acid monomer and flexible bifunctional monomer; (3) Crosslinking: Components A and B are crosslinked using natural polyphenol compounds as supramolecular crosslinking agent C to obtain a binder for silicon-carbon / graphite composite negative electrode.
[0008] The technical principle of this invention is as follows: First, hydrophobic component A is synthesized. This component is obtained by emulsion copolymerization of acrylate monomers. This component has strong hydrophobicity, good compatibility with graphite materials, and certain flexibility and high elasticity, effectively adapting to the volume changes of silicon. Then, component B is synthesized. This component is obtained by controlled free radical polymerization of acrylic acid and a flexible bifunctional monomer. This component has strong hydrophilicity. The high modulus and dense carboxyl groups of polyacrylic acid have strong interfacial interactions with silicon, which can effectively inhibit the expansion of silicon and maintain the integrity of the electrode. At the same time, the introduction of the bifunctional monomer reduces the brittleness of PAA. Finally, a supramolecular crosslinking agent is used to combine component A and component B to form an amphiphilic binder with strong cohesion.
[0009] In step (1), the functional monomer is selected from one or more of acrylic acid, methacrylic acid, hydroxyethyl methacrylate or hydroxypropyl methacrylate; the hard monomer is selected from one or more of methyl acrylate, methyl methacrylate or ethyl methacrylate or styrene; and the soft monomer is selected from one or more of ethyl acrylate, isooctyl acrylate, n-butyl acrylate or hydroxyethyl acrylate.
[0010] Preferably, the functional monomer is selected from acrylic acid and / or methacrylic acid, the hard monomer is selected from one or more of methyl methacrylate, ethyl methacrylate or styrene, and the soft monomer is selected from one or more of isooctyl acrylate, n-butyl acrylate or hydroxyethyl acrylate, which is more conducive to simultaneously improving the mechanical properties and cycle stability of the adhesive.
[0011] In step (1), the mass ratio of the functional monomer: hard monomer: soft monomer is 1:10-16:20-26.
[0012] In step (1), the emulsion copolymerization is carried out under the conditions of emulsifier and initiator. The reaction temperature of the emulsion copolymerization is 60-85℃, the reaction time of the emulsion copolymerization is 1-4h, and the reaction system is deionized water.
[0013] Preferably, the emulsifier is selected from one or more of OP-10, sodium dodecylbenzenesulfonate, or sodium dodecyl sulfate, and the total amount of the emulsifier is 1.5-3% of the total mass of the functional monomer, hard monomer, and soft monomer; the initiator is selected from one or more of azobisisobutyronitrile, azoisobutyronitrile cyanoformamide, ammonium persulfate, potassium persulfate, sodium persulfate, or benzoyl peroxide, and the total amount is 0.5-1.5% of the total mass of the functional monomer, hard monomer, and soft monomer.
[0014] In step (2), the flexible bifunctional monomer is selected from one or more of polyethylene glycol diacrylate, tri(ethylene glycol) diacrylate, dipropylene glycol diacrylate or polypropylene glycol diacrylate; the mass ratio of the flexible bifunctional monomer to the acrylic monomer is 0.4-2.0:100.
[0015] Preferably, the flexible bifunctional monomer is selected from polyethylene glycol diacrylate and / or tri(ethylene glycol) diacrylate, which is more conducive to simultaneously improving the mechanical properties and cycle stability of the adhesive.
[0016] In step (2), the controlled free radical polymerization is carried out in the presence of a chain transfer agent and an initiator; the reaction temperature of the controlled free radical polymerization is 60-80℃, and the reaction time of the controlled free radical polymerization is 5-12h; the reaction system is DMF, DMSO or deionized water, and the reaction system requires 30-60min of nitric acid gas to maintain an oxygen-free environment.
[0017] Preferably, the chain transfer agent is a dithioester, selected from one of cyanoisopropyl dithiobenzoate, cumyl dithiobenzoate, or cyanoisopropyl dithioacetate, and the amount used is 0.2-0.5% of the total mass of the acrylic monomer and the flexible bifunctional monomer; the initiator is selected from one or more of azobisisobutyronitrile, azoisobutyl cyanoformamide, ammonium persulfate, potassium persulfate, sodium persulfate, and benzoyl peroxide, and the total amount used is 0.1-0.3% of the total mass of the acrylic monomer and the flexible bifunctional monomer.
[0018] In step (3), the supramolecular crosslinking agent is selected from tartaric acid or tannic acid, and the mass ratio of component A, component B and supramolecular crosslinking agent C is 3-5:8-9:1-3.
