Compositions for dry electrodes, dry electrode sheets and their preparation methods, and batteries.
By adding polyether oligomers to the dry electrode composition, the problems of poor electrode mechanical strength and interface instability in the dry electrode process are solved, achieving efficient electrode processing and stable solid electrolyte interface film formation, thus improving the overall performance of sodium-ion batteries.
Patent Information
- Application Number
- CN202611110954.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-24
- Publication Date
- 2026-11-10
AI Technical Summary
In existing dry electrode processes, the interface compatibility between the negative electrode material and the binder in sodium-ion batteries is poor, resulting in poor electrode mechanical strength, discontinuous electronic conduction network, and unstable solid electrolyte interface film, which affects battery performance and cycle life.
Introducing polyether oligomers into dry electrode compositions utilizes the ether oxygen groups on their molecular chains to transform into a liquid state during shearing, promoting fibrillation of the binder, improving electrode processing performance, and inducing the formation of a stable solid electrolyte interface film on the negative electrode surface during battery charging and discharging.
It significantly improves the processing and mechanical properties of the electrode, reduces the electrode resistivity, enhances the interface stability and cycle life of sodium-ion batteries, and reduces the energy consumption and cost of preparation.
Smart Images

Figure CN123073067A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery technology, and more particularly to compositions for dry electrode fabrication, dry electrode sheets and their preparation methods, and batteries. Background Technology
[0002] Sodium-ion batteries are considered one of the most promising technologies in large-scale energy storage and low-cost power batteries due to their abundant resources, low cost, and good safety. However, their energy density, cycle life, and manufacturing cost still need further optimization. On the manufacturing side, traditional wet electrode processes use large amounts of organic solvents such as N-methylpyrrolidone (NMP), resulting in high costs, high energy consumption, environmental pollution, and solvent residue affecting battery performance. Therefore, solvent-free dry electrode processes have attracted widespread attention, offering advantages such as shorter processes, reduced energy consumption, and increased electrode compaction density, and are considered a next-generation battery manufacturing technology.
[0003] The core binder for dry-process electrodes is typically polytetrafluoroethylene (PTFE), which relies on fibrillation under shear force to form a three-dimensional microfiber network, providing mechanical strength and electronic conduction pathways. However, key anode materials in sodium-ion batteries (such as hard carbon) have strong chemical inertness, irregular morphology, and poor interfacial compatibility with PTFE. This results in low shear force transfer efficiency, insufficient fibrillation of PTFE, and uneven fiber distribution during dry mixing. This directly leads to poor mechanical strength of the electrode film and discontinuous electronic conduction network, severely affecting electrode processability and battery performance.
[0004] Meanwhile, sodium ions have a large ionic radius and weak solvation energy, resulting in an initial solid electrolyte interphase (SEI) film formed on the negative electrode surface that is typically thicker, more porous, and has poorer mechanical strength and ionic conductivity. This unstable SEI film cannot effectively passivate the interface, leading to continuous consumption of active sodium and electrolyte, manifested as low initial coulombic efficiency and a sharp decline in cycle life. This is one of the core issues restricting the commercialization of sodium-ion batteries.
[0005] To improve interfacial stability, film-forming additives such as fluoroethylene carbonate and vinylene carbonate are often introduced in wet electrode processes. However, in solvent-free dry processes, these liquid or low-melting-point solid additives are difficult to disperse uniformly in the electrode active material. Simple physical mixing can lead to excessively high local concentrations, which not only interferes with the fibrillation process of PTFE and affects the mechanical properties of the electrode, but may also form an uneven and unstable SEI inside the electrode during cycling, thus deteriorating battery performance. Some studies have attempted to add solid lubricants or plasticizers (such as zinc stearate and paraffin) to dry electrodes to improve powder flowability or film formation, but these substances are usually electrochemically inert and cannot solve the problem of interfacial stability of sodium electrode anodes.
[0006] An ideal additive for dry electrode should have the dual functions of a processing aid and an interface modifier: it can improve the fibrillation uniformity of PTFE and the processing performance of the electrode, and participate in the regulation of the formation of the SEI film on the negative electrode surface to enhance interface stability.
[0007] Therefore, there is an urgent need to develop an electrode composition and its preparation method that are compatible with dry processes, so as to improve the electrode processing performance while enhancing the interface stability and cycle life of sodium-ion batteries. Summary of the Invention
[0008] The purpose of this invention is to address the deficiencies of existing technologies by providing a dry electrode composition, a dry electrode sheet, a method for preparing the same, and a battery. This invention adds polyether oligomers to the dry electrode composition. The molecular chains of polyether oligomers contain ether oxygen groups, which can liquefy during the dry electrode preparation process. As a processing aid, they promote the fibrillation of the binder and improve the processing and mechanical properties of the electrode. At the same time, polyether oligomers can induce the formation of a stable solid electrolyte interface film on the negative electrode surface during battery charging and discharging, thereby improving the interface stability and cycle life of sodium-ion batteries.
[0009] To achieve the above objectives, in a first aspect, the present invention provides a composition for dry electrode fabrication, the composition comprising an electrode active material, a conductive agent, a binder, and a polyether oligomer; The polyether oligomer contains etheroxy groups on its molecular chain; the polyether oligomer is in a liquid state during the dry electrode preparation process, so that the polyether oligomer acts as a processing aid to promote the fibrillation of the binder during the dry electrode preparation process; and the polyether oligomer induces the formation of a solid electrolyte interface film on the negative electrode surface during battery charging and discharging.
[0010] Preferably, the polyether oligomