A device and method for controlling internal stress in high-strength and high-toughness ductile iron castings

By dividing the casting into control zones and dynamically adjusting the cooling intensity and constraint relationship, the problem of residual stress not being effectively reduced during the cooling process of castings in the prior art is solved, and the effect of reducing residual stress is achieved without extending the cooling cycle.

CN123067583APending Publication Date: 2026-11-10临清市金光机械制造有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202611577156.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies cannot effectively reduce the residual stress of castings without extending the cooling cycle, and the mechanical constraint relationship between various parts during the casting cooling process cannot be dynamically controlled, resulting in a tradeoff between cooling efficiency and residual stress.

Method used

By establishing units based on partitioning and coupling relationships, the casting is divided into multiple control partitions. Through state sensing units, soft and hard state determination units, obstructed state determination units, and partitioned cooling adjustment units, and by utilizing partitionable constraint clutch units and adaptive control units, the cooling intensity and constraint relationships of each part of the casting are dynamically adjusted to achieve adaptive decoupling control.

Benefits of technology

Without extending the cooling cycle, it effectively reduces residual stress in castings, improves dimensional stability, avoids deformation, and is compatible with existing cooling processes without changing the overall cooling regime.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123067583A_ABST
    Figure CN123067583A_ABST
Patent Text Reader

Abstract

This invention provides a device and method for controlling internal stress in high-strength and high-toughness ductile iron castings, belonging to the field of casting technology. The device includes a partitioning and coupling relationship establishment unit, a state sensing unit, a soft / hard state determination unit, an obstruction state determination unit, a partitioned cooling adjustment unit, a partitionable constraint clutch unit, and an adaptive control unit. It uses the combination of obstruction and soft / hard states of each control partition as the judgment basis, and uses the state switching of constraint elements between adjacent partitions as the control action. Within each control cycle, it sequentially executes decoupling judgment, window delay judgment, peak shifting judgment, and recovery judgment according to a fixed priority. Upon the success of the previous judgment, the corresponding action is executed and the cycle ends. The beneficial effect of this invention is that it allows the shrinkage of each part of the casting to be completed freely within its plastic yielding capacity, reducing residual stress without prolonging the cooling cycle, thus breaking the inherent trade-off between cooling rate and residual stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of casting technology, specifically relating to a device and method for controlling internal stress in high-strength and high-toughness ductile iron castings. Background Technology

[0002] During the cooling process of castings such as drive wheels for heavy-duty vehicles after casting, the uneven wall thickness distribution leads to significant differences in the cooling rate of different parts of the casting. During the cooling and shrinkage process, these areas exert mutual tension and restraint, ultimately leaving residual stress inside the casting. This residual stress significantly reduces the dimensional stability of the casting and easily causes deformation during subsequent machining.

[0003] Existing technologies offer various solutions to the problems of residual stress and machining deformation in castings, addressing issues at different stages of the process. Among them, Chinese inventions with publication numbers CN122665978A and CN122559182A employ zoned temperature control during the casting cooling process to balance the temperature field across different parts of the casting and reduce temperature differences. Chinese inventions with publication numbers CN121592846A and CN122722820A utilize vibration aging and thermal aging processes to eliminate residual stress within the casting after it has fully cooled and solidified. Chinese inventions with publication numbers CN122807308A and CN122807161A address workpiece deformation problems in the welding field through deformation prediction and motion trajectory compensation technologies.

[0004] However, all the aforementioned existing technologies share a common limitation: their implementation presupposes that the mechanical constraints of each part of the casting remain fixed. This constraint is determined once before pouring by the mold structure and the arrangement of the gating system, and remains constant throughout the entire cooling process. Based on this fixed constraint, existing technologies can only passively optimize stress and deformation by adjusting cooling temperature, aging vibration parameters, and compensating for deformation trajectories, exhibiting significant technical shortcomings. While zoned cooling processes can balance the temperature of different parts of the casting, the rigid connection structure of the casting is fixed. Even if the temperature of each part is consistent, stress will still be generated during the cooling shrinkage process due to mutual restraint. Aging treatment is carried out after the casting is fully hardened, missing the optimal time to dissipate shrinkage stress at low cost during the soft stage of the material, resulting in limited stress relief. Deformation compensation technology can only correct existing deformation defects after they have formed, and cannot eliminate the generation of residual stress at its source. In other words, existing technologies have never dynamically controlled the mechanical constraints during the casting cooling process. To reduce residual stress, they can only passively reduce the overall cooling rate, ultimately creating an inherent technical contradiction where "cooling efficiency" and "low residual stress" cannot be simultaneously achieved. Summary of the Invention

[0005] The purpose of this invention is to provide a device and method for controlling internal stress in high-strength and high-toughness ductile iron castings, and to solve the problem that existing casting technology only controls the cooling process itself and cannot regulate the mutual constraint relationship between different parts of the casting during the cooling process. Therefore, it can only reduce residual stress at the cost of reducing the cooling rate, and cannot reduce residual stress without extending the cooling cycle.

