A polyacrylonitrile-based carbon fiber precursor, carbon fiber, and method for producing the same

By employing a multi-temperature zone washing process to adjust the pH of the washing water to 6.0–6.9 during the preparation of polyacrylonitrile-based carbon fibers, metal complexes were removed, solving the problems of excessive fuzz and poor drawability, and improving the quality of the carbon fibers.

CN123063876APending Publication Date: 2026-11-10CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202510597107.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the existing technology, the presence of metal-carboxyl complexes leads to problems such as excessive fuzz and poor drawability in polyacrylonitrile-based carbon fiber precursors during the spinning process.

Method used

The process employs wet spinning or dry-jet wet spinning, adjusting the pH of the washing water to 6.0–6.9, and performing multi-temperature zone washing to remove metal complexes. Specifically, this includes 5–12 temperature zones, a temperature range of 30–85°C, and the pH of the washing water is adjusted by adding citric acid, dilute hydrochloric acid, and acetic acid. The water-to-wash volume ratio is 5:1–30:1, and the washing time is 0.5–5 minutes, combined with water circulation or ultrasonic treatment.

Benefits of technology

It significantly reduces the number of filaments in the precursor fiber, improves the drawability, reduces the solvent residue to ≤0.03wt%, and enhances the physical properties of carbon fiber.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application provides a polyacrylonitrile-based carbon fiber precursor, a carbon fiber and a preparation method thereof, and mainly solves the problems of many broken filaments and poor drawability in the prior art. The preparation steps of the polyacrylonitrile-based carbon fiber precursor include the following steps: preparation of a stock solution, extrusion and coagulation molding of the stock solution, hot water drawing, washing, oiling, drying and densification, steam drawing and heat setting; in the washing stage, the pH value of the washing water is 6.0-6.9, and the technical scheme preferably solves the problems in the prior art, and can be used in industrial production in the field of polyacrylonitrile-based precursors and carbon fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of carbon fiber technology, specifically relating to a polyacrylonitrile-based carbon fiber precursor, carbon fiber, and its preparation method. Background Technology

[0002] Carbon fiber possesses excellent properties such as lightweight, high strength, high modulus, high temperature resistance, and corrosion resistance, making it a key material in aerospace, automotive, and wind energy industries. In these fields, carbon fiber is commonly used to manufacture structural components, composite material reinforcements, and sensors, becoming an indispensable strategic material. Furthermore, carbon fiber is widely used in building reinforcement, sporting goods, and medical devices. With technological advancements and the continuous expansion of the carbon fiber market demand, the carbon fiber industry is currently expanding from traditional high-end technology applications to mass-market applications, and the market is expected to continue growing in the coming years.

[0003] Polyacrylonitrile (PAC) is an important precursor material for carbon fiber, and the choice of polymerization method and solvent system has a significant impact on the properties of the precursor fiber and carbon fiber. Currently, common solvent systems include sodium thiocyanate (NaSCN), dimethyl sulfoxide (DMSO), and dimethylacetamide (DMAc). Common polymerization methods include one-step and two-step methods. The one-step method uses homogeneous solution polymerization, while the two-step method uses heterogeneous solution polymerization, where the polymer is first obtained, and then further processed after separation and dissolution.

[0004] In the NaSCN system, the Na in the solvent dissociation products + The ions can form metal complexes through coordination with a small amount of carboxyl groups introduced by the second or third comonomer (such as the commonly used itaconic acid). This is because Na... + The ions are relatively reactive metal cations, while the carboxyl group is a functional group containing an oxygen atom with a lone pair of electrons. The DMSO system cannot completely avoid the formation of metal complexes. The containers and pipes of the entire polymerization system are made of stainless steel, which, under the long-term corrosive action of DMSO, may release free Fe. 2+ or Fe 3+ Through similar coordination interactions, metal-carboxyl coordination complexes may also be formed. These complexes are highly compatible with solvents and, after stirring, disperse throughout the spinning solution. Because there are no large particles, obvious precipitation, or color changes in the solution, they are almost imperceptible to the naked eye.

[0005] The main methods for preparing carbon fiber precursor from polyacrylonitrile (PAN) dosage are wet spinning and dry-jet wet spinning. In wet spinning, the PAN raw material is dissolved in a solvent, and the solution is spun into fibers through a spinneret and then cured in a water bath. This method is mature, the spinning process is stable, and the resulting fiber surface groove structure provides excellent reinforcement in composite materials. Dry-jet wet spinning, on the other hand, first evaporates the solvent through an air layer before curing in a coagulation bath. Compared to wet spinning, dry-jet wet spinning produces a smoother, denser fiber surface with superior mechanical properties, making it suitable for preparing high-strength, low-defect carbon fiber products. Both processes include steps such as dosage extrusion coagulation, hot water drawing, washing, oiling, drying densification, steam drawing, and heat setting.

