Var melting process for producing high purity titanium

By employing a three-stage adaptive current melting and directional argon beam arc stabilization control, the problems of arc drift and vacuum fluctuation in the VAR melting of high-purity titanium were solved, enabling the preparation of high-purity, high-quality ingots.

CN123063631APending Publication Date: 2026-11-10CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202611554665.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The existing VAR melting process for preparing high-purity titanium suffers from problems such as arc drift causing molten pool tumbling, high subcutaneous porosity, and independent vacuum and current control, making it difficult to meet high purity requirements and also resulting in excessive interstitial elements.

Method used

A three-stage adaptive current melting process is adopted, combined with local arc stabilization control of directional argon beam, and vacuum degree and current linkage regulation. Through deep degassing of high-purity sponge titanium electrode and gradient water cooling solidification, a full-link impurity control process is formed.

Benefits of technology

It significantly reduces subcutaneous porosity and interstitial impurity content, improves finished product yield, ensures uniformity of ingot composition and head quality, and enhances process stability and adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063631A_ABST
    Figure CN123063631A_ABST
Patent Text Reader

Abstract

The application discloses a VAR smelting process, in particular to a VAR smelting process for preparing high-purity pure titanium, and belongs to the technical field of vacuum smelting of titanium metal. The application provides a VAR smelting process for preparing high-purity pure titanium, which can significantly reduce vacuum fluctuation, and the vacuum degree control and the current control can be adapted to each other, and the molten pool state can be dynamically matched. The VAR smelting process uses high-purity titanium sponge electrodes as consumable electrodes, adopts three-stage self-adaptive current smelting including an arc striking stage, a main smelting stage and a feeding stage in a vacuum furnace, and outputs the high-purity pure titanium liquid that meets the smelting requirements to a crystallizer to obtain high-purity pure titanium ingots by gradient directional water cooling solidification, finally, the high-purity pure titanium is prepared by heat preservation cooling, furnace discharge and continuous cooling, the vacuum degree in the furnace is coupled and controlled by the input directional argon beam and the smelting current of the corresponding smelting sub-stage, and is matched with the dynamic state of the molten pool of the corresponding sub-stage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a VAR melting process, and more particularly to a VAR melting process for preparing high-purity titanium, belonging to the field of titanium metal vacuum smelting technology. Background Technology

[0002] Vacuum self-consuming arc melting (VAR) is the mainstream industrial method for preparing titanium and titanium alloy ingots. Its basic principle is that in a vacuum environment, a self-consuming electrode is used as the cathode and a water-cooled copper crystallizer is used as the anode. The high temperature generated by the DC arc gradually melts the electrode tip, and the molten droplets fall into the crystallizer and solidify into ingots [1].

[0003] For industrial pure titanium such as TA2, especially for high-purity titanium (oxygen content ≤500ppm, or ≤300ppm when lower requirements are needed) for cold-rolled thin sheets, high-end medical, and electronic applications, the existing VAR smelting process has three major technical pain points that are difficult to avoid: (1) Arc drift causes the molten pool to roll and air to be trapped, forming subcutaneous pores. When pure titanium is melted in a vacuum environment, the electric arc is prone to drift, diverge and oscillate, causing the molten pool to churn violently, and gas is drawn into the surface of the molten metal, forming a large number of subcutaneous pore defects after solidification. Luo Wenzhong et al. [2] showed through numerical simulation that the stability of the electric arc during VAR melting directly affects the surface quality of the ingot, and the electric arc deviation and molten pool fluctuation are the main causes of surface cold shuts and subcutaneous pores.

[0004] In current production, AC arc stabilization is commonly used to assist in arc stabilization. Chinese patent CN115896472A[3] discloses an argon-filled melting method for titanium alloy ingots, in which 10-50Pa of argon gas is filled before the arc-starting stage, and argon is continued to be filled during the stabilization melting stage, with the aim of suppressing the volatilization of alloy elements. Chinese patent CN113174501B[4] discloses a method to improve the visibility and stability of the argon-filled melting process of titanium alloys, with an argon filling pressure as high as 15000Pa, which is also aimed at the titanium alloy system. However, high-pressure argon filling will cause a large amount of argon gas and the impurities it carries to dissolve in the titanium liquid, resulting in a significant increase in the content of interstitial elements (especially oxygen, hydrogen, and nitrogen) in pure titanium, which cannot meet the purity requirements of high-purity titanium at all.

[0005] (2) Defects at each stage are caused by constant current or simple segmented current. Traditional pure titanium VAR melting often adopts constant current mode (such as 28kA for primary melting and 38kA for secondary melting), or simply divides it into three stages of stepped current: arc initiation, main melting, and shrinkage compensation. Each stage is independently controlled and not matched with the dynamic state of the molten pool. Chinese patent CN113088719B[5] discloses a melting method to improve the bottom quality of VAR titanium alloy primary ingots. It uses segmented current control to improve the bottom quality, but it only targets the bottom of the primary ingot and does not involve the current-vacuum linkage of the entire process. Chinese patent CN105039760A[6] discloses a shrinkage compensation method for titanium alloy ingot melting. It uses a stepped current reduction method for shrinkage compensation, but it only targets the shrinkage compensation stage and is for titanium alloy systems.

[0006] Existing segmented current technology has the following problems: ① Excessive current during the arc ignition stage causes instantaneous arc impact, resulting in splashing and air entrapment; ② The current is constant during the main smelting stage and cannot be dynamically adjusted according to the depth of the molten pool and the height of the liquid surface, which leads to overheating and oxygenation of the molten pool and component segregation; ③ During the feeding stage, the current drops sharply or decreases in a simple stepwise manner, which can easily cause shrinkage cavities and looseness in the center of the ingot.

[0007] Jing Zhenquan et al. [7] showed that VAR smelting process parameters (especially smelting current and molten pool depth) have a significant impact on the macrosegregation of titanium alloy ingots, and excessively deep molten pools will exacerbate element segregation.

[0008] (3) Vacuum degree and current are independently controlled, and vacuum fluctuations affect the quality of ingot casting. In the existing technology, vacuum degree control and current control are two independent systems, lacking linkage matching logic. In actual production, the vacuum degree has intermittent small fluctuations, and the vacuum degree of secondary melting often exceeds the requirements of the scheme (≤1.1Pa), and some furnaces even reach 3 to 4Pa. Vacuum fluctuations directly lead to unstable molten pool, poor degassing effect, and insufficient uniformity of ingots. Cao Rui et al. [8] pointed out in their analysis of deoxidation in the VAR melting process of titanium and titanium alloys that the stability of vacuum degree directly affects the deoxidation effect of the melting process and the final interstitial element content.

[0009] The literature contains a simple segmentation idea of ​​"low vacuum for arc initiation and high vacuum for melting," but this is only a rough switching method. It does not accurately control the vacuum gradient according to the dynamic state of the molten pool, nor does it have adaptive linkage with the current, making it difficult to achieve coordinated control of low porosity and low gap impurities.

[0010] In addition, although electrode pretreatment (vacuum baking degassing) and crystallizer cooling (partitioned water cooling) are mentioned sporadically—such as patent CN105238936A[9] which involves the structure of water-cooled crystallizers—they are all single processes or equipment structures, lacking a complete set of processes from electrode degassing to melting arc control and solidification segregation control. Huang Liqing et al.

[10] studied the influence of electromagnetic field on flow field and segregation during the VAR process of titanium alloys, but did not involve the coupling control of vacuum-current-arc stabilization. Guo Jie et al.

[11] studied the transmission behavior of macrosegregation during three VAR melting processes, further confirming the limitations of single parameter optimization.

[0011] Summary of the main shortcomings of existing technologies: ① The effect of AC arc stabilization is limited, and arc drift leads to many subcutaneous pores, resulting in a serious over-extraction of skin. ② The high-pressure argon-filled arc stabilization scheme for titanium alloys (CN113174501B, CN115896472A, etc.) is not suitable for high-purity titanium, as it will cause the interstitial element content to exceed the standard. ③ The short-term argon purging scheme for pure titanium arc initiation cannot solve the problems of arc drift and microporosity in the main melting stage; ④ The current segment (CN113088719B, CN105039760A, etc.) is independent of the vacuum segment and does not form a coupled control logic; ⑤ There is a lack of a complete set of low-oxygen and low-porosity impurity control processes for high-purity titanium, covering the entire chain from electrode to solidification.

[0012] References: [1] Deoxidation analysis of VAR melting process of titanium and titanium alloys [J]. Cao Rui, Li Nan, Lü Huajiang et al. Metal World, 2021 (4): 49-52; [2] Numerical simulation method was used to analyze the factors affecting the surface quality of VAR smelted titanium alloy ingots [J]. Luo Wenzhong, Zhao Xiaohua, Liu Peng et al. Rare Metals Materials and Engineering, 2020, 49 (3):927-932; [3] Titanium alloy ingot and its preparation method [P]. Chinese Patent: CN115896472A, 2023-04-04; [4] A method for improving visibility and stability in the argon-filled melting process of titanium alloys [P]. Chinese Patent: CN113174501B, 2022-08-02; [5] A smelting method for improving the bottom quality of VAR titanium alloy primary ingots [P]. Chinese Patent: CN113088719B, 2023-03-28; [6] A method for feeding and melting TC4-DT titanium alloy ingots with a diameter of Φ720~Φ1000mm [P]. Chinese Patent: CN105039760A, 2015-11-11; [7] Influence of process parameters of vacuum consumable melting of titanium alloy TC4 on macrosegregation [J]. Jing Zhenquan, Sun Yanhui, Liu Rui et al. Rare Metals Materials and Engineering, 2023, 52 (3):815-822; [8] Deoxidation analysis of VAR melting process of titanium and titanium alloys [J]. Cao Rui, Li Nan, Lü Huajiang et al. Metal World, 2021 (4): 49-52; [9] A vacuum consumable electrode arc melting and drawing device for smelting metal materials [P]. Chinese Patent: CN105238936A, 2016-01-13;

[10] Influence of self-induced electromagnetic field on flow field and segregation behavior during VAR process of titanium alloy [J]. Huang Liqing, Wu Jingyang, Guo Jie et al. Iron & Steel Vanadium Titanium, 2023, 44 (4):55-61;

[11] Macroscopic segregation transport behavior during the three-stage vacuum arc melting process of titanium alloys [J]. Guo Jie, Huang Liqing, Wu Jingyang, et al. Acta Metallurgica Sinica, 2024, 60 (11): 1531-15. Summary of the Invention

[0013] The technical problem to be solved by the present invention is to provide a VAR melting process for preparing high-purity titanium that can significantly reduce vacuum fluctuations, allow vacuum degree control and current control to adapt to each other, and dynamically match the state of the molten pool.

[0014] The technical solution adopted to solve the above-mentioned technical problems is: a VAR melting process for preparing high-purity titanium. The VAR melting process uses a high-purity sponge titanium electrode that has passed pressure degassing as a consumable electrode. In a vacuum furnace, a three-stage adaptive current melting process is employed, sequentially including an arc-ignition stage, a main melting stage, and a feeding stage. The melted high-purity titanium liquid is then output to a crystallizer where it undergoes gradient-directional water cooling and solidification to obtain a high-purity titanium ingot. Finally, the ingot is held at the desired temperature, cooled, and then further cooled after being removed from the furnace to complete the preparation of high-purity titanium. The main melting stage consists of three sub-melting stages: the molten pool formation stage, the steady-state melting stage, and the molten pool expansion stage. During the melting process of each sub-melting stage, the vacuum level inside the furnace is adaptively coupled and controlled by the input directional argon beam with the melting current of the corresponding melting sub-stage, and adaptively matched with the dynamic state of the molten pool in the corresponding sub-stage. Throughout the entire melting process, the furnace cavity is maintained at a relatively high vacuum of no more than 3 Pa. Argon gas is only applied locally to the core area of ​​the electric arc in the form of a directional beam, without being diffused throughout the entire area.

[0015] Furthermore, the arc initiation stage employs a medium-vacuum substrate combined with a directional micro-argon beam for soft arc initiation. The specific process and requirements are as follows: The furnace cavity is evacuated to a medium vacuum state of 3-6 Pa. Then, a small amount of high-purity argon gas is directionally introduced into the core area of ​​the electric arc through a directional argon beam nozzle at a flow rate of 0.1-0.5 L / min, so that the argon partial pressure in the local area of ​​the electric arc is maintained at 10-50 Pa, while the entire furnace cavity remains in a medium vacuum state. The arc ignition current is 3-7 kA, and a low-current, slow-speed soft arc ignition is adopted, with an arc ignition time of 7-9 minutes.

