A method for extracting vanadium-molybdenum from vanadium-bearing shale ore
By employing decarbonization roasting, sodium roasting, and sulfuric acid leaching combined with amine and phosphorus extractants in vanadium-shale coal ore, the simultaneous separation and recovery of vanadium and molybdenum in a single liquid phase system is achieved. This solves the problems of molybdenum resource waste and complex processes, improves resource utilization and product purity, and is suitable for petroleum refining and high-end vanadium-based energy storage materials.
Patent Information
- Application Number
- CN202611560060.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, the separation and extraction of vanadium and molybdenum from shale coal vanadium ore is difficult, molybdenum resources are not effectively recovered, resulting in resource waste. Furthermore, traditional processes are complex and costly, and the extractants are not industrially applicable.
After decarbonization roasting, sodium roasting, and sulfuric acid leaching, vanadium and molybdenum are simultaneously separated and recovered in a single liquid phase system by adjusting the pH value and using amine and phosphorus extractants. The anion exchange mechanism of amine extractants and the cation exchange mechanism of phosphorus extractants are used for preliminary impurity removal and deep impurity removal. Finally, high-purity ammonium molybdate and vanadium pentoxide are obtained by evaporation and crystallization.
It achieves efficient and comprehensive utilization of coal mineral resources, simplifies the process flow, improves the efficiency of molybdenum ion separation and recovery, reduces costs, and produces ammonium molybdate and vanadium pentoxide products with a purity of over 99%, which are suitable for petroleum refining hydrogenation catalysts and high-end vanadium-based energy storage materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of vanadium extraction technology from vanadium-bearing coal ore, and specifically to a method for extracting vanadium and molybdenum from vanadium-bearing coal ore. Background Technology
[0002] Shale oil is an important supplementary raw material for the development and utilization of vanadium resources in my country. In addition to vanadium, the ore also contains various valuable metals and impurities such as molybdenum, iron, aluminum, calcium, magnesium, phosphorus, and silicon. Vanadium in shale oil is mostly hosted in the crystal lattice of aluminosilicate minerals, while associated molybdenum exists in a fine-grained disseminated form, closely coexisting with vanadium minerals. The intergrowth relationship between the two is complex, and the overall grade is relatively low. Coupled with the characteristics of the ore having a wide variety of impurities and large fluctuations in their content, the separation, extraction, and refining of vanadium and molybdenum are quite difficult.
[0003] Currently, the mainstream industrial processes for vanadium extraction from coal shale in China all follow a continuous operation process of roasting, leaching, impurity removal, enrichment, and vanadium precipitation. During the leaching stage, vanadium and molybdenum dissolve together with impurity ions such as iron, aluminum, phosphorus, and silicon, forming a complex mixture. However, subsequent processes only focus on enriching, removing impurities, and precipitating vanadium, while the associated molybdenum is never effectively recovered. Ultimately, it is directly discharged with the production tailings and slag, resulting in a serious waste of molybdenum resources and significantly reducing the comprehensive utilization rate of coal shale mineral resources.
[0004] Chinese patent CN121204435B discloses a method for extracting vanadium and molybdenum from shale vanadium ore. This patent involves decarbonizing and roasting, sodium roasting, and acid leaching of shale ore samples to obtain an acid leaching solution and acid leaching residue. Trihexyl(xophiano)phosphonyl chloride is used as the extractant. Based on the differences in the extraction behavior of this extractant for vanadium and molybdenum at different pH ranges, the stepwise extraction, separation, and recovery of molybdenum and vanadium are first completed within the acid leaching solution system. Subsequently, the remaining molybdenum element in the acid leaching residue is further extracted and recovered, ultimately achieving the synergistic recovery of vanadium and molybdenum from shale resources. However, the molybdenum recovery process in this technology is split into two independent steps: acid leaching solution extraction and acid leaching residue re-extraction. The overall process is relatively long and the process connections are complex. Furthermore, the core extractant, trihexyl(xophiano)phosphonyl chloride, is not a commonly used industrial extractant in hydrometallurgy, and its market procurement cost is much higher than that of conventional extractants, resulting in high extraction costs. Summary of the Invention
[0005] The purpose of this invention is to provide a method for extracting vanadium and molybdenum from vanadium shale ore. This method is simple, has a short process, and can simultaneously and efficiently extract vanadium and molybdenum from vanadium shale ore, thereby effectively improving the comprehensive utilization rate of vanadium shale ore resources.
[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for extracting vanadium-molybdenum from vanadium shale ore includes the following steps: Step S01: Crush and decarbonize the coal ore, add sodium salt, and perform sodium roasting to obtain roasted material; add the roasted material to acid solution for leaching to obtain acid leaching solution, and oxidize the acid leaching solution to obtain extraction solution; Step S02: Adjust the pH of the extraction solution to 1.5-1.8, use an amine extraction system for extraction, take the extract, use an alkaline solution to back-extract the extract, and take the back-extract as a low-impurity vanadium-molybdenum solution. Step S03: Adjust the pH of the low-impurity vanadium-molybdenum solution to 8.5-9.5, add magnesium salt for dephosphorization, adjust the pH to 2-2.5, use a phosphorus extraction system for extraction, collect the raffinate, reduce the raffinate to obtain a high-purity vanadium-molybdenum solution. Step S04: Adjust the pH of the high-purity vanadium-molybdenum solution to 1.5-1.8, and use an amine extraction system for extraction. Take the extract and raffinate as the molybdenum-rich solution and the vanadium-containing solution, respectively. Use ammonia water to back-extract the molybdenum-rich solution, take the back-extract, evaporate, crystallize, filter, and dry the back-extract to obtain ammonium molybdate. Oxidize the vanadium-containing solution, adjust the pH to 2-3, add ammonium salt for precipitation, filter, and calcine to obtain vanadium pentoxide.
[0007] Preferably, in step S01, during crushing, the particle size after crushing is 0.1-1 mm; During decarburization roasting, the temperature is 650-700℃ and the time is 10-20 minutes; The sodium salt is sodium chloride; The amount of sodium salt added is 5-10% of the mass of the decarbonized roasted coal ore; In the sodium calcination process, the sodium calcination temperature is 850-900℃ and the sodium calcination time is 1-2 hours. The acid solution is a sulfuric acid solution with a mass concentration of 2-5%; The liquid-to-solid ratio of acid solution to calcined material is 2-4 mL: 1 g; During leaching, the leaching temperature is 60-90℃ and the leaching time is 1-2 hours; In the oxidation process, the oxidant is either sodium chlorate or hydrogen peroxide. During oxidation, the amount of oxidant added is 0.05-0.1 times the molar amount of vanadium ions in the acid leaching solution; During oxidation, the oxidation time is 0.5-1 hour.
[0008] Furthermore, in step S01, after leaching, the filter cake is washed with water at a ratio of 0.1-0.3 times the mass of the calcined material, and the washing liquid and filtrate are collected and mixed as an acid leaching solution.
[0009] Preferably, in step S02, the amine extraction system consists of an amine extractant, bis(2,4,4-trimethylpentyl)-thiophosphonic acid (Cyanex302), and sulfonated kerosene, wherein the volume ratio of the amine extractant, bis(2,4,4-trimethylpentyl)-thiophosphonic acid, and sulfonated kerosene is 15-30:5:65-80, and the amine extractant is one of trialkylamine (N235) and trioctylamine (TOA); When using an amine extraction system, the extraction ratio O / A is 1:3-6; When using an amine extraction system, the extraction time is 5-10 minutes. The alkaline solution is one of sodium hydroxide solution, ammonia water, sodium carbonate solution, or ammonium bicarbonate solution, and the concentration of the alkaline solution is 1-2 mol / L. When back-extracting the extract using an alkaline solution, the back-extraction ratio O / A is 1-2:1; When back-extracting the extract using an alkaline solution, a three-stage countercurrent back-extraction method is employed.
[0010] Furthermore, in step S02, an amine extraction system is used for extraction. After taking the extract, it is washed with water for 5-10 minutes, with an O / A ratio of 4-6:1 during washing.
[0011] Preferably, in step S03, the magnesium salt is magnesium chloride; The amount of magnesium salt added is 1.1-1.2 times the molar amount of phosphorus in the low-impurity vanadium-molybdenum solution; During dephosphorization, the dephosphorization time is 10-30 minutes.
[0012] Preferably, in step S03, the phosphorus extraction system consists of a phosphorus extractant, tributyl phosphate (TBP), and sulfonated kerosene, wherein the volume ratio of the phosphorus extractant, tributyl phosphate (TBP), and sulfonated kerosene is 15-30:5:65-80, the phosphorus extractant is one of dioctyl phosphate (P204) or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester (P507), and the saponification degree of the phosphorus extractant is 30-80%. When using a phosphorus-based extraction system, the extraction ratio O / A is 1:3-6; When using a phosphorus-based extraction system, the extraction time is 5-10 minutes.
[0013] Preferably, in step S03, when reducing the raffinate, the reduction method is to adjust the pH of the raffinate to 1.5-1.8, add 1-1.5 times the molar amount of sodium sulfite of vanadium, stir to dissolve, adjust the pH to 1.5-1.8, and reduce for 2-4 hours.
[0014] Preferably, in step S04, the amine extraction system consists of an amine extractant, tributyl phosphate (TBP), and sulfonated kerosene, wherein the volume ratio of the amine extractant, tributyl phosphate (TBP), and sulfonated kerosene is 15-30:5:65-80, and the amine extractant is one of trialkylamine (N235) and trioctylamine (TOA). When using an amine extraction system, the extraction ratio O / A is 1:4-8; After extraction using an amine extraction system, the extract is collected and washed with water for 5-10 minutes, with an O / A ratio of 4-6:1 during washing.
[0015] Preferably, in step S04, the concentration of ammonia is 1-3 mol / L; When using ammonia to back-extract molybdenum-rich solutions, the back-extraction ratio (O / A) is 3-5:1. When using ammonia water for back-extraction of molybdenum-rich solution, a three-stage countercurrent back-extraction method is employed. The evaporation is vacuum evaporation, with a temperature of 40-60℃ and a vacuum degree of 0.06-0.08MPa. During crystallization, the crystallization temperature is 20-30℃ and the crystallization time is 10-12h; The drying process is vacuum drying, with a temperature of 40-50℃ and a drying time of 3-6 hours.
[0016] Preferably, in step S04, during oxidation, the oxidant is hydrogen peroxide, and the amount of hydrogen peroxide added is 1.05-1.1 times the molar amount of vanadium ions in the vanadium-containing solution; During oxidation, the oxidation time is 0.5-1 hour; The ammonium salt is ammonium chloride; The amount of ammonium salt added is 1.1-1.2 times the molar amount of vanadium ions in the vanadium-containing solution.
[0017] Preferably, in step S04, the precipitation temperature is 90-100℃ and the precipitation time is 0.5-1h. During roasting, the roasting temperature is 400-500℃ and the roasting time is 2-3 hours.
[0018] Furthermore, in step S04, after precipitation, the sediment is aged, filtered, and washed. The aging temperature is 100℃, the aging time is 0.5-1h, and the washing is done with deionized water.
[0019] The beneficial effects of this invention are as follows: (1) This invention removes carbonaceous components from the shale coal by decarbonization roasting, fully exposing valuable minerals such as vanadium-containing mica; then, vanadium and molybdenum are activated simultaneously by sodium roasting, so that they are fully converted into soluble sodium salts; subsequently, vanadium-molybdenum mixed acid leaching solution is obtained by sulfuric acid leaching, so that the vanadium and molybdenum elements present in the shale coal mine enter the acid leaching solution, and then the residual low-valent vanadium in the acid leaching solution system is converted into pentavalent vanadate ions by oxidation process, which creates favorable conditions for the efficient separation of vanadium and molybdenum in the future.
[0020] (2) In this invention, after adjusting the pH value of the extraction solution, the anion exchange mechanism of amine extractant is used to allow pentavalent vanadium ions and molybdenum ions to enter the organic phase in anionic form simultaneously, while more than 95% of cationic impurities such as iron and aluminum are retained in the raffinate, thus completing the enrichment and preliminary removal of vanadium and molybdenum ions in one step, so that the enrichment and removal processes are carried out efficiently and simultaneously. Then, the cation exchange mechanism of phosphorus extractant is used to deeply remove cationic impurities carried in the extraction process of amine extractant, so as to obtain high-purity vanadium-molybdenum solution. Finally, by utilizing the difference in valence state of vanadium and molybdenum ions in the high-purity vanadium-molybdenum solution before and after reduction, the efficient separation and simultaneous recovery of vanadium and molybdenum ions are achieved.
[0021] (3) In this invention, molybdenum in the coal mine can be leached into the acid leaching solution simultaneously with vanadium, and the separation and recovery of vanadium and molybdenum can be completed directly in a single liquid phase system. Compared with the traditional acid leaching-ammonia leaching process for vanadium and molybdenum extraction, which involves extracting vanadium and a small amount of molybdenum from the acid leaching solution first, and then using ammonia leaching to extract residual molybdenum from the acid leaching residue, the solution of this invention can significantly shorten the process flow and significantly improve the efficiency of molybdenum ion separation and recovery.
[0022] (4) In this invention, the extractants used in the amine extraction system and the phosphorus extraction system are conventional industrial extractants that are mass-produced in the field of hydrometallurgy. There are no expensive special reagents throughout the process, the cost is controllable, and the economy is good.
[0023] (5) The method of the present invention has the advantages of simple process and short process, and can realize the separation and recovery of vanadium and molybdenum at the same time. Compared with the prior art, it significantly improves the separation efficiency of vanadium and molybdenum, and the purity of the vanadium pentoxide and ammonium molybdate products prepared is over 99%. Vanadium pentoxide can be directly adapted to the demand scenarios of high-purity vanadium raw materials such as all-vanadium redox flow battery electrolyte and high-end vanadium-based energy storage materials. Ammonium molybdate can be directly applied to industrial fields such as petroleum refining hydrogenation catalyst preparation and special alloy smelting, which greatly enhances the comprehensive utilization value of coal resources. Detailed Implementation
[0024] The present invention will be further illustrated below with reference to examples. It should be understood that these embodiments are merely illustrative and are not intended to limit the scope of the present invention.