[0006] To achieve the above objectives, firstly, the present invention provides an internal stress control device for high-strength and high-toughness ductile iron castings, comprising: The partitioning and coupling relationship establishment unit is used to divide the casting into N control partitions according to the wall thickness distribution, hot spot location and structural continuity, and record the coupling mode between any two adjacent control partitions. The coupling mode includes decoupling and non-decoupling. Decoupling is a coupling mode in which a partitionable constraint clutch unit can be set between two adjacent control partitions. Non-decoupling is a coupling mode in which two adjacent control partitions belong to the same continuous entity and a partitionable constraint clutch unit cannot be set. The state sensing unit includes a temperature sensing part distributed in the mold and each control zone, a displacement sensing part for sensing the actual relative displacement between each adjacent control zone, and a state output part for outputting the soft and hard state and the obstructed state of each control zone. The soft / hard state determination unit is connected to the temperature sensing part and is used to compare the current temperature of each control zone with the preset plastic temperature limit to determine whether the corresponding control zone is in a plastic state, a transitional state or a rigid state. The obstructed state determination unit, connected to the displacement sensing part, is used to compare the amount of contraction that each control zone should have completed according to its temperature history with the actual amount of contraction that the control zone has actually experienced. When the difference exceeds the allowable range, the control zone is determined to be in an obstructed state. The zoned cooling adjustment unit includes cooling circuits that correspond one-to-one with each control zone and are independently controllable, and each cooling circuit has an independent cooling intensity adjustment element; A partitionable constraint clutch unit is disposed between adjacent control partitions that are determined to be decoupled. It has a constraint state that restricts the relative displacement between the corresponding adjacent control partitions and a release state that allows free relative displacement between the corresponding adjacent control partitions, and can switch between the constraint state and the release state under control. An adaptive control unit is connected to the soft / hard state determination unit, the obstructed state determination unit, the partitioned cooling adjustment unit, and the partitionable constraint clutch unit, respectively. The adaptive control unit is configured to perform hierarchical decoupling control judgment based on the partitioned soft / hard state and obstructed state in each control cycle, and to perform the corresponding action and end the current control cycle when the previous judgment is true.

[0007] Furthermore, the hierarchical decoupling control decision includes the following steps executed sequentially: Firstly, if there are adjacent control partition pairs that are both in a malleable state and both in a restricted state, then the partitionable constraint clutch unit between the adjacent control partition pairs is switched to the released state. The second judgment is that if there is a control zone that is currently in a blocked state and in a malleable state, while its adjacent control zone is currently in a rigid state, then the cooling intensity of the cooling circuit of that control zone is reduced. The third judgment is that if there is an adjacent control partition pair whose coupling mode is non-decoupling, whose plastic state periods overlap in time, and both are in a blocked state, then the cooling sequence of the adjacent control partition pair is adjusted so that one of them completes free contraction and enters a rigid state first, and then the other is cooled. The fourth determination is that if there is a control zone that has been released from obstruction or has entered a rigid state, the cooling intensity of the cooling circuit of that control zone is restored to the standard strong cooling intensity, and the partitionable constraint clutch unit between that control zone and the adjacent control zone is restored to the constraint state.

[0008] Furthermore, the condition for the soft / hard state determination unit to determine the plastic state is that the current temperature of the control zone is higher than the plastic temperature limit; the condition for determining the rigid state is that the current temperature of the control zone is lower than the plastic temperature limit; and the condition for determining the transition state is that the current temperature of the control zone is within a predetermined range above or below the plastic temperature limit. The plastic temperature limit is pre-calibrated according to the temperature corresponding to the ratio of the yield strength of the casting material to its room temperature yield strength, and once calibrated, it remains fixed during the cooling process.

[0009] Furthermore, the obstructed state determination unit includes a free contraction amount conversion part and a comparison part. The free contraction amount conversion part calculates the contraction amount that the corresponding control zone should have completed when it is unobstructed by converting the temperature history of the control zone with the pre-calibrated linear expansion characteristics. The comparison part calculates the difference between the actual contraction amount of the control zone and the contraction amount that should have been completed, and outputs the determination result that the corresponding control zone is in an obstructed state when the absolute value of the difference exceeds the allowable range.

[0010] Furthermore, the displacement sensing part is a high-temperature displacement sensor or a non-contact vision measuring device, and the displacement sensing part is installed at the boundary between two adjacent control zones and avoids the gating and riser area of ​​the casting.

[0011] Furthermore, each cooling circuit of the partitioned cooling adjustment unit operates under negative pressure conditions, and the cooling intensity adjustment element is a negative pressure adjustment valve installed on each cooling circuit. The cooling intensity is independently adjusted by adjusting the negative pressure value of each cooling circuit.

[0012] Furthermore, the adaptive control unit also includes a batch adaptive module, which is used to correct the linear expansion characteristics used in the obstructed state determination unit to calculate the amount of shrinkage that should have been completed, based on the measured expansion characteristics of the casting material in the current furnace.

