A method for lead quenching and online phosphating heat treatment of galvanized aluminum spring steel wire
By integrating the phosphating process into the lead quenching production line through online phosphating heat treatment, the problems of secondary acid corrosion and lengthy processes in the production of galvanized aluminum spring steel wire are solved, achieving efficient production and excellent microstructure control, and ensuring the torsional performance and surface quality of the steel wire.
Patent Information
- Application Number
- CN202611421080.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-10
AI Technical Summary
In the current production of galvanized aluminum spring steel wire, the offline phosphating mode leads to problems such as secondary acid corrosion risk, lengthy process, surface quality fluctuation and low production efficiency. In particular, the traditional TT2 direct heat treatment leads to the deterioration of the martensitic structure in the core and the torsional properties after plating.
The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire is adopted, integrating the phosphating process into the lead quenching production line. The lead quenching heating, isothermal transformation, online pickling, phosphating and saponification processes are continuously completed on the same production line. The heat treatment parameters are optimized to obtain a uniform sorbite + pearlite structure and avoid the formation of martensite.
Eliminates secondary acid corrosion, increases sorbitization rate, improves surface quality and production efficiency, ensures stable torsional performance after plating, simplifies the process, and reduces equipment occupation and transfer time.
Smart Images

Figure CN123063705A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of galvanized aluminum spring steel wire preparation technology, and in particular to a lead-quenched online phosphating heat treatment method for galvanized aluminum spring steel wire. Background Technology
[0002] Lead quenching (Pyden quenching) is the most critical heat treatment process in the production of galvanized aluminum carbon spring steel wire. Its core purpose is to obtain a fine lamellar sorbite structure, providing the microstructure basis for subsequent high-compression cold drawing. After lead quenching, the steel wire needs to undergo phosphating treatment to form a phosphating film, which serves as a lubricant for subsequent drawing.
[0003] Existing technical solution: Currently, the industry generally adopts the offline phosphating mode, where lead quenching and phosphating are two independent processes. After lead quenching, the steel wire is transferred to the phosphating line, where it is then pickled, phosphating, saponified, and dried.
[0004] Disadvantages of existing technology:
[0005] (1) Risk of secondary acid corrosion: Offline phosphating requires secondary pickling of the steel wire after lead quenching, which increases the chance of chloride ions corroding the surface of the steel wire, aggravates surface corrosion pits, and becomes the cause of subsequent zinc pot breakage.
[0006] (2) The process is lengthy: lead quenching and phosphating are carried out separately, which requires a lot of equipment, takes a long time to transfer, and has low production efficiency.
[0007] (3) Surface quality fluctuation: damage and contamination occur during transportation, resulting in poor uniformity and continuity of the phosphating film.
[0008] (4) Poor microstructure control: Traditional TT2 direct heat treatment results in martensite microstructure in the core, with a surface shrinkage rate of only 24% to 34%, and the torsion performance after plating is reduced from 22 times to 12 times. Summary of the Invention
[0009] The traditional lead quenching process is as follows: heating → lead quenching → pickling → phosphating → saponification → drying. The steel wire needs to be transported offline to the phosphating process, which is prone to damage and contamination, and the secondary pickling introduces the risk of chloride ion corrosion. To overcome the shortcomings of existing technologies, this invention solves the problems of secondary acid corrosion risk, lengthy process, and surface quality fluctuations inherent in the traditional offline phosphating mode for lead quenching in the production of galvanized aluminum spring steel wire. These problems lead to increased LME sensitivity and low production efficiency during subsequent hot-dip galvanizing.
[0010] The objective of this invention is achieved through the following technical solution:
[0011] A method for lead-quenched online phosphating heat treatment of galvanized aluminum spring steel wire, with specific process steps:
[0012] Step 1, lead quenching and heating: The semi-finished steel wire after the billet drawing is heated to the austenitizing temperature of 880-930℃ in sections to avoid overheating of the steel wire;
[0013] Step 2, lead bath isothermal transformation: The steel wire is immersed in a molten lead bath at a temperature of 500-530℃ for isothermal transformation. The temperature fluctuation of the lead bath is controlled within ±5℃, the machine speed is 18-20m / min, the DV value is controlled at 50-70, and the sorbite conversion rate is greater than 90% to obtain a fine lamellar sorbite structure.
