A strong corrosion-resistant Ti-Si-C MAX phase coating and a preparation method and application thereof
By using DC/HiPIMS technology and designing a Ti-C/Ti-Si-C layer structure, the challenge of low-temperature composition control in Ti3SiC2MAX phase coatings was solved, resulting in a high-purity, uniform equiaxed nanocrystalline coating that improves the overall performance of the coating and is suitable for protection of marine and aerospace equipment.
Patent Information
- Application Number
- CN202611447404.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies make it difficult to achieve precise composition control of Ti3SiC2MAX phase coatings at low temperatures, leading to the formation of competing phases and the volatilization of Si elements in the coating, which affects the fracture toughness, thermal shock resistance, and service stability of the coating in harsh corrosive environments.
A uniformly distributed equiaxed nanocrystalline Ti3SiC2MAX phase coating was prepared by employing a two-step deposition strategy combining a Ti-C transition layer and a Ti-Si-C functional layer using single-target DC/HiPIMS co-sputtering technology and vacuum annealing.
It achieves precise control of the composition of Ti3SiC2MAX phase coating, suppresses the formation of competing phases, improves the density and bonding strength of the coating, and extends the anti-corrosion and anti-oxidation life. It is suitable for high-temperature and high-salt harsh environment protection for marine engineering and aerospace equipment.
Smart Images

Figure CN123063735A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional coating materials technology, specifically relating to a tough and corrosion-resistant Ti-Si-C MAX phase coating, its preparation method, and its application. Background Technology
[0002] MAX phase (M n+1 AX n Ti3SiC2 is a class of nanolayered ternary compounds that combine the excellent properties of metals and ceramics. M represents an early transition metal, A is primarily a group IIIA or IVA element, and X is C or N. These materials, with their unique layered crystal structure, exhibit excellent electrical and thermal conductivity, high hardness, outstanding thermal shock resistance, and good corrosion resistance and high-temperature oxidation resistance. Among the many MAX phases, Ti3SiC2, as a typical representative of the 312 type, not only possesses higher hardness, elastic modulus, and fracture toughness, but also exhibits good corrosion resistance in intermediate-temperature salt spray corrosion environments, with extremely low electrochemical corrosion rates and high corrosion activation energy. Therefore, the Ti3SiC2 MAX phase is considered an ideal candidate material for surface protection of hot-end components in marine engineering equipment and aero-engines.
[0003] However, the preparation of Ti3SiC2MAX phase coatings still faces significant technical bottlenecks. Firstly, the Ti3SiC2 crystal structure has a long c-axis, resulting in long diffusion paths and high potential barriers for atoms along this direction, requiring high thermodynamic driving forces for phase formation. Traditional preparation processes such as chemical vapor deposition (CVD) and solid-state reaction sintering typically require temperatures above 1000 °C, with bulk synthesis temperatures even exceeding ~1200 °C. These high-temperature processes not only significantly limit the selection range of substrate materials (such as titanium alloys and stainless steel) but also easily induce substrate grain coarsening, elemental segregation, or interfacial interdiffusion, leading to severe deterioration of the substrate's mechanical properties and dimensional accuracy.
[0004] Secondly, in the Ti-Si-C ternary system, thermodynamic equilibrium calculations show that TiC and TiSi... x Competing phases have lower formation free energy and are therefore more likely to preferentially nucleate during deposition. Especially during non-equilibrium deposition or subsequent heat treatment, Si atoms, due to their high vapor pressure, are prone to desorption and volatilization, causing the actual composition of the coating to deviate from the ideal stoichiometry, thus inducing the formation of large amounts of TiC and TiSi. x The precipitation of brittle impurity phases. The enrichment of impurity phases will significantly disrupt the layered topology unique to the MAX phase, greatly reducing the fracture toughness, thermal shock resistance, and long-term service stability of the coating in harsh corrosive environments.
[0005] Currently, existing technologies have developed various methods for preparing Ti-Si-C MAX phase coatings. For example, patent CN118345336 A employs high-power pulsed magnetron sputtering (HiPIMS) technology to alternately deposit Ti. Si coating and Ti Si C coating effectively reduces the formation temperature of the MAX phase, but the multilayer alternating deposition process is complex. Moreover, the alloy target cannot independently adjust the Ti and Si content, only the C content, resulting in low precision. In addition, the element ratio of the alloy target is locked, which reduces the flexibility and precision of composition control. Furthermore, in reactive sputtering, CH4 gas readily reacts with the alloy target surface, forming a high-resistivity carbide layer (i.e., target poisoning), and there is a possibility of hydrogen inclusions and defects.
[0006] In summary, achieving independent and precise control of the deposition fluxes of Ti, Si, and C elements through a direct deposition process at relatively low substrate temperatures, while suppressing the formation of competing phases and Si volatilization, to prepare a high-purity, uniformly composed, strongly interfacially bonded Ti3SiC2MAX phase coating with excellent comprehensive mechanical and corrosion resistance properties, has become a key technical challenge urgently needing to be overcome in this field. Therefore, there is an urgent need to develop a novel, low-damage, high-precision, and engineerable MAX phase coating preparation process to meet the stringent performance requirements of surface protective coatings for high-end marine and aerospace equipment. Summary of the Invention
[0007] The main objective of this invention is to provide a tough and corrosion-resistant Ti-Si-C MAX phase coating, its preparation method, and its application, so as to overcome the shortcomings of the prior art.