[0013] Furthermore, the adaptive control unit is also equipped with a control cycle setting module, which determines the control cycle according to the wall thickness of the control zone, and the determined control cycle is less than a set proportion of the duration of the plastic state of the corresponding control zone.

[0014] Secondly, a method for controlling the internal stress of high-strength and high-toughness ductile iron castings is also disclosed, employing the aforementioned internal stress control device for high-strength and high-toughness ductile iron castings, comprising: Step S1: Divide the casting into N control zones, record the coupling mode between any two adjacent control zones as decoupling or non-decoupling, set up a zoned constraint clutch unit at the decoupling point, configure an independent and controllable cooling circuit for each control zone, and calibrate the plastic temperature limit according to the casting material. Step S2: The casting enters the cooling stage; Step S3: Collect the temperature of each control zone and the actual relative displacement between adjacent control zones; Step S4: Compare the current temperature of each control zone with the plastic temperature limit to determine whether the corresponding control zone is in a plastic state, a transitional state, or a rigid state. Step S5: Compare the actual amount of contraction that occurs in each control zone with the amount of contraction that should have been completed according to the temperature history to determine whether the corresponding control zone is in an obstructed state. Step S6: Perform the first judgment. If there are adjacent control partition pairs where both are currently in a malleable state and both are currently in a blocked state, then switch the partitionable constraint clutch unit between the corresponding adjacent control partition pairs to the released state. This control cycle ends and returns to step S2. Step S7: Perform the second judgment. If there is a control zone that is currently in a blocked state and in a malleable state while its adjacent control zone is currently in a rigid state, then reduce the cooling intensity of the cooling circuit of the corresponding control zone. This control cycle ends and returns to step S2. Step S8: Perform the third judgment. If there are adjacent control partition pairs whose coupling mode is non-decoupling, whose plastic state time periods overlap in time, and both are currently in a blocked state, then adjust the cooling sequence of the corresponding adjacent control partition pairs so that one of them completes free contraction and enters a rigid state first, and then applies cooling to the other. This control cycle ends and returns to step S2. Step S9: Perform the fourth judgment. For the control zone whose obstruction state has been released or has entered the rigid state, restore the cooling intensity of its cooling circuit to the standard strong cooling intensity, and restore the partitionable constraint clutch unit between it and the adjacent control zone to the constraint state. Step S10: Repeat steps S2 to S9 until the casting has cooled down.

[0015] Furthermore, it also includes step S11: outputting the obstruction state history record and residual stress assessment results of each control zone as quality traceability data for the casting.

[0016] Furthermore, the fixed priority order is determined according to the principle of increasing cost, where the cost of the first judgment is less than the cost of the second judgment, the cost of the second judgment is less than the cost of the third judgment, and the cost of the third judgment is less than the cost of the fourth judgment.

[0017] As can be seen from the above technical solutions, the present invention has the following advantages: Firstly, residual stress is reduced without extending the cooling cycle. In this invention, the action of reducing the cooling intensity only occurs during a limited period when the control zone is still soft and obstructed. Once the obstructed state is lifted or the control zone enters a rigid state, the cooling intensity is immediately restored to the standard strong cooling intensity through the fourth judgment. Therefore, the overall cooling cycle of the casting remains basically unchanged, which is fundamentally different from all schemes that reduce stress through overall slow cooling. Secondly, intervention is applied at a time when the cost is relatively low. This invention focuses the intervention on the stage when the casting is still soft. At this stage, the material can absorb the shrinkage difference with very small local plastic deformation. However, after the casting hardens, the same shrinkage difference can only be converted into considerable elastic stress. The timing itself brings about the difference in technical effect. Third, it transforms constraints from a prerequisite into a means; the introduction of partitionable constraint engagement and disengagement units makes the previously passively accepted constraint relationships in casting adjustable, providing a degree of freedom for stress control of castings that is not available in existing technologies. Fourth, it provides observable state quantities during the cooling process; the obstructed state is a state quantity that can be determined in real time during the cooling process, making the control an object with an immediate response; in contrast, existing technologies can only detect residual stress after cooling is completed, which is a result quantity and cannot be used for process intervention. Fifth, it provides a time-dimensional alternative for situations where constraints cannot be physically removed; for partitioned pairs of constraint-engaged units with continuous structures and no partitionable partitioning, this invention achieves equivalent decoupling by staggering peaks in shrinking windows. Sixth, it is compatible with existing forced cooling processes rather than conflicting with them; this invention does not change the overall system of forced cooling processes, but only makes local concessions within key windows, and can be used in conjunction with existing processes such as vacuum cooling casting and forced cooling to shorten production cycles. Attached Figure Description

[0018] To more clearly illustrate the technical solution of the present invention, the accompanying drawings used in the description will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a structural block diagram of the internal stress control device for high-strength and high-toughness ductile iron castings in this invention. Figure 2 This is a flowchart of the internal stress control method for high-strength and high-toughness ductile iron castings in this invention.