[0014] Step 3, Online Phosphating: After the steel wire completes the lead quenching isothermal transformation, it directly enters the online pickling, phosphating, saponification and drying processes without the need for off-line transfer. The entire process is completed continuously on the same production line.
[0015] Step 4, Cooling: Use two air cooling systems for uniform cooling.
[0016] In more advanced technical solutions, the commonly used acids for steel wire pickling include hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid. These acids are highly irritating, corrosive, and even systemically toxic to humans, requiring strict protective measures during operation. The pickling process also generates acid mist, containing acid vapors and toxic gases such as nitrogen oxides (e.g., nitrogen dioxide). To address the issue of existing pickling tanks requiring frequent opening for steel wire pickling, a closable pickling tank is designed to reduce the risk of injury from human operation.
[0017] In step three, the online pickling process uses a pickling box, which includes a box body with a pickling tank inside. A vertical frame is provided on one side of the box body, with a vertical groove inside the vertical frame and a vertical screw installed thereon. A lifting motor is installed at the top of the vertical screw, which drives the vertical screw to rotate and drives the moving block threaded on the vertical screw to rise and fall.
[0018] A movable plate is integrally mounted on the movable block, and multiple sets of pull rollers are provided at the bottom of the movable plate for driving the steel wire;
[0019] The bottom of the box is equipped with an acid drain pipe and a corrosion-resistant valve to control the opening and closing of the acid drain pipe;
[0020] The pickling tank is filled with pickling solution for online pickling of steel wire; the multiple sets of pull rollers move and lift inside and outside the box, and the box is equipped with an opening and closing door for closing the pickling tank.
[0021] In a further technical solution, support plates are provided at both ends of multiple sets of pull rollers and are fixedly connected to the moving plate; at least the middle pull roller immerses the steel wire in the pickling solution;
[0022] The size of the moving plate is not smaller than the size of the pickling tank.
[0023] In a further technical solution, a feed pipe is installed at one end of the box, and two sets of guide wheels are installed at the inlet of the feed pipe. Guide grooves are opened on the guide wheels to constrain the steel wire from entering the box.
[0024] The guide wheel is provided with a bracket plate and an adjusting rod is installed. The adjusting rod extends through the feed pipe to the outside and is equipped with a locking nut.
[0025] In a further technical solution, a position plate is provided on one side of the housing; two sets of constraint plates are provided in the middle of the position plate, and limit plates are installed at both ends; a bidirectional motor is installed between the two sets of constraint plates; the output end of the bidirectional motor passes through the constraint plate and is coaxially mounted with a side lead screw; a bearing is installed between the end of the side lead screw away from the bidirectional motor and the limit plate;
[0026] A side block is threaded onto the side lead screw, and the side block moves along the axis of the side lead screw; an opening and closing door is installed on the side block.
[0027] In a further technical solution, one bottom side of the opening and closing door is fixedly connected to a side block, and the other side is connected to a guide rail; the guide rail is fixedly connected to the side of the housing opposite to the position plate, and a hemispherical part is bent on one side of the opening and closing door and constrained on the guide rail; the two sides of the opening and closing door are supported and slid on the side block and the guide rail respectively.
[0028] The opening and closing door has a long groove along the length of the box body, which runs through the top and bottom of the opening and closing door; a sliding block is installed in the long groove, and elastic folding plates are installed on both sides of the sliding block to close the gap between the long groove and the sliding block; a guide hole is opened in the middle of the sliding block for the steel wire to pass through.
[0029] In a further technical solution, the lengths of both the position plate and the guide rail are greater than the length of the housing, and a connecting plate is installed between the position plate and the guide rail, with the connecting plate fixed to the end of the housing.