[0016] The preferred method of the above scheme is that the argon beam nozzle is located above the electrode side, with an angle of 15°-30° with the vertical direction, and the diameter of the argon beam is controlled at 10-30mm, covering only the core area of ​​the electric arc, without full-area diffusion gas filling.

[0017] Furthermore, during the molten pool formation period, the vacuum level inside the smelting furnace, the smelting current, and the dynamic state of the molten pool are linked, matched, and controlled according to the following requirements: The vacuum level in the furnace cavity is gradually increased from medium vacuum to high vacuum of 1.5-3 Pa; a directional argon beam is continuously introduced at a flow rate of 0.05-0.2 L / min, with local partial pressure of 5-20 Pa in the arc zone; the melting current is increased from 7 kA to 26-28 kA for primary melting or 36-38 kA for secondary melting, with the rate of increase divided into three stages: 0.5 kA / min for the first 10 kA, 1 kA / min for the middle 10-20 kA, and 2 kA / min for the final 20 kA to the target current; the vacuum level is increased synchronously with the current, and the vacuum level in the furnace cavity decreases by 5%-10% for every 1 kA increase in current, dynamically matching the expansion process of the molten pool.

[0018] The preferred method of the above scheme is that the vacuum degree inside the smelting furnace during the steady-state smelting period is linked and matched with the smelting current and the dynamic state of the molten pool according to the following requirements: The furnace cavity vacuum is controlled at a high vacuum of 0.8-1.5 Pa, with continuous deep degassing; the directional argon beam flow rate is reduced to 0.02-0.1 L / min, and the local partial pressure in the arc zone is 2-10 Pa; the melting current is stabilized at 27-28 kA for the first melting or 37-38 kA for the second melting, and the current is finely adjusted in real time according to the height of the molten pool to ensure consistent depth and uniform solidification, with an adjustment range of ±0.5 kA; the arc position offset is monitored in real time by an arc sensor, and when the offset exceeds 5 mm, the argon beam flow rate and direction are automatically finely adjusted to bring the arc back to the center.

[0019] Furthermore, during the molten pool expansion period, the vacuum level inside the smelting furnace, the smelting current, and the dynamic state of the molten pool are linked, matched, and controlled according to the following requirements: The furnace cavity vacuum is controlled at 0.5-1.0 Pa; the directional argon beam flow rate is reduced to 0.01-0.05 L / min, and the local partial pressure in the arc zone is 1-5 Pa; the melting current is gradually reduced from 28 kA for the first melting or 38 kA for the second melting to 20-22 kA for the first melting or 30-32 kA for the second melting, with a reduction rate of 0.5-1 kA / min; the vacuum level increases synchronously with the decrease in current, and the furnace cavity vacuum level decreases by 8%-15% for every 1 kA decrease in current.

[0020] The preferred method of the above scheme is to use a small-amplitude vacuum voltage stabilization + stepped current reduction delay to obtain a high-purity titanium billet with complete elimination of shrinkage cavities at the head and central porosity defects in the pure titanium ingot under high vacuum conditions during the feeding stage. The total time for delayed melting and feeding is 200-300 minutes.

[0021] Furthermore, the small-amplitude vacuum voltage stabilization employs intermittent directional argon beam injection to maintain arc stability. The specific process of small-amplitude vacuum voltage stabilization combined with stepped current reduction and time-delayed melt preservation is as follows: The vacuum level in the furnace cavity was slightly adjusted to a stable 1.0-2.0 Pa. Argon beams were introduced intermittently every 30 seconds for 2 seconds at a flow rate of 0.01-0.03 L / min to maintain the arc basically stable. The compensation current was reduced from 20-22 kA in the first stage or 30-32 kA in the second stage to 3-5 kA in 4-6 stages, with each stage held for 30 minutes to achieve delayed melting.

[0022] The preferred method of the above scheme is that the gradient directional water cooling solidification ingot in the crystallizer adopts the upper and lower partition gradient water cooling control to solidify the pure titanium ingot sequentially from bottom to top. The cooling water volume of the upper part is 0.6-0.8 times that of the lower part, the inlet water temperature is controlled at 25-30℃, and the outlet water temperature is controlled at 37-41℃.

[0023] Furthermore, the production of high-purity sponge titanium consumable electrodes by pressing and degassing is carried out according to the following steps: First, high-purity sponge titanium of grade 0A or grade 0 is pressed into a consumable electrode. The diameter of one side of the consumable electrode is 40-100 mm smaller than the diameter of the crystallizer. Then, the consumable electrode is placed in a vacuum baking furnace for high-vacuum long-term baking and degassing. The baking temperature is 280-350℃, the holding time is 6-12 hours, and the vacuum degree is ≤0.5Pa. This yields a consumable electrode with surface adsorbed water, hydroxyl groups and trace adsorbed oxygen removed.

[0024] The beneficial effects of this invention are as follows: The technical solution provided in this application, during the entire melting process using high-purity sponge titanium electrodes as consumable electrodes, achieves adaptive linkage control between the input directional argon beam and the melting current of the corresponding melting sub-stage, and adaptive matching with the dynamic state of the molten pool in the corresponding sub-stage. Furthermore, the furnace cavity is maintained at a relatively high vacuum of no more than 3 Pa throughout the entire melting process, with argon gas acting only locally on the arc core region in the form of a directional beam, without full-area diffusion. This not only significantly reduces vacuum fluctuations but also allows vacuum and current control to adapt to each other, and the molten pool state to be dynamically matched. This effectively solves the problems of high subcutaneous porosity and excessive interstitial impurities caused by arc drift and molten pool tumbling in the main stage of existing high-purity titanium VAR melting, achieving the goal of effectively reducing or even eliminating axial or radial component segregation and head shrinkage porosity in finished high-purity titanium ingots, thus significantly improving the yield of finished products. Attached Figure Description

[0025] Figure 1 The flowchart of the VAR melting process for preparing high-purity titanium in this invention shows the complete 7-step process from electrode pretreatment to cooling and unloading, with the core features of each stage clearly marked. Figure 2 This is a schematic diagram of the directional argon beam arc stabilization structure involved in the VAR melting process for preparing high-purity titanium according to the present invention. It shows the relative positional relationship of the consumable electrode, the arc core region, the directional argon beam nozzle, the argon beam, the molten pool, and the crystallizer. The argon beam nozzle is obliquely pointed to the arc core region at an angle of about 20°, and only local arc stabilization is achieved without diffusion. Figure 3 This is a schematic diagram of the gradient water-cooling structure of the crystallizer involved in the VAR melting process for preparing high-purity titanium according to the present invention. It shows the partitioned structure of the crystallizer cylinder, the upper weak cooling water-cooling zone, and the lower strong cooling water-cooling zone. The cooling water volume in the upper part is 0.6-0.8 times that in the lower part, so as to achieve sequential solidification from bottom to top. Detailed Implementation