[0006] The resulting metal-carboxyl complexes mainly cause two problems in the spinning process. First, during the drafting stage of spinning, the complexes restrict the free movement of polymer chains, leading to chain confinement and reduced chain segment freedom, thus decreasing drafting performance. At high draft ratios, especially in high-speed, high-draft-ratio dry-jet wet spinning technologies, fuzzing is likely to occur. Second, after the dopant solution is ammoniated, some NH4+ is released... + Ions may remain on the molecular chains. If not effectively removed during the washing stage, these NH4+ ions... + The ions will volatilize into ammonia gas during the drying process, causing pores or other defects on the surface of the precursor fiber, ultimately affecting the physical properties of the precursor fiber and carbon fiber. Furthermore, these NH4 ions... + Ions may form metal-carboxyl complexes with carboxyl groups, and due to the weak coordination, the release of a small amount of ammonia gas during the decomposition of the complexes during drying may also cause defects in the precursor fiber.

[0007] Currently, existing technologies all use deionized water to wash the filament bundles, such as patents CN118007284A, CN117802592A, and CN101724922A. However, deionized water is neutral and cannot effectively remove complexes, thus failing to eliminate the negative impact of complexes on drawability. Furthermore, research related to pH control in the spinning process mainly focuses on adjusting the pH of the coagulation bath, such as patents CN116427059A, CN109137117A, and CN103290527A. The main purpose of these studies is to optimize the uniformity of coagulation diffusion, resulting in dense and transparent filaments after the bath.

[0008] To address the limitation on the maximum draw ratio of polyacrylonitrile precursor fibers, patent CN106939439A describes poor draw performance of fibers formed under highly alkaline conditions. Therefore, by controlling the pH of the coagulation bath to a weakly acidic condition, the double diffusion during the coagulation process is slowed down, thereby achieving homogenization of fiber formation and improving the drawability of the precursor fibers. Patent CN117535815A employs a ternary copolymerization scheme of acrylonitrile, an acidic second monomer, and a neutral third monomer. While this allows for a higher total draw ratio, the high monomer mass percentage (2.5%) leads to a decrease in carbon yield. Patent CN115707801A designs a drying and densification unit using heat-conducting oil as the circulating medium. By performing a drying and densification process under a certain tension, the precursor fiber pores are closed, resulting in a dense fiber network structure, which is beneficial for further high-ratio drawing. Summary of the Invention

[0009] This invention mainly addresses the problem in the prior art where the presence of a small amount of metal-carboxyl complexes leads to excessive fuzz and poor drawability of the precursor fiber. It provides a method for preparing carbon fiber precursor and carbon fiber, which has the advantages of reducing the number of fuzz and improving the drawability of the precursor fiber.

[0010] One of the objectives of this invention is to provide a method for preparing polyacrylonitrile-based carbon fiber precursor, which employs a wet spinning process or a dry-jet wet spinning process, including a water washing step, wherein the pH of the washing water is 6.0 to 6.9.

[0011] According to an embodiment of the present invention, in the water washing step:

[0012] The water washing process employs at least 5 water washing temperature zones, preferably 5 to 12 water washing temperature zones; for example, the water washing temperature zones can be 5, 6, 7, 8, 9, 10, 11 or 12 temperature zones.

[0013] The washing operation temperature is 30-85℃, for example, any temperature among 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, and 85℃, or any two of the above temperature ranges; according to a preferred embodiment of the present invention, the temperature of the washing temperature zone increases along the fiber running direction; according to a preferred embodiment of the present invention, in the washing process, the temperature value of each washing temperature zone and the pH value of the washing water satisfy the following relationship: A = 0.0174B + 5.5076, where A is the pH value of the washing water and B is the temperature value, with the temperature unit being ℃;

[0014] The pH of the wash water can be adjusted using commonly used acidic compounds. For example, the pH of the wash water can be adjusted by adding organic and / or inorganic acids, preferably by adding at least one of citric acid, dilute hydrochloric acid, and acetic acid. The pH of the wash water is adjusted to 6.0–6.9, for example, any value among 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, and 6.9, or any value within the range of the above values. When the pH of the wash water is lower than 6.0, it will cause the molecular structure of the emulsifier to be damaged in the subsequent oiling process, thereby weakening the binding force between the emulsifier and the oil phase, ultimately leading to oil phase stratification or coagulation, causing oil demulsification.

[0015] The amount of washing water used in the washing process can be adjusted within a wide range. Specifically, the ratio of the weight of the washing water to the weight of the running yarn bundle is (5-30):1, for example, it can be any ratio among 5:1, 8:1, 10:1, 15:1, 20:1, 25:1, 30:1 or any ratio between any two of the above ratios; preferably, the ratio of the weight of the washing water to the weight of the running yarn bundle is (8-20):1.

[0016] The washing time can be selected from commonly used washing times. Specifically, the total washing time is 0.5 to 5 minutes, for example, it can be any time from 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 minutes or any time between any two of the above values.

[0017] The washing method is not particularly limited, and a commonly used washing method in the prior art can be selected. For example, the washing method can be at least one of water circulation, ultrasonic, and compressed air.

[0018] The residual solvent content in the washed filament bundle is ≤0.03wt%.

[0019] According to an embodiment of the present invention, the preparation method of the polyacrylonitrile-based carbon fiber precursor specifically includes: extruding polyacrylonitrile stock solution, solidifying and molding, hot water stretching, washing with water, oiling, drying and densifying, steam stretching, and steam heat setting to obtain the polyacrylonitrile-based carbon fiber precursor.