[0030] In a further technical solution, a liquid outlet pipe is installed at the end of the box away from the feed pipe and a water tank is installed thereon; flow pipe one and flow pipe two are respectively installed on both sides of the water tank, with flow pipe one for liquid inlet and flow pipe two for liquid outlet.
[0031] Two sets of parallel filter screens are installed inside the water tank, and the steel wire passes through the two sets of filter screens; the filter screens are perpendicular to the liquid inlet direction of the flow pipe.
[0032] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0033] This invention integrates the phosphating process into the lead quenching production line. After the steel wire completes the isothermal transformation of lead quenching, it directly enters the online pickling, phosphating, saponification and drying processes without the need for off-line transfer. At the same time, it uses optimized heat treatment parameters to obtain a uniform sorbite + pearlite structure, and with the optimized heat treatment parameters, it obtains a high sorbitization rate structure, avoiding the formation of martensite.
[0034] This invention has the following advantages:
[0035] (1) Eliminate secondary acid corrosion: avoid secondary pickling, reduce the chance of chloride ions corroding the steel wire surface, and reduce the sensitivity of subsequent LME.
[0036] (2) Excellent structure: a uniform sorbite + pearlite structure is obtained, the sorbitization rate is ≥90%, and the area shrinkage is increased to 35%~40%.
[0037] (3) Avoid martensite: Completely eliminate the problem of martensite structure in the core caused by direct heat treatment of TT2.
[0038] (4) Stable torsional performance: The torsional performance after plating is normal, and there is no deterioration in the TT2 process where the torsional count drops from 22 to 12.
[0039] (5) Improved surface quality: The phosphating film is more uniform and continuous, with no lead residue defects.
[0040] (6) Improved production efficiency: Simplified processes reduce equipment usage and transfer time.
[0041] This invention features a movable plate that can be raised and lowered, which drives a pull roller to pull a steel wire, allowing the plate to move up and down while closing at the top opening of the pickling tank, reducing acid mist overflow and minimizing its impact on operators. Furthermore, it incorporates two sets of opening and closing doors that can be driven by a bidirectional motor and a side-mounted lead screw to open and close the top opening of the pickling tank when not in use; the doors are opened during pickling. Attached Figure Description
[0042] Figure 1 This is a schematic diagram of the pickling tank structure of the present invention. Figure 1 ;
[0043] Figure 2 This is a schematic diagram of the pickling tank structure of the present invention. Figure 2 ;
[0044] Figure 3 This is a schematic diagram of the pickling tank structure of the present invention. Figure 3 ;
[0045] Figure 4 for Figure 3 Enlarged view of part A;
[0046] Figure 5for Figure 3 Enlarged view of part B;
[0047] Figure 6 This is a front view of the pickling tank of the present invention;
[0048] Figure 7 This is a schematic diagram of the operation of the pickling tank in Embodiment 1 of the present invention;
[0049] Figure 8 This is a top view of the pickling tank of the present invention;
[0050] Figure 9 for Figure 8 CC section view;
[0051] Figure 10 This is a side sectional view of the water tank of the present invention;
[0052] Figure 11 This is a schematic diagram of the online wire movement of the pickling tank of the present invention;
[0053] Figure 12 This is a schematic diagram of the pickling tank in Embodiment 2 of the present invention;
[0054] Figure 13 This is a schematic diagram of online wire movement according to Embodiment 2 of the present invention;
[0055] Figure 14 for Figure 13 Enlarged view of part D.
[0056] In the diagram: 1. Box body; 2. Vertical frame; 3. Vertical lead screw; 4. Lifting motor; 5. Moving block; 6. Moving plate; 7. Pull roller; 8. Anti-corrosion valve; 9. Opening and closing door; 10. Support plate; 11. Pickling tank; 12. Feed pipe; 13. Guide wheel; 14. Support plate; 15. Adjusting rod; 16. Position plate; 17. Constraint plate; 18. Limiting plate; 19. Bidirectional motor; 20. Side lead screw; 21. Side block; 22. Guide rail; 23. Long groove; 24. Sliding block; 25. Elastic folding plate; 26. Connecting plate; 27. Water tank; 28. Flow pipe one; 29. Flow pipe two; 30. Filter screen; 31. Liquid outlet pipe. Detailed Implementation
[0057] The present invention will now be further described in conjunction with the accompanying drawings and specific embodiments. It should be noted that, without conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments. Unless otherwise specified, the materials and equipment used in this embodiment are commercially available. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.