[0020] In the diagram: 1. Partition and coupling relationship establishment unit; 2. State perception unit; 3. Soft and hard state determination unit; 4. Obstructed state determination unit; 5. Partition cooling adjustment unit; 6. Partitionable constraint clutch unit; 7. Adaptive control unit. Detailed Implementation

[0021] To make the objectives, features, and advantages of this invention more apparent and understandable, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings of the specific embodiments. Obviously, the embodiments described below are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0022] Example 1 like Figure 1 As shown, this embodiment provides an internal stress control device for high-strength and high-toughness ductile iron castings, including a partitioning and coupling relationship establishment unit 1, a state sensing unit 2, a soft and hard state determination unit 3, a blocked state determination unit 4, a partitioned cooling adjustment unit 5, a partitionable constraint clutch unit 6, and an adaptive control unit 7.

[0023] The partitioning and coupling relationship establishment unit 1 is used to divide the casting into N (N is an integer not less than 2) control partitions according to wall thickness distribution, hot spot location, and structural continuity. Taking a heavy-duty vehicle drive wheel casting as an example, its material is QT900-5 ductile iron, with a wall thickness distribution ranging from 15mm to 45mm. There is a hot spot at the hub and a thin wall at the spokes. Based on this, the casting is divided into 6 control partitions. After partitioning, the coupling mode between each pair of adjacent control partitions is recorded. In this embodiment, two pairs of adjacent control partitions at the junction of the hub and spokes can be partitioned by a constraint clutch unit 6, which is denoted as decoupling; there is one pair of adjacent control partitions inside the spokes, which belong to the same continuous entity and cannot be partitioned by a constraint clutch unit 6, which is denoted as non-decoupling.

[0024] Furthermore, in this first embodiment, the core principle of the partitioning and coupling relationship establishment unit 1 lies in transforming the interrelationships between various parts of the casting during the cooling process from static conditions given all at once in the casting process plan into explicit data structures that can be invoked by the control device. Its theoretical basis is the structural continuity analysis and thermal point identification of the casting. The purpose is to provide object definitions for subsequent obstruction state determination and constraint switching, avoiding misjudgments of independent parts by the control device without coupling relationship records, and realizing the transformation from passively accepting constraint relationships to actively managing constraint relationships.

[0025] The state sensing unit 2 includes a temperature sensing section, a displacement sensing section, and a state output section. The temperature sensing section uses thermocouples distributed throughout the mold and each control zone to sense the temperature of each control zone. The displacement sensing section uses a high-temperature displacement sensor or a non-contact vision measuring device, installed at the boundary between two adjacent control zones, avoiding the gating and riser area of ​​the casting, to sense the actual relative displacement between adjacent control zones. The state output section outputs the soft / hard state and obstructed state of each control zone to the adaptive control unit 7.

[0026] The soft / hard state determination unit 3 is connected to the temperature sensing part and is used to compare the current temperature of each control zone with a preset plastic temperature limit to determine whether the control zone is in a plastic, transitional, or rigid state. The condition for determining the plastic state is that the current temperature of the control zone is higher than the plastic temperature limit; the condition for determining the rigid state is that the current temperature of the control zone is lower than the plastic temperature limit; and the condition for determining the transitional state is that the current temperature of the control zone is within a predetermined neighborhood above or below the plastic temperature limit.

[0027] Furthermore, in this first embodiment, the plasticity temperature limit is pre-calibrated according to the temperature corresponding to the ratio of the yield strength of the casting material to its room temperature yield strength. For QT900-5 ductile iron, the value of this plasticity temperature limit is determined according to the above calibration method, and once calibrated, it remains fixed during the cooling process of the castings in the same batch. The purpose of using a fixed limit instead of a dynamic limit that changes with temperature is to ensure that the determination of the soft and hard state is not affected by measurement noise, thereby providing a definite input for subsequent judgment steps.

[0028] The obstruction state determination unit 4 is connected to the displacement sensing part and is used to determine whether the current contraction of each control zone is obstructed. The obstruction state determination unit 4 includes a free contraction amount conversion part and a comparison part. The free contraction amount conversion part calculates the amount of contraction that the control zone should have completed when there is no obstruction, based on the temperature history of the control zone and the pre-calibrated linear expansion characteristics. The comparison part calculates the difference between the actual contraction amount and the expected contraction amount of the control zone, and outputs a determination result that the control zone is in an obstructed state when the absolute value of the difference exceeds the allowable range.

[0029] A hindered state refers to a state in which the contraction that a control zone should have completed is not completed due to constraints imposed by adjacent control zones. Constructing this state variable requires simultaneously knowing and comparing the temperature history and measured displacement of the control zones; it cannot be directly read from the temperature field. When there is no coupling relationship between control zones, the actual contraction amount is consistent with the expected contraction amount, and the hindered state is always invalid; separation only occurs when coupling constraints exist. Therefore, the validity of this criterion itself depends on the existence of a coupling relationship and has a definite physical meaning. Furthermore, the hindered state is a state variable during the cooling process, not a result variable after cooling is complete, and thus can be used as an input for process control.