[0026] like Figure 1 , Figure 2 as well as Figure 3 This invention illustrates a VAR (Vacuum Aperture Reduction) melting process for preparing high-purity titanium, which significantly reduces vacuum fluctuations, allows for mutual adaptation between vacuum and current control, and dynamically matches the molten pool state. The VAR melting process uses a high-purity sponge titanium electrode that has passed pressure degassing as a consumable electrode. In a vacuum furnace, it employs a three-stage adaptive current melting process, sequentially including an arc-ignition stage, a main melting stage, and a feeding stage. The melted high-purity titanium liquid is then output to a crystallizer where it undergoes gradient-directional water cooling and solidification to obtain a high-purity titanium ingot. Finally, the ingot is held at the furnace for cooling and further cooling to complete the preparation of high-purity titanium. The main melting stage consists of three sub-melting stages: the molten pool formation stage, the steady-state melting stage, and the molten pool expansion stage. During the melting process of each sub-melting stage, the vacuum level inside the furnace is adaptively coupled and controlled by the input directional argon beam with the melting current of the corresponding melting sub-stage, and adaptively matched with the dynamic state of the molten pool in the corresponding sub-stage. Throughout the entire melting process, the furnace cavity is maintained at a relatively high vacuum of no more than 3 Pa. Argon gas only acts locally on the core region of the arc in the form of a directional beam, without being diffused throughout the entire process. The technical solution provided in this application achieves this by adaptively coupling the input directional argon beam with the melting current of the corresponding melting sub-stage and adaptively matching it with the dynamic state of the molten pool in the corresponding sub-stage throughout the entire melting process. Moreover, the furnace cavity is maintained at a relatively high vacuum of no more than 3 Pa throughout the entire melting process, and argon gas only acts locally on the core region of the arc in the form of a directional beam, without being diffused throughout the entire process. This not only significantly reduces vacuum fluctuations, but also allows vacuum degree control and current control to adapt to each other, and the molten pool state to be dynamically matched. This effectively solves the problems of high subcutaneous porosity and excessive interstitial impurities caused by arc drift and molten pool tumbling in the main stage of existing high-purity titanium VAR melting. It effectively reduces or even eliminates axial or radial component segregation and head shrinkage porosity in finished high-purity titanium ingots, thus significantly improving the yield of finished products.

[0027] Accordingly, in order to improve the reliability of each step of the operation and the quality of the finished high-purity titanium ingot, the arc initiation stage of this application adopts a medium-vacuum substrate + directional micro-argon beam soft arc initiation. The specific process and requirements are as follows. The furnace cavity is evacuated to a medium vacuum state of 3-6 Pa. Then, a small amount of high-purity argon gas is directionally introduced into the arc core area through a directional argon beam nozzle at a flow rate of 0.1-0.5 L / min, maintaining the argon partial pressure in the local arc area at 10-50 Pa, while the entire furnace cavity remains in a medium vacuum state. The arc ignition current is 3-7 kA, employing low-current, slow-speed soft arc ignition, with an ignition time of 7-9 minutes. During the molten pool formation period, the vacuum state inside the furnace, the molten current, and the dynamic state of the molten pool are linked and controlled according to the following requirements. The furnace vacuum level is gradually increased from medium vacuum to high vacuum of 1.5-3 Pa; a directional argon beam is continuously introduced at a flow rate of 0.05-0.2 L / min, with localized pressure distribution of 5-20 Pa in the arc zone; the melting current is increased from 7 kA to 26-28 kA for primary melting or 36-38 kA for secondary melting, with the increase rate divided into three stages: 0.5 kA / min for the first 10 kA, 1 kA / min for the middle 10-20 kA, and 2 kA / min for the final 20 kA to the target current; the vacuum level increases synchronously with the current, with a corresponding decrease of 5%-10% in the furnace vacuum level for every 1 kA increase in current, dynamically matching the expansion of the molten pool. In this application, the furnace vacuum level, melting current, and dynamic state of the molten pool during the steady-state melting period are linked and controlled according to the following requirements. The furnace vacuum is controlled at a high vacuum of 0.8-1.5 Pa, with continuous deep degassing; the directional argon beam flow rate is reduced to 0.02-0.1 L / min, and the local partial pressure in the arc zone is 2-10 Pa; the melting current is stabilized at 27-28 kA for primary melting or 37-38 kA for secondary melting, and the current is finely adjusted in real time according to the molten pool height to ensure consistent molten pool depth and uniform solidification, with an adjustment range of ±0.5 kA; the arc position offset is monitored in real time by an arc sensor, and when the offset exceeds 5 mm, the argon beam flow rate and direction are automatically finely adjusted to bring the arc back to the center. In this application, the furnace vacuum, melting current, and dynamic state of the molten pool during the molten pool expansion period are linked and matched with the following requirements for control. The furnace cavity vacuum is controlled at 0.5-1.0 Pa; the directional argon beam flow rate is reduced to 0.01-0.05 L / min, and the local partial pressure in the arc zone is 1-5 Pa; the melting current is gradually reduced from 28 kA in the first melting or 38 kA in the second melting to 20-22 kA in the first melting or 30-32 kA in the second melting, with a reduction rate of 0.5-1 kA / min; the vacuum level increases synchronously with the decrease in current, and the furnace cavity vacuum level decreases by 8%-15% for every 1 kA decrease in current. The feeding stage of this application is to obtain high-purity titanium billets with complete elimination of shrinkage cavities at the head and central porosity defects by using small-amplitude vacuum stabilization and stepped current reduction for delayed melting under high vacuum conditions. The total duration of delayed melting and feeding is 200-300 min. The gradient directional water cooling solidification of the ingot in this application employs a top-to-bottom gradient water cooling system with weak cooling at the top and strong cooling at the bottom, controlling the solidification of the pure titanium ingot sequentially from bottom to top. The cooling water volume in the upper part is 0.6-0.8 times that in the lower part, the inlet water temperature is controlled at 25-30℃, and the outlet water temperature is controlled at 37-41℃. The pressing and degassing process for producing high-purity sponge titanium consumable electrodes in this application is carried out according to the following steps. First, high-purity sponge titanium of grade 0A or grade 0 is pressed into a consumable electrode. The diameter of one side of the consumable electrode is 40-100 mm smaller than the diameter of the crystallizer. Then, the consumable electrode is placed in a vacuum baking furnace for high-vacuum long-term baking and degassing. The baking temperature is 280-350℃, the holding time is 6-12 hours, and the vacuum degree is ≤0.5Pa. This yields a consumable electrode with surface adsorbed water, hydroxyl groups and trace adsorbed oxygen removed.

