A pretreatment solution and method for chemical copper plating on organic polymer substrates

By using an alkaline aqueous solution pretreatment solution and a graded activation mechanism, the problems of cumbersome steps and coating quality in the chemical copper plating process of organic polymer substrates have been solved, and the density of the coating and the interfacial bonding force have been improved, making it suitable for high-frequency communication and flexible electronic devices.

CN123063753APending Publication Date: 2026-11-10UNIV OF ELECTRONICS SCI & TECH OF CHINA +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611296582.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing pretreatment processes for chemical copper plating on organic polymer substrates are cumbersome, resulting in high resistivity and large surface roughness of the plating layer, making it difficult to guarantee the uniformity of active centers and interfacial adhesion.

Method used

The pretreatment solution, which uses an alkaline aqueous solution system, contains transition metal coordination compounds, molybdates, silicates, and phosphates, to achieve a one-step process of cleaning, micro-etching and roughening, and active site implantation. Combined with a graded activation mechanism, the density and uniformity of catalytic active centers are improved through two activation site implantation and reduction activation treatments.

Benefits of technology

It simplifies the pretreatment process, improves the density and smoothness of the coating, enhances the interfacial bonding strength between the coating and the substrate, and reduces the surface roughness of the coating, making it suitable for high-frequency communication and flexible electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063753A_ABST
    Figure CN123063753A_ABST
Patent Text Reader

Abstract

This invention provides a pretreatment solution and method for electroless copper plating on organic polymer substrates, belonging to the field of surface metallization technology for non-conductive materials. The pretreatment solution is an alkaline aqueous solution system containing 0.01~100 g / L of transition metal coordination compounds or complexes, 0.02~20 g / L of molybdate, 0.05~500 g / L of silicate, 0.05~50 g / L of phosphate, and 0~1.0 g / L of organic additives. It can simultaneously perform substrate cleaning and micro-etching roughening to achieve the first implantation of copper plating active sites. The pretreatment method includes: after substrate pretreatment, it is placed in the pretreatment solution for the first active site implantation, followed by a second active site implantation in a post-activation solution and a reduction activation treatment in a reducing agent solution, finally performing electroless copper plating. This invention integrates the traditional multi-step processes of degreasing, roughening, and activation into one step, combined with a two-stage activation mechanism, significantly simplifying the pretreatment process, improving the density of the copper plating layer and the interfacial adhesion, and is suitable for printed circuit boards, flexible electronics, and sensors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallization technology for non-conductive material surfaces, and more specifically, to a pretreatment solution and method for electroless copper plating on organic polymer substrates. Background Technology

[0002] With the increasing penetration of electronic technology into various application fields of the national economy, the technical approach of metallizing non-conductive materials through surface modification has attracted widespread attention. This mainly includes methods such as electroless plating, vacuum phase deposition (e.g., PVD, CVD), and conductive adhesive sintering. Electroless plating, with its advantages of preparing uniform and continuous metal coatings on complex three-dimensional irregularly shaped insulating substrates, lower equipment investment, and ease of large-scale production, has become an important technical means for metallizing non-metallic surfaces in printed circuit boards (PCBs), chip manufacturing, and flexible electronics. With the evolution of high-frequency communication technologies such as 5G and the rapid popularization of electronic devices such as the Internet of Things, the skin effect and signal integrity are receiving increasing attention. This places higher demands on the resistivity, corrosion resistance, and interlayer adhesion of conductive layers prepared using electroless plating technology. Therefore, developing new electroless copper plating technologies to meet the iterative needs of electronic products has become a current research hotspot.

[0003] Currently, the mainstream technology for metallizing non-conductive substrates using electroless copper plating includes three stages: pretreatment, copper plating, and post-treatment. Pretreatment, encompassing basic processes such as degreasing, micro-etching / roughening, sensitization, and activation, is responsible for cleaning and roughening the substrate surface and forming copper plating growth centers. It plays a decisive role in the quality of the copper plating layer and is one of the key steps in electroless copper plating.

[0004] Zheng Anni et al., in their paper "Research Progress on Pretreatment of Electroless Copper Plating on Polymer Materials" (Acta Chimica Sinica, 2022, 80(05): 659-667), provided a relatively complete literature review on the important applications of surface metallization of organic polymer materials in fields such as communication electronics and the current status of electroless copper plating technology. They proposed that the surface pretreatment of polymer materials directly affects the adhesion and smoothness of the electroless copper plating layer. Chinese patents such as "A Method for Electroless Copper Plating with Ionic Liquids (CN105063582B)" and "A Method for Forming Metal Mesh on a Substrate (CN114489373B)" explored new systems and application areas for electroless copper plating. Chinese invention "A Pretreatment Process and Equipment for Electroless Copper Plating on Double-Sided Printed Circuit Boards (CN113174591B)" disclosed a pretreatment process and equipment for electroless copper plating on double-sided printed circuit boards. In their paper “Study on the Micromorphology of Interface Failure in PCB Chemical Copper Plating” (Printed Circuit Information, 2023, 31(12): 59-65), He Guanghui et al. proposed that the quality of the chemical copper plating layer is a key influencing factor on the interface bonding strength.

[0005] However, the aforementioned research findings and technological innovations are all based on the mature process of traditional electroless copper plating on organic substrates. Each step in the substrate pretreatment stage requires a different treatment solution, and deionized water is needed for rinsing between steps to prevent cross-contamination and interference between the treatment solutions. This process is extremely complex and poses significant challenges to product quality control. Furthermore, the copper deposition centers in the electroless plating process are only formed in the "sensitization and activation" step, making it difficult to guarantee the uniformity of the active centers. The performance of copper layers deposited on non-conductive substrates such as organic polymers using existing activation solutions based on "tin + palladium" and silver nitrate systems still needs improvement in terms of density, interfacial adhesion, and long-term service stability. Summary of the Invention

[0006] The purpose of this invention is to provide a pretreatment solution and method for electroless copper plating of organic polymer substrates, which can simplify the pretreatment operation, improve the uniformity of the distribution of catalytic active centers and enhance the quality of the plating layer, and solve the problems of cumbersome steps, high resistivity of copper plating layer and large surface roughness of plating layer in the existing electroless copper plating pretreatment process for organic polymer substrates.

[0007] This invention is implemented as follows: A pretreatment solution for electroless copper plating on an organic polymer substrate, wherein the pretreatment solution is an alkaline aqueous solution system comprising the following components: Transition metal coordination compounds or transition metal complexes, with a concentration of 0.01–100 g / L; Molybdate, with a concentration of 0.02–20 g / L; Silicates, with a concentration of 0.05–500 g / L; Phosphate, with a concentration of 0.05–50 g / L; And organic additives, at a concentration of 0–1.0 g / L; The pretreatment solution is used to simultaneously clean, micro-etch and roughen the surface of the organic polymer substrate, and perform the first implantation of active sites for chemical copper plating.

[0008] Further, the transition metal coordination compound or transition metal complex is selected from one or more of tetraamminecopper(II) sulfate, copper(II) citrate, disodium ethylenediaminetetraacetate copper(II) ester, copper(II) tartrate complex, disodium ethylenediaminetetraacetate nickel(II) ester, and disodium ethylenediaminetetraacetate palladium(II) ester.

[0009] Furthermore, the molybdate is selected from one or more of potassium molybdate, sodium molybdate, ammonium molybdate, and magnesium molybdate; The silicate is selected from one or more of sodium silicate, aluminum silicate, and potassium silicate; The phosphate is selected from one or more of trisodium phosphate, tripotassium phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, sodium pyrophosphate, potassium pyrophosphate, and sodium tripolyphosphate.

[0010] Furthermore, the organic additive is selected from one or more of the following: silane coupling agent, potassium sulfonylbenzenesulfonate, sodium stearate, potassium myristate, potassium laurate, and alkenyl sulfonate.

[0011] A pretreatment method for electroless copper plating on an organic polymer substrate includes the following steps: After pretreatment to remove surface contaminants, the organic polymer substrate is placed in the pretreatment solution as described above for a first immersion treatment to achieve cleaning, micro-etching roughening, and the first implantation of active sites for chemical copper plating on the substrate surface. The substrate treated as described above is placed in a post-activation solution for a second immersion treatment, thereby achieving a second implantation of chemically plated copper active sites on the substrate surface. The substrate treated as described above is placed in a reducing agent solution for reduction and activation treatment, which reduces the active sites implanted on the substrate surface into catalytically active metal catalytic centers. The substrate, after reduction and activation treatment, is placed in a chemical copper plating solution for chemical copper plating to form a copper plating layer on the substrate surface, and then the copper-plated substrate is post-treated.

[0012] Further, the step of pretreating the organic polymer substrate to remove surface contaminants includes: The organic polymer substrate is placed in an alcohol solvent and immersed in an ultrasonic environment at 25–60°C for 1–30 minutes. After completion, the substrate is removed, cleaned with deionized water, and dried.