[0058] In the description of this application, it should be understood that the terms "upper," "lower," "front," "rear," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on this application. In the description of this application, "a plurality of" means two or more, unless otherwise precisely specified.
[0059] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "connected," "linked," and "connected" should be interpreted broadly. For example, they can refer to a fixed connection, a connection through an intermediary, the internal connection of two elements, or the interaction between two elements. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0060] The terms "first," "second," etc., in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such process, method, product, or apparatus.
[0061] This invention relates to a method for lead quenching and online phosphating heat treatment of galvanized aluminum spring steel wire, with the following specific process steps:
[0062] Step 1, lead quenching and heating: The semi-finished steel wire after the billet drawing is heated to the austenitizing temperature of 880-930℃ in sections to avoid overheating of the steel wire;
[0063] Step 2, lead bath isothermal transformation: The steel wire is immersed in a molten lead bath at a temperature of 500-530℃ for isothermal transformation. The temperature fluctuation of the lead bath is controlled within ±5℃, the machine speed is 18-20m / min, the DV value is controlled at 50-70, and the sorbite conversion rate is greater than 90% to obtain a fine lamellar sorbite structure.
[0064] Step 3, Online Phosphating: After the steel wire completes the lead quenching isothermal transformation, it directly enters the online pickling, phosphating, saponification and drying processes without the need for off-line transfer. The entire process is completed continuously on the same production line.
[0065] Step 4, Cooling: Use two air cooling systems for uniform cooling.
[0066] The lead quenching process parameters in step 1 of this invention (based on a semi-finished product diameter of 6.4 mm) are shown in Table 1:
[0067] Table 1. Process Parameter Table
[0068] parameter numerical values Key Control Points austenitizing temperature 880~930℃ Segmented heating to avoid overheating Lead bath temperature 500~530℃ Fluctuation within ±5℃ Speed 18~20m / min Control DV value Cooling method Two air cooling Uniform cooling
[0069] The core advantages of online phosphating in step three:
[0070] (1) Eliminate secondary acid corrosion: avoid the secondary pickling of steel wire after lead quenching, and reduce the chance of chloride ions corroding the surface of steel wire.
[0071] (2) Improved surface quality: Online continuous processing reduces transport damage and contamination, resulting in a more uniform and continuous phosphating film.
[0072] (3) Simplified process: Reduce equipment occupation and transfer time, and improve production efficiency.
[0073] Table 2 shows a comparison between TT1 heat treatment and TT2 direct heat treatment:
[0074] Table 2. Performance Comparison Table
[0075] Comparison Projects TT2 direct heat treatment (comparative example) TT1 heat treatment (this invention) organize Martensite in the core + surface roughening Sorbite + Pearlite + Small Amount of Bainite Soxhletization rate Approximately 70% ≥90% Lead hanging situation serious none surface shrinkage rate 24%~34% 35%~40% Pre-plating twist 22 times normal Twisting after plating 12 times (a decrease of 45%) normal Overall evaluation Not feasible feasible
[0076] Sorbiticization rate refers to the percentage of sorbite (fine pearlite) in the microstructure of high-carbon steel wire rod or wire after sorbiticization treatment. Controlling the sorbiticization rate: The key to obtaining a high sorbiticization rate (≥90%) lies in precise austenitizing temperature, rapid lead immersion cooling, and appropriate isothermal temperature and time.
[0077] This invention has the following advantages:
[0078] (1) Online phosphating process: lead quenching (heating → lead bath isothermal transformation) → online pickling → online phosphating → online saponification → online drying. The whole process is completed continuously on the same production line without the need for offline transfer.