[0028] More specifically, the argon beam nozzle is located above the electrode side, at an angle of 15°-30° to the vertical direction. The argon beam diameter is controlled at 10-30mm, covering only the core area of ​​the arc and not performing full-area diffusion gas filling. Small-amplitude vacuum stabilization is achieved by intermittent directional argon beam injection to maintain arc stability. The specific process of small-amplitude vacuum stabilization + stepped current reduction delay for melt preservation is as follows: The vacuum level in the furnace cavity was slightly adjusted to a stable 1.0-2.0 Pa. Argon beams were introduced intermittently every 30 seconds for 2 seconds at a flow rate of 0.01-0.03 L / min to maintain the arc basically stable. The compensation current was reduced from 20-22 kA in the first stage or 30-32 kA in the second stage to 3-5 kA in 4-6 stages, with each stage held for 30 minutes to achieve delayed melting.

[0029] In summary, the technical solution provided in this application also has the following advantages: ① Subcutaneous porosity significantly decreased, and peeling amount greatly reduced: By using directional micro-argon beams to stabilize the arc, the arc offset during the main melting stage was reduced from 10-20mm in the traditional process to less than 3mm, effectively suppressing molten pool tumbling and gas entrapment. The subcutaneous porosity depth of the secondary ingot decreased from 8-12mm in the traditional process to 2-3mm, and the peeling amount during secondary ingot turning decreased from 500-750kg to 200-280kg, increasing the yield by 3.3%-5.2%.

[0030] ② Significantly reduced interstitial impurity content: The scheme of a high-vacuum substrate throughout the process + localized directional argon beam ensures arc stability while avoiding excessive interstitial elements caused by full-area argon purging. The oxygen content of the ingot can be reduced by 15%-25%, the hydrogen content by 20%-30%, and the nitrogen content by 10%-20% compared to traditional processes.

[0031] ③ Improved vacuum stability: The vacuum gradient and current linkage control reduces the vacuum fluctuation range during the melting process from ±2Pa to within ±0.3Pa. The vacuum level during secondary melting can be stably controlled at ≤1.1Pa, which greatly improves the process stability and the consistency of ingot quality.

[0032] ④ Improved composition uniformity: Dynamic fine-tuning of the constant melting pool power in the main melting section + gradient directional cooling of the crystallizer reduces the axial oxygen content deviation of the ingot from ±50ppm to within ±20ppm, significantly reduces radial segregation, and completely suppresses dendrite coarsening.

[0033] ⑤ Improved head quality: The stepped current reduction and delayed melting system during the feeding stage, combined with small-amplitude vacuum voltage stabilization, completely eliminated shrinkage cavities and central porosity in the ingot head. The head yield increased by 10%-15% based on the amount of material removed after forging.

[0034] ⑥ Strong process adaptability: By controlling the argon beam flow rate, vacuum degree, and current in a coordinated manner, it can adapt to the production of pure titanium ingots with different specifications and purity requirements, with a wide process window and strong controllability.

[0035] The technical solution of this application will be further described below through specific embodiments: The purpose of this invention is to overcome the shortcomings of existing technologies and provide a vacuum gradient voltage-stabilized directional argon beam arc-stabilized VAR melting process for high-purity titanium, solving the following technical problems: ① The problem of high subcutaneous porosity and excessive peeling caused by arc drift and molten pool tumbling in the main stage of VAR melting of high-purity titanium is avoided, while avoiding excessive interstitial impurities caused by full-area argon purging. ② The vacuum level control and current control are independent of each other, which cannot match the dynamic state of the molten pool and result in large vacuum fluctuations; ③ The problem of further reducing the content of interstitial impurities such as oxygen, nitrogen, and hydrogen in high-purity titanium; ④ Problems such as axial or radial component segregation in ingots and porosity due to shrinkage cavities at the head.

[0036] The main technical solution is a vacuum gradient voltage-stabilized directional argon beam arc-stabilized VAR melting process for high-purity titanium, comprising five core modules for coordinated control: pre-electrode deep degassing pretreatment, vacuum gradient graded control, three-stage adaptive current melting, micro-volume high-purity argon beam directional arc stabilization, and crystallizer gradient directional cooling. The specific steps are as follows: ① Pre-treatment of electrode pre-degassing: High-purity sponge titanium (0A grade or 0 grade) is pressed into consumable electrodes, with the diameter of one side of the electrode being 40-100mm lower than the diameter of the crystallizer; the entire electrode is placed in a vacuum baking furnace for high-vacuum long-term baking degassing, with a baking temperature of 280-350℃, a holding time of 6-12 hours, and a vacuum degree ≤0.5Pa, to remove adsorbed water, hydroxyl groups and trace amounts of adsorbed oxygen from the electrode surface, thus blocking oxygenation during smelting from the source.

[0037] ② Arc Ignition Stage—Medium Vacuum Substrate + Directional Micro-Argon Beam Soft Arc Ignition: Evacuate the furnace cavity to a vacuum level of 3-6 Pa (medium vacuum) to prevent instantaneous arc ignition and splashing; introduce a small amount of high-purity argon gas into the core area of ​​the arc through a directional argon beam nozzle at a flow rate of 0.1-0.5 L / min, maintaining the argon partial pressure in the local area of ​​the arc at 10-50 Pa, while the entire furnace cavity remains in a medium vacuum state; the arc ignition current is 3-7 kA, using low current and slow soft arc ignition, with an arc ignition time of 7-9 minutes to prevent instantaneous arc impact from causing splashing and gas entrapment; the argon beam nozzle is located above the electrode side, at an angle of 15°-30° to the vertical direction, and the diameter of the argon beam is controlled at 10-30 mm, covering only the core area of ​​the arc, without full-area diffusion gas filling.

[0038] ③ Main melting stage—vacuum gradient voltage stabilization and current adaptive linkage coupling control: The main melting stage is divided into three sub-stages: early stage, middle stage and late stage. The vacuum degree of the furnace cavity and the melting current in each stage are adaptively linked to match the dynamic state of the molten pool.

[0039] Early stage of main melting (molten pool formation stage): The vacuum degree of the furnace cavity is gradually increased from medium vacuum to high vacuum, controlled at 1.5-3 Pa; directional argon beam is continuously introduced at a flow rate of 0.05-0.2 L / min, and the local partial pressure in the arc zone is 5-20 Pa; the melting current is gradually increased from 7 kA to 26-28 kA (primary melting) or 36-38 kA (secondary melting), with the rate of increase divided into three stages: 0.5 kA / min for the first 10 kA, 1 kA / min for 10-20 kA, and 2 kA / min for the target current after 20 kA; the vacuum degree is synchronously increased with the increase of current, and for every 1 kA increase in current, the vacuum degree of the furnace cavity decreases by 5%-10% (i.e., the vacuum degree increases), dynamically matching the expansion process of the molten pool.

[0040] Mid-stage of main melting (steady-state melting period): The vacuum degree of the furnace cavity is controlled at 0.8-1.5Pa (high vacuum), and deep degassing is continuously carried out; the directional argon beam flow rate is reduced to 0.02-0.1L / min, and the local partial pressure in the arc zone is 2-10Pa; the melting current is stabilized at 27-28kA (primary melting) or 37-38kA (secondary melting), and the current is finely adjusted in real time according to the height of the molten pool to ensure that the depth of the molten pool is consistent and the solidification is uniform, with an adjustment range of ±0.5kA; the arc position offset is monitored in real time by an arc sensor, and when the offset exceeds 5mm, the argon beam flow rate and direction are automatically finely adjusted to bring the arc back to the center.

[0041] During the later stages of the main melting process (molten pool expansion phase): the furnace vacuum is controlled at 0.5-1.0 Pa; the directional argon beam flow rate is further reduced to 0.01-0.05 L / min, and the local partial pressure in the arc zone is 1-5 Pa; the melting current is gradually reduced from 28 kA (primary) or 38 kA (secondary) to 20-22 kA (primary) or 30-32 kA (secondary), with a reduction rate of 0.5-1 kA / min; the vacuum level increases synchronously with the decrease in current, and for every 1 kA decrease in current, the furnace vacuum level decreases by 8%-15%.

[0042] ④ Feeding Stage—Small Vacuum Stabilization + Stepped Current Reduction for Delayed Melting: The vacuum level in the furnace cavity is slightly reduced to 1.0-2.0 Pa for stabilization to prevent backflow from the ingot head; directional argon beams are intermittently introduced, with a flow rate of 0.01-0.03 L / min every 30 seconds for 2 seconds, maintaining a basically stable arc; the feeding current is stepped down from 20-22 kA (primary) or 30-32 kA (secondary) to 3-5 kA, in 4-6 stages, with each stage lasting 30 minutes, to achieve delayed melting; the total feeding time is 200-300 minutes, completely eliminating shrinkage cavities at the head and central porosity of the pure titanium ingot.

[0043] ⑤ Gradient directional cooling of the crystallizer: The crystallizer adopts an upper and lower partitioned gradient water cooling structure. The upper part is weakly cooled and the lower part is strongly cooled. The cooling water volume of the upper part is 0.6-0.8 times that of the lower part. The inlet water temperature is controlled at 25-30℃ and the outlet water temperature is controlled at 37-41℃. This achieves the sequential solidification of pure titanium ingots from bottom to top, suppressing radial segregation and dendrite coarsening.

[0044] ⑥ Cooling and unloading: After melting, keep the furnace under vacuum for 2-4 hours, then fill it with high-purity argon gas to atmospheric pressure and continue cooling for 4-6 hours before unloading.

[0045] The core technical principle of the technical solution in this application is: ① Directional micro-argon beam arc stabilization mechanism: Unlike traditional full-area diffused gas filling, this invention uses a directional beam to confine the arc. Argon gas only acts on the core region of the arc and will not diffuse and dissolve into the pure titanium matrix over a large area. The angle, position, and flow rate of the argon beam nozzle are precisely designed to ensure arc stability while minimizing the contact area between argon gas and molten titanium, achieving "arc stabilization without oxygenation and without contamination of high-purity titanium." Compared with existing AC arc stabilization, the arc offset is reduced from 10-20 mm to less than 3 mm.

[0046] ② Coupling of Vacuum Gradient and Current: The core innovation of this invention lies in the adaptive linkage control of vacuum level and current. When the current increases, the molten pool temperature rises and the titanium vapor pressure increases, requiring a corresponding increase in vacuum level to maintain molten pool stability and enhance degassing; when the current decreases, the molten pool contracts, allowing for further improvement in vacuum level. The two form a closed-loop linkage, rather than independent control, achieving precise matching between the vacuum gradient and the dynamic state of the molten pool, effectively suppressing vacuum fluctuations.

[0047] ③ Full-link oxygen and gas control system: from electrode depth degassing (source oxygen reduction) → directional micro argon beam arc stabilization (process gas reduction) → vacuum gradient linkage (continuous degassing) → gradient cooling directional solidification (reducing segregation), a complete set of impurity control processes is formed from electrode to solidification.

[0048] Example 1: Secondary melting of Φ1000mm TA2 cold-rolled high-purity titanium ingot Raw materials: primary ingot (obtained from grade 0 sponge titanium pressed electrode through one VAR melting), oxygen content approximately 400 ppm, hydrogen content approximately 15 ppm, nitrogen content approximately 30 ppm.

[0049] Equipment: 10-ton vacuum consumable electric arc furnace, crystallizer diameter 1000mm, equipped with directional argon beam nozzle, arc monitoring system and vacuum-current linkage control system.

[0050] Process steps: ① Electrode pretreatment: The entire surface of the ingot is peeled off in one go (approximately 300 kg of peeling material) to remove the black shell and defects. After peeling, the electrode surface is polished and cleaned to remove the discolored oxide layer. The electrode is then degassed in a vacuum oven at 200℃ for 5 hours with a vacuum degree of 10 Pa.

[0051] ② Loading the furnace: After welding the auxiliary electrode to the main electrode, load it into the crystallizer. The electrode diameter is approximately 920 mm, and the distance between the electrode end and the bottom pad is 30 mm. Seal the furnace body and evacuate the furnace.