[0013] Furthermore, the process conditions for the first soaking treatment are: a treatment temperature of 25–65°C, a treatment time of 10–300 min, and stirring during the soaking process; After soaking, remove the substrate, clean it with deionized water, and then dry it.

[0014] Further, the post-activation solution is a palladium salt activation solution or a silver salt activation solution, and the concentration of the active component in the post-activation solution is 0.05–5 g / L; The process conditions for the second soaking treatment are: temperature 20-50℃, time 0.1-30 min; After soaking, remove the substrate and rinse it with deionized water for 2-5 seconds.

[0015] Further, the reducing agent solution is selected from one of sodium borohydride solution, hydrazine hydrate solution, hydroxylamine solution, and hydrazine sulfate solution; wherein the mass concentration of the reducing agent in the solution is 0.01–10 g / L; The process conditions for the reduction and activation treatment are: temperature of 10-30℃ and time of 2-50 s.

[0016] Furthermore, the temperature for the electroless copper plating is 30–50°C, and the plating time is 10–120 min.

[0017] The beneficial effects of this invention are: (1) The pretreatment solution proposed in this invention has the functions of multiple pretreatment solutions (degreasing solution, roughening solution / micro-etching solution, sensitizing solution) in the traditional chemical copper plating process, and can realize the implantation of active sites in chemical copper plating. It integrates the degreasing, micro-etching / roughening and first activation site implantation in the traditional process into one step, which simplifies the pretreatment process and operation difficulty of chemical copper plating and is conducive to improving quality.

[0018] (2) The pretreatment technology proposed in this invention applies a graded activation mechanism (firstly, transition metal active sites are implanted through the pretreatment solution, and secondly, noble metal active sites are implanted through the post-activation solution), which can improve the density and uniformity of copper growth catalytic centers in the copper plating process, and is beneficial to enhancing the interfacial bonding strength between the copper plating layer and the substrate, as well as the density and flatness of the plating layer. Experimental data show that the surface roughness Sa of the electroless copper plating layer prepared on the polyimide (PI) substrate using the method of this invention can reach 0.060 μm, the bonding force between the copper layer and the substrate reaches the 5B standard, and the surface roughness is reduced by more than 10% compared with the traditional method.

[0019] (3) The pretreatment technology proposed in this invention bypasses the two processes of sensitization and desizing acceleration in traditional chemical copper plating, which not only further simplifies the operation, but also avoids the adverse factors that affect the quality caused by these processes.

[0020] (4) The present invention has good compatibility with existing processes, which can reduce the risk of technology iteration and provide a green, economical and efficient solution to the technical problems encountered by chemical copper plating technology in high frequency communication, flexible electronic devices, sensors and other fields such as high insertion loss and difficulty in ensuring reliability. Attached Figure Description

[0021] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained from these drawings without creative effort.

[0022] Figure 1 This is a flowchart of the pretreatment method for chemical copper plating on an organic polymer substrate provided in the application embodiment; Figure 2This is a 500x scanning electron microscope (SEM) image of the electroless copper plating layer prepared on a polyimide (PI) substrate in Example 1 of the application; Figure 3 This is a 3D confocal microscope image of the surface morphology of the electroless copper plating layer prepared on a polyimide (PI) substrate in Example 1 of the application. Detailed Implementation

[0023] This embodiment provides a pretreatment solution for electroless copper plating on an organic polymer substrate. The pretreatment solution is an alkaline aqueous solution system containing the following components: a transition metal coordination compound or transition metal complex at a concentration of 0.01–100 g / L; molybdate at a concentration of 0.02–20 g / L; silicate at a concentration of 0.05–500 g / L; phosphate at a concentration of 0.05–50 g / L; and organic additives at a concentration of 0–1.0 g / L. The pretreatment solution is used to simultaneously clean, micro-etch and roughen the surface of the organic polymer substrate, and implant the active sites for electroless copper plating for the first time.

[0024] A pretreatment solution was formulated using transition metal complexes (or complexes) and polyacid salts to replace traditional degreasing and roughening / micro-etching solutions. Polyacid salts (molybdates, silicates, phosphates) synergistically regulate the substrate surface state and solution pH to induce micro-etching. Simultaneously, silicate hydrolysis makes the pretreatment solution alkaline, facilitating substrate roughening and degreasing. Silicate ions form a silica film, creating an intermediate layer that increases the substrate's adsorption of activators and reduces the aggregation effect of activating ions. Phosphate ions wet the substrate and adjust its charge, promoting activator adsorption and forming effective catalytic centers. Phosphate hydrolysis also makes the pretreatment solution alkaline, contributing to micro-etching and increasing substrate roughness. Molybdate ions in molybdates act as precursors for non-precious metal activators, participating in surface micro-etching, increasing surface energy, and forming a multi-dimensional network-like corrosion-inhibiting barrier, providing a limited-domain effect for substrate micro-etching. Organic additives are mainly used to adjust the wettability of organic polymer substrates and enhance the effectiveness of the pretreatment solution.

[0025] This pretreatment solution integrates the functions of degreasing solution, roughening solution / micro-etching solution, and sensitizing solution in traditional technologies into a unique new pretreatment solution. It can not only achieve functions such as cleaning and modifying the surface of organic substrates, but also has the function of implanting active sites in copper plating layers. In practical applications, it greatly simplifies the operation steps of traditional pretreatment processes.

[0026] In one embodiment of this application, the aforementioned transition metal coordination compound or transition metal complex is a coordination compound or complex that does not produce precipitation in an alkaline system, and is selected from one or more of tetraamminecopper(II) sulfate, copper(II) citrate, disodium ethylenediaminetetraacetate copper(II) ester, copper(II) tartrate complex, disodium ethylenediaminetetraacetate nickel(II) ester, and disodium ethylenediaminetetraacetate palladium(II) ester.

[0027] The use of transition metal complexes (or complexes) provides a metal ion source and a coordinating agent (or complexing agent) for the pretreatment solution, so that an appropriate amount of metal ions are present on the substrate surface to complete the first activation site implantation.

[0028] In one embodiment of this application, the molybdate is selected from one or more of potassium molybdate, sodium molybdate, ammonium molybdate, and magnesium molybdate; the silicate is selected from one or more of sodium silicate, aluminum silicate, and potassium silicate; and the phosphate is selected from one or more of trisodium phosphate, tripotassium phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, sodium pyrophosphate, potassium pyrophosphate, and sodium tripolyphosphate.

[0029] In one embodiment of this application, the aforementioned organic additive is one or more selected from silane coupling agents, potassium sulfonylbenzenesulfonate, sodium stearate, potassium myristate, potassium laurate, and alkenyl sulfonate. The organic additive is a surface-modifying compound that does not precipitate in an alkaline system.

[0030] In one embodiment of this application, the pH value of the pretreatment solution is 9-13. It is understood that the pH value of the pretreatment solution is spontaneously adjusted by the hydrolysis of silicates and phosphates, without the need for additional pH adjusters.

[0031] In one embodiment of this application, the preparation method of the above-mentioned pretreatment solution includes the following steps: Step 1: Add silicate to deionized water and stir at 20-40℃ until completely dissolved to obtain a clear solution; Step 2: Add phosphate and molybdate to the solution obtained in Step 1, and stir at 20-40°C until completely dissolved; Step 3: Add a transition metal coordination compound or transition metal complex to the solution obtained in Step 2, and optionally add an organic additive. Stir at 20-40°C until the mixture is homogeneous, and cool to obtain the pretreatment solution.

[0032] It should be noted that when the composite inorganic system consisting of transition metal coordination compounds (or complexes), molybdates, silicates and phosphates is sufficient to complete the one-step treatment on the substrate surface, there is no need to introduce additional organic additives.

[0033] Please refer to Figures 1-3 This embodiment also provides a pretreatment method for electroless copper plating on an organic polymer substrate, including the following steps: S110. After pretreating the organic polymer substrate to remove surface contaminants, it is placed in the pretreatment solution as described above for the first immersion treatment to achieve cleaning, micro-etching roughening and the first implantation of active sites for chemical copper plating on the substrate surface. S120. The substrate after the above treatment is placed in the post-activation solution for a second immersion treatment, so as to realize the second implantation of chemical copper plating active sites on the substrate surface. S130. The substrate after the above treatment is placed in a reducing agent solution for reduction and activation treatment, so as to reduce the active sites implanted on the substrate surface into metal catalytic centers with catalytic activity. S140. The substrate after reduction and activation treatment is placed in a chemical copper plating solution for chemical copper plating to form a copper plating layer on the substrate surface, and the copper-plated substrate is then post-treated.

[0034] The pretreatment method of this invention includes two steps: implantation of active sites for copper plating on the surface and reduction and activation of active sites. By combining traditional activation solution-based secondary activation center implantation with strong reducing agents such as sodium borohydride for active site reduction and activation, the density and uniformity of active sites in the copper plating layer can be improved through two activation center implantations. Based on this, Pd-containing... 2+ By implanting secondary active sites of metal ions and undergoing reduction and activation treatment with a strong reducing agent, a high-density, highly active nucleation catalytic site for electroless copper plating is constructed. This establishes the theoretical and material basis for the dense and smooth growth of electroless copper plating, overcoming the technical bottlenecks of high surface roughness and high resistivity in existing electroless copper plating. Furthermore, this invention bypasses the two steps of tin-containing solution sensitization and desizing acceleration in traditional electroless copper plating, further simplifying the operation and avoiding the adverse effects on quality caused by these steps.

[0035] In one embodiment of this application, step S110, which involves pretreating the organic polymer substrate to remove surface contaminants, specifically includes: placing the organic polymer substrate in an alcohol solvent and immersing it in an ultrasonic environment at 25–60°C for 1–30 min; after completion, removing the substrate, washing it with deionized water, and drying it.

[0036] The alcohol solvent is preferably ethanol or propanol. The frequency of the ultrasonic treatment is preferably 40–100 kHz, and the power density is preferably 0.1–1.0 W / cm³. 2 The preferred drying conditions are drying at 60–80°C for 30–90 minutes.

[0037] The process conditions for the first immersion treatment are as follows: treatment temperature of 25–65℃, treatment time of 10–300 min, with stirring during the immersion process. The stirring speed is preferably 50–500 rpm. After immersion, the substrate is removed, rinsed with deionized water, and then dried at 60–80℃ for 30–90 min.

[0038] During the first immersion process, the polyacid salts in the pretreatment solution work synergistically to clean and micro-etch the substrate surface, while the transition metal coordination compound is adsorbed on the substrate surface and implanted into the first activation site.

[0039] In one embodiment of this application, in step S120, the post-activation solution is a palladium salt activation solution or a silver salt activation solution. Specifically, the palladium salt activation solution is an aqueous solution of palladium chloride in hydrochloric acid, and the silver salt activation solution is an aqueous solution of silver nitrate. The concentration of the active component in the post-activation solution is 0.05–5 g / L.

[0040] The second immersion treatment conditions were: temperature 20–50℃, time 0.1–30 min. After immersion, the substrate was removed and rinsed with deionized water for 2–5 s. The Pd in ​​the subsequent activation solution was then removed. 2+ or Ag + Ions are adsorbed on the substrate surface, enabling the implantation of a second activation site.

[0041] In one embodiment of this application, in step S130, the reducing agent solution is selected from one of sodium borohydride solution, hydrazine hydrate solution, hydroxylamine solution, and hydrazine sulfate solution. The mass concentration of the reducing agent in the solution is 0.01–10 g / L.

[0042] The reduction activation process conditions are: temperature 10–30℃, time 2–50 s. The reducing agent will implant into the active sites of metal ions (such as Cu) on the substrate surface. 2+ Pd 2+ Ag + (etc.) is reduced to a catalytically active metal elemental catalytic center (Cu) 0 Pd 0 Ag 0 wait).

[0043] In one embodiment of this application, in step S140, the temperature for the electroless copper plating is 30–50°C, and the plating time is 10–120 min. The electroless copper plating solution can be a conventional electroless copper plating solution in the art, such as an alkaline aqueous solution containing copper salts (e.g., copper sulfate), complexing agents (e.g., EDTA·2Na or potassium sodium tartrate), reducing agents (e.g., formaldehyde), and pH adjusting agents (e.g., sodium hydroxide).

[0044] The technical solutions of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0045] Example 1 A pretreatment solution and method for chemical copper plating on an organic polymer substrate, comprising the following steps: (1) Preparation of pretreatment solution: First, 5.000 g of potassium silicate hydrate was added to 100 ml of deionized water and stirred at 30 °C until completely dissolved to obtain a clear solution. Then, 0.100 g of sodium phosphate and 0.040 g of sodium molybdate were added to the obtained solution and stirred at 30 °C until completely dissolved. Finally, 1.000 g of copper citrate (II) was added and stirred at 30 °C for 30 min until homogeneous. The mixture was then cooled to obtain the pretreatment solution.

[0046] In this embodiment, the concentrations of each component in the pretreatment solution are as follows: copper citrate (II) approximately 10 g / L, sodium molybdate approximately 0.4 g / L, potassium silicate hydrate approximately 50 g / L, and sodium phosphate approximately 1 g / L. The pH value of the pretreatment solution is approximately 11.