[0020] Among them, the dope extrusion, coagulation molding, hot water drawing, oiling, drying densification, steam drawing, and steam heat setting in wet spinning and dry-jet wet spinning processes can all adopt the commonly used process equipment and process conditions in existing technologies. Specifically, the wet spinning process can employ the following conditions: coagulation conditions: at least two coagulation baths, coagulation bath temperature range 20–80℃, total draw ratio 0.8–1.5; hot water drawing conditions: temperature 90–99℃, hot water drawing total draw ratio 3–6; washing conditions: three washings at 50–70℃, washing total draw ratio 0.8–1.2; oiling conditions: residence time 3–6s, no drawing; drying and densification conditions: temperature range 120–160℃, using four temperature zones, with gradual temperature increase; steam drawing conditions: pressure 0.2–0.8MPa, draw ratio 2–6 times; steam heat setting: pressure 0.05–0.50MPa, draw ratio 0.5–1.2; finally, the yarn is wound up to obtain polyacrylonitrile-based carbon fiber precursor. The following operating conditions can be used in the dry-jet wet spinning process: After the dope is extruded, it passes through an air section of 1-15 mm and enters the coagulation bath at a temperature of 0-15 degrees Celsius with a concentration of 20-50%; hot water drawing conditions: temperature 90-99℃, total hot water drawing ratio 3-6; washing conditions: three washes at 50-70℃, total washing drawing ratio 0.8-1.2; oiling conditions: residence time 3-6 seconds, no drawing; drying and densification using a two-stage gradient temperature increase, 110-150℃; steam drawing conditions: pressure 0.2-0.8 MPa, drawing ratio 2-6 times; steam heat setting: pressure 0.05-0.50 MPa, drawing ratio 0.5-1.2; finally, the yarn is wound up to obtain polyacrylonitrile-based carbon fiber precursor.

[0021] According to an embodiment of the present invention, the polyacrylonitrile stock solution is obtained by polymerizing a monomer containing acrylonitrile and then sequentially undergoing monomer removal, degassing, amination treatment, and filtration.

[0022] According to a specific embodiment of the present invention, the polymeric monomer may further include comonomers commonly used in the prior art. Specifically, the polymeric monomer further includes at least one comonomer. Preferably, the comonomer is selected from at least one of itaconic acid, acrylic acid, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, vinyl acetate, isobutyl acrylate, butyl itaconic acid, mesoaconic acid, 2-butenoic acid, maleic acid, methylmaleic acid, acrylamide, acrylamide oxime, hydroxyethyl acrylonitrile, α-chloroacrylonitrile, and diacetone acrylamide.

[0023] The polymerization is carried out in an organic solvent and / or an inorganic solvent, which can be solvents commonly used in existing polyacrylonitrile preparation processes. Preferably, the organic solvent is selected from at least one of dimethyl sulfoxide, dimethylformamide, dimethylacetamide, and ethylene carbonate; the inorganic solvent is selected from at least one of zinc chloride aqueous solution, nitric acid aqueous solution, sodium thiocyanate aqueous solution, and sodium bisulfate aqueous solution; the amount of solvent used is 70-85 wt% of the total weight of the polymerization reaction system.

[0024] The polymerization is carried out under the action of an initiator, which can be an initiator commonly used in the existing polyacrylonitrile preparation process. Preferably, the initiator is selected from at least one of azo compounds, and more preferably at least one of azobisisobutyronitrile and azobisisoheptanenitrile.

[0025] The polymer monomer contains acrylonitrile at a mass percentage of not less than 95 wt%, preferably 95-99 wt%.

[0026] The polymerization reaction can be carried out under common polymerization conditions, for example, the temperature of the polymerization reaction is 30-70°C; the time of the polymerization reaction is 10-40 hours; the polymerization reaction is carried out under protective gas conditions, and the protective gas can be commonly used nitrogen, etc.

[0027] The number-average molecular weight of the polyacrylonitrile copolymer obtained by the polymerization reaction is 50,000 to 120,000.

[0028] The ammoniation treatment can be carried out using common ammoniation treatment processes, such as using at least one of ammonia gas, ammonia water, and ammonium carbonate; the ammoniation treatment yields a stock solution with a pH of 7.0 to 10.5.

[0029] The second objective of this invention is to provide a polyacrylonitrile-based carbon fiber precursor obtained by the above preparation method.

[0030] The third objective of this invention is to provide a carbon fiber prepared from polyacrylonitrile-based carbon fiber precursor, wherein the polyacrylonitrile-based carbon fiber precursor is the aforementioned polyacrylonitrile-based carbon fiber precursor.

[0031] The fourth objective of this invention is to provide a method for preparing the above-mentioned carbon fiber, comprising: obtaining polyacrylonitrile-based carbon fiber precursor by means of the preparation method described in one objective of this invention, and subjecting the polyacrylonitrile-based carbon fiber precursor to pre-oxidation treatment and carbonization treatment in sequence to obtain the carbon fiber.

[0032] According to embodiments of the present invention, the pre-oxidation treatment and carbonization treatment in the carbon fiber preparation method can both adopt the process conditions used in the prior art. For example, the conditions for the pre-oxidation treatment are: pre-oxidation temperature of 180-300℃ and treatment time of 10-60 min; the carbonization treatment includes low-temperature carbonization and high-temperature carbonization. Preferably, the carbonization treatment is carried out under protective gas conditions, and the protective gas can be commonly used nitrogen, etc.; the conditions for the low-temperature carbonization are: temperature of 350-700℃ and treatment time of 2-4 min; the conditions for the high-temperature carbonization are: temperature of 1300-1400℃ and treatment time of 2-4 min.

[0033] This invention effectively removes metal complexes by adjusting the pH value of the washing water. After a weakly acidic washing treatment, the stability of the complexes formed by metal ions and carboxylic acid groups decreases. In an environment with a pH of 6.0–6.9, the coordination bond strength is weakened, promoting the dissociation of metal complexes into soluble free ions. By reducing the residual metal impurities on the surface of the precursor fiber, the generation and propagation of cracks caused by localized stress concentration of impurities on the fiber surface during high-temperature processes (such as drying densification and steam drawing) can be reduced, thereby significantly reducing the fuzz production rate. In addition, it also effectively avoids the void defects in the precursor fiber caused by the volatilization of these unstable metal complexes during high-temperature processes. These void defects would remain in the carbon fiber stage, deteriorating the performance of the final carbon fiber. Detailed Implementation

[0034] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.

[0035] The testing instruments and conditions used in this embodiment are as follows:

[0036] In the embodiments, the tensile strength and tensile modulus of carbon fibers were tested according to the test methods of GB / T3362-2005.

[0037] The determination of solvent residue in chemical fibers shall be performed in accordance with the test method of GB / T41671-2022.

[0038] Unless otherwise specified, the raw materials used in the examples and comparative examples are all disclosed in the prior art, such as those that can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0039] Example 1

[0040] Preparation of polyacrylonitrile copolymers:

[0041] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethyl sulfoxide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 2.8. After monomer removal, the copolymer was ammonified with ammonia to obtain a highly hydrophilic solution with a pH of 9.5. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0042] Preparation of polyacrylonitrile carbon fiber:

[0043] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. The process first involved solution extrusion and coagulation (coagulation bath temperatures of 55℃, 60℃, and 70℃; DMSO concentrations of 90%, 60%, and 30%; total draw ratio of 1.1) and hot water drawing (temperatures of 96℃, 97℃, and 98℃; total draw ratio of 3). During the washing stage, the fiber passed through 10 temperature zones along the fiber's direction of travel. The washing temperatures were 45℃, 50℃, 53℃, 57℃, 61℃, 63℃, 69℃, 71℃, 73℃, and 75℃, respectively. The pH values ​​of the washing water were 6.3, 6.4, 6.4, 6.5, 6.6, 6.6, 6.7, 6.7, 6.8, and 6.8 (the pH of the washing water was adjusted using citric acid). The total draw ratio for the washing process was 1.17. The washing process combines water circulation and ultrasonic methods. The counter-current water circulation rate in each tank is 50 L / h, the ultrasonic power is 300 W, the oscillation frequency is 40 kHz, and the wave count is 12 per meter. The ratio of water weight to the weight of the running filament is 17.5, and the total washing time is 4 minutes. After washing, the solvent residue in the filament is less than 0.01%. After washing, the filament undergoes oiling (6-second dwell time, no stretching), drying and densification (using a four-zone stepped heating method at 120℃, 125℃, 130℃, and 135℃), steam stretching (pressure 0.3 MPa, steam stretching ratio 2.5), and steam heat setting (steam pressure 0.38 MPa, steam heat setting stretching ratio 0.75) before winding to obtain polyacrylonitrile precursor fibers.

[0044] The polyacrylonitrile precursor fiber further undergoes a pre-oxidation process; the pre-oxidation temperature zones are 185℃, 222℃, 234℃, 252℃, and 273℃, with a total processing time of 30 minutes. Subsequently, low-temperature carbonization and high-temperature carbonization are carried out in a nitrogen atmosphere to obtain carbon fibers; the low-temperature carbonization temperature is 600℃, and the high-temperature carbonization temperature is 1300℃, with each taking 4 minutes.

[0045] The total weight of fuzz collected at the drying and densification and steam stretching stages within one hour is defined as the "fuzz weight." A fuzz weight of less than 20 mg is considered acceptable. At a total stretching ratio of 5.5, the fuzz weight was measured to be 5 mg. The final carbon fiber tensile strength was 5.7 GPa, and the carbon fiber tensile modulus was 292 GPa.

[0046] Example 2

[0047] Preparation of polyacrylonitrile copolymers:

[0048] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethyl sulfoxide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 2.8. After monomer removal, the copolymer was aminated with ammonia to obtain a highly hydrophilic solution with a pH of 8.8. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0049] Preparation of polyacrylonitrile carbon fiber:

[0050] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 1. The process first involved solution extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through eight temperature zones along the fiber's direction of travel. The temperatures of these zones were 55°C, 60°C, 65°C, 69°C, 71°C, 72°C, 74°C, and 76°C, with pH values ​​of 6.5, 6.6, 6.6, 6.7, 6.7, 6.8, 6.8, and 6.8 (the pH of the washing water was adjusted using citric acid). The washing process was a circulating water system, with a counter-current circulation rate of 60 L / h in each tank. The ratio of the weight of the washing water to the weight of the fiber bundle was 12. The total washing time was 3 minutes, and the solvent residue in the fiber bundle after washing was 0.02%. After washing, the polyacrylonitrile precursor fiber is obtained by oiling, drying and densification, steam drawing, heat setting and winding.

[0051] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0052] At a total draw ratio of 5.5, the filament weight was measured to be 11 mg. The final carbon fiber tensile strength was 5.3 GPa, and the carbon fiber tensile modulus was 279 GPa.

[0053] Example 3

[0054] Preparation of polyacrylonitrile copolymers:

[0055] Acrylonitrile, itaconic acid, and methyl acrylate were mixed in a mass ratio of 98:1:1, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethyl sulfoxide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 87,000, and the molecular weight distribution was approximately 3.0. After monomer removal, the copolymer was ammonified with ammonium carbonate to obtain a highly hydrophilic solution with a pH of 8.1. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0056] Preparation of polyacrylonitrile carbon fiber:

[0057] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 1. The process first involved solution extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through 10 temperature zones along the fiber's direction of travel. The temperatures of these zones were 45℃, 50℃, 53℃, 57℃, 61℃, 63℃, 69℃, 71℃, 73℃, and 75℃, respectively. The pH values ​​of the washing water were 6.3, 6.4, 6.4, 6.5, 6.6, 6.6, 6.7, 6.7, 6.8, and 6.8, respectively (the pH of the washing water was adjusted using citric acid). The washing process was a water circulation system, with a counter-current circulation rate of 60 L / h in each tank. The ratio of the weight of the water used for washing to the weight of the fiber bundle was 11. The total washing time was 3 minutes, and the solvent residue in the fiber bundle after washing was 0.02%. After washing, the polyacrylonitrile precursor fiber is obtained by oiling, drying and densification, steam drawing, heat setting and winding.

[0058] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0059] At a total draw ratio of 5.5, the filament weight was measured to be 12 mg. The final carbon fiber tensile strength was 5.3 GPa, and the carbon fiber tensile modulus was 284 GPa.

[0060] Example 4

[0061] Preparation of polyacrylonitrile copolymers:

[0062] Acrylonitrile, itaconic acid, and acrylic acid were added to a reactor at a mass ratio of 98:1.2:0.8, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). The reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 100,000, and the molecular weight distribution was approximately 2.7. After monomer removal, the copolymer was ammonified with ammonia to obtain a highly hydrophilic solution with a pH of 8.6. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0063] Preparation of polyacrylonitrile carbon fiber:

[0064] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 1. The process first involved solution extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through seven temperature zones along the fiber's direction of travel. The temperatures of these zones were 57°C, 59°C, 61°C, 62°C, 65°C, 73°C, and 76°C, with pH values ​​of 6.5, 6.5, 6.6, 6.6, 6.6, 6.8, and 6.8, respectively (the pH of the washing water was adjusted using citric acid). The washing process was a circulating water system, with a counter-current circulation rate of 70 L / h in each tank. The ratio of the weight of the washing water to the weight of the fiber bundle was 15. The total washing time was one minute, and the solvent residue in the fiber bundle after washing was 0.03%. After washing, the polyacrylonitrile precursor fiber is obtained by oiling, drying and densification, steam drawing, heat setting and winding.

[0065] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0066] At a total draw ratio of 5.5, the filament weight was measured to be 15 mg. The final carbon fiber tensile strength was 5.2 GPa, and the carbon fiber tensile modulus was 269 GPa.

[0067] Example 5

[0068] Preparation of polyacrylonitrile copolymers:

[0069] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethylacetamide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 3.1. After monomer removal, the copolymer was aminated with ammonia to obtain a highly hydrophilic solution with a pH of 8.3. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0070] Preparation of polyacrylonitrile carbon fiber:

[0071] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 1. The process first involved solution extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through eight temperature zones along the fiber's direction of travel. The temperatures of these zones were 55℃, 60℃, 65℃, 69℃, 71℃, 72℃, 74℃, and 76℃, and the pH values ​​were 6.5, 6.6, 6.6, 6.7, 6.7, 6.8, 6.8, and 6.8, respectively (the pH of the washing water was adjusted using citric acid). The washing process combined water circulation and ultrasonic methods. The counter-current circulation rate in each tank was 50 L / h, the ultrasonic power was 350 W, the oscillation frequency was 40 kHz, and the wave count was 10 waves / meter. The ratio of water weight to the weight of the running filament bundle in the water washing process is 8. The total water washing time is 4 minutes, and the solvent residue in the filament bundle after water washing is 0.03%. After water washing, the filament bundle is oiled, dried and densified, steam drawn, heat-set, and then wound to obtain polyacrylonitrile precursor fibers.

[0072] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0073] At a total draw ratio of 5.5, the filament weight was measured to be 13 mg. The final carbon fiber tensile strength was 5.1 GPa, and the carbon fiber tensile modulus was 263 GPa.

[0074] Example 6

[0075] Preparation of polyacrylonitrile copolymers:

[0076] Acrylonitrile, itaconic acid, and ethyl methacrylate were added to a reactor at a mass ratio of 98:1:1 (with initiator at 0.1 wt% of the total monomers), using azobisisobutyronitrile as the initiator and dimethyl sulfoxide as the solvent. The reaction was carried out under nitrogen atmosphere and at a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 85,000, and the molecular weight distribution was approximately 3.3. After monomer removal, the copolymer was ammonified with ammonia to obtain a highly hydrophilic solution with a pH of 10.0. Following degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0077] Preparation of polyacrylonitrile carbon fiber:

[0078] The polyacrylonitrile copolymer spinning solution was spun using a dry-jet wet spinning process. First, after extrusion of the solution, it passed through a 5mm air section and then entered a coagulation bath containing a 30% DMSO aqueous solution at 7℃. The draw ratio was 1.5. During the washing stage, the fiber passed through 12 temperature zones along the fiber's direction of travel. The temperatures of these zones were 40℃, 43℃, 46℃, 49℃, 52℃, 55℃, 58℃, 61℃, 64℃, 67℃, 70℃, and 73℃, respectively. The pH values ​​of the washing water were 6.2, 6.3, 6.3, 6.4, 6.4, 6.5, 6.5, 6.6, 6.6, 6.7, 6.7, and 6.8 (the pH of the washing water was adjusted using citric acid). The total draw ratio for washing was 1.1. The washing process was a water circulation system, with a counter-current circulation rate of 50L / h in each tank. The ratio of water weight to the weight of the running filament bundle in the washing process was 17, and the total washing time was 5 minutes. After washing, the solvent residue in the filament bundle was less than 0.01%. After washing, the filament bundle underwent hot water drawing (temperatures of 95℃, 96℃, 97℃, and 99℃, with a total draw ratio of 4.536), oiling (residence time of 3 seconds, no drawing), drying and densification (two-stage drying and densification at temperatures of 115℃ and 125℃), steam drawing (pressure of 0.3MPa, steam draw ratio of 2.5), and steam heat setting (steam pressure of 0.4MPa, steam heat setting draw ratio of 0.75) before being wound up to obtain polyacrylonitrile precursor fibers.

[0079] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0080] At a total draw ratio of 37, the filament weight was measured to be 17 mg. The final carbon fiber tensile strength was 5.4 GPa, and the carbon fiber tensile modulus was 295 GPa.

[0081] Example 7

[0082] Preparation of polyacrylonitrile copolymers:

[0083] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethylformamide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 2.8. After monomer removal, the copolymer was aminated with ammonia to obtain a highly hydrophilic solution with a pH of 8.4. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0084] Preparation of polyacrylonitrile carbon fiber:

[0085] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 1. The process first involved solution extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through 11 temperature zones along the fiber's direction of travel. The temperatures of these zones were 43℃, 46℃, 49℃, 52℃, 55℃, 58℃, 61℃, 64℃, 67℃, 75℃, and 81℃, with pH values ​​of 6.3, 6.3, 6.4, 6.4, 6.5, 6.5, 6.6, 6.6, 6.7, 6.8, and 6.9 (the pH of the washing water was adjusted using citric acid). The washing process was ultrasonic, with an ultrasonic power of 400W, an oscillation frequency of 30kHz, and a wave count of 12 per meter. The ratio of water weight to the weight of the running filament bundle in the water washing process was 14. The total water washing time was 4 minutes, and the solvent residue in the filament bundle after water washing was 0.02%. After water washing, the filament bundle was oiled, dried and densified, steam-drawn, heat-set, and then wound to obtain polyacrylonitrile precursor fibers.

[0086] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0087] At a total draw ratio of 5.5, the filament weight was measured to be 20 mg. The final carbon fiber tensile strength was 5.0 GPa, and the carbon fiber tensile modulus was 252 GPa.

[0088] Comparative Example 1

[0089] Preparation of polyacrylonitrile copolymers:

[0090] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethyl sulfoxide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 2.8. After monomer removal, the copolymer was ammonified with ammonia to obtain a highly hydrophilic solution with a pH of 9.1. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0091] Preparation of polyacrylonitrile carbon fiber:

[0092] The polyacrylonitrile copolymer spinning solution was spun using a dry-jet wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 6. First, the solution underwent extrusion and coagulation. During the washing stage, the fiber passed through five temperature zones along the fiber's running direction. The temperatures of these zones were 38℃, 47℃, 56℃, 65℃, and 74℃, and the pH values ​​were 6.2, 6.3, 6.5, 6.7, and 7.8, respectively (the pH of the washing water was adjusted using citric acid or ammonia). The washing process combined water circulation and ultrasonic methods. The counter-current circulation rate in each tank was 50 L / h, the ultrasonic power was 100 W, the oscillation frequency was 20 kHz, and the wave count was 8 per meter. The ratio of the weight of the water used for washing to the weight of the running fiber bundle was 6. The total washing time was 0.6 minutes, and the solvent residue in the fiber bundle after washing was 0.07%. After washing, the polyacrylonitrile precursor fiber is obtained by hot water stretching, oiling, drying and densification, steam stretching, heat setting and winding.