[0025] Embodiments of the present invention provide a method for extracting vanadium and molybdenum from vanadium shale ore, comprising the following steps: Step S01: Crush and decarbonize the coal ore, add sodium salt, and perform sodium roasting to obtain roasted material; add the roasted material to acid solution for leaching to obtain acid leaching solution, and oxidize the acid leaching solution to obtain extraction solution; Step S02: Adjust the pH of the extraction solution to 1.5-1.8, use an amine extraction system for extraction, take the extract, use an alkaline solution to back-extract the extract, and take the back-extract as a low-impurity vanadium-molybdenum solution. Step S03: Adjust the pH of the low-impurity vanadium-molybdenum solution to 8.5-9.5, add magnesium salt for dephosphorization, adjust the pH to 2-2.5, use a phosphorus extraction system for extraction, collect the raffinate, reduce the raffinate to obtain a high-purity vanadium-molybdenum solution. Step S04: Adjust the pH of the high-purity vanadium-molybdenum solution to 1.5-1.8, and use an amine extraction system for extraction. Take the extract and raffinate as the molybdenum-rich solution and the vanadium-containing solution, respectively. Use ammonia water to back-extract the molybdenum-rich solution, take the back-extract, evaporate, crystallize, filter, and dry the back-extract to obtain ammonium molybdate. Oxidize the vanadium-containing solution, adjust the pH to 2-3, add ammonium salt for precipitation, filter, and calcine to obtain vanadium pentoxide.
[0026] Preferably, in step S01, the particle size after crushing is 0.1-1 mm.
[0027] Preferably, in step S01, the decarburization roasting temperature is 650-700℃ and the time is 10-20min.
[0028] Preferably, in step S01, the sodium salt is sodium chloride.
[0029] Preferably, in step S01, the amount of sodium salt added is 5-10% of the mass of the decarbonized roasted coal ore.
[0030] Preferably, in step S01, the sodium calcination temperature is 850-900℃ and the sodium calcination time is 1-2h.
[0031] Preferably, in step S01, the acid solution is a sulfuric acid solution with a mass concentration of 2-5%.
[0032] Preferably, in step S01, the liquid-to-solid ratio of the acid solution to the calcining material is 2-4 mL:1 g.
[0033] Preferably, in step S01, the leaching temperature is 60-90℃ and the leaching time is 1-2h.
[0034] Furthermore, in step S01, after leaching, the filter cake is washed with water at a ratio of 0.1-0.3 times the mass of the calcined material, and the washing liquid and filtrate are collected and mixed as an acid leaching solution.
[0035] Preferably, in step S01, the oxidant used in the oxidation process is either sodium chlorate or hydrogen peroxide.
[0036] Preferably, in step S01, during oxidation, the amount of oxidant added is 0.05-0.1 times the molar amount of vanadium ions in the acid leaching solution.
[0037] Preferably, in step S01, the oxidation time is 0.5-1h.
[0038] Preferably, in step S02, the amine extraction system consists of an amine extractant, bis(2,4,4-trimethylpentyl)-thiophosphonic acid (Cyanex302), and sulfonated kerosene, wherein the volume ratio of the amine extractant, bis(2,4,4-trimethylpentyl)-thiophosphonic acid, and sulfonated kerosene is 15-30:5:65-80, and the amine extractant is one of trialkylamine (N235) and trioctylamine (TOA).
[0039] Preferably, in step S02, when using an amine extraction system for extraction, the extraction ratio O / A is 1:3-6.
[0040] Preferably, in step S02, when using an amine extraction system for extraction, the extraction time is 5-10 minutes.
[0041] Preferably, in step S02, the alkaline solution is one of sodium hydroxide solution, ammonia water, sodium carbonate solution, and ammonium bicarbonate solution, and the concentration of the alkaline solution is 1-2 mol / L.
[0042] Preferably, in step S02, when back-extracting the extract with alkali solution, the back-extraction ratio O / A is 1-2:1.
[0043] Preferably, in step S02, when back-extracting the extract with alkaline solution, a three-stage countercurrent back-extraction method is used.
[0044] Furthermore, in step S02, an amine extraction system is used for extraction. After taking the extract, it is washed with water for 5-10 minutes, with an O / A ratio of 4-6:1 during washing.
[0045] Preferably, in step S03, the magnesium salt is magnesium chloride.
[0046] Preferably, in step S03, the amount of magnesium salt added is 1.1-1.2 times the molar amount of phosphorus in the low-impurity vanadium-molybdenum solution.
[0047] Preferably, in step S03, the dephosphorization time is 10-30 min.
[0048] Preferably, in step S03, the phosphorus extraction system consists of a phosphorus extractant, tributyl phosphate (TBP), and sulfonated kerosene, wherein the volume ratio of the phosphorus extractant, tributyl phosphate (TBP), and sulfonated kerosene is 15-30:5:65-80, the phosphorus extractant is one of dioctyl phosphate (P204) or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester (P507), and the saponification degree of the phosphorus extractant is 30-80%.
[0049] Preferably, in step S03, when using a phosphorus-based extraction system for extraction, the extraction ratio O / A is 1:3-6.
[0050] Preferably, in step S03, when using a phosphorus-based extraction system for extraction, the extraction time is 5-10 minutes.
[0051] Preferably, in step S03, when reducing the raffinate, the reduction method is to adjust the pH of the raffinate to 1.5-1.8, add 1-1.5 times the molar amount of sodium sulfite of vanadium, stir to dissolve, adjust the pH to 1.5-1.8, and reduce for 2-4 hours.
[0052] Preferably, in step S04, the amine extraction system consists of an amine extractant, tributyl phosphate (TBP), and sulfonated kerosene, wherein the volume ratio of the amine extractant, tributyl phosphate (TBP), and sulfonated kerosene is 15-30:5:65-80, and the amine extractant is one of trialkylamine (N235) and trioctylamine (TOA).
[0053] Preferably, in step S04, when using an amine extraction system for extraction, the extraction ratio O / A is 1:4-8.
[0054] Preferably, in step S04, after extraction using an amine extraction system, the extract is washed with water for 5-10 minutes, with an O / A ratio of 4-6:1 during washing.
[0055] Preferably, in step S04, the concentration of ammonia is 1-3 mol / L.
[0056] Preferably, in step S04, when using ammonia to back-extract the molybdenum-rich solution, the back-extraction ratio O / A is 3-5:1.
[0057] Preferably, in step S04, when using ammonia to back-extract the molybdenum-rich solution, a three-stage countercurrent back-extraction method is adopted.
[0058] Preferably, in step S04, the evaporation is vacuum evaporation, the temperature of vacuum evaporation is 40-60℃, and the vacuum degree is 0.06-0.08MPa.
[0059] Preferably, in step S04, the crystallization temperature is 20-30℃ and the crystallization time is 10-12h.
[0060] Preferably, in step S04, the drying is vacuum drying, the temperature of vacuum drying is 40-50℃, and the vacuum drying time is 3-6 hours.
[0061] Preferably, in step S04, during oxidation, the oxidant is hydrogen peroxide, and the amount of hydrogen peroxide added is 1.05-1.1 times the molar amount of vanadium ions in the vanadium-containing solution.
[0062] Preferably, in step S04, the oxidation time is 0.5-1h.
[0063] Preferably, in step S04, the ammonium salt is ammonium chloride.
[0064] Preferably, in step S04, the amount of ammonium salt added is 1.1-1.2 times the molar amount of vanadium ions in the vanadium-containing solution.
[0065] Preferably, in step S04, the precipitation temperature is 90-100℃ and the precipitation time is 0.5-1h.
[0066] Furthermore, in step S04, after precipitation, the sediment is aged, filtered, and washed. The aging temperature is 100℃, the aging time is 0.5-1h, and the washing is done with deionized water.
[0067] Preferably, in step S04, the roasting temperature is 400-500℃ and the roasting time is 2-3h.
[0068] The main components of a certain coal sample used in subsequent embodiments and comparative examples are shown in Table 1: Table 1. Main components of a coal mine sample.
[0069] In subsequent examples and comparative examples, before using TOA / N235, it was first pre-acidified with a 1 mol / L sulfuric acid solution. During pre-acidification, the O / A ratio was controlled to be 1:1. After pre-acidification, TOA / N235 was protonated into an amine salt before being used in the preparation of the amine extraction system.
[0070] In the subsequent examples and comparative examples, the leaching rate in the acid leaching solution is calculated using the following formula: Leaching rate (%) = (volume of acid leaching solution × concentration of target ion in acid leaching solution) / (mass of coal sample before roasting × content of target ion in ore sample) × 100%; When using an amine extraction system, the formula for calculating the extraction rate in the resulting extract is as follows: Extraction rate (%) = (Target ion content in the original extract - Target ion content in the raffinate) / Target ion content in the original extract × 100%; When using sodium hydroxide solution for back-extraction, the formula for calculating the back-extraction rate in the resulting low-impurity vanadium-molybdenum solution (back-extraction solution) is as follows: Back-extraction rate (%) = Target ion content in back-extraction solution / [(Target ion content in original extract - Target ion content in raffinate) / Extraction ratio (O / A) × Back-extraction ratio (O / A)] × 100%.
[0071] Example 1 A sample from a coal mine was crushed to a particle size of 0.1 mm using a jaw crusher and a double roll crusher. It was then decarburized and roasted at 700℃ for 10 min, allowed to cool naturally, and 10% sodium chloride was added. The sample was then soda-roasted at 850℃ for 2 h and allowed to cool naturally to obtain the roasted material.
[0072] The calcined material was added to a 5% sulfuric acid solution (mass fraction) at a liquid-to-solid ratio of 3 mL:1 g, and leached at 90℃ for 2 hours. The solution was filtered, and the filtrate was collected. The filter cake was washed once with water equal to 0.2 times the mass of the calcined material. The washing liquid and filtrate were mixed to obtain an acid leaching solution. The vanadium leaching rate was 91.36%, and the molar ... Table 2. Concentrations of various ions in the extract solution Unit: mg / L
[0073] The pH of the extraction solution was adjusted to 1.8 with sodium hydroxide. At an extraction ratio of O / A = 1:5, 20% TOA + 5% Cyanex 302 + 75% sulfonated kerosene (amine extraction system) was added by volume and extracted for 6 minutes to achieve preliminary separation and enrichment of vanadium and molybdenum ions. The extraction rates were 99.23% for vanadium ions, 99.32% for molybdenum ions, 2.86% for iron ions, 0.25% for aluminum ions, and 12.5% for phosphorus ions. Over 95% of the cation impurities such as iron and aluminum remained in the raffinate, while vanadium and molybdenum ions entered the extract. The extract contained only a small amount of impurity ions. The extract was washed with water at an O / A ratio of 5:1 for 6 min, and then subjected to three-stage countercurrent back-extraction with a 1 mol / L sodium hydroxide solution at an O / A ratio of 1:1. This achieved efficient back-extraction of vanadium and molybdenum ions, yielding a low-impurity vanadium-molybdenum solution. The vanadium ion back-extraction rate in the obtained low-impurity vanadium-molybdenum solution was 99.82%, the molybdenum ion back-extraction rate was 99.72%, and the concentrations of vanadium ions, molybdenum ions, and phosphorus ions in the obtained low-impurity vanadium-molybdenum solution were 10.39 g / L, 0.44 g / L, and 1.69 g / L.
[0074] The low-impurity vanadium-molybdenum solution was adjusted to pH 8.5 with 98% concentrated sulfuric acid (mass fraction), resulting in a phosphorus ion concentration of 1.69 g / L. Magnesium chloride with 1.2 times the molar amount of phosphorus was added, and the mixture was stirred for 20 min. The solution was then filtered, and the filtrate was collected. The phosphorus removal rate was 91.12%, the residual phosphorus concentration in the filtrate was 150 mg / L, the vanadium ion loss rate was 0.8%, and the molybdenum ion loss rate was 0.5%. The filtrate was then adjusted to pH 2.0 with sulfuric acid. At an extraction ratio of O / A = 1:5, a saponification degree of 60% was achieved by adding 20% P₂O₄ + 5% TBP + 75% sulfonium chloride solution. Extraction with kerosene (phosphorus extraction system) for 6 min removes calcium and other metal ions. The concentration of calcium, iron, aluminum and other metal impurities in the raffinate is controlled below 10 mg / L. Vanadium and molybdenum ions are not co-extracted during the process and remain in the raffinate. The pH of the raffinate is adjusted to 1.5 with 98% concentrated sulfuric acid (mass fraction), and 1.2 times the molar amount of vanadium sodium sulfite is added. The mixture is stirred to dissolve, and the pH is adjusted to 1.5. After reduction for 4 h, a high-purity vanadium-molybdenum solution is obtained. The vanadium ion concentration in the high-purity vanadium-molybdenum solution is 10.12 g / L, and the molybdenum ion concentration is 0.43 g / L. The pH of the high-purity vanadium-molybdenum solution was adjusted to 1.5. Then, 20% TOA + 5% TBP + 75% sulfonated kerosene were added by volume at an extraction ratio of O / A = 1:5 for 6 min. The molybdenum extraction rate was 99.86%, and the vanadium co-extraction rate was 0.082%, yielding a molybdenum-containing extract and a vanadium-containing solution. The molybdenum-containing extract was washed with water at an O / A ratio of 5:1 for 6 min, and then back-extracted with a 2.5 mol / L ammonia solution at a back-extraction ratio of O / A = 3:1 in a three-stage countercurrent process to obtain an ammonium molybdate solution with a molybdenum ion concentration of 6.42 g / L and a molybdenum ion back-extraction rate of 99.75%. The ammonium molybdate solution was evaporated under reduced pressure at 40℃ and 0.08 MPa until saturation, cooled to 25℃ for constant temperature crystallization for 10 h, filtered, and vacuum dried at 40℃ for 6 h to obtain the ammonium molybdate product with a purity of 99.36%. The ion concentrations in the obtained ammonium molybdate solution are shown in Table 3. Table 3 Ion concentrations in ammonium molybdate solution: Unit: mg / L
[0075] The ion concentrations in the obtained vanadium-containing solution are shown in Table 4: Table 4 Vanadium-containing liquid ion concentration Unit: mg / L
[0076] As shown in Table 4, the vanadium concentration in the vanadium-containing solution was 10.01 g / L. Hydrogen peroxide with 1.05 times the molar amount of vanadium was added, and the mixture was stirred for 0.5 h to oxidize the tetravalent vanadium to the pentavalent vanadium. The pH was adjusted to 2.5 with ammonia, and ammonium chloride with 1.1 times the molar amount of vanadium was added. The mixture was stirred at 100℃ for 1 h, aged at 100℃ for 1 h, filtered, and ammonium metavanadate was obtained. The product was washed twice with deionized water and calcined at 500℃ for 2 h to obtain vanadium pentoxide with a purity of 99.62%.
[0077] Example 2 A sample from a coal mine was crushed to a particle size of 0.1 mm using a jaw crusher and a double roll crusher. It was then decarburized and roasted at 650℃ for 20 min, allowed to cool naturally, and 10% sodium chloride was added. The sample was then soda-roasted at 900℃ for 2 h and allowed to cool naturally to obtain the roasted material.
[0078] The calcined material was added to a 5% sulfuric acid solution (mass fraction) at a liquid-to-solid ratio of 4 mL:1 g, and leached at 90℃ for 2 hours. The solution was filtered, and the filtrate was collected. The filter cake was washed once with water equal to 0.2 times the mass of the calcined material. The washing liquid and filtrate were mixed to obtain an acid leaching solution. The vanadium leaching rate was 90.72%, and the molybdenum leaching rate was 94.58%. Hydrogen peroxide, equal to 0.05 times the molar amount of vanadium, was added to the acid leaching solution, and the mixture was stirred for 1 hour to oxidize the residual low-valent vanadium to pentavalent vanadium, thus obtaining the extraction solution. The ion concentrations in the extraction solution are shown in Table 5. Table 5. Concentrations of various ions in the extract. Unit: mg / L
[0079] The pH of the extraction solution was adjusted to 1.5 with sodium hydroxide. At an extraction ratio of O / A = 1:6, 15% N235 + 5% Cyanex 302 + 80% sulfonated kerosene (amine extraction system) was added by volume and extracted for 6 minutes to achieve preliminary separation and enrichment of vanadium and molybdenum ions. The extraction rates were 99.02% for vanadium ions, 99.29% for molybdenum ions, 4.36% for iron ions, 3.04% for aluminum ions, and 11.08% for phosphorus ions. Over 95% of the cationic impurities such as iron and aluminum remained in the raffinate, while vanadium and molybdenum ions entered the raffinate. The extract contained only a small amount of impurity ions. The extract was washed with water at an O / A ratio of 5:1 for 6 minutes, and then subjected to a three-stage countercurrent back-extraction process using a 2 mol / L sodium carbonate solution at an O / A ratio of 1.5:1. This process achieved efficient back-extraction of vanadium and molybdenum ions, yielding a low-impurity vanadium-molybdenum solution. The vanadium ion back-extraction rate in the resulting low-impurity vanadium-molybdenum solution was 99.12%, the molybdenum ion back-extraction rate was 99.78%, and the concentrations of vanadium ions, molybdenum ions, and phosphorus ions were 14.20 g / L, 0.61 g / L, and 1.22 g / L, respectively.
[0080] The low-impurity vanadium-molybdenum solution was adjusted to pH 9.5 with 98% concentrated sulfuric acid (mass fraction), resulting in a phosphorus ion concentration of 1.22 g / L. Magnesium chloride with 1.15 times the molar amount of phosphorus was added, and the mixture was stirred for 20 min. The solution was then filtered, and the filtrate was collected. The phosphorus removal rate was 90.38%, the residual phosphorus concentration in the filtrate was 118 mg / L, the vanadium ion loss rate was 0.92%, and the molybdenum ion loss rate was 0.35%. The filtrate was then adjusted to pH 2.0 with sulfuric acid. 25% P2O4+ with a saponification degree of 60% was added by volume at an extraction ratio of O / A = 1:4. Extraction with 5% TBP and 70% sulfonated kerosene for 6 minutes removes calcium and other metal ions. The concentration of calcium, iron, aluminum and other metal impurities in the raffinate is controlled below 10 mg / L. Vanadium and molybdenum ions are not co-extracted during the process and remain in the raffinate. The pH of the raffinate is adjusted to 1.5 with 98% concentrated sulfuric acid (mass fraction), and 1.5 times the molar amount of sodium sulfite is added. After stirring and dissolving, the pH is adjusted to 1.5, and after reduction for 4 hours, a high-purity vanadium-molybdenum solution is obtained with a vanadium ion concentration of 14.02 g / L and a molybdenum ion concentration of 0.59 g / L.
[0081] The pH of a high-purity vanadium-molybdenum solution was adjusted to 1.8. Then, 25% N235 + 5% TBP + 70% sulfonated kerosene were added by volume at an extraction ratio of O / A = 1:6 for 6 min. The molybdenum extraction rate was 99.85%, and the vanadium co-extraction rate was 0.058%, yielding a molybdenum-containing extract and a vanadium-containing solution. The extract was washed with water at an O / A ratio of 5:1 for 6 min, and then back-extracted with a 2 mol / L ammonia solution at a back-extraction ratio of O / A = 3:1 in a three-stage countercurrent process to obtain an ammonium molybdate solution with a molybdenum ion concentration of 10.57 g / L and a molybdenum ion back-extraction rate of 99.75%. The ammonium molybdate solution was evaporated under reduced pressure at 60℃ and 0.08 MPa until saturation, cooled to 25℃ for constant temperature crystallization for 10 h, filtered, and vacuum dried at 50℃ for 6 h to obtain the ammonium molybdate product with a purity of 99.47%. The ion concentrations in the obtained ammonium molybdate solution are shown in Table 6. Table 6 Ion Concentrations of Ammonium Molybdate Solution Unit: mg / L
[0082] The ion concentrations in the obtained vanadium-containing solution are shown in Table 7: Table 7 Vanadium-containing liquid ion concentration Unit: mg / L
[0083] As shown in Table 7, the vanadium concentration in the vanadium-containing solution was 13.72 g / L. Hydrogen peroxide with a molar amount of 1.05 times that of vanadium was added, and the mixture was stirred for 1 hour to oxidize the tetravalent vanadium into the pentavalent vanadium. The pH was adjusted to 2.0 with ammonia water, and ammonium chloride with a molar amount of 1.2 times that of vanadium was added. The mixture was stirred at 90°C for 1 hour, aged at 100°C for 1 hour, filtered, and ammonium metavanadate was obtained. After washing twice with deionized water, the product was calcined at 500°C for 3 hours to obtain vanadium pentoxide with a purity of 99.53%.