[0019] Preferably, the mass ratio of the functional monomer:hard monomer:soft monomer is 1:13-16:23-26, the mass ratio of the flexible bifunctional monomer to the acrylic monomer is 0.45-1.8:100, and the mass ratio of component A, component B, and supramolecular crosslinking agent C is 3-4.5:8-9:1.5-3. Under these ratios, it is more beneficial to improve the cycle stability and mechanical properties of lithium batteries: the elongation at break is at least 210%, and the stable cycle life is at least more than 550 cycles.
[0020] Preferably, the mass ratio of the functional monomer to the hard monomer to the soft monomer is 1:13-16:23-26, the mass ratio of the flexible bifunctional monomer to the acrylic monomer is 0.45-1.8:100, and the mass ratio of component A, component B, and supramolecular crosslinking agent C is 4.5:9:3. Under the above ratio conditions, the cycling stability can be further improved to a stable cycle of at least 700 cycles.
[0021] Preferably, the mass ratio of the functional monomer to the hard monomer to the soft monomer is 1:13-16:23-26, the mass ratio of the flexible bifunctional monomer to the acrylic monomer is 0.9:100, and the mass ratio of component A, component B, and supramolecular crosslinking agent C is 4.5:9:3. Under these conditions, the cycling stability can be further improved to a stable cycle length of at least 750 cycles.
[0022] The present invention also provides a binder for silicon-carbon / graphite composite negative electrodes prepared according to the above preparation method.
[0023] The present invention also provides an application of the above-mentioned binder for silicon-carbon / graphite composite negative electrode in lithium batteries.
[0024] Compared with the prior art, the present invention has the following superior effects: 1. In this invention, emulsion component A and block component B serve as strong binders for carbon and silicon, respectively. Under the action of supramolecular crosslinking agent C, they form a supramolecular crosslinking amphiphilic binder, achieving stable interfacial compatibility. This binder has excellent adhesion ability (achieving strong adhesion to both silicon and graphite) and mechanical properties (elongation at break of at least 210%). 2. The binder provided by this invention maintains high stability of the binder system during electrode cycling: For example, when the binder provided by this invention is applied to a SiC anode, it can be stably cycled at 1C for at least 550 cycles with a capacity retention of 80% and an average coulombic efficiency of >99%. 3. The adhesive provided by this invention has a simple preparation process, low raw material cost and easy availability, and meets the requirements of green chemistry. Attached Figure Description
[0025] Figure 1 A process flow diagram of the preparation method of the binder for silicon-carbon / graphite composite negative electrode provided by the present invention; Figure 2 This is a comparison chart of the cyclic performance of Application Example 1 and Comparative Example 1. Detailed Implementation
[0026] To better clarify and understand the objectives, process solutions, and advantages of this invention, the technical solutions and implementation methods of this invention will be further described clearly, completely, and in detail below through specific embodiments and in conjunction with the accompanying drawings. It should be understood that the embodiments described in this invention are implemented under the premise of the technical solutions of this invention, providing detailed implementation methods and specific operating procedures, but are only some embodiments of this invention, not all embodiments. The specific implementation methods described are limited to illustrating and explaining this invention and do not limit this invention. Based on the embodiments of this invention, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0027] Unless otherwise specified, the experimental methods and conditions used in the embodiments of this invention are conventional methods and conditions. The materials, reagents, and instruments used in the embodiments, unless otherwise specified, can be obtained commercially or prepared by conventional methods. The reaction conditions described in the invention can all achieve the reactions and obtain the desired products. Due to space limitations, some embodiments are listed below to further illustrate the advantages of the technical solution of this invention.
[0028] Example 1 like Figure 1 As shown, the preparation method of the binder for the silicon-carbon / graphite composite negative electrode provided in this embodiment includes: (1) Add 20g of deionized water to a four-necked flask, heat to 80℃ and keep warm, then add 7.5g of 1wt% APS aqueous solution and stir for 5-10min; (2) In a single-necked flask, add 30g of deionized water, 23g of butyl acrylate, 16g of methyl methacrylate, 1g of acrylic acid, 0.5g of OP-10, and 0.5g of sodium dodecylbenzenesulfonate, and stir until homogeneous to prepare a pre-emulsion. (3) Add 10 wt% of pre-emulsion to a four-necked flask. After the seed emulsion is formed (about 20 min), add the remaining pre-emulsion dropwise into the four-necked flask at a constant rate through a dropping funnel (the addition is completed in about 2 h). Prepare 6.5 g of 2 wt% APS aqueous solution and add it dropwise into the four-necked flask at a constant rate (the addition is completed in about 2 h). After all monomers have been added, keep the temperature for 30 min to end the reaction, and filter to obtain component A. (4) Add 12g N,N-dimethylformamide, 10mg azobisisobutyronitrile, 20mg dithioacetic acid cyanoisopropyl ester, 6.6g acrylic acid and 60mg tri(ethylene glycol) diacrylate to a three-necked flask. After purging the system with nitrogen for 40min, react at 70℃ for 12h. After the reaction is complete, dry the product to obtain component B. (5) Dissolve component A, tannic acid and component B in deionized water at a mass ratio of 3:2:6 and stir for 10 h to obtain an amphiphilic supramolecular crosslinking composite binder (binder for silicon carbon / graphite composite negative electrode).