[0079] (2) Lead quenching process parameters: austenitizing temperature 880~930℃ segmented heating, lead bath temperature 500~530℃ (fluctuation within ±5℃), machine speed 18~20m / min, two-stage air cooling.
[0080] (3) TT1 heat treatment characteristics: obtain a uniform sorbite + pearlite + a small amount of bainite structure, sorbitization rate ≥90%, area shrinkage rate 35%~40%, and no martensite structure.
[0081] (4) Eliminate secondary acid corrosion: avoid secondary pickling after lead quenching, and reduce chloride ion corrosion from the source.
[0082] (5) Phosphating film quality: uniform and continuous, without lead residue defects, providing a lubricating carrier for subsequent drawing.
[0083] Example 1
[0084] Taking the production of SH-grade galvanized spring steel wire with a diameter of 2.9mm as an example, the 6.4mm semi-finished product undergoes heat treatment.
[0085] Step S1, lead quenching heating: austenitizing temperature 900~930℃, segmented heating.
[0086] Step S2, isothermal transformation in lead bath: lead bath temperature 500~520℃, lead bath temperature fluctuation within ±5℃, vehicle speed 18.75m / min.
[0087] Step S3, Online Phosphating: After lead quenching, it directly enters the online pickling, phosphating, saponification, and drying processes.
[0088] Step S4, Cooling: Uniform cooling with two air cooling systems.
[0089] Results: The metallographic structure consists of sorbite, pearlite, a very small amount of ferrite, and a small amount of bainite, with no martensite at the beginning and end, and good uniformity. The 6.4mm semi-finished product has a strength of 1350MPa, a shrinkage rate of 38%, and an elongation of 10% to 11%. There are no lead residue defects. The torsional performance after plating is normal and has not deteriorated. The phosphating film is uniform and continuous.
[0090] Comparative Example 1 (TT2 direct heat treatment + offline phosphating): Martensite structure appeared in the core, the area shrinkage rate was only 28%, the lead plating was serious, and the number of twists after plating decreased from 22 to 12, which is not feasible.
[0091] Example 2: Taking the production of SH-grade galvanized spring steel wire with a diameter of 2.6mm as an example, the austenitizing temperature is 910-930℃, the lead bath temperature is 510-525℃, and the machine speed is 19m / min. The sorbitization rate is 93%, the area reduction rate is 39%, there is no martensite, and the torsional performance after plating is normal.
[0092] Example 3: Taking the production of galvanized spring steel wire with a diameter of 4.5mm as an example, the austenitizing temperature is 890-910℃, the lead bath temperature is 500-520℃, and the machine speed is 18m / min. The sorbitization rate is 90%, the area shrinkage rate is 36%, there is no martensite, and the torsional performance after plating is normal.
[0093] Table 3, Performance Parameters of Multiple Embodiments
[0094] Example 1 Example 2 Example 3 Comparative Example 1 austenitizing temperature 900~930℃ 910~930℃ 890~910℃ Martensitic structure none none none exist surface shrinkage rate 38% 39% 36% 28% Soxhletization rate 95% 93% 90% Approximately 70% Post-plating torsional performance (passing at 22 cycles as the standard value) normal normal normal 12 times
[0095] As can be seen from Examples 1-3 in Table 3, the austenitizing temperature is between 880 and 930℃. The martensite structure transforms into a uniform sorbite + pearlite + a small amount of bainite structure, resulting in a high sorbitization rate and good torsional properties after plating, ensuring the torsional performance of the finished steel wire. In Comparative Example 1, due to direct heat treatment, the microstructure control is poor, the surface quality is poor, and the torsional performance of the galvanized wire is insufficient.
[0096] Example 4
[0097] Based on the aforementioned online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire, an acid pickling tank is used in the online pickling process of step three, such as... Figure 1 As shown, the pickling tank includes a tank body 1, and a pickling tank 11 is provided inside the tank body 1; a vertical frame 2 is provided on one side of the tank body 1, and a vertical groove is provided inside the vertical frame 2, and a vertical lead screw 3 is installed thereon; a lifting motor 4 is installed on the top of the vertical lead screw 3, and the lifting motor 4 is used to drive the vertical lead screw 3 to rotate, thereby driving the moving block 5 threaded on the vertical lead screw 3 to rise and fall; in order to control the acid temperature and ensure a stable chemical reaction rate, a heating layer and a temperature sensing element can be added to the pickling tank to detect and control the heating temperature.