[0008] To achieve the aforementioned objectives, the technical solution adopted by this invention includes: The first aspect of the present invention provides a tough and corrosion-resistant Ti-Si-C MAX phase coating, comprising: A transition layer is located on the surface of the alloy substrate, and the transition layer includes a Ti-C transition layer or a T-Si transition layer; The Ti-Si-C functional layer is stacked on the surface of the transition layer opposite to the alloy matrix. The Ti-Si-C functional layer includes a Ti3SiC2MAX phase, and the Ti3SiC2MAX phase has a close-packed hexagonal crystal structure. The tough and corrosion-resistant Ti-Si-C MAX phase coating has a uniformly distributed equiaxed nanocrystalline structure.
[0009] A second aspect of the present invention provides a method for preparing a tough and corrosion-resistant Ti-Si-C MAX phase coating, comprising: A single-target DC / HiPIMS technique is used, with a Ti target as the high-power pulsed sputtering target and a C or Si target as the DC sputtering target, to deposit a Ti-C transition layer or a T-Si transition layer on the surface of a pretreated alloy substrate. A multi-target DC and high-power pulsed magnetron co-sputtering technology is used, with Ti target as high-power pulsed sputtering target and C target and Si target as DC sputtering targets respectively, to perform synchronous sputtering and deposit on the surface of Ti-C transition layer or T-Si transition layer to obtain Ti-Si-C functional layer; A strong, tough, and corrosion-resistant Ti-Si-C MAX phase coating was obtained by vacuum annealing an alloy substrate with the Ti-Si-C functional layer on its surface.
[0010] A third aspect of the invention provides the application of the Ti-Si-C MAX phase coating in the field of surface protection for marine engineering equipment or key aerospace components.
[0011] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The present invention adopts a two-step deposition strategy. First, Ti is prepared on the substrate surface. C transition layer or Ti A Si transition layer is then deposited on top of it, followed by the deposition of Ti. Si C functional layer. The transition layer acts as a mechanical buffer zone between the coating and the substrate, while also playing a role in elemental regulation. Ti is selected. When using a Si transition layer, it serves two purposes: firstly, it replenishes Si in situ when losses occur in the outer functional layers; secondly, it effectively prevents the diffusion of Si from the outer layers into the deeper substrate. Ti is selected. In the C transition layer, a dense covalent bond network ensures strong interfacial element bonding. Both transition layers establish interlayer chemical potential equilibrium, ensuring that the outer Ti3SiC2MAX phase maintains a precise stoichiometric ratio throughout long-term high-temperature service, thus significantly extending the coating's corrosion and oxidation resistance lifespan. Therefore, the transition layer not only blocks the interfacial diffusion channels of light elements but also provides continuous compositional self-sustaining capability throughout service life. The functional layer and the transition layer work synergistically to construct a robust and corrosion-resistant dense MAX phase coating system.
[0012] (2) This invention also differs from the macroscopic diffusion kinetics path relied upon by traditional alternating deposition to construct multilayer modulated structures. It adopts a three-target co-sputtering process to construct an atomically homogeneous, interface-free precursor structure in the early stage of Ti-Si-C functional layer deposition. This structure transforms the long-range heterogeneous diffusion process in the subsequent annealing process into in-situ short-range crystallization behavior, which not only significantly reduces the nucleation barrier of the Ti3SiC2MAX phase and improves the phase purity, but more importantly, it avoids Kirkendal voids caused by differences in element diffusion rates, as well as the interlayer stress concentration and peeling failure problems inherent in traditional multilayer coatings. Ultimately, it achieves a synergistic improvement in coating density, bonding strength, and high-temperature oxidation resistance.
[0013] (3) The coating composition of this invention is precisely controlled, resulting in high purity of the main phase. The use of independent sputtering sources for Ti, Si, and C elemental targets breaks the limitations of traditional alloy targets or reactive gases introducing carbon sources, achieving dynamic and precise matching of the three-element deposition flux. This design effectively suppresses the thermodynamically stable deposition of TiC and TiSi. x The formation of competing phases makes the Ti3SiC2MAX phase the main phase, fully preserving the intrinsic toughness of the MAX phase.
[0014] (4) This invention employs low-temperature phase formation, avoiding thermal damage to the substrate. By introducing DC / HiPIMS composite sputtering technology, the ionization rate and surface migration ability of the deposited particles are significantly improved, effectively reducing the nucleation energy barrier of the Ti3SiC2MAX phase, and the annealing phase formation temperature of the coating is greatly reduced to 750 ℃, which is 200 ℃ lower than the traditional method. This process avoids the thermal damage to the substrate structure caused by traditional high-temperature synthesis, and significantly broadens the engineering application range of the coating on heat-sensitive substrates such as titanium alloys, titanium-aluminum alloys, and stainless steel.
[0015] (5) The coating obtained by this invention has excellent comprehensive performance through structural design. By constructing an interface structure of "Ti-C / Ti-Si transition layer / Ti-Si-C functional layer" and combining it with a vacuum annealing process of 750~900 ℃, the preferred diffusion of atoms and grain boundary reconstruction within the coating are promoted, ultimately obtaining a dense and uniformly distributed equiaxed nanocrystalline structure. This structure not only significantly improves the film-substrate bonding strength and coating hardness, but also endows it with excellent resistance to seawater corrosion and salt spray corrosion, making it particularly suitable for long-term protection of equipment under harsh marine high-temperature and high-salt conditions. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 This is a scanning electron microscope cross-sectional morphology image of the Ti3SiC2MAX phase coating prepared in Example 1 of this invention; Figure 2 The XRD patterns of the coatings prepared in Examples 1, 2 and Comparative Example 3 of this invention are shown below. Figure 3a The image shows the surface morphology of the coating prepared in Example 2 of this invention under an optical microscope. Figure 3b This is a surface morphology image of the coating prepared in Comparative Example 1 of the present invention under an optical microscope; Figure 4 This is a comparison chart of the nanoindentation hardness data of the coatings prepared in Example 2 and Comparative Example 2 of the present invention; Figure 5a This is a scanning electron microscope (SEM) image of the coating cube indenter toughness test prepared in Example 1 of the present invention. Figure 5b The image shows the scanning electron microscope (SEM) morphology of the coated Cube indenter prepared in Comparative Example 3 of this invention for toughness testing. Figure 6 The above are the potentiodynamic polarization curves of the coatings prepared in Examples 2, 3 and 4 of this invention; Figure 7 This is a macroscopic morphology diagram of the coating of Comparative Example 4 of the present invention. Detailed Implementation
[0018] In view of the problems existing in the above-mentioned prior art, after in-depth research, a tough and corrosion-resistant Ti-Si-C MAX phase coating, its preparation method and application are provided.