[0093] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0094] At a total draw ratio of 37, the filament weight was measured to be 62 mg. The final tensile strength of the carbon fiber was 4.7 GPa, and the tensile modulus of the carbon fiber was 238 GPa.

[0095] Comparative Example 2

[0096] Preparation of polyacrylonitrile copolymers:

[0097] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethyl sulfoxide was added to the reactor as the solvent. The reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 2.8. After monomer removal, no amination treatment was performed; instead, the copolymer was directly degassed and filtered to obtain a polyacrylonitrile copolymer spinning solution with a solid content of 23%.

[0098] Preparation of polyacrylonitrile carbon fiber:

[0099] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 1. The process first involved solution extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through seven temperature zones along the fiber's direction of travel. The temperatures of these zones were 33°C, 39°C, 45°C, 51°C, 57°C, 63°C, and 66°C, with pH values ​​of 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, and 6.7 (the pH of the washing water was adjusted using citric acid). The washing process was a circulating water system, with a counter-current circulation rate of 60 L / h in each tank. The ratio of the weight of the washing water to the weight of the fiber bundle was 5. The total washing time was 3 minutes, and the solvent residue in the fiber bundle after washing was 0.08%. After washing, the polyacrylonitrile precursor fiber is obtained by oiling, drying and densification, steam drawing, heat setting and winding.

[0100] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0101] Multiple demulsification events were observed during the oiling stage, reducing production efficiency. At a total draw ratio of 5.5, the filament weight was measured to be 31 mg. The final carbon fiber tensile strength was 4.5 GPa, and the carbon fiber tensile modulus was 217 GPa.

[0102] Comparative Example 3

[0103] Preparation of polyacrylonitrile copolymers:

[0104] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethyl sulfoxide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 2.8. After monomer removal, the copolymer was aminated with ammonia to obtain a highly hydrophilic solution with a pH of 8.5. After degassing and filtration, a polyacrylonitrile copolymer spinning solution was obtained, with a solid content of 23%.

[0105] Preparation of polyacrylonitrile carbon fiber:

[0106] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 1. First, the solution underwent extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through three temperature zones along the fiber's direction of travel: 55°C, 72°C, and 64°C. The washing water was adjusted to pH 7.3 with ammonia. The washing process was a circulating water system, with a counter-current circulation rate of 50 L / h in each tank. The ratio of water weight to fiber weight was 10, and the washing process lasted 2 minutes. After washing, the solvent residue in the fiber was 0.05%. After washing, the fiber underwent oiling, drying and densification, steam drawing, heat setting, and winding to obtain polyacrylonitrile precursor fibers.

[0107] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0108] At a total draw ratio of 5.5, the filament weight was measured to be 59 mg. The final carbon fiber tensile strength was 4.4 GPa, and the carbon fiber tensile modulus was 219 GPa.

[0109] Comparative Example 4

[0110] Preparation of polyacrylonitrile copolymers:

[0111] Acrylonitrile and itaconic acid were mixed at a mass ratio of 98:2, with azobisisobutyronitrile (AIB) as the initiator (0.1 wt% of the total monomers). Dimethyl sulfoxide was added to the reactor as the solvent, and the reaction was carried out under nitrogen atmosphere and a constant temperature of 70°C for 20 hours to obtain a copolymer. The number average molecular weight of the polyacrylonitrile copolymer was approximately 90,000, and the molecular weight distribution was approximately 2.8. After monomer removal, the copolymer was aminated with ammonia to obtain a highly hydrophilic solution with a pH of 8.8. After degassing and filtration, the polyacrylonitrile copolymer spinning solution was obtained.

[0112] Preparation of polyacrylonitrile carbon fiber:

[0113] The polyacrylonitrile copolymer spinning solution was spun using a wet spinning process. Except for different washing conditions, the other process conditions were the same as in Example 2. First, the solution underwent extrusion coagulation and hot water drawing. During the washing stage, the fiber passed through eight temperature zones along the fiber's direction of travel. The temperatures of these zones were 55℃, 60℃, 65℃, 69℃, 71℃, 72℃, 74℃, and 76℃, and the pH value of each zone was 7.0. The washing process was a water circulation system, with a counter-current circulation rate of 60 L / h in each tank. The ratio of water weight to the weight of the fiber bundle was 12, and the washing process lasted for 3 minutes. After washing, the solvent residue in the fiber bundle was 0.02%. After washing, the fiber underwent oiling, drying and densification, steam drawing, heat setting, and winding to obtain polyacrylonitrile precursor fibers.

[0114] The pre-oxidation and carbonization conditions were the same as in Example 1.

[0115] At a total draw ratio of 5.5, the filament weight was measured to be 36 mg. The final carbon fiber tensile strength was 4.9 GPa, and the carbon fiber tensile modulus was 241 GPa.

[0116] As can be clearly seen from Examples 1-7 and Comparative Examples 1-4, during the washing process, the use of the present invention to set the temperature and pH value of each washing zone, as well as other washing parameters, plays an important role in reducing the total amount of fuzz at the drying and steam stretching points, and improves the stretchability of the raw yarn.

Claims

1. A method for preparing polyacrylonitrile-based carbon fiber precursor, employing a wet spinning process or a dry-jet wet spinning process, including a water washing step, wherein the pH of the washing water is 6.0 to 6.