[0030] The zoned cooling regulation unit 5 includes cooling circuits that correspond one-to-one with each control zone and are independently controllable. Each cooling circuit has an independent cooling intensity regulation element. In this embodiment, each cooling circuit operates under negative pressure conditions. The cooling intensity regulation element is a negative pressure regulating valve installed on each cooling circuit. The cooling intensity is independently regulated by adjusting the negative pressure value of each cooling circuit. Negative pressure regulation is used instead of regulating the flow rate of the cooling medium because the strong cooling process of castings is often carried out under vacuum or negative pressure conditions. The negative pressure value itself is an adjustable parameter, eliminating the need for additional piping.

[0031] The partitionable constraint clutch unit 6 is disposed between adjacent control partitions that are determined to be decoupled, and has two working states: a constrained state and a released state. In the constrained state, the unit restricts the relative displacement between two adjacent control partitions; in the released state, the unit allows free relative displacement between two adjacent control partitions. The unit can switch between the two states under controlled conditions. In this embodiment, the partitionable constraint clutch unit 6 adopts a hydraulic constraint clutch element, and its residual constraint force in the released state does not exceed a set value. The partitionable constraint clutch unit 6 is the landmark component of this invention. In the art, the constraints between various parts of a casting have traditionally been passively provided by the core and mold, and remain fixed throughout the cooling process. This embodiment uses this constraint as a switchable element and connects it to the control loop as an actuator, thus making the constraint a control means that can be switched on and off at any time for the first time.

[0032] The adaptive control unit 7 is connected to the soft and hard state determination unit 3, the obstructed state determination unit 4, the partitioned cooling adjustment unit 5, and the partitionable constraint clutch unit 6, respectively. It is configured to perform hierarchical decoupling control judgment based on the partitioned soft and hard state and the obstructed state in each control cycle. That is, it executes the following four judgment steps in a fixed priority order, and executes the corresponding action and ends the current control cycle when the previous judgment is true.

[0033] Specifically, the first judgment (decoupling judgment) has the highest priority. This judgment determines whether there exists an adjacent control partition pair that simultaneously satisfies the condition that both are currently in a plastic state and both are currently in a restricted state. If this judgment is true, the partitionable constraint clutch unit 6 between the adjacent control partition pair is switched to the released state. The design basis for the first judgment is that both are currently in a plastic state, meaning that allowing them to contract freely at this time has the lowest cost and best effect. If this point is missed, releasing the constraint after either one enters a rigid state is meaningless, because the already rigid one cannot eliminate stress through plastic yielding. Therefore, this judgment must be executed first.

[0034] The second judgment (window-based judgment) has lower priority. This judgment checks whether there exists a control partition that is currently in a blocked and malleable state while its adjacent control partition is currently in a rigid state. If this judgment is true, the cooling intensity of the cooling circuit of that control partition is reduced. The design basis for the second judgment is that if an adjacent control partition has entered a rigid state, it means that the control partition is likely being held up by this rigid neighbor. In this case, releasing the constraint cannot solve the problem because the adjacent control partition is either non-decoupled or already solidified. The only effective means is to make the control partition complete its contraction before it also becomes rigid; therefore, its cooling must be slowed down to extend the duration of its malleable state.

[0035] It is important to note that the action direction of the second judgment is opposite to the prevailing teachings in the art. The prevailing practice is to intensify the cooling of a region or its adjacent regions when a temperature is found to be too high, in order to achieve temperature convergence. The action of the second judgment, however, is to actively reduce the cooling intensity of the control zone, artificially maintaining the temperature difference between it and adjacent control zones. The reason for the opposite action direction is that the control objectives are opposite: the prevailing practice aims to achieve temperature convergence, while the objective of this invention is to fully utilize the flexible shrinkage window in terms of time. This invention artificially prolongs the temperature difference, not to abandon uniform cooling, but to extend the time the control zone remains soft enough to complete the required shrinkage; once the window is used up, strong cooling is immediately restored through the fourth judgment.

[0036] The third judgment (peak-shifting judgment) has the next highest priority. This judgment determines whether there exists a pair of adjacent control zones that satisfy the following conditions: the coupling mode is non-decoupling, the plastic state periods overlap in time, and both are currently in a blocked state. If this judgment is true, the cooling sequence of the adjacent control zone pair is adjusted so that one of them completes free contraction and enters a rigid state first, before cooling is applied to the other. The design basis of the third judgment is that for two control zones that are structurally inseparable, the physical constraints cannot be removed; therefore, their contractions must be queued, with only one contracting at a time to avoid simultaneous contraction and mutual obstruction. The adjusted result is that the contraction windows of the two control zones are staggered in time and do not overlap. One of them completes free contraction and enters a rigid state first, after which it becomes a rigid reference that no longer moves; then cooling is applied to the other to cause it to contract, at which point the contraction of the other is no longer affected by a contracting living body. Furthermore, the object of staggering in the third judgment is the timing of the contraction windows of each control zone, i.e., the response timing, not the timing of the heat source input. While staggered welding techniques such as segmented back-welding and skip welding exist in the welding field, they only stagger the order of heat source input, controlling the input quantity, which differs from this invention. The cooling timing adjustment in the third judgment is determined based on the thermal diffusion characteristics of adjacent control zones, with its lower limit being the time required for the control zone that is cooled first to complete free contraction and enter a rigid state.