[0084] Example 3 A sample from a coal mine was crushed to a particle size of 1 mm using a jaw crusher and a double roll crusher. It was then decarburized and roasted at 650℃ for 20 minutes, allowed to cool naturally, and 10% sodium chloride was added. The sample was then soda-roasted at 900℃ for 1 hour and allowed to cool naturally to obtain the roasted material.
[0085] The calcined material was added to a 5% sulfuric acid solution (mass fraction) at a liquid-to-solid ratio of 2 mL:1 g, and leached at 60℃ for 2 h. The solution was filtered, and the filtrate was collected. The filter cake was washed once with water equal to 0.2 times the mass of the calcined material. The washing liquid and filtrate were mixed to obtain an acid leaching solution. The vanadium leaching rate was 93.62%, and the molybdenum leaching rate was 96.82%. Hydrogen peroxide, with a molar weight equal to that of vanadium, was added to the acid leaching solution, and the mixture was stirred for 1 h to oxidize the residual low-valent vanadium to pentavalent vanadium, thus obtaining the extraction solution. The concentrations of various ions in the extraction solution are shown in Table 8. Table 8. Summary of Ion Concentrations in the Extract Solution Unit: mg / L
[0086] The pH of the extraction solution was adjusted to 1.5 with sodium hydroxide. At an extraction ratio of O / A = 1:6, 30% N235 + 5% Cyanex 302 + 65% sulfonated kerosene (amine extraction system) was added by volume and extracted for 6 minutes to achieve preliminary separation and enrichment of vanadium and molybdenum ions. The extraction rates were 99.16% for vanadium ions, 99.50% for molybdenum ions, 2.86% for iron ions, 0.29% for aluminum ions, and 12.5% for phosphorus ions. Over 95% of the cationic impurities such as iron and aluminum remained in the raffinate, while vanadium and molybdenum ions... The extract contains only a small amount of impurity ions. The extract is washed with water at an O / A ratio of 5:1 for 6 minutes, and then back-extracted with 2 mol / L ammonia water at an O / A ratio of 1:1 in a three-stage countercurrent process. This achieves efficient back-extraction of vanadium and molybdenum ions, resulting in a low-impurity vanadium-molybdenum solution. The vanadium ion back-extraction rate in the obtained low-impurity vanadium-molybdenum solution is 99.42%, the molybdenum ion back-extraction rate is 99.32%, and the concentrations of vanadium ions, molybdenum ions, and phosphorus ions in the obtained low-impurity vanadium-molybdenum solution are 19.10 g / L, 0.80 g / L, and 1.95 g / L.
[0087] The low-impurity vanadium-molybdenum solution was adjusted to pH 9.5 with 98% concentrated sulfuric acid (mass fraction), resulting in a phosphorus ion concentration of 1.95 g / L. Magnesium chloride with a phosphorus ion molar ratio of 1.1 was added, and the mixture was stirred for 20 min. After filtration, the filtrate was collected, showing a phosphorus removal rate of 94.44%, a residual phosphorus concentration of 108 mg / L, a vanadium ion loss rate of 1%, and a molybdenum ion loss rate of 0.8%. The filtrate was then adjusted to pH 2.5 with sulfuric acid, and 30% P507+ with a saponification degree of 30% was added by volume at an extraction ratio of O / A = 1:3. Extraction with 5% TBP and 65% sulfonated kerosene for 6 minutes removes calcium and other metal ions. The concentration of calcium, iron, aluminum and other metal impurities in the raffinate is controlled below 10 mg / L. Vanadium and molybdenum ions are not co-extracted during the process and remain in the raffinate. The pH of the raffinate is adjusted to 1.8 with 98% concentrated sulfuric acid (mass fraction), and an equal molar amount of sodium sulfite is added. The mixture is stirred to dissolve, and the pH is adjusted to 1.5. After reduction for 2 hours, a high-purity vanadium-molybdenum solution is obtained with a vanadium ion concentration of 18.73 g / L and a molybdenum ion concentration of 0.79 g / L.
[0088] The pH of the high-purity vanadium-molybdenum solution was adjusted to 1.5. Then, 30% N235 + 5% TBP + 65% sulfonated kerosene were added by volume at an extraction ratio of O / A = 1:8 for 6 min. The molybdenum extraction rate was 99.75%, and the vanadium co-extraction rate was 0.072%, yielding a molybdenum-containing extract and a vanadium-containing solution. The extract was washed with water at an O / A ratio of 5:1 for 6 min, and then back-extracted with a 3 mol / L ammonia solution at a three-stage countercurrent extraction ratio of O / A = 3:1 to obtain an ammonium molybdate solution with a molybdenum ion concentration of 18.84 g / L and a molybdenum ion back-extraction rate of 99.58%. The ammonium molybdate solution was evaporated under reduced pressure at 50℃ and 0.06 MPa until saturation, cooled to 25℃ for constant temperature crystallization for 10 h, filtered, and vacuum dried at 50℃ for 3 h to obtain the ammonium molybdate product with a purity of 99.52%. The ion concentrations in the obtained ammonium molybdate solution are shown in Table 9. Table 9 Ion Concentrations of Ammonium Molybdate Solution Unit: mg / L
[0089] The ion concentrations in the obtained vanadium-containing solution are shown in Table 10: Table 10 Vanadium-containing liquid ion concentration Unit: mg / L
[0090] As shown in Table 10, the vanadium concentration in the vanadium-containing solution was 18.69 g / L. Hydrogen peroxide with 1.1 times the molar amount of vanadium was added, and the mixture was stirred for 1 hour to oxidize the tetravalent vanadium into the pentavalent vanadium. The pH was adjusted to 3.0 with ammonia water, and ammonium chloride with 1.1 times the molar amount of vanadium was added. The mixture was stirred at 90°C for 0.6 hours, aged at 100°C for 0.5 hours, filtered, and ammonium metavanadate was obtained. After washing twice with deionized water, the product was calcined at 450°C for 3 hours to obtain vanadium pentoxide with a purity of 99.51%.
[0091] Example 4 A sample of a certain coal mine was crushed to a particle size of 0.5 mm by a jaw crusher and a double roll crusher, then decarburized and roasted at 700℃ for 20 min, allowed to cool naturally, 5% sodium chloride was added, and the sample was sodaified and roasted at 850℃ for 2 h, and then allowed to cool naturally to obtain the roasted material.