[0019] The following will provide a further explanation of the technical solution, its implementation process, and its principles.
[0020] The first aspect of the present invention provides a tough and corrosion-resistant Ti-Si-C MAX phase coating comprising: A transition layer is located on the surface of the alloy substrate, and the transition layer includes a Ti-C transition layer or a T-Si transition layer; The Ti-Si-C functional layer is stacked on the surface of the transition layer opposite to the alloy matrix. The Ti-Si-C functional layer includes a Ti3SiC2MAX phase, and the Ti3SiC2MAX phase has a close-packed hexagonal crystal structure. The tough and corrosion-resistant Ti-Si-C MAX phase coating has a uniformly distributed equiaxed nanocrystalline structure.
[0021] In this invention, the hexagonal crystal structure is a spatial structure, and the equiaxed nanocrystal structure is a microstructure.
[0022] In some implementations, the Ti3SiC2MAX phase is the main phase of the coating.
[0023] In some embodiments, the atomic percentage of Ti in the Ti-Si-C functional layer is 40-50%, the atomic percentage of Si is 13-25%, and the atomic percentage of C is 30-42%.
[0024] In some implementations, the thickness of the Ti-C transition layer is 0.2~1 μm.
[0025] In some implementations, the thickness of the T-Si transition layer is 0.2~1 μm.
[0026] In some implementations, the thickness of the Ti-Si-C functional layer is 3~5 μm.
[0027] In some embodiments, the total thickness of the tough and corrosion-resistant Ti-Si-C MAX phase coating is 3~7 μm.
[0028] A second aspect of the present invention provides a method for preparing a tough and corrosion-resistant Ti-Si-C MAX phase coating, comprising: A single-target DC / HiPIMS technique is used, with a Ti target as the high-power pulsed sputtering target and a C or Si target as the DC sputtering target, to deposit a Ti-C transition layer or a T-Si transition layer on the surface of a pretreated alloy substrate. A multi-target DC and high-power pulsed magnetron co-sputtering technology is used, with Ti target as high-power pulsed sputtering target and C target and Si target as DC sputtering targets respectively, to perform synchronous sputtering and deposit on the surface of Ti-C transition layer or T-Si transition layer to obtain Ti-Si-C functional layer; The alloy substrate with the Ti-Si-C functional layer was subjected to vacuum annealing to obtain a tough and corrosion-resistant Ti-Si-CMAX phase coating.
[0029] In some embodiments, the alloy substrate is pretreated before the preparation of the tough and corrosion-resistant Ti-Si-C MAX phase coating. The pretreatment includes mechanical polishing, ultrasonic cleaning and plasma glow etching of the alloy substrate in sequence.
[0030] In some preferred embodiments, the plasma glow etching includes: in a vacuum environment, introducing an inert gas and applying a DC negative bias voltage to the alloy substrate to perform the plasma glow etching.
[0031] Furthermore, the process parameters for plasma glow etching include: substrate temperature of 200~400 ℃, argon flow rate of 40~60 sccm, working pressure of 1.5~2.5 Pa, substrate bias voltage of -500~-300 V, and etching time of 20~60 min.
[0032] In some embodiments, the process parameters for depositing the Ti-C transition layer include: argon as the working gas, working pressure of 0.5~1.0 Pa, substrate bias of -100~-50 V, argon flow rate of 20~40 sccm, deposition temperature of 200~400 ℃, and deposition time of 0.5~1.0 h; The Ti target is sputtered using high-power pulsed sputtering with an average power of 100-150 W, a duty cycle of 5-10%, and a frequency of 500-1000 Hz; the C target is sputtered using DC sputtering with an average power of 80-120 W.
[0033] In some embodiments, the process parameters for depositing the Ti-Si transition layer include: argon as the working gas, working pressure of 0.5~1.0 Pa, substrate bias of -100~-50 V, argon flow rate of 20~40 sccm, deposition temperature of 200~400 ℃, and deposition time of 0.5~1.0 h; The Ti target is sputtered using high-power pulsed sputtering with an average power of 100-150 W, a duty cycle of 5-10%, and a frequency of 500-1000 Hz; the Si target is sputtered using DC sputtering with an average power of 60-100 W.
[0034] In some implementations, the process parameters for depositing the Ti-Si-C functional layer include: argon as the working gas, working pressure of 0.5~1.0 Pa, substrate bias of -100~-50 V, argon flow rate of 20~40 sccm, and deposition temperature of 200~400 ℃; The Ti target is sputtered using high-power pulsed sputtering with an average power of 100-150 W, a duty cycle of 5-10%, and a frequency of 500-1000 Hz; the Si target is sputtered using DC sputtering with an average power of 60-100 W; and the C target is sputtered using DC sputtering with an average power of 80-120 W.
[0035] In some implementations, the vacuum annealing process specifically includes: annealing at a vacuum level of less than 1×10⁻⁶. -3Under Pa conditions, the alloy substrate with the Ti-Si-C functional layer is heated to 750-900 ℃ at a heating rate of 10-20 ℃ / min, and held at that temperature for 1-24 h, and then naturally cooled to room temperature.