[0047] (2) Substrate pretreatment: Place a 1×2 cm polyimide (PI) substrate into a beaker containing anhydrous ethanol, ensuring the PI substrate is completely submerged in the ethanol. Place the beaker in an ultrasonic cleaner at an ultrasonic frequency of 60 kHz and a power density of approximately 0.5 W / cm². 2 The PI substrate was ultrasonically cleaned for 5 minutes at a temperature of 25°C. After cleaning, the substrate was removed, rinsed with deionized water, and then dried in a 75°C oven for 60 minutes.

[0048] (3) First immersion treatment (first active site implantation): The dried PI substrate is placed in a pretreatment solution at 50°C to completely immerse the substrate. The substrate is treated for 60 min with stirring (stirring speed of about 200 rpm). The PI substrate is then removed from the pretreatment solution, rinsed with deionized water for 2 s, and dried in an oven at 75°C for 60 min.

[0049] (4) Second immersion treatment (secondary active site implantation): Take out the dried PI substrate and put it into 0.5 g / L palladium chloride activation solution (hydrochloric acid aqueous solution of palladium chloride) and treat it at 25°C for 20 min; take out the PI substrate from the activation solution and wash it in deionized water for 2 s.

[0050] (5) Reduction and activation treatment: The PI substrate is placed in a 0.5 g / L sodium borohydride solution and treated at 20°C for 5 s; the PI substrate is then removed and cleaned with deionized water.

[0051] (6) Chemical copper plating: The PI substrate is placed in the chemical copper plating solution and copper is plated at 35°C for 30 min; the plated part is taken out and cleaned to obtain PI material with a dense chemical copper plating layer.

[0052] The chemical copper plating solution used in this embodiment has the following formula: 6 g / L copper sulfate, 30 g / L EDTA·2Na, 5 mL / L formaldehyde (37%), and sodium hydroxide to adjust the pH to 12.5.

[0053] (7) Performance testing: The surface roughness parameters of the electroless copper plating layer prepared in this embodiment were obtained by 3D confocal microscopy testing: Sa = 0.060 μm, Sz = 1.016 μm. The adhesion between the copper layer and the substrate was tested by cross-cut test according to ASTM D3359 standard, and the rating reached 5B (the highest level), indicating that the copper layer and the PI substrate have excellent interfacial bonding strength.

[0054] Figure 2 This is a 500x SEM image of the electroless copper plating layer prepared on the PI substrate in this embodiment. As can be seen from the image, the surface of the copper plating layer is uniform and dense, without obvious cracks or pore defects. Figure 3 This is a 3D confocal microscope image of the surface morphology of the electroless copper plating layer prepared on the PI substrate in this embodiment. As can be seen from the image, the plating surface is smooth and has low roughness.

[0055] Example 2 A pretreatment solution and method for electroless copper plating on organic polymer substrates, comprising the following steps: (1) Preparation of pretreatment solution: First, 1.000 g of potassium silicate hydrate was added to 100 ml of deionized water and stirred at 30°C until completely dissolved to obtain a clear solution. 4.000 g of sodium phosphate and 1.900 g of sodium molybdate were added to the obtained solution and stirred at 30°C until completely dissolved. Finally, 8.000 g of copper citrate (II) and 0.100 g of silane coupling agent (KH-550, γ-aminopropyltriethoxysilane) were added and stirred at 30°C for 30 min until homogeneous. The mixture was then cooled to obtain the pretreatment solution.

[0056] In this embodiment, the concentrations of each component in the pretreatment solution are as follows: copper citrate (II) approximately 80 g / L, sodium molybdate approximately 19 g / L, potassium silicate hydrate approximately 10 g / L, sodium phosphate approximately 40 g / L, and silane coupling agent approximately 1 g / L. The pH of the pretreatment solution is approximately 10.5.

[0057] (2) Substrate pretreatment: Place a 1×2 cm PI substrate into a beaker containing anhydrous ethanol, ensuring the PI substrate is completely submerged in the ethanol. Place the beaker in an ultrasonic cleaner and perform ultrasonic cleaning for 10 min at an ultrasonic frequency of 60 kHz and a cleaning temperature of 25℃. After cleaning, remove the PI substrate, rinse it with deionized water, and then dry it in a 70℃ oven for 60 min.

[0058] (3) First immersion treatment (first active site implantation): Place the dried PI substrate into a pretreatment solution at 50°C to completely immerse the substrate; treat for 30 min with stirring (stirring speed about 200 rpm). Remove the PI substrate from the pretreatment solution, rinse with deionized water for 2 s, and dry in an oven at 70°C for 60 min.

[0059] (4) Second immersion treatment (secondary active site implantation): Take out the dried PI substrate and place it in 0.25 g / L palladium chloride activation solution and treat it at 25°C for 25 min. Take out the PI substrate from the activation solution and wash it in deionized water for 2 s.