9.

2. The preparation method according to claim 1, characterized in that, The water washing process employs at least five water washing temperature zones, preferably five to twelve water washing temperature zones; and / or, The operating temperature for the water washing is 30–85°C; and / or, The pH of the wash water is adjusted by adding an organic acid and / or an inorganic acid, preferably by adding at least one of citric acid, dilute hydrochloric acid, and acetic acid; and / or, The washing process uses a water weight to running yarn weight ratio of (5-30):1, preferably (8-20):1; and / or, The total washing time is 0.5 to 5 minutes; and / or, The water washing method employs at least one of the following: water circulation type, ultrasonic type, and compressed air type; and / or, The residual solvent content in the washed filament bundle is ≤0.03wt%.

3. The preparation method according to claim 2, characterized in that, Along the fiber running direction, the temperature of the washing zone increases; and / or, In the water washing process, the temperature values ​​of each water washing zone and the pH value of the washing water satisfy the following relationship: A = 0.0174B + 5.5076, where A is the pH value of the washing water and B is the temperature value.

4. The preparation method according to any one of claims 1 to 3, characterized in that, The preparation method of the polyacrylonitrile-based carbon fiber precursor specifically includes: extruding polyacrylonitrile solution, solidifying and molding, hot water stretching, washing, oiling, drying and densifying, steam stretching, and steam heat setting to obtain the polyacrylonitrile-based carbon fiber precursor.

5. The preparation method according to claim 4, characterized in that, The polyacrylonitrile stock solution is obtained by polymerizing monomers including acrylonitrile and then sequentially undergoing monomer removal, degassing, ammonia treatment, and filtration.

6. The preparation method according to claim 5, characterized in that, The polymeric monomer further comprises at least one comonomer, preferably selected from at least one of itaconic acid, acrylic acid, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, vinyl acetate, isobutylacrylic acid, butyl itaconic acid, mesoaconic acid, 2-butenoic acid, maleic acid, methylmaleic acid, acrylamide, acrylamide oxime, hydroxyethyl acrylonitrile, α-chloroacrylonitrile, and diacetone acrylamide; and / or, The polymerization is carried out in an organic solvent and / or an inorganic solvent, preferably, the organic solvent is selected from at least one of dimethyl sulfoxide, dimethylformamide, dimethylacetamide, and ethylene carbonate; and / or, the inorganic solvent is selected from at least one of aqueous solutions of zinc chloride, nitric acid, sodium thiocyanate, and sodium bisulfate; and / or, The polymerization is carried out under the action of an initiator, preferably selected from at least one azo compound, more preferably at least one of azobisisobutyronitrile and azobisisoheptanenitrile; and / or The polymeric monomers contain acrylonitrile at a mass percentage of not less than 95 wt%, preferably 95–99 wt%; and / or, The amount of solvent used is 70-85 wt% of the total weight of the polymerization reaction system; and / or, The polymerization reaction is carried out at a temperature of 30–70°C; and / or, The polymerization reaction takes 10–40 hours; and / or, The number-average molecular weight of the polyacrylonitrile copolymer obtained by the polymerization reaction is 50,000 to 120,000.

7. The preparation method according to claim 5, characterized in that, The ammoniation treatment uses at least one of ammonia gas, ammonia water, and ammonium carbonate; and / or, The ammoniation treatment yields a stock solution with a pH of 7.0–10.

5.

8. A polyacrylonitrile-based carbon fiber precursor, obtained by the preparation method according to any one of claims 1 to 7.

9. A carbon fiber prepared from polyacrylonitrile-based carbon fiber precursor, wherein the polyacrylonitrile-based carbon fiber precursor is the polyacrylonitrile-based carbon fiber precursor as described in claim 8.

10. A method for preparing carbon fiber, comprising: Polyacrylonitrile-based carbon fiber precursor is obtained by the preparation method according to any one of claims 1 to 7, and the carbon fiber is obtained by subjecting the polyacrylonitrile-based carbon fiber precursor to pre-oxidation treatment and carbonization treatment in sequence.

11. The method for preparing carbon fiber according to claim 10, characterized in that, The pre-oxidation treatment conditions are: a pre-oxidation temperature of 180–300°C and a treatment time of 10–60 min; and / or, The carbonization process includes low-temperature carbonization and high-temperature carbonization. Preferably, the conditions for low-temperature carbonization are: temperature 350-700℃ and processing time 2-4 min; and / or, the conditions for high-temperature carbonization are: temperature 1300-1400℃ and processing time 2-4 min.

Citation Information

Patent Citations

  • Method for preparing high-strength polyacrylonitrile-based precursor for carbon fiber

    CN101724922A

  • Method for lowering ash content of polyacrylonitrile-based carbon fiber

    CN103290527A

  • Continuous shallow groove polyacrylonitrile carbon fibre precursor consolidation forming method

    CN106939439A

  • Method for dry spraying and wet spinning low-grade polyacrylonitrile nascent fiber

    CN109137117A

  • Preparation method of polyacrylonitrile pre-oxidized fiber and obtained polyacrylonitrile pre-oxidized fiber

    CN115707801A