[0036] In some embodiments, the alloy matrix includes at least one of stainless steel, titanium alloy, titanium-aluminum alloy, etc., but is not limited to this.
[0037] In some more specific implementations, the preparation method specifically includes the following four core steps: Step S1: Plasma glow etching cleaning and activation The alloy matrix (such as stainless steel, titanium alloy, or titanium-aluminum alloy) is loaded into the vacuum magnetron sputtering reaction chamber and evacuated to a background vacuum (≤1×10⁻⁶). -3 After passing through a pressure of 1.5 Pa, high-purity argon gas is introduced. The substrate temperature is set to 200–400 °C, the argon flow rate to 40–60 sccm, the working pressure to 1.5–2.5 Pa, and a DC negative bias of -500 to -300 V is applied for glow etching for 20–60 min. This step utilizes high-energy Ar... + The bombardment effectively removes the oxide film and adsorbed impurities from the substrate surface, forming a micro-activated surface with moderate roughness, providing high-density chemical bonding sites for subsequent coatings and significantly improving the film-substrate bonding strength.
[0038] Step S2: Deposit Ti-C / Ti-Si transition layer A single-target DC / HiPIMS co-sputtering technique was employed, using a high-purity Ti target as the HiPIMS target and a C / Si target as the DC target, to deposit a Ti-C / Ti-Si transition layer under a pure argon atmosphere. The process parameters were controlled as follows: working pressure 0.5–1.0 Pa, substrate bias -100–-50 V, argon flow rate 20–40 sccm, and deposition temperature 200–400 °C. The Ti target was used in high-power pulse mode with an average power of 100–150 W (duty cycle 5–10%, pulse frequency 500–1000 Hz); the optional Ti-C transition layer C target was used in DC mode with an average power of 80–120 W. The deposition time was controlled at 0.5–1.0 h to achieve a transition layer thickness of 0.2–1.0 μm, with the optimal Ti to C atomic ratio maintained at 0.6–1.25. The optional Ti-Si transition layer Si target is used in DC mode with an average power of 60~100 W. The deposition time is controlled at 0.5~1.0 h to achieve a transition layer thickness of 0.2~1.0 μm, and the Ti to Si atomic ratio within the layer is preferably maintained at 1~2. The high ionization rate plasma generated by HiPIMS enhances the surface migration ability of the deposited particles, enabling a gradient transition between the transition layer and the substrate, effectively alleviating the thermal expansion coefficient mismatch stress.
[0039] Step S3: Deposit Ti-Si-C functional layer A Ti-Si-C functional layer was deposited on the Ti-C / Ti-Si transition layer surface using multi-target DC and high-power pulsed magnetron co-sputtering technology. The Ti target maintained HiPIMS sputtering mode, while the Si and C targets were sputtered using DC sputtering modes. The process parameters were: operating pressure 0.5–1.0 Pa, substrate bias -100–-50 V, argon flow rate 20–40 sccm, and deposition temperature 200–400 °C. The average power of the Ti target was 100–150 W (duty cycle 5–10%, pulse frequency 500–1000 Hz), the average power of the Si target was 60–100 W, and the average power of the C target was 80–120 W. By independently adjusting the sputtering power and bias of the three targets, the deposition flux of each element was precisely controlled, ensuring that the Si content in the functional layer was stabilized at 13–20 at%, and the Ti to Si atomic ratio was controlled within the range of 2.5–3.2. The total thickness of the transition layer and functional layer was preferably controlled within 3–7 μm.
[0040] Step S4: Vacuum annealing induces in-situ precipitation of MAX phase The deposited sample was transferred to a high-vacuum annealing furnace, maintaining a vacuum level ≤1×10⁻⁶. -3 Pa. The temperature was increased to 750–900 °C at a heating rate of 10–20 °C / min and held for 1–24 h, followed by natural cooling to room temperature in a vacuum chamber. The annealing process provided a suitable thermodynamic driving force for the coating, promoting the ordered rearrangement of atoms and grain boundary diffusion in the amorphous / nanocrystalline precursor, driving the in-situ nucleation and growth of the Ti3SiC2MAX phase, ultimately yielding a dense coating with a uniform equiaxed nanocrystalline structure.
[0041] The third aspect of the present invention provides the application of the tough and corrosion-resistant Ti-Si-C MAX phase coating in the field of surface protection for marine engineering equipment or key aerospace components.
[0042] The technical solution of the present invention will be further described below with reference to the embodiments. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available. Other unmentioned raw materials and instruments are all conventionally selected and do not involve the core technical means of the present invention.
[0043] Example 1 In this embodiment, the specific preparation method of the high-purity, strong, tough, and corrosion-resistant Ti-Si-C MAX phase coating is as follows: (1) The TC4 titanium alloy substrate was subjected to mechanical polishing, ultrasonic cleaning, and plasma glow discharge etching in sequence. First, the substrate was polished with silicon carbide metallographic sandpaper from low to high grit up to 3000#, and then polished to a mirror finish with diamond polishing agent. The polished substrate was then ultrasonically cleaned for 15 min each with acetone and ethanol in sequence. The plasma glow discharge etching specifically included the following steps: the substrate was placed in the vacuum magnetron sputtering reaction chamber and evacuated to a background vacuum (≤1×10). -4 After heating the substrate to 300 °C, high-purity argon gas was introduced. The argon gas flow rate was set to 50 sccm, the working pressure was 2 Pa, and a DC substrate bias voltage of -400 V was applied for glow discharge etching for 30 min.
[0044] (2) A Ti-C transition layer was deposited on the surface of the alloy substrate using DC composite high-power pulsed magnetron sputtering technology. The argon flow rate was 30 sccm, the working pressure was 0.6 Pa, the substrate bias was -70 V, the deposition temperature was 300℃, the Ti single-element target was used as the high-power pulsed sputtering target, the average sputtering power of the Ti target was 120 W (duty cycle 5%, pulse width frequency 500 Hz), the C single-element target was used as the DC sputtering target, the average sputtering power of the C target was 110 W, the deposition time was 0.5 h, and a Ti-C transition layer with a thickness of 0.5 μm was obtained.
[0045] (3) A Ti-Si-C coating was deposited on the surface of the Ti-C transition layer using DC composite high-power pulsed magnetron sputtering technology. The argon flow rate was 30 sccm, the working pressure was 0.6 Pa, the substrate bias was -70 V, and the deposition temperature was 300℃. The Ti elemental target was used as the high-power pulsed sputtering target. The average sputtering power of the Ti target was 120 W, the pulse time was 2000 μs, and the duty cycle was 5%. The Si elemental target and the C elemental target were used as DC sputtering targets. The average sputtering power of the Si target was 75 W, and the average sputtering power of the C target was 100 W. The functional layer was obtained by deposition for 6 h. The thickness of the functional layer was 4.5 μm, and the atomic ratios of Ti, Si, and C in the layer were 49.75%, 14.92%, and 35.33%, respectively.
[0046] (4) Place the prepared Ti-Si-C coating in a tube furnace and wait for the vacuum level in the furnace to reach 1×10⁻⁶. -3 When the Pa is below 800 ℃, the sample is heated to 800 ℃ at a heating rate of 10 ℃ / min and held at this temperature for 120 min. The sample is then cooled to room temperature in the furnace to obtain a Ti3SiC2MAX phase coating with a total thickness of 4.5 μm.
[0047] The coating prepared in Example 1 was characterized and its performance was tested. Its cross-sectional morphology is as follows: Figure 1 As shown, from Figure 1It can be seen that the entire coating structure consists of a functional Ti-C transition layer and a Ti-Si-C functional layer.
[0048] XRD pattern as follows Figure 2 As shown, from Figure 2 It can be seen that the prepared coating is mainly composed of the Ti3SiC2MAX phase.
[0049] Cube indentation morphology as follows Figure 5a As shown, from Figure 5a It can be seen that the coating has no cracks and has good toughness.
[0050] All nanoindentation mechanical property tests in this experiment were performed using the continuous stiffness method; the Cube indentation test was performed using the fixed load method.
[0051] Example 2 (1) The TC4 titanium alloy substrate was subjected to mechanical polishing, ultrasonic cleaning, and plasma glow discharge etching in sequence. First, the substrate was polished with silicon carbide metallographic sandpaper from low to high grit up to 3000#, and then polished to a mirror finish with diamond polishing agent. The polished substrate was then ultrasonically cleaned for 15 min each with acetone and ethanol in sequence. The plasma glow discharge etching specifically included the following steps: the substrate was placed in the vacuum magnetron sputtering reaction chamber and evacuated to a background vacuum (≤1×10). -4 After passing through the substrate (Pa), high-purity argon gas is introduced. The substrate is heated to 300 °C, the argon gas flow rate is 50 sccm, the working pressure is 2 Pa, and a DC substrate bias voltage of -400 V is applied for glow discharge etching for 30 min.
[0052] (2) A Ti-Si transition layer was deposited on the surface of the alloy substrate using DC composite high-power pulsed magnetron sputtering technology. The argon flow rate was 30 sccm, the working pressure was 0.6 Pa, the substrate bias voltage was -70 V, the deposition temperature was 300 ℃, the Ti elemental target was used as the high-power pulsed sputtering target, the average sputtering power of the Ti target was 120 W (duty cycle 5%, frequency 500 Hz), the Si elemental target was used as the DC sputtering target, the average sputtering power of the Si target was 75 W, the deposition time was 0.5 h, and a Ti-Si transition layer with a thickness of 0.5 μm was obtained.
[0053] (3) A Ti-Si-C coating was deposited on the surface of the Ti-Si transition layer using DC composite high-power pulsed magnetron sputtering technology. The argon flow rate was 30 sccm, the working pressure was 0.6 Pa, the substrate bias was -70 V, and the deposition temperature was 300 ℃. The Ti elemental target was used as the high-power pulsed sputtering target. The average sputtering power of the Ti target was 120 W, the pulse time was 2000 μs, and the duty cycle was 5%. The Si elemental target and the C elemental target were used as DC sputtering targets. The average sputtering power of the Si target was 75 W, and the average sputtering power of the C target was 100 W. The three targets were deposited together for 6 h to obtain the functional layer. The thickness of the functional layer was 4.5 μm, and the atomic ratios of Ti, Si, and C in the layer were 45.52%, 21.22%, and 33.26%, respectively.
[0054] (4) Place the prepared Ti-Si-C coating in a tube furnace and wait for the vacuum level in the furnace to reach 1×10⁻⁶. -3 When the pressure is below Pa, the sample is heated to 850 °C at a heating rate of 10 °C / min and held at this temperature for 90 min. The sample is then cooled to room temperature in the furnace to obtain a Ti3SiC2MAX phase coating. The total thickness is 5 μm, and Ti3SiC2MAX is the main phase in the Ti3SiC2MAX phase coating.
[0055] The coating prepared in Example 2 was characterized and its performance was tested. Its XRD pattern is shown below. Figure 2 As shown, the surface morphology image under an optical microscope is as follows. Figure 3a As shown in the figure, the nanoindentation mechanical test data is as follows: Figure 4 As shown, the coating has no cracks and good toughness; the potentiodynamic polarization test results are as follows. Figure 6 As shown, it has a lower corrosion current density.