[0037] The fourth judgment (restoration judgment) has the lowest priority. This judgment determines whether there is a control zone whose obstructed state has been released or has entered a rigid state. If this judgment is true, the cooling intensity of the cooling circuit of that control zone is restored to the standard strong cooling intensity (the standard strong cooling intensity is the preset cooling intensity for the corresponding control zone under unobstructed intervention), and the partitionable constraint clutch unit 6 between it and the adjacent control zone is restored to the constrained state. The design basis of the fourth judgment is that reducing the cooling intensity in the second judgment comes at a cost, prolonging the local cooling time of the control zone. Once the plastic window has been used up, the cooling intensity must be immediately restored to ensure that the overall cooling cycle of the casting is not affected. This judgment is a key finishing step in this invention that enables both residual stress and cooling efficiency to be reduced. Furthermore, restoring the constraint state between the control zone and the solidified adjacent control zone after it has entered a rigid state will not generate new stress because both sides are no longer contracting.

[0038] The fixed priority order of the above four judgments is determined based on the principle of increasing cost. Removing the constraint does not cause any loss in cooling efficiency, so its cost is the lowest, and it is ranked first with the highest priority; extending the plastic window causes a local loss in cooling efficiency, so its cost is in the middle and it is ranked second; staggered waiting causes a waiting loss in terms of timing, so its cost is next; the fourth judgment itself does not cause any additional loss to the cooling process, so it is ranked last because a closing action is only required when the first three judgments are all false. This order is not arbitrary, and there is no corresponding teaching in the prior art that reflects the considerations of this technology.

[0039] To illustrate the above process using a control zone as an example: Initially, the control zone has a high temperature and is in a plastic state during the cooling process. As cooling progresses, its temperature decreases. At a certain point, the actual amount of contraction begins to fall short of the contraction it should have completed according to the temperature history, and the obstructed state changes from invalid to valid. If its adjacent control zone is simultaneously in a plastic state and obstructed, the first judgment is valid, and the constraint is released. If its adjacent control zone has already entered a rigid state, the first judgment is invalid, the second judgment is valid, the cooling intensity of the control zone is reduced, its temperature decreases more slowly, and the duration of the plastic state is extended. After the control zone completes its expected contraction, the obstructed state changes from valid to invalid, the fourth judgment is valid, its cooling intensity is restored to the standard strong cooling intensity, and the temperature then accelerates its decrease and enters a rigid state.

[0040] In addition, the adaptive control unit 7 also includes a batch adaptive module and a control cycle setting module. The batch adaptive module is used to correct the linear expansion characteristics used in the obstructed state determination unit 4 to calculate the shrinkage amount that should have been completed, based on the measured expansion characteristics of the casting material in the current heat. This is because ductile iron from different heats has fluctuations in graphite spheroidization rate and matrix structure, and its linear expansion characteristics are not exactly the same. If a fixed linear expansion characteristic is used, the calculation result of the shrinkage amount that should have been completed will have device deviation, thus causing misjudgment of the obstructed state. The control cycle setting module determines the control cycle according to the wall thickness of the control zone, and the determined control cycle is less than the set proportion of the duration of the plastic state of the control zone. The control cycle needs to be significantly shorter than the duration of the plastic state to ensure that the above judgment and action can be completed within the plastic window; moreover, the greater the wall thickness, the longer the duration of the plastic state, and the longer the control cycle that can be used.

[0041] Example 2 like Figure 2 As shown, this embodiment two discloses a method for controlling the internal stress of high-strength and high-toughness ductile iron castings, which adopts the internal stress control device for high-strength and high-toughness ductile iron castings described in embodiment one, including steps S1 to S11.

[0042] Step S1: Divide the casting into N control zones, record the coupling mode between each pair of adjacent control zones as decoupling or non-decoupling, set up a partitioned constraint clutch unit 6 at the decoupling point, configure an independent and controllable cooling circuit for each control zone, and calibrate the plastic temperature limit according to the casting material.

[0043] In step S2, the casting enters the cooling stage, and subsequent steps are executed cyclically according to the control cycle.

[0044] Step S3: Collect the temperature of each control zone and the actual relative displacement between adjacent control zones.

[0045] Step S4: Compare the current temperature of each control zone with the plastic temperature limit to determine whether the control zone is in a plastic state, a transitional state, or a rigid state.

[0046] Step S5: Compare the actual amount of contraction that occurs in each control zone with the amount of contraction that should have been completed according to the temperature history to determine whether the control zone is in a blocked state.

[0047] Step S6: Perform the first judgment. If there is an adjacent control partition pair where both are currently in a malleable state and both are currently in a restricted state, then switch the partitionable constraint clutch unit 6 between the adjacent control partition pair to the released state, the current control cycle ends and returns to step S2.