[0060] (5) Reduction and activation treatment: The PI substrate was placed in a 1.0 g / L sodium borohydride solution and treated at 20°C for 8 s. The PI substrate was then removed and cleaned with deionized water.

[0061] (6) Chemical copper plating: The PI substrate is placed in the chemical copper plating solution and copper is plated at 35°C for 30 min; the plated part is taken out and cleaned to obtain PI material with a dense chemical copper plating layer.

[0062] The chemical copper plating solution used in this embodiment has the same formulation as in Example 1.

[0063] (7) Performance testing: The surface roughness parameters of the electroless copper plating layer prepared in this embodiment, obtained by 3D confocal microscopy, are: Sa = 0.100 μm, Sz = 2.753 μm. The adhesion between the copper layer and the substrate was tested by cross-cut test according to ASTM D3359 standard, and the rating reached 5B.

[0064] Example 3 A pretreatment solution and method for electroless copper plating on organic polymer substrates, comprising the following steps: (1) Preparation of pretreatment solution: First, 36.000 g of potassium silicate hydrate was placed in 100 ml of deionized water and stirred at 30°C until completely dissolved to obtain a clear solution. 2.000 g of sodium phosphate and 0.970 g of sodium molybdate were added to the obtained solution and stirred at 30°C until completely dissolved. Finally, 0.070 g of copper citrate (II) and 0.050 g of silane coupling agent (KH-550) were added and stirred at 30°C for 30 min until homogeneous. The mixture was then cooled to obtain the pretreatment solution.

[0065] The concentrations of each component in the pretreatment solution in this embodiment are as follows: copper citrate (II) approximately 0.7 g / L, sodium molybdate approximately 9.7 g / L, potassium silicate hydrate approximately 360 g / L, sodium phosphate approximately 20 g / L, and silane coupling agent approximately 0.5 g / L. The pH value of the pretreatment solution is approximately 12.

[0066] (2) Substrate pretreatment: Place a 1×2 cm PI substrate into a beaker containing anhydrous ethanol, ensuring the PI substrate is completely submerged in the ethanol. Place the beaker in an ultrasonic cleaner and perform ultrasonic cleaning for 10 min at an ultrasonic frequency of 60 kHz and a cleaning temperature of 25℃. After cleaning, remove the PI substrate, rinse it with deionized water, and then dry it in a 75℃ oven for 60 min.

[0067] (3) First immersion treatment (first active site implantation): The dried PI substrate is placed in a pretreatment solution at 50°C to completely immerse the substrate; it is treated for 30 min with stirring (stirring speed of about 200 rpm). The PI substrate is removed from the pretreatment solution, rinsed with deionized water for 2 s, and dried in an oven at 75°C for 60 min.

[0068] (4) Second immersion treatment (secondary active site implantation): Take out the dried PI substrate and place it in 0.50 g / L palladium chloride activation solution and treat it at 25°C for 20 min. Take out the PI substrate from the activation solution and wash it in deionized water for 4 s.

[0069] (5) Reduction and activation treatment: The PI substrate is placed in a 1.0 g / L sodium borohydride solution and treated at 20°C for 30 s; the PI substrate is then removed and cleaned with deionized water.

[0070] (6) Chemical copper plating: The PI substrate is placed in the chemical copper plating solution and copper is plated at 35°C for 30 min; the plated part is taken out and cleaned to obtain PI material with a dense chemical copper plating layer.

[0071] The chemical copper plating solution used in this embodiment has the same formulation as in Example 1.

[0072] (7) Performance testing: The surface roughness parameters of the electroless copper plating layer prepared in this embodiment, obtained by 3D confocal microscopy, are: Sa = 0.192 μm, Sz = 5.232 μm. The adhesion between the copper layer and the substrate was tested by cross-cut test according to ASTM D3359 standard, and the rating reached 5B.

[0073] The above embodiments demonstrate that the process of the present invention can stably and efficiently achieve chemical copper plating on organic polymer substrates, and the prepared copper plating layer has advantages such as good density and excellent interlayer adhesion. The present invention is applicable to the pretreatment of chemical copper plating on various organic polymer substrates such as polyimide (PI), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), liquid crystal polymer (LCP), and polytetrafluoroethylene (PTFE), and can be widely used in printed circuit boards, flexible electronic devices, chip packaging, sensors, and other fields.

[0074] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the invention by those skilled in the art. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the invention should be included within the scope of protection of the invention.