[0056] Example 3 The preparation method is basically the same as in Example 1, with the only difference being: The substrate selected in step (1) is 316L stainless steel alloy; Step (3) The bias voltage is -80 V. The functional layer thickness is 4.5 μm.
[0057] The total thickness of the obtained Ti3SiC2MAX phase coating is 5 μm.
[0058] Example 4 The preparation method is basically the same as in Example 1, with the only difference being: The matrix selected in step (1) is Ti-45Al-2Mn-2Nb-0.8vol%TiB2 (grade TiAl-45XD) alloy; In step (3), the average power of sputtering on the Si target was 70 W, and the average power of sputtering on the C target was 80 W. The thickness of the functional layer was 4 μm.
[0059] The total thickness of the obtained Ti3SiC2MAX phase coating is 4.5 μm.
[0060] The performance tests of the coatings prepared in Examples 3 and 4 were conducted, and the results of the potentiodynamic polarization test are as follows: Figure 6 As shown, its overall corrosion resistance is good.
[0061] Example 5 The preparation method is basically the same as in Example 1, with the only difference being: In step (3), the average power of the Ti target sputtering was 150 W, the pulse time was 2000 μs, the duty cycle was 10%, and the average power of the Si single-element DC sputtering target was 80 W. The functional layer thickness was 4.5 μm.
[0062] The total thickness of the obtained Ti3SiC2MAX phase coating is 5 μm.
[0063] Example 6 The preparation method is basically the same as in Example 1, with the only difference being: In step (3), the average power of sputtering on the Ti target is 150 W, and the average power of the DC sputtering on the Si single-element target is 100 W; the C target is sputtered by DC with an average power of 120 W. The thickness of the functional layer is 4.5 μm.
[0064] The total thickness of the obtained Ti3SiC2MAX phase coating is 5 μm.
[0065] Comparative Example 1 (1) The TC4 titanium alloy substrate was subjected to mechanical polishing, ultrasonic cleaning, and plasma glow discharge etching in sequence. First, the substrate was polished with silicon carbide metallographic sandpaper from low to high grit up to 3000#, and then polished to a mirror finish with diamond polishing agent. The polished substrate was then ultrasonically cleaned for 15 min each with acetone and ethanol in sequence. The plasma glow discharge etching specifically included the following steps: the substrate was placed in the vacuum magnetron sputtering reaction chamber and evacuated to a background vacuum (≤1×10). -3 After passing through the substrate (Pa), high-purity argon gas is introduced. The substrate is heated to 300°C, the working pressure is 2 Pa, the argon flow rate is 50 sccm, and a DC substrate bias voltage of -400 V is applied for glow discharge etching for 30 min.
[0066] (2) A Ti-Si transition layer was deposited on the surface of the alloy substrate using DC composite high-power pulsed magnetron sputtering technology. The working pressure was 0.6 Pa, the substrate bias voltage was -120 V, the argon flow rate was 30 sccm, the deposition temperature was 300℃, the Ti single-element target was used as the high-power pulsed sputtering target, the average sputtering power of the Ti target was 120 W (duty cycle 5%, frequency 500 Hz), the Si single-element target was used as the DC sputtering target, the average sputtering power of the Si target was 75 W, the deposition time was 0.5 h, and a Ti-Si transition layer with a thickness of 0.5 μm was obtained.
[0067] (3) A Ti-Si-C coating was deposited on the surface of the Ti-Si transition layer using a dual-target DC composite high-power pulsed magnetron sputtering technique. The working pressure was 0.6 Pa, the substrate bias was -120 V, the argon flow rate was 30 sccm, and the deposition temperature was 300℃. The Ti single-element target was used as the high-power pulsed sputtering target. The average power of the Ti target sputtering was 120 W, the pulse time was 2000 μs, and the duty cycle was 5%. The Si single-element target and the C single-element target were used as DC sputtering targets. The average power of the Si target sputtering was 75 W, and the average power of the C target sputtering was 100 W. The deposition time was 6 h, and a functional layer with a thickness of 4 μm was obtained.
[0068] (4) Place the prepared Ti-Si-C coating in a tube furnace and wait for the vacuum level in the furnace to reach 1×10⁻⁶. -3 When the temperature was below Pa, the sample was heated to 850 °C at a heating rate of 10 °C / min and held at this temperature for 1.5 h. After cooling to room temperature in the furnace, the target coating was not obtained.
[0069] The coating prepared in Comparative Example 1 was characterized, and its surface morphology under an optical microscope is as follows: Figure 3b As shown, the coating is cracked.
[0070] Comparative Example 2 (1) The TC4 titanium alloy substrate was subjected to mechanical polishing, ultrasonic cleaning, and plasma glow discharge etching in sequence. First, the substrate was polished with silicon carbide metallographic sandpaper from low to high grit up to 3000#, and then polished to a mirror finish with diamond polishing agent. The polished substrate was then ultrasonically cleaned for 15 min each with acetone and ethanol in sequence. The plasma glow discharge etching specifically included the following steps: the substrate was placed in the vacuum magnetron sputtering reaction chamber and evacuated to a background vacuum (≤1×10). -3 After passing through the substrate (Pa), high-purity argon gas is introduced. The substrate is heated to 300°C, the working pressure is 2 Pa, the argon flow rate is 50 sccm, and a DC substrate bias voltage of -400 V is applied for glow discharge etching for 30 min.