[0048] Step S7: Perform the second judgment. If there is a control zone that is currently in a blocked state and a malleable state while its adjacent control zone is currently in a rigid state, then reduce the cooling intensity of the cooling circuit of that control zone, end the current control cycle, and return to step S2.

[0049] Step S8: Perform the third judgment. If there are adjacent control partition pairs whose coupling mode is non-decoupling, whose plastic state periods overlap in time, and both are currently in a blocked state, then adjust the cooling sequence of the adjacent control partition pairs so that one of them completes free contraction and enters a rigid state first, and then applies cooling to the other. This control cycle ends and returns to step S2.

[0050] Step S9, execute the fourth judgment. For control zones whose obstructed state has been released or have entered a rigid state, restore the cooling intensity of their cooling circuit to the standard strong cooling intensity, and restore the partitionable constraint clutch unit 6 between them and the adjacent control zones to the constraint state.

[0051] Step S10: Repeat steps S2 to S9 until the casting has cooled down.

[0052] Step S11: Output the obstruction state history record and residual stress assessment results of each control zone as the quality traceability data of the casting.

[0053] Furthermore, the first, second, third, and fourth judgments in steps S6 to S9 are executed sequentially according to a fixed priority order, and subsequent judgments are not executed if a previous judgment is true. This fixed priority order is determined based on the principle of increasing cost. After step S9, the process also includes: after the casting has cooled, keeping each partitionable constraint clutch unit 6 in a released state to facilitate sand removal and casting extraction.

[0054] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A device for controlling internal stress in high-strength and high-toughness ductile iron castings, characterized in that, include: The partitioning and coupling relationship establishment unit is used to divide the casting into N control partitions according to the wall thickness distribution, hot spot location and structural continuity, and record the coupling mode between any two adjacent control partitions. The coupling mode includes decoupling and non-decoupling. Decoupling is a coupling mode in which a partitionable constraint clutch unit can be set between two adjacent control partitions. Non-decoupling is a coupling mode in which two adjacent control partitions belong to the same continuous entity and a partitionable constraint clutch unit cannot be set. The state sensing unit includes a temperature sensing part distributed in the mold and each control zone, a displacement sensing part for sensing the actual relative displacement between each adjacent control zone, and a state output part for outputting the soft and hard state and the obstructed state of each control zone. The soft / hard state determination unit is connected to the temperature sensing part and is used to compare the current temperature of each control zone with the preset plastic temperature limit to determine whether the corresponding control zone is in a plastic state, a transitional state or a rigid state. The obstructed state determination unit, connected to the displacement sensing part, is used to compare the amount of contraction that each control zone should have completed according to its temperature history with the actual amount of contraction that the control zone has actually experienced. When the difference exceeds the allowable range, the control zone is determined to be in an obstructed state. The zoned cooling adjustment unit includes cooling circuits that correspond one-to-one with each control zone and are independently controllable, and each cooling circuit has an independent cooling intensity adjustment element; A partitionable constraint clutch unit is disposed between adjacent control partitions that are determined to be decoupled. It has a constraint state that restricts the relative displacement between the corresponding adjacent control partitions and a release state that allows free relative displacement between the corresponding adjacent control partitions, and can switch between the constraint state and the release state under control. An adaptive control unit is connected to the soft / hard state determination unit, the obstructed state determination unit, the partitioned cooling adjustment unit, and the partitionable constraint clutch unit, respectively. The adaptive control unit is configured to perform hierarchical decoupling control judgment based on the partitioned soft / hard state and obstructed state in each control cycle, and to perform the corresponding action and end the current control cycle when the previous judgment is true.

2. The internal stress control device for high-strength and high-toughness ductile iron castings according to claim 1, characterized in that, The hierarchical decoupling control judgment includes the following steps executed sequentially: Firstly, if there are adjacent control partition pairs that are both in a malleable state and both in a restricted state, then the partitionable constraint clutch unit between the adjacent control partition pairs is switched to the released state. The second judgment is that if there is a control zone that is currently in a blocked state and in a malleable state, while its adjacent control zone is currently in a rigid state, then the cooling intensity of the cooling circuit of that control zone is reduced. The third judgment is that if there is an adjacent control partition pair whose coupling mode is non-decoupling, whose plastic state periods overlap in time, and both are in a blocked state, then the cooling sequence of the adjacent control partition pair is adjusted so that one of them completes free contraction and enters a rigid state first, and then the other is cooled. The fourth determination is that if there is a control zone that has been released from obstruction or has entered a rigid state, the cooling intensity of the cooling circuit of that control zone is restored to the standard strong cooling intensity, and the partitionable constraint clutch unit between that control zone and the adjacent control zone is restored to the constraint state.