[0098] A movable plate 6 is integrally mounted on the movable block 5. Multiple sets of pull rollers 7 are provided at the bottom of the movable plate 6 for driving the steel wire.
[0099] The bottom of the box 1 is equipped with an acid drain pipe and an anti-corrosion valve 8 to control the opening and closing of the acid drain pipe; both the acid drain pipe and the anti-corrosion valve require professional pipes and valves to deal with acid liquid.
[0100] The pickling tank 11 is filled with pickling solution for online pickling of steel wire; the multiple sets of pull rollers 7 move and lift inside and outside the box 1, and the box 1 is provided with an opening and closing door 9 for closing the pickling tank.
[0101] like Figure 2 As shown, multiple sets of pull rollers 7 are equipped with support plates 10 at both ends and are fixedly connected to the moving plate 6; at least the middle pull roller 7 immerses the steel wire in the pickling solution; as Figure 7 As shown, the size of the movable plate 6 is not smaller than the size of the pickling tank 11.
[0102] like Figure 3 and 4 As shown, a feed pipe 12 is installed at one end of the box body 1, and two sets of guide wheels 13 are installed at the inlet of the feed pipe 12. Guide grooves are opened on the guide wheels 13 to constrain the steel wire from entering the box body 1.
[0103] The guide wheel 13 is provided with a bracket plate 14 and an adjusting rod 15 is installed on it. The adjusting rod 15 extends through the feed pipe 12 to the outside and is equipped with a locking nut.
[0104] like Figure 2 and 3 As shown, a position plate 16 is provided on one side of the housing 1; two sets of constraint plates 17 are provided in the middle of the position plate 16, and limit plates 18 are installed at both ends; a bidirectional motor 19 is installed between the two sets of constraint plates 17; the output end of the bidirectional motor 19 passes through the constraint plate 17 and is coaxially mounted with a side lead screw 20; a bearing is installed between the end of the side lead screw 20 away from the bidirectional motor 19 and the limit plate 18; since the side lead screw is long, the limit plates and constraint plates at both ends need to be lengthened to enhance the support effect; secondly, the bottom of the side block is pressed on the position plate to ensure sufficient support to achieve the lateral movement effect of opening and closing the door.
[0105] A side block 21 is threaded onto the side lead screw 20, and the side block 21 moves along the axis of the side lead screw 20; an opening and closing door 9 is installed on the side block 21.
[0106] like Figure 2 The bottom of one side of the opening / closing door 9 is fixedly connected to the side block 21, and the other side is connected to the guide rail 22; the guide rail 22 is fixedly connected to the side of the housing 1 opposite to the position plate 16, such as... Figure 3 and 5 A hemispherical portion is bent on one side of the opening / closing door 9. The hemispherical portion is strip-shaped and located at the upper part of the bend of the opening / closing door. Figure 5 In the middle, the synchronous guide rail is T-shaped, fixed on one side of the box body, and has a groove at the bottom to fit the connection of the hemispherical part. Since the opening and closing door bends upward at the connection and is constrained on the guide rail 22, it can achieve the effect of sliding and preventing bending. The two sides of the opening and closing door 9 are supported on the side block 21 and the guide rail 22 respectively and slide.
[0107] like Figure 2 As shown, the lengths of the position plate 16 and the guide rail 22 are both greater than the length of the housing 1, and a connecting plate 26 is installed between the position plate 16 and the guide rail 22, with the connecting plate 26 fixed to the end of the housing 1.