[0071] (2) A Ti-Si-C coating was deposited on the substrate surface using a dual-target DC composite high-power pulsed magnetron sputtering technique. The working pressure was 0.6 Pa, the substrate bias was -70 V, the argon flow rate was 30 sccm, and the deposition temperature was 300℃. The Ti single-element target was used as the high-power pulsed sputtering target. The average sputtering power of the Ti target was 120 W, the pulse time was 2000 μs, and the duty cycle was 5%. The Si single-element target and the C single-element target were used as DC sputtering targets. The average sputtering power of the Si target was 75 W, and the average sputtering power of the C target was 100 W. The deposition time was 6 h. The functional layer was obtained with a thickness of 4 μm.
[0072] (3) Place the prepared Ti-Si-C coating in a tube furnace and wait for the vacuum degree in the furnace to reach 1×10 -3 When the temperature was below Pa, the sample was heated to 850 °C at a heating rate of 10 °C / min and held at this temperature for 1.5 h. After cooling to room temperature in the furnace, the target coating was not obtained.
[0073] The coating prepared in Comparative Example 2 was subjected to performance testing, and its nanoindentation mechanical test data were obtained. Figure 4 As shown, the overall mechanical properties are significantly reduced compared to Example 2.
[0074] Comparative Example 3 (1) The TC4 titanium alloy substrate was subjected to mechanical polishing, ultrasonic cleaning, and plasma glow discharge etching in sequence. First, the substrate was polished with silicon carbide metallographic sandpaper from low to high grit up to 3000#, and then polished to a mirror finish with diamond polishing agent. The polished substrate was then ultrasonically cleaned for 15 min each with acetone and ethanol in sequence. The plasma glow discharge etching specifically included the following steps: the substrate was placed in the vacuum magnetron sputtering reaction chamber and evacuated to a background vacuum (≤1×10). -4 After passing through the substrate (Pa), high-purity argon gas is introduced. The substrate is heated to 300 °C, the argon gas flow rate is 50 sccm, the working pressure is 2 Pa, and a DC substrate bias voltage of -400 V is applied for glow discharge etching for 30 min.
[0075] (2) A Ti-C transition layer was deposited on the surface of the alloy substrate using DC composite high-power pulsed magnetron sputtering technology. The argon flow rate was 30 sccm, the working pressure was 0.6 Pa, the substrate bias voltage was -70 V, the deposition temperature was 350℃, the Ti single-element target was used as the high-power pulsed sputtering target, the average sputtering power of the Ti target was 120 W (duty cycle 5%, frequency 500 Hz), the C single-element target was used as the DC sputtering target, the average sputtering power of the C target was 110 W, the deposition time was 0.5 h, and a Ti-C transition layer with a thickness of 0.5 μm was obtained.
[0076] (3) A Ti-Si-C coating was deposited on the surface of the Ti-C transition layer using a dual-target DC composite high-power pulsed magnetron sputtering technique. The argon flow rate was 30 sccm, the working pressure was 0.6 Pa, the substrate bias was -70 V, the deposition temperature was 300℃, the Ti single-element target was used as the high-power pulsed sputtering target, the average sputtering power of the Ti target was 120 W, the pulse time was 2000 μs, and the duty cycle was 5%. The Si single-element target and the C single-element target were used as DC sputtering targets, the average sputtering power of the Si target was 50 W, the average sputtering power of the C target was 110 W, and the deposition time was 6 h.
[0077] (4) Place the prepared Ti-Si-C coating in a tube furnace and wait for the vacuum level in the furnace to reach 1×10⁻⁶. -3 When the Pa is below 850 °C, the sample is heated to 850 °C at a heating rate of 10 °C / min and held at this temperature for 90 min. It is then cooled to room temperature in the furnace to obtain a hard and brittle TiC phase. x The coating with Ti3SiC2MAX as the main phase did not yield the Ti3SiC2MAX phase.
[0078] The coating prepared in Comparative Example 3 was characterized and its performance was tested. Its XRD pattern is shown below. Figure 2 As shown; the morphology of the cube indentation is as follows. Figure 5b As shown, the coating surface exhibits long cracks and poor toughness.
[0079] Comparative Example 4 (1) The TC4 titanium alloy substrate was subjected to mechanical polishing, ultrasonic cleaning, and plasma glow discharge etching in sequence. First, the substrate was polished with silicon carbide metallographic sandpaper from low to high grit up to 3000#, and then polished to a mirror finish with diamond polishing agent. The polished substrate was then ultrasonically cleaned with acetone and ethanol for 15 min each. The plasma glow discharge etching specifically included the following steps: the substrate was placed in the vacuum magnetron sputtering reaction chamber and evacuated to a background vacuum (≤1×1×10). -4 After passing through the substrate (Pa), high-purity argon gas is introduced. The substrate is heated to 300 °C, the argon gas flow rate is 50 sccm, the working pressure is 2 Pa, and a DC substrate bias voltage of -400 V is applied for glow discharge etching for 30 min.
[0080] (2) A Ti-C coating was deposited on the surface of the alloy substrate using DC composite high-power pulsed magnetron sputtering technology. The argon flow rate was 30 sccm, the working pressure was 0.6 Pa, the substrate bias was -70 V, the deposition temperature was 350℃, the Ti single-element target was used as the high-power pulsed sputtering target, the average sputtering power of the Ti target was 120 W (duty cycle 5%, frequency 500 Hz), the C single-element target was used as the DC sputtering target, the average sputtering power of the C target was 110 W, and the deposition time was 6h to obtain the Ti-C coating.
[0081] (3) Place the prepared Ti-C coating in a tube furnace and wait for the vacuum degree in the furnace to reach 1×10 -3 When the Pa is below 850 °C, the sample is heated to 850 °C at a heating rate of 10 °C / min and held at this temperature for 90 min. It is then cooled to room temperature in the furnace to obtain TiC. x Coating. The total thickness of the resulting coating is approximately 4 μm.