[0052] ③ Arc ignition stage: The furnace cavity vacuum is evacuated to 4Pa; the directional argon beam is turned on with a flow rate of 0.6L / min and a local partial pressure of about 30Pa in the arc zone; the arc ignition current is 5kA and the arc ignition time is 8 minutes, with low current soft arc ignition; the argon beam nozzle angle is 20° and the beam diameter is 40mm.

[0053] ④ In the early stage of main melting: the current is increased from 13kA to 38kA, with the rate of increase in three steps: 0.5kA / min, 1kA / min, and 2kA / min; the vacuum degree of the furnace cavity is gradually reduced from 4Pa to 1.2Pa; the argon beam flow rate is reduced from 0.6L / min to 0.15L / min; for every 1kA increase in current, the vacuum degree decreases by about 8% (vacuum degree increases).

[0054] ⑤ Mid-stage of main melting: The current is stabilized at 37-38kA, and is adaptively fine-tuned according to the height of the molten pool, with an amplitude of ±0.5kA; the vacuum degree of the furnace cavity is stabilized at 1.0Pa; the argon beam flow rate is 0.08L / min, and the arc zone pressure is about 5Pa; the arc sensor monitors in real time, and the arc offset is controlled within 5mm; the outlet water temperature is controlled at 37-41℃.

[0055] ⑥ Later stage of main melting: The current is reduced from 38kA to 32kA at a rate of 0.8kA / min; the vacuum degree of the furnace cavity is gradually reduced from 1.0Pa to 0.6Pa; the argon beam flow rate is reduced from 0.08L / min to 0.03L / min; for every 1kA decrease in current, the vacuum degree decreases by about 10% (vacuum degree increases).

[0056] ⑦ Compensation stage: The vacuum level in the furnace cavity is slightly reduced to a stable 1.5Pa; the argon beam is intermittently introduced, for 2 seconds every 30 seconds, at a flow rate of 0.04L / min; the current decreases in four stages: 32kA→18kA→10kA→8kA→3kA, with dwell times of 20, 20, 50, and 160 minutes respectively. ⑧ Crystallizer cooling: The cooling water volume in the upper part is 0.7 times that in the lower part, the inlet water temperature is 28℃, and the outlet water temperature is 38~40℃.

[0057] ⑨ Cooling and unloading: After vacuum cooling for 4 hours, argon is purged for 5 hours before unloading.

[0058] Test results: Ingot surface quality: no cold shuts, no obvious ripples, smooth surface, and slight oxidation. Secondary spindle peeling capacity: 220kg Oxygen content: Head 322ppm, Middle 341ppm, Bottom 353ppm, Average 340ppm, Axial deviation ±20ppm; Hydrogen content: 8 ppm at the head, 11 ppm in the middle, 11 ppm at the bottom, and 10 ppm on average; Nitrogen content: Head 23ppm, Middle 24ppm, Bottom 28ppm, Average 25ppm; Flaw detection: No internal micropores or inclusions, subcutaneous pore depth ≤2mm, flaw detection pass rate 100%; Head quality: No shrinkage cavities, no central porosity, head yield rate 92%; Vacuum fluctuation: ±0.2Pa, stable at around 1.0Pa throughout.

[0059] Example 2: Secondary melting of Φ1000mm medical-grade high-purity titanium ingot Raw material: Small-particle titanium ingots from a certain steel company, with an oxygen content of approximately 200 ppm, a hydrogen content of approximately 8 ppm, and a nitrogen content of approximately 15 ppm.

[0060] Equipment: 10-ton vacuum consumable electric arc furnace, crystallizer diameter 1000mm, equipped with directional argon beam nozzle, arc monitoring system and vacuum-current linkage control system.

[0061] Process steps: Electrode Φ940mm, vacuum baked at 220℃ / 12 hours, vacuum degree 0.5-1Pa; Arc ignition: vacuum degree 3Pa, argon beam flow rate 0.4L / min, current 3-7kA, 8 minutes; During the initial stage of main melting: current 7→38kA, vacuum degree 3→1Pa, argon beam 0.4→0.1L / min; Mid-stage of main melting: current 37-38kA, vacuum degree 0.8-1Pa, argon beam 0.06L / min; Later stage of main melting: current 38→30kA, vacuum degree 0.8→0.4Pa, argon beam 0.06→0.02L / min; Compensation: Vacuum level adjusted back to 1.2 Pa, argon beam intermittent, current 30→3kA in four stages, 280 minutes; Crystallizer: The water volume in the upper part is 0.65 times that in the lower part, and the inlet water temperature is 26℃.

[0062] Test results: Secondary stripping amount: 274kg (meets standards); The average oxygen content is 180 ppm, the average hydrogen content is 5 ppm, and the average nitrogen content is 12 ppm. The flaw detection pass rate is 100%, and there are no micropores or inclusions inside; It meets the requirements for medical-grade high-purity titanium; Axial oxygen deviation: ±15ppm, excellent compositional uniformity.

Claims

1. A VAR melting process for preparing high-purity titanium, characterized in that: The VAR melting process described above uses a high-purity sponge titanium electrode that has passed pressure degassing as a consumable electrode. In a vacuum furnace, a three-stage adaptive current melting process is employed, consisting of an arc-ignition stage, a main melting stage, and a feeding stage. The melted high-purity titanium liquid is then output to a crystallizer where it undergoes gradient-directional water cooling and solidification to obtain a high-purity titanium ingot. Finally, the ingot is held at the furnace temperature, cooled further, and then continuously cooled to complete the preparation of the high-purity titanium. The main melting stage consists of three sub-melting stages: the molten pool formation stage, the steady-state melting stage, and the molten pool expansion stage. During the melting process of each sub-melting stage, the vacuum level inside the furnace is adaptively coupled and controlled by the input directional argon beam with the melting current of the corresponding melting sub-stage, and adaptively matched with the dynamic state of the molten pool in the corresponding sub-stage. Throughout the entire melting process, the furnace cavity is maintained at a relatively high vacuum of no more than 3 Pa. Argon gas is only applied locally to the core area of ​​the electric arc in the form of a directional beam, without being diffused throughout the entire area.