[0108] like Figure 11When pickling is required, the steel wire is first threaded into the feed pipe and then through the traction rope, then wound around the roller, and finally threaded into the outlet pipe to complete the pickling process. Afterwards, it is introduced into a water tank for cooling and deacidification. During pickling, the opening and closing door is opened, and the lifting motor drives the moving block to descend, causing the moving plate to descend and pull the steel wire down, immersing it in the acid solution. The steel wire is then continuously fed in to complete the online steel wire pickling.
[0109] like Figure 2 On the right side, an outlet pipe 31 is installed at the end of the housing 1 furthest from the feed pipe 12, and a water tank 27 is also installed thereon; Figure 10 The water tank 27 has two flow pipes, one (28) and two (29), installed on its sides respectively. Flow pipe one (28) is for liquid inlet, and flow pipe two (29) is for liquid outlet. The flowing water forms a continuous water curtain through a water pump, which allows the steel wire to pass through continuously while effectively preventing acid mist from flowing out with the pipes. The cleaned steel wire can be dried subsequently to thoroughly degrease and pickle before the phosphating process, thus obtaining a clean active surface.
[0110] Two sets of parallel filter screens 30 are installed inside the water tank 27, and the steel wire passes through the two sets of filter screens 30; the filter screens 30 are perpendicular to the liquid inlet direction of the flow pipe 28.
[0111] This invention features a movable plate that can be raised and lowered, which drives a pull roller to pull a steel wire, allowing the plate to move up and down while closing at the top opening of the pickling tank, reducing acid mist overflow and minimizing its impact on operators. Furthermore, it incorporates two sets of opening and closing doors that can be driven by a bidirectional motor and a side-mounted lead screw to open and close the top opening of the pickling tank when not in use; the doors are opened during pickling.
[0112] Example 5
[0113] like Figure 12-14 As shown, this is another embodiment of the present invention, based on embodiment 4, as follows. Figure 12 As shown, a long groove 23 along the length of the housing 1 is provided on the opening and closing door 9, and the long groove 23 runs through the top and bottom of the opening and closing door 9; a sliding block 24 is installed in the long groove 23, and elastic folding plates 25 are installed on both sides of the sliding block 24 to close the distance between the long groove 23 and the sliding block 24; a guide hole is provided in the middle of the sliding block 24 for the steel wire to pass through.
[0114] like Figure 13 As shown, the steel wire is directly threaded through the guide hole of the sliding block of the opening and closing gate, inserting one end of the wire. At this time, the opening and closing gate opens, and the sliding block on the left moves to the left, away from the pickling tank. After the wire passes through, the two sets of opening and closing gates are closed by a bidirectional motor, at which point the pickling tank closes. Then, one end of the wire continues to pass over multiple sets of pull rollers; then the two sets of closing gates are opened again, as shown... Figure 13On the right side, the end of the steel wire is then inserted into the water tank. During the steel wire pulling process, operators stay away from the pickling tank to reduce the impact of acid mist, and it is not necessary to insert the wire into the acid tank. The steel wire moves up and down with the moving plate and is immersed in the acid solution for pickling.
[0115] Finally, it should be noted that the above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.
Claims
1. A method for lead-quenching and online phosphating heat treatment of galvanized aluminum spring steel wire, characterized in that: Specific process steps: Step 1, lead quenching and heating: The semi-finished steel wire after the billet drawing is heated to the austenitizing temperature of 880-930℃ in sections to avoid overheating of the steel wire; Step 2, lead bath isothermal transformation: The steel wire is immersed in a molten lead bath at a temperature of 500-530℃ for isothermal transformation. The temperature fluctuation of the lead bath is controlled within ±5℃, the machine speed is 18-20m / min, the DV value is controlled at 50-70, and the sorbite conversion rate is greater than 90% to obtain a fine lamellar sorbite structure. Step 3, Online Phosphating: After the steel wire completes the lead quenching isothermal transformation, it directly enters the online pickling, phosphating, saponification and drying processes; Step 4, Cooling: Use two air cooling systems for uniform cooling.
2. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 1, characterized in that: In the online pickling process in step three, a pickling box is used. The pickling box includes a box body (1) and a pickling tank (11) is provided inside the box body (1). A vertical frame (2) is provided on one side of the box body (1). A vertical groove is provided inside the vertical frame (2) and a vertical screw (3) is installed. A lifting motor (4) is installed on the top of the vertical screw (3). The lifting motor (4) is used to drive the vertical screw (3) to rotate and drive the moving block (5) threaded on the vertical screw (3) to rise and fall. A movable plate (6) is integrally mounted on the movable block (5), and multiple sets of pull rollers (7) are provided at the bottom of the movable plate (6) for driving the steel wire; The bottom of the box (1) is provided with an acid drain pipe and an anti-corrosion valve (8) is installed to control the opening and closing of the acid drain pipe; The pickling tank (11) is filled with pickling liquid for online pickling of steel wire; the multiple sets of pull rollers (7) move and lift inside and outside the box (1), and the box (1) is provided with an opening and closing door (9) for closing the pickling tank.
3. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 2, characterized in that, Multiple sets of pull rollers (7) are provided with support plates (10) at both ends and are fixedly connected to the moving plate (6); at least the middle pull roller (7) immerses the steel wire in the pickling solution; The size of the moving plate (6) is not smaller than the size of the pickling tank (11).
4. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 3, characterized in that, A position plate (16) is provided on one side of the housing (1); two sets of constraint plates (17) are provided in the middle of the position plate (16), and limit plates (18) are installed at both ends; a bidirectional motor (19) is installed between the two sets of constraint plates (17); the output end of the bidirectional motor (19) passes through the constraint plate (17) and is coaxially mounted with a side screw (20); a bearing is installed between the end of the side screw (20) away from the bidirectional motor (19) and the limit plate (18); A side block (21) is threaded onto the side screw (20), and the side block (21) moves along the axis of the side screw (20); an opening and closing door (9) is installed on the side block (21).
5. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 4, characterized in that, The bottom of one side of the opening and closing door (9) is fixedly connected to the side block (21), and the other side is connected to the guide rail (22); the guide rail (22) is fixedly connected to the side of the housing (1) facing away from the position plate (16), and a hemispherical part is bent on one side of the opening and closing door (9) and constrained on the guide rail (22); the two sides of the opening and closing door (9) are supported on the side block (21) and the guide rail (22) respectively and slide.
6. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 5, characterized in that, The lengths of the position plate (16) and the guide rail (22) are both greater than the length of the box (1), and a connecting plate (26) is installed between the position plate (16) and the guide rail (22), with the connecting plate (26) fixed to the end of the box (1).
7. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 6, characterized in that, The box (1) is equipped with a liquid outlet pipe (31) and a water tank (27) at one end away from the feed pipe (12); a flow pipe one (28) and a flow pipe two (29) are respectively installed on both sides of the water tank (27), with the flow pipe one (28) for liquid inlet and the flow pipe two (29) for liquid outlet; Two sets of parallel filter screens (30) are installed in the water tank (27), and the steel wire passes through the two sets of filter screens (30); the filter screens (30) are perpendicular to the liquid inlet direction of the flow pipe (28).
8. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 7, characterized in that, A feed pipe (12) is installed at one end of the box (1), and two sets of guide wheels (13) are installed at the opening of the feed pipe (12). Guide grooves are opened on the guide wheels (13) to constrain the steel wire from entering the box (1). The guide wheel (13) is provided with a bracket plate (14) and an adjusting rod (15) is installed. The adjusting rod (15) extends through the feed pipe (12) to the outside and is equipped with a locking nut.
9. The online phosphating heat treatment method for lead quenching of galvanized aluminum spring steel wire according to claim 5, characterized in that, The opening and closing door (9) is provided with a long groove (23) along the length of the box body (1), and the long groove (23) runs through the top and bottom of the opening and closing door (9); a sliding block (24) is installed in the long groove (23), and elastic folding plates (25) are installed on both sides of the sliding block (24) to close the distance between the long groove (23) and the sliding block (24); a guide hole is provided in the middle of the sliding block (24) for the steel wire to pass through.