[0092] The calcined material was added to a 2% sulfuric acid solution (mass fraction) at a liquid-to-solid ratio of 2 mL:1 g, and leached at 90℃ for 1 h. The solution was then filtered, and the filtrate was collected. The filter cake was washed once with water equal to 0.2 times the mass of the calcined material. The washing liquid and filtrate were mixed to obtain an acid leaching solution. The vanadium leaching rate was 95.36%, and the molar ... Table 11 Concentrations of various ions in the extract solution Unit: mg / L
[0093] The pH of the extraction solution was adjusted to 1.8 with sodium hydroxide. At an extraction ratio of O / A = 1:3, 15% TOA + 5% Cyanex 302 + 80% sulfonated kerosene (amine extraction system) was added by volume and extracted for 6 minutes to achieve preliminary separation and enrichment of vanadium and molybdenum ions. The extraction rates were 99.28% for vanadium ions, 99.59% for molybdenum ions, 3.21% for iron ions, 0.34% for aluminum ions, and 16.9% for phosphorus ions. Over 95% of the iron, aluminum, and other cationic impurities remained in the raffinate. The vanadium and molybdenum ions enter the extract, carrying only a small amount of impurity ions. The extract is washed with water at an O / A ratio of 5:1 for 6 minutes, and then back-extracted with ammonium bicarbonate at a concentration of 2 mol / L using a three-stage countercurrent back-extraction method with an O / A ratio of 2:1. This achieves efficient back-extraction of vanadium and molybdenum ions, with a vanadium ion back-extraction rate of 99.43% and a molybdenum ion back-extraction rate of 99.85%. The resulting low-impurity vanadium-molybdenum solution has a vanadium ion concentration of 19.73 g / L, a molybdenum ion concentration of 0.81 g / L, and a phosphorus ion concentration of 2.52 g / L.
[0094] The low-impurity vanadium-molybdenum solution was adjusted to pH 9.0 with 98% concentrated sulfuric acid (mass fraction), resulting in a phosphorus ion concentration of 2.52 g / L. Magnesium chloride with 1.2 times the molar amount of phosphorus ions was added, and the mixture was stirred for 10 min. After filtration, the filtrate was collected, showing a phosphorus removal rate of 93.12%, a residual phosphorus concentration of 173 mg / L, a vanadium ion loss rate of 0.76%, and a molybdenum ion loss rate of 0.52%. The filtrate was then adjusted to pH 2.0 with sulfuric acid. At an extraction ratio of O / A = 1:6, 15% P507 + 5% T (80% saponification degree) was added by volume. Extraction with BP + 80% sulfonated kerosene (phosphorus extraction system) for 6 min removes calcium and other metal ions. The concentration of calcium, iron, aluminum and other metal impurities in the raffinate is controlled below 10 mg / L. Vanadium and molybdenum ions are not co-extracted during the process and remain in the raffinate. The pH of the raffinate is adjusted to 1.5 with 98% concentrated sulfuric acid (mass fraction), and an equal molar amount of sodium sulfite is added. The mixture is stirred to dissolve, and the pH is adjusted to 1.5. After reduction for 3 h, a high-purity vanadium-molybdenum solution is obtained with a vanadium ion concentration of 19.48 g / L and a molybdenum ion concentration of 0.80 g / L.
[0095] The pH of the high-purity vanadium-molybdenum solution was adjusted to 1.8. Then, 15% TOA + 5% TBP + 80% sulfonated kerosene were added by volume at an extraction ratio of O / A = 1:4 for 6 min. The molybdenum extraction rate was 99.80%, and the vanadium co-extraction rate was 0.067%, yielding a molybdenum-containing extract and a vanadium-containing solution. The extract was washed with water at an O / A ratio of 5:1 for 6 min, and then back-extracted with a 1 mol / L ammonia solution at a three-stage countercurrent extraction ratio of O / A = 5:1 to obtain an ammonium molybdate solution with a molybdenum ion concentration of 16.32 g / L and a molybdenum ion back-extraction rate of 99.88%. The ammonium molybdate solution was evaporated under reduced pressure at 50℃ and 0.06 MPa until saturation, cooled to 25℃ for 12 h of constant-temperature crystallization, filtered, and vacuum dried at 50℃ for 6 h to obtain the ammonium molybdate product with a purity of 99.58%. The ion concentrations in the obtained ammonium molybdate solution are shown in Table 12. Table 12 Summary of Ion Concentrations in Ammonium Molybdate Solution Unit: mg / L
[0096] The ion concentrations in the obtained vanadium-containing solution are shown in Table 13: Table 13 Summary of Vanadium-Containing Liquid Ion Concentration Unit: mg / L
[0097] As shown in Table 13, the vanadium concentration in the vanadium-containing solution was 19.42 g / L. Hydrogen peroxide with 1.1 times the molar amount of vanadium was added, and the mixture was stirred for 1 hour to oxidize the tetravalent vanadium into the pentavalent vanadium. The pH was adjusted to 2.0 with ammonia water, and ammonium chloride with 1.2 times the molar amount of vanadium was added. The mixture was stirred at 100°C for 0.5 hours, aged at 100°C for 1 hour, filtered, and ammonium metavanadate was obtained. The product was washed twice with deionized water and calcined at 500°C for 3 hours to obtain vanadium pentoxide with a purity of 99.64%.
[0098] Comparative Example 1 The same process as in Example 1 was used to prepare the extraction solution for the extraction of vanadium and molybdenum ions. However, when extracting the extraction solution, the extraction system composition was 25% TOA + 75% sulfonated kerosene, that is, the amine extraction system used did not contain 5% Cyanex 302. The other conditions were the same as in Example 1.
[0099] The results showed that the vanadium ion extraction rate was 88.23%, and the molybdenum ion extraction rate was 99.65%, indicating a significant decrease in the vanadium ion extraction rate. Analysis revealed that in sulfuric acid medium with a pH less than 2, pentavalent vanadium mainly exists as VO2+. + It exists in the form of vanadium; some vanadium complexes with sulfate to form VO2SO4. - Anions. The amine extractant TOA, which utilizes anion exchange mechanisms, can extract VO2SO4. - This process achieves the extraction of most of the vanadium within the system, but some VO2 still exists in the form of cationic ions. + It cannot be captured by anionic extractants. Introducing a small amount of Cyanex 302 into the extraction system allows the P=OH group of Cyanex 302 to react with the R3N-H group of the protonated TOA. + Intermolecular hydrogen bonds are formed, with hydrogen atoms on the P-SH in Cyanex 302 serving as active exchange sites, and residual VO2 is achieved through a cation exchange mechanism. + This improves the overall extraction efficiency of vanadium in the system.
[0100] Comparative Example 2 Low-impurity vanadium-molybdenum solution was prepared using the same process as in Example 1, except that after phosphorus removal using the same process, sodium sulfite reduction was omitted, i.e., the reduction step was eliminated, and instead, extraction was performed directly using 20% TOA + 5% TBP + 75% sulfonated kerosene. The results showed that the molybdenum extraction rate was 99.86%, and the vanadium extraction rate was 77.81%. A large amount of vanadium ions were co-extracted into the organic phase. Analysis revealed that after ammonia back-extraction, some vanadium ions entered the back-extraction solution along with molybdenum, resulting in the inability to achieve effective separation of vanadium and molybdenum. The reason for this is that in the unreduced solution after phosphorus removal, vanadium exists as a pentavalent oxyacid anion, which can be extracted by anionic amine extractants. After reduction, pentavalent vanadium is converted to tetravalent vanadium cations and is no longer extracted by anionic extractants. Molybdenum, however, exists in solution as anion both before and after reduction. By utilizing the change in the morphology and charge of vanadium ions before and after reduction, while the charge of molybdenum ions remains unchanged, efficient separation of vanadium and molybdenum ions was achieved.
[0101] The above embodiments are merely preferred results of the present invention and do not limit the scope of the present invention. All modifications, equivalent substitutions, improvements, and other variations and modifications made in accordance with the scope of this application should be covered within the scope of protection of the present invention.