[0029] Example 2 In step (2), the monomers are replaced with: 23g butyl acrylate, 16g methyl methacrylate, 1g methacrylic acid, and the remaining feed ratios are the same as in Example 1.
[0030] Example 3 In step (2), the monomers are replaced with: 23g butyl acrylate, 3g isooctyl acrylate, 13g methyl methacrylate, 1g acrylic acid, and the remaining feed ratios are the same as in Example 1.
[0031] Example 4 In step (2), the monomers are replaced with: 23g butyl acrylate, 3g hydroxyethyl acrylate, 7g methyl methacrylate, 6g styrene, 1g acrylic acid, and the remaining feed ratios are the same as in Example 1.
[0032] Example 5 In step (2), the monomers are replaced with: 23g butyl acrylate, 3g hydroxyethyl acrylate, 7g ethyl methacrylate, 6g styrene, 1g acrylic acid, and the remaining feed ratios are the same as in Example 1.
[0033] Example 6 In step (4), the monomers are replaced with 6.6g of acrylic acid and 60mg of polyethylene glycol diacrylate, and the remaining feed ratios are the same as in Example 1.
[0034] Example 7 In step (4), the monomers are replaced with 6.6g of acrylic acid and 120mg of tri(ethylene glycol) diacrylate, and the remaining feed ratios are the same as in Example 1.
[0035] Example 8 In step (4), the monomers are replaced with 6.6g of acrylic acid and 30mg of tri(ethylene glycol) diacrylate, and the remaining feed ratios are the same as in Example 1.
[0036] Example 9 In step (5), component A, tannic acid and component B are dissolved in deionized water at a mass ratio of 3:3:9 and stirred for 10 hours to obtain an amphiphilic supramolecular crosslinked composite adhesive.
[0037] Example 10 In step (5), component A, tannic acid and component B are dissolved in deionized water at a mass ratio of 3:1:6 and stirred for 10 hours to obtain an amphiphilic supramolecular crosslinked composite adhesive.
[0038] Application Example 1-10 The active material SiO in a mass ratio of 7:2:1 x C. The conductive agent (acetylene black in this example) is mixed with the binder prepared in Examples 1-10, and stirred in a degassing machine for 30 minutes to obtain a uniformly dispersed slurry. This slurry is then coated onto copper foil and vacuum dried at 80°C for 12 hours to form a circular electrode sheet with a diameter of 14 mm. The electrode sheet is then transferred to an argon-filled glove box for battery assembly. The electrolyte is 1 M / L LiPF6 lithium salt, the solvent is ethylene carbonate (EC) and diethyl carbonate (DEC) in a 1:1 volume ratio, and the additive is 10 wt% fluoroethylene carbonate (FEC). The separator is Celgar 2500, and CR2032 coin cells are used for assembly.
[0039] Peel strength, electrolyte swelling rate, elongation at break and 80% capacity retention cycle number at 1C were tested. The test methods were as follows: (1) Peel strength test: The electrode was placed on the peel strength test equipment and the result was obtained by peeling at 180°. (2) Electrolyte swelling rate: The film was dried and weighed, then soaked in the electrolyte for 24 hours. After wiping off the surface liquid, it was weighed to obtain the swelling rate. (3) Elongation at break: The adhesive was prepared into a dumbbell-shaped film using a mold and tested on a tensile testing machine. The ratio of the length of the film at break minus the original length to the original length was obtained. The test results are detailed in Table 1.
[0040] Table 1 Performance test results of the adhesives prepared in Examples 1-10
[0041] Comparative Example 1 PAA, CMC, and SBR were dissolved in deionized water at a mass ratio of 8:3:2 and stirred for 10 hours to obtain a composite binder. The active material SiO₂ was added at a mass ratio of 7:2:1. x / C, the conductive agent and this binder are mixed and stirred in a degassing machine for 30 minutes to obtain a uniformly dispersed slurry, which is then coated onto copper foil. After vacuum drying at 80°C for 12 hours, a circular electrode sheet with a diameter of 14 mm is formed. Battery assembly is the same as in Application Example 1.
[0042] Comparative Example 2 Components A, CMC, and B from Example 1 were dissolved in deionized water at a mass ratio of 3:2:6 to obtain a composite binder.
[0043] Comparative Example 3 Components A and B from Example 1 were dissolved in deionized water at a mass ratio of 3:6 to obtain a composite binder.