2. The VAR melting process for preparing high-purity titanium according to claim 1, characterized in that: The arc initiation stage employs a medium-vacuum substrate combined with a directional micro-argon beam for soft arc initiation. The specific process and requirements are as follows. The furnace cavity is evacuated to a medium vacuum state of 3-6 Pa. Then, a small amount of high-purity argon gas is directionally introduced into the core area of ​​the electric arc through a directional argon beam nozzle at a flow rate of 0.1-0.5 L / min, so that the argon partial pressure in the local area of ​​the electric arc is maintained at 10-50 Pa, while the entire furnace cavity remains in a medium vacuum state. The arc ignition current is 3-7 kA, and a low-current, slow-speed soft arc ignition is adopted, with an arc ignition time of 7-9 minutes.

3. The VAR melting process for preparing high-purity titanium according to claim 2, characterized in that: The argon beam nozzle is located above the electrode side, at an angle of 15°-30° to the vertical direction. The diameter of the argon beam is controlled at 10-30mm, covering only the core area of ​​the electric arc, without full-area diffusion gas filling.

4. The VAR melting process for preparing high-purity titanium according to any one of claims 1 to 3, characterized in that: During the molten pool formation period, the vacuum level inside the smelting furnace, the smelting current, and the dynamic state of the molten pool should be linked, matched, and controlled according to the following requirements. The vacuum level in the furnace cavity is gradually increased from medium vacuum to high vacuum of 1.5-3 Pa; a directional argon beam is continuously introduced at a flow rate of 0.05-0.2 L / min, with local partial pressure of 5-20 Pa in the arc zone; the melting current is increased from 7 kA to 26-28 kA for primary melting or 36-38 kA for secondary melting, with the rate of increase divided into three stages: 0.5 kA / min for the first 10 kA, 1 kA / min for the middle 10-20 kA, and 2 kA / min for the final 20 kA to the target current; the vacuum level is increased synchronously with the current, and the vacuum level in the furnace cavity decreases by 5%-10% for every 1 kA increase in current, dynamically matching the expansion process of the molten pool.

5. The VAR melting process for preparing high-purity titanium according to claim 4, characterized in that: During the steady-state smelting period, the vacuum level inside the smelting furnace, the smelting current, and the dynamic state of the molten pool should be linked, matched, and controlled according to the following requirements. The furnace cavity vacuum is controlled at a high vacuum of 0.8-1.5 Pa, with continuous deep degassing; the directional argon beam flow rate is reduced to 0.02-0.1 L / min, and the local partial pressure in the arc zone is 2-10 Pa; the melting current is stabilized at 27-28 kA for the first melting or 37-38 kA for the second melting, and the current is finely adjusted in real time according to the height of the molten pool to ensure consistent depth and uniform solidification, with an adjustment range of ±0.5 kA; the arc position offset is monitored in real time by an arc sensor, and when the offset exceeds 5 mm, the argon beam flow rate and direction are automatically finely adjusted to bring the arc back to the center.

6. The VAR melting process for preparing high-purity titanium according to claim 5, characterized in that: During the molten pool expansion period, the vacuum level inside the smelting furnace, the smelting current, and the dynamic state of the molten pool should be linked, matched, and controlled according to the following requirements. The furnace cavity vacuum is controlled at 0.5-1.0 Pa; the directional argon beam flow rate is reduced to 0.01-0.05 L / min, and the local partial pressure in the arc zone is 1-5 Pa; the melting current is gradually reduced from 28 kA for the first melting or 38 kA for the second melting to 20-22 kA for the first melting or 30-32 kA for the second melting, with a reduction rate of 0.5-1 kA / min; the vacuum level increases synchronously with the decrease in current, and the furnace cavity vacuum level decreases by 8%-15% for every 1 kA decrease in current.

7. The VAR melting process for preparing high-purity titanium according to any one of claims 1 to 3, characterized in that: During the feeding stage, under high vacuum conditions, a small-amplitude vacuum voltage stabilization and stepped current reduction are used to delay the melting process to obtain high-purity titanium billets with complete elimination of shrinkage cavities at the head and central porosity defects in pure titanium ingots. The total time for delayed melting and feeding is 200-300 minutes.

8. The VAR melting process for preparing high-purity titanium according to claim 7, characterized in that: The small-amplitude vacuum voltage regulation uses intermittent directional argon beam to maintain arc stability. The specific process of small-amplitude vacuum voltage regulation + stepped current reduction delay to maintain melting is as follows: The vacuum level in the furnace cavity was slightly adjusted to a stable 1.0-2.0 Pa. Argon beams were introduced intermittently every 30 seconds for 2 seconds at a flow rate of 0.01-0.03 L / min to maintain the arc basically stable. The compensation current was reduced from 20-22 kA in the first stage or 30-32 kA in the second stage to 3-5 kA in 4-6 stages, with each stage held for 30 minutes to achieve delayed melting.

9. The VAR melting process for preparing high-purity titanium according to any one of claims 1 to 3, characterized in that: The gradient directional water cooling solidification ingot in the crystallizer adopts a gradient water cooling control system with weak cooling at the top and strong cooling at the bottom to control the solidification of pure titanium ingots from bottom to top. The cooling water volume at the top is 0.6-0.8 times that at the bottom, the inlet water temperature is controlled at 25-30℃, and the outlet water temperature is controlled at 37-41℃.

10. The VAR melting process for preparing high-purity titanium according to claim 9, characterized in that: The preparation of high-purity sponge titanium consumable electrodes by pressing and degassing is carried out according to the following steps. First, high-purity sponge titanium of grade 0A or grade 0 is pressed into a consumable electrode. The diameter of one side of the consumable electrode is 40-100 mm smaller than the diameter of the crystallizer. Then, the consumable electrode is placed in a vacuum baking furnace for high-vacuum long-term baking and degassing. The baking temperature is 280-350℃, the holding time is 6-12 hours, and the vacuum degree is ≤0.5Pa. This yields a consumable electrode with surface adsorbed water, hydroxyl groups and trace adsorbed oxygen removed.

Citation Information

Patent Citations

  • Smelting feeding method for TC4-DT titanium alloy cast ingot of phi 720-phi 1000 mm specification

    CN105039760A

  • Vacuum consumable-electrode arc melting ingot pulling device for metal material melting

    CN105238936A

  • Smelting method for improving bottom quality of VAR titanium alloy primary ingot

    CN113088719A

  • A smelting method for improving the bottom quality of VAR titanium alloy primary ingots

    CN113088719B

  • Method for improving visibility and stability in titanium alloy argon-filled smelting process

    CN113174501A