Claims

1. A pretreatment solution for electroless copper plating on an organic polymer substrate, characterized in that, The pretreatment solution is an alkaline aqueous solution system, comprising the following components: Transition metal coordination compounds or transition metal complexes, with a concentration of 0.01–100 g / L; Molybdate, with a concentration of 0.02–20 g / L; Silicates, with a concentration of 0.05–500 g / L; Phosphate, with a concentration of 0.05–50 g / L; And organic additives, at a concentration of 0–1.0 g / L; The pretreatment solution is used to simultaneously clean, micro-etch and roughen the surface of the organic polymer substrate, and perform the first implantation of active sites for chemical copper plating.

2. The pretreatment solution for electroless copper plating on organic polymer substrates according to claim 1, characterized in that, The transition metal coordination compound or transition metal complex is selected from one or more of the following: copper(II) tetraammine sulfate, copper(II) citrate, disodium ethylenediaminetetraacetate copper(II) ester, copper(II) tartrate complex, disodium ethylenediaminetetraacetate nickel(II) ester, and disodium ethylenediaminetetraacetate palladium(II) ester.

3. The pretreatment solution for electroless copper plating of organic polymer substrates according to claim 1, characterized in that, The molybdate is selected from one or more of potassium molybdate, sodium molybdate, ammonium molybdate, and magnesium molybdate; The silicate is selected from one or more of sodium silicate, aluminum silicate, and potassium silicate; The phosphate is selected from one or more of trisodium phosphate, tripotassium phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, sodium pyrophosphate, potassium pyrophosphate, and sodium tripolyphosphate.

4. The pretreatment solution for electroless copper plating on organic polymer substrates according to claim 1, characterized in that, The organic additive is selected from one or more of the following: silane coupling agent, potassium sulfonylbenzenesulfonate, sodium stearate, potassium myristate, potassium laurate, and alkenyl sulfonate.

5. A pretreatment method for electroless copper plating on an organic polymer substrate, characterized in that, Includes the following steps: After pretreatment to remove surface contaminants from the organic polymer substrate, it is placed in the pretreatment solution as described in any one of claims 1-4 for a first immersion treatment to achieve cleaning, micro-etching roughening, and the first implantation of active sites for chemical copper plating on the substrate surface. The substrate treated as described above is placed in a post-activation solution for a second immersion treatment, thereby achieving a second implantation of chemically plated copper active sites on the substrate surface. The substrate treated as described above is placed in a reducing agent solution for reduction and activation treatment, which reduces the active sites implanted on the substrate surface into catalytically active metal catalytic centers. The substrate, after reduction and activation treatment, is placed in a chemical copper plating solution for chemical copper plating to form a copper plating layer on the substrate surface, and then the copper-plated substrate is post-treated.

6. The pretreatment method for electroless copper plating on an organic polymer substrate according to claim 5, characterized in that, The step of pretreating the organic polymer substrate to remove surface contaminants includes: The organic polymer substrate is placed in an alcohol solvent and immersed in an ultrasonic environment at 25–60°C for 1–30 minutes. After completion, the substrate is removed, cleaned with deionized water, and dried.

7. The pretreatment method for electroless copper plating on an organic polymer substrate according to claim 5, characterized in that, The process conditions for the first soaking treatment are: a treatment temperature of 25-65℃, a treatment time of 10-300 min, and stirring during the soaking process; After soaking, remove the substrate, clean it with deionized water, and then dry it.

8. The pretreatment method for electroless copper plating on an organic polymer substrate according to claim 5, characterized in that, The post-activation solution is a palladium salt activation solution or a silver salt activation solution, and the concentration of the active component in the post-activation solution is 0.05–5 g / L; The process conditions for the second soaking treatment are: temperature 20-50℃, time 0.1-30 min; After soaking, remove the substrate and rinse it with deionized water for 2-5 seconds.

9. The pretreatment method for electroless copper plating on an organic polymer substrate according to claim 5, characterized in that, The reducing agent solution is selected from one of sodium borohydride solution, hydrazine hydrate solution, hydroxylamine solution, and hydrazine sulfate solution; wherein the mass concentration of the reducing agent in the solution is 0.01–10 g / L; The process conditions for the reduction and activation treatment are: temperature of 10-30℃ and time of 2-50 s.

10. The pretreatment method for electroless copper plating on an organic polymer substrate according to claim 5, characterized in that, The temperature for the electroless copper plating is 30–50°C, and the plating time is 10–120 min.

Citation Information

Patent Citations

  • A kind of method of ionic liquid electroless copper plating

    CN105063582B

  • A pretreatment process and equipment for chemical copper plating on double-sided printed circuit boards