[0044] Comparative Example 4 Component A, tannic acid and component B from Example 1 were dissolved in deionized water at a mass ratio of 3:0.5:6 to obtain a composite binder.
[0045] The test methods are the same as in Application Examples 1-10. The performance test results of the adhesives prepared in Comparative Examples 1-4 are detailed in Table 2.
[0046] Table 2 Performance test results of the binders prepared in Comparative Examples 1-4
[0047] Combining Tables 1 and 2, and Figure 2 The comparison chart of the cycle performance of Application Example 1 and Comparative Example 1 (the capacity of a 1Ah pouch cell remains at 80% of the cycle count at 1C) shows that Examples 1-10 are significantly better than the comparative examples in terms of overall performance.
[0048] The above-described specific embodiments are preferred examples of the present invention. Although they are quite detailed, they do not limit the claims of the present invention. Any changes, modifications, substitutions, combinations, or simplifications made using the technical content disclosed in the present invention should be considered equivalent embodiments and should not depart from the technical features of the present invention. They should all fall within the scope of the technical features of the present invention and should be included within the protection scope of the present invention.
[0049] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a binder for a silicon-carbon / graphite composite negative electrode, characterized in that, Includes the following steps: (1) Preparation of component A by emulsion copolymerization: at least two of the functional monomer, hard monomer and soft monomer are emulsion copolymerized to obtain component A; wherein the functional monomer and soft monomer are both selected from acrylate monomers, and the hard monomer is selected from acrylate monomers and / or styrene; (2) Preparation of component B by controlled free radical polymerization: component B is obtained by controlled free radical polymerization of acrylic acid monomer and flexible bifunctional monomer; (3) Crosslinking: Components A and B are crosslinked using natural polyphenol compounds as supramolecular crosslinking agent C to obtain a binder for silicon-carbon / graphite composite negative electrode.
2. The method for preparing the binder for the silicon-carbon / graphite composite negative electrode according to claim 1, characterized in that, In step (1), the functional monomer is selected from one or more of acrylic acid, methacrylic acid, hydroxyethyl methacrylate or hydroxypropyl methacrylate; the hard monomer is selected from one or more of methyl acrylate, methyl methacrylate or ethyl methacrylate or styrene; and the soft monomer is selected from one or more of ethyl acrylate, isooctyl acrylate, n-butyl acrylate or hydroxyethyl acrylate.
3. The method for preparing the binder for the silicon-carbon / graphite composite negative electrode according to claim 2, characterized in that, In step (1), the mass ratio of the functional monomer: hard monomer: soft monomer is 1:10-16:20-26.
4. The method for preparing the binder for the silicon-carbon / graphite composite negative electrode according to claim 1, characterized in that, In step (1), the emulsion copolymerization is carried out in the presence of an emulsifier and an initiator, the reaction temperature of the emulsion copolymerization is 60-85℃, and the reaction time of the emulsion copolymerization is 1-4h.
5. The method for preparing the binder for the silicon-carbon / graphite composite negative electrode according to claim 1, characterized in that, In step (2), the flexible bifunctional monomer is selected from one or more of polyethylene glycol diacrylate, tri(ethylene glycol) diacrylate, dipropylene glycol diacrylate or polypropylene glycol diacrylate; the mass ratio of the flexible bifunctional monomer to the acrylic monomer is 0.4-2.0:
100.
6. The method for preparing the binder for the silicon-carbon / graphite composite negative electrode according to claim 1, characterized in that, In step (2), the controlled free radical polymerization is carried out in the presence of a chain transfer agent and an initiator; the reaction temperature of the controlled free radical polymerization is 60-80℃, and the reaction time of the controlled free radical polymerization is 5-12h.
7. The method for preparing the binder for the silicon-carbon / graphite composite negative electrode according to claim 1, characterized in that, In step (3), the supramolecular crosslinking agent is selected from tartaric acid or tannic acid, and the mass ratio of component A, component B and supramolecular crosslinking agent C is 3-5:8-9:1-3.
8. The method for preparing the binder for the silicon-carbon / graphite composite negative electrode according to claim 1, characterized in that, The mass ratio of the functional monomer: hard monomer: soft monomer is 1:13-16:23-26, the mass ratio of the flexible bifunctional monomer to the acrylic monomer is 0.45-1.8:100, and the mass ratio of component A, component B and supramolecular crosslinking agent C is 3-4.5:8-9:1.5-3.
9. A binder for a silicon-carbon / graphite composite negative electrode prepared by the preparation method according to any one of claims 1-8.
10. The application of the binder for the silicon-carbon / graphite composite negative electrode according to any one of claims 9 in a lithium battery.
Citation Information
Patent Citations
Silicon-based negative electrode slurry, preparation method thereof and negative electrode plate
CN116230849A
Binder for silicon-carbon negative electrode and lithium ion battery containing binder
CN117777891A