[0082] The coating prepared in Comparative Example 4 is as follows Figure 7 As shown. From Figure 7 It can be seen that the target coating cracked after annealing.
[0083] In addition, the present invention has also conducted experiments with other raw materials, process operations and process conditions described in this specification, with reference to the foregoing embodiments, and has obtained relatively ideal results in all cases.
[0084] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.
Claims
1. A tough and corrosion-resistant Ti-Si-C MAX phase coating, characterized in that, include: A transition layer is located on the surface of the alloy substrate, and the transition layer includes a Ti-C transition layer or a T-Si transition layer; The Ti-Si-C functional layer is stacked on the surface of the transition layer opposite to the alloy matrix. The Ti-Si-C functional layer includes a Ti3SiC2MAX phase, and the Ti3SiC2MAX phase has a close-packed hexagonal crystal structure. The tough and corrosion-resistant Ti-Si-C MAX phase coating has a uniformly distributed equiaxed nanocrystalline structure.
2. The tough and corrosion-resistant Ti-Si-C MAX phase coating according to claim 1, characterized in that: The Ti3SiC2MAX phase is the main phase of the coating; And / or, in the Ti-Si-C functional layer, the atomic percentage of Ti is 40-50%, the atomic percentage of Si is 13-25%, and the atomic percentage of C is 30-42%.
3. The tough and corrosion-resistant Ti-Si-C MAX phase coating according to claim 1, characterized in that: The thickness of the Ti-C transition layer is 0.2~1 μm; And / or, the thickness of the T-Si transition layer is 0.2~1 μm; And / or, the thickness of the Ti-Si-C functional layer is 3~5μm; And / or, the total thickness of the tough and corrosion-resistant Ti-Si-C MAX phase coating is 3~7μm.
4. A method for preparing a tough and corrosion-resistant Ti-Si-C MAX phase coating, characterized in that, include: A single-target DC and high-power pulsed magnetron co-sputtering technique is used, with a Ti target as the high-power pulsed sputtering target and a C or Si target as the DC sputtering target, to deposit a Ti-C transition layer or a Ti-Si transition layer on the surface of a pretreated alloy substrate. A multi-target DC and high-power pulsed magnetron co-sputtering technology is used, with Ti target as high-power pulsed sputtering target and C target and Si target as DC sputtering targets respectively, to perform synchronous sputtering and deposit on the surface of Ti-C transition layer or T-Si transition layer to obtain Ti-Si-C functional layer; A strong, tough, and corrosion-resistant Ti-Si-C MAX phase coating was obtained by vacuum annealing an alloy substrate with the Ti-Si-C functional layer on its surface.
5. The preparation method according to claim 4, characterized in that, Before preparing the tough and corrosion-resistant Ti-Si-C MAX phase coating, the alloy substrate is pretreated, which includes mechanical polishing, ultrasonic cleaning and plasma glow etching of the alloy substrate in sequence. Preferably, the plasma glow etching includes: in a vacuum environment, introducing an inert gas and applying a DC negative bias voltage to the alloy substrate to perform the plasma glow etching; Particularly preferred are the following process parameters for plasma glow etching: substrate temperature of 200~400 ℃, argon flow rate of 40~60 sccm, working pressure of 1.5~2.5 Pa, substrate bias of -500~-300 V, and etching time of 20~60 min.
6. The preparation method according to claim 4, characterized in that, The process parameters for depositing the Ti-C transition layer include: argon as the working gas, working pressure of 0.5~1.0 Pa, substrate bias of -100~-50 V, argon flow rate of 20~40 sccm, deposition temperature of 200~400 ℃, and deposition time of 0.5~1.0 h; The Ti target is sputtered using high-power pulsed sputtering with an average power of 100-150 W, a duty cycle of 5-10%, and a frequency of 500-1000 Hz; the C target is sputtered using DC sputtering with an average power of 80-120 W.
7. The preparation method according to claim 4, characterized in that, The process parameters for depositing the Ti-Si transition layer include: argon as the working gas, working pressure of 0.5~1.0 Pa, substrate bias of -100~-50 V, argon flow rate of 20~40 sccm, deposition temperature of 200~400 ℃, and deposition time of 0.5~1.0 h; The Ti target is sputtered using high-power pulsed sputtering with an average power of 100-150 W, a duty cycle of 5-10%, and a frequency of 500-1000 Hz; the Si target is sputtered using DC sputtering with an average power of 60-100 W.
8. The preparation method according to claim 4, characterized in that, The process parameters for depositing Ti-Si-C functional layers include: argon as the working gas, working pressure of 0.5~1.0 Pa, substrate bias of -100~-50 V, argon flow rate of 20~40 sccm, and deposition temperature of 200~400 ℃; The Ti target is sputtered using high-power pulsed sputtering with an average power of 100-150 W, a duty cycle of 5-10%, and a frequency of 500-1000 Hz; the Si target is sputtered using DC sputtering with an average power of 60-100 W; and the C target is sputtered using DC sputtering with an average power of 80-120 W.
9. The preparation method according to claim 4, characterized in that, The vacuum annealing process specifically includes: annealing at a vacuum level less than 1×10⁻⁶. -3 Under Pa conditions, the alloy substrate with the Ti-Si-C functional layer is heated to 750-900 ℃ at a heating rate of 10-20 ℃ / min, and held at that temperature for 1-24 h, and then naturally cooled to room temperature. And / or, the alloy matrix includes at least one of stainless steel, titanium alloy, and titanium-aluminum alloy.
10. The application of the tough and corrosion-resistant Ti-Si-C MAX phase coating according to any one of claims 1-3 in the field of surface protection of marine engineering equipment or key components of aerospace.