Claims
1. A method for extracting vanadium-molybdenum from vanadium-bearing shale ore, characterized in that, Includes the following steps: Step S01: Crush and decarbonize the coal ore, add sodium salt, and perform sodium roasting to obtain roasted material; The roasted material is added to an acid solution for leaching to obtain an acid leaching solution. The acid leaching solution is then oxidized to obtain the original extract. Step S02: Adjust the pH of the extraction solution to 1.5-1.8, use an amine extraction system for extraction, take the extract, use an alkaline solution to back-extract the extract, and take the back-extract as a low-impurity vanadium-molybdenum solution. Step S03: Adjust the pH of the low-impurity vanadium-molybdenum solution to 8.5-9.5, add magnesium salt for dephosphorization, adjust the pH to 2-2.5, use a phosphorus extraction system for extraction, collect the raffinate, reduce the raffinate to obtain a high-purity vanadium-molybdenum solution. Step S04: Adjust the pH of the high-purity vanadium-molybdenum solution to 1.5-1.8, and use an amine extraction system for extraction. Take the extract and raffinate as the molybdenum-rich solution and the vanadium-containing solution, respectively. Use ammonia water to back-extract the molybdenum-rich solution, take the back-extract, evaporate, crystallize, filter, and dry the back-extract to obtain ammonium molybdate. Oxidize the vanadium-containing solution, adjust the pH to 2-3, add ammonium salt for precipitation, filter, and calcine to obtain vanadium pentoxide.
2. The method for extracting vanadium and molybdenum from vanadium shale ore according to claim 1, characterized in that, In step S01, during crushing, the particle size after crushing is 0.1-1mm; During decarburization roasting, the temperature is 650-700℃ and the time is 10-20 minutes; The sodium salt is sodium chloride; The amount of sodium salt added is 5-10% of the mass of the decarbonized roasted coal ore; In the sodium calcination process, the sodium calcination temperature is 850-900℃ and the sodium calcination time is 1-2 hours. The acid solution is a sulfuric acid solution with a mass concentration of 2-5%; The liquid-to-solid ratio of acid solution to calcined material is 2-4 mL: 1 g; During leaching, the leaching temperature is 60-90℃ and the leaching time is 1-2 hours; In the oxidation process, the oxidant is either sodium chlorate or hydrogen peroxide. During oxidation, the amount of oxidant added is 0.05-0.1 times the molar amount of vanadium ions in the acid leaching solution; During oxidation, the oxidation time is 0.5-1 hour.
3. The method for extracting vanadium and molybdenum from vanadium shale ore according to claim 1, characterized in that, In step S02, the amine extraction system consists of an amine extractant, bis(2,4,4-trimethylpentyl)thiophosphonic acid, and sulfonated kerosene. The volume ratio of the amine extractant, bis(2,4,4-trimethylpentyl)thiophosphonic acid, and sulfonated kerosene is 15-30:5:65-80. The amine extractant is one of trialkylamine or trioctylamine. When using an amine extraction system, the extraction ratio O / A is 1:3-6; When using an amine extraction system, the extraction time is 5-10 minutes. The alkaline solution is one of sodium hydroxide solution, ammonia water, sodium carbonate solution, or ammonium bicarbonate solution, and the concentration of the alkaline solution is 1-2 mol / L. When back-extracting the extract using an alkaline solution, the back-extraction ratio O / A is 1-2:1; When back-extracting the extract using an alkaline solution, a three-stage countercurrent back-extraction method is employed.
4. The method for extracting vanadium and molybdenum from vanadium shale ore according to claim 1, characterized in that, In step S03, the magnesium salt is magnesium chloride; The amount of magnesium salt added is 1.1-1.2 times the molar amount of phosphorus in the low-impurity vanadium-molybdenum solution; During dephosphorization, the dephosphorization time is 10-30 minutes.
5. The method for extracting vanadium-molybdenum from vanadium-bearing shale ore according to claim 1, characterized in that, In step S03, the phosphorus extraction system consists of a phosphorus extractant, tributyl phosphate, and sulfonated kerosene. The volume ratio of the phosphorus extractant, tributyl phosphate, and sulfonated kerosene is 15-30:5:65-80. The phosphorus extractant is one of dioctyl phosphate or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester, and the saponification degree of the phosphorus extractant is 30-80%. When using a phosphorus-based extraction system, the extraction ratio O / A is 1:3-6; When using a phosphorus-based extraction system, the extraction time is 5-10 minutes.
6. The method for extracting vanadium-molybdenum from vanadium-bearing shale according to claim 1, characterized in that, In step S03, when reducing the raffinate, the reduction method is to adjust the pH of the raffinate to 1.5-1.8, add 1-1.5 times the molar amount of sodium sulfite of vanadium, stir to dissolve, adjust the pH to 1.5-1.8, and reduce for 2-4 hours.
7. The method for extracting vanadium-molybdenum from vanadium-bearing shale ore according to claim 1, characterized in that, In step S04, the amine extraction system consists of an amine extractant, tributyl phosphate, and sulfonated kerosene, wherein the volume ratio of the amine extractant, tributyl phosphate, and sulfonated kerosene is 15-30:5:65-80, and the amine extractant is one of trialkylamine or trioctylamine. When using an amine extraction system, the extraction ratio O / A is 1:4-8; After extraction using an amine extraction system, the extract is collected and washed with water for 5-10 minutes, with an O / A ratio of 4-6:1 during washing.
8. The method for extracting vanadium-molybdenum from vanadium-bearing shale according to claim 1, characterized in that, In step S04, the concentration of ammonia is 1-3 mol / L; When using ammonia to back-extract molybdenum-rich solutions, the back-extraction ratio (O / A) is 3-5:
1. When using ammonia water for back-extraction of molybdenum-rich solution, a three-stage countercurrent back-extraction method is employed. The evaporation is vacuum evaporation, with a temperature of 40-60℃ and a vacuum degree of 0.06-0.08MPa. During crystallization, the crystallization temperature is 20-30℃ and the crystallization time is 10-12h; The drying process is vacuum drying, with a temperature of 40-50℃ and a drying time of 3-6 hours.
9. The method for extracting vanadium and molybdenum from vanadium shale ore according to claim 1, characterized in that, In step S04, during oxidation, the oxidant is hydrogen peroxide, and the amount of hydrogen peroxide added is 1.05-1.1 times the molar amount of vanadium ions in the vanadium-containing solution. During oxidation, the oxidation time is 0.5-1 hour; The ammonium salt is ammonium chloride; The amount of ammonium salt added is 1.1-1.2 times the molar amount of vanadium ions in the vanadium-containing solution.
10. The method for extracting vanadium-molybdenum from vanadium shale ore according to claim 1, characterized in that, During precipitation, the precipitation temperature is 90-100℃ and the precipitation time is 0.5-1h; During roasting, the roasting temperature is 400-500℃ and the roasting time is 2-3 hours.
Citation Information
Patent Citations
A method for extracting vanadium-molybdenum from vanadium-bearing shale ore
CN121204435B