3. The internal stress control device for high-strength and high-toughness ductile iron castings according to claim 2, characterized in that, The condition for the soft / hard state determination unit to determine the plastic state is that the current temperature of the control zone is higher than the plastic temperature limit; the condition for determining the rigid state is that the current temperature of the control zone is lower than the plastic temperature limit; and the condition for determining the transition state is that the current temperature of the control zone is within a set range above or below the plastic temperature limit. The plastic temperature limit is pre-calibrated according to the temperature corresponding to the ratio of the yield strength of the casting material to its room temperature yield strength, and once calibrated, it remains fixed during the cooling process.

4. The internal stress control device for high-strength and high-toughness ductile iron castings according to claim 2, characterized in that, The obstructed state determination unit includes a free contraction amount conversion part and a comparison part. The free contraction amount conversion part calculates the contraction amount that the corresponding control zone should have completed when it is unobstructed by converting the temperature history of the control zone and the pre-calibrated linear expansion characteristics. The comparison part calculates the difference between the actual contraction amount of the control zone and the contraction amount that should have been completed, and outputs the determination result that the corresponding control zone is in an obstructed state when the absolute value of the difference exceeds the allowable range.

5. The internal stress control device for high-strength and high-toughness ductile iron castings according to claim 2, characterized in that, The displacement sensing part is a high-temperature displacement sensor or a non-contact vision measuring device. The displacement sensing part is installed at the boundary between two adjacent control zones and avoids the gating and riser area of ​​the casting.

6. The internal stress control device for high-strength and high-toughness ductile iron castings according to claim 2, characterized in that, Each cooling circuit of the partitioned cooling regulation unit operates under negative pressure conditions, and the cooling intensity regulating element is a negative pressure regulating valve installed on each cooling circuit.

7. The internal stress control device for high-strength and high-toughness ductile iron castings according to claim 2, characterized in that, The adaptive control unit also includes a batch adaptive module, which is used to correct the linear expansion characteristics in the obstructed state determination unit for calculating the amount of shrinkage that should have been completed, based on the measured expansion characteristics of the casting material in the current furnace.

8. The internal stress control device for high-strength and high-toughness ductile iron castings according to claim 2, characterized in that, The adaptive control unit is also equipped with a control cycle setting module, which determines the control cycle according to the wall thickness of the control zone, and the determined control cycle is less than the set ratio of the duration of the plastic state of the corresponding control zone.

9. A method for controlling internal stress in high-strength and high-toughness ductile iron castings, characterized in that, The internal stress control device for high-strength and high-toughness ductile iron castings according to any one of claims 1-8 includes: Step S1: Divide the casting into N control zones, record the coupling mode between any two adjacent control zones as decoupling or non-decoupling, set up a zoned constraint clutch unit at the decoupling point, configure an independent and controllable cooling circuit for each control zone, and calibrate the plastic temperature limit according to the casting material. Step S2: The casting enters the cooling stage; Step S3: Collect the temperature of each control zone and the actual relative displacement between adjacent control zones; Step S4: Compare the current temperature of each control zone with the plastic temperature limit to determine whether the corresponding control zone is in a plastic state, a transitional state, or a rigid state. Step S5: Compare the actual amount of contraction that occurs in each control zone with the amount of contraction that should have been completed according to the temperature history to determine whether the corresponding control zone is in an obstructed state. Step S6: Perform the first judgment. If there are adjacent control partition pairs where both are currently in a malleable state and both are currently in a blocked state, then switch the partitionable constraint clutch unit between the corresponding adjacent control partition pairs to the released state. This control cycle ends and returns to step S2. Step S7: Perform the second judgment. If there is a control zone that is currently in a blocked state and in a malleable state while its adjacent control zone is currently in a rigid state, then reduce the cooling intensity of the cooling circuit of the corresponding control zone. This control cycle ends and returns to step S2. Step S8: Perform the third judgment. If there are adjacent control partition pairs whose coupling mode is non-decoupling, whose plastic state time periods overlap in time, and both are currently in a blocked state, then adjust the cooling sequence of the corresponding adjacent control partition pairs so that one of them completes free contraction and enters a rigid state first, and then applies cooling to the other. This control cycle ends and returns to step S2. Step S9: Perform the fourth judgment. For the control zone whose obstruction state has been released or has entered the rigid state, restore the cooling intensity of its cooling circuit to the standard strong cooling intensity, and restore the partitionable constraint clutch unit between it and the adjacent control zone to the constraint state. Step S10: Repeat steps S2 to S9 until the casting has cooled down.

10. The method for controlling internal stress in high-strength and high-toughness ductile iron castings according to claim 9, characterized in that, It also includes step S11: outputting the obstruction state history record and residual stress assessment results of each control zone as quality traceability data for the casting.

Citation Information

Patent Citations

  • Partitioned self-adaptive vibration aging control method and system for residual stress of steel box girder

    CN121592846A

  • Alloy wheel low-pressure casting device with mold partitioned cooling function

    CN122559182A

  • A partitioned cooling mechanism and cooling method for casting molds

    CN122665978A

  • A method for producing a gray cast iron machine tool bed casting with low residual stress

    CN122722820A

  • A method for processing a blade body after welding deformation of a hollow web plate of an aero-engine fan

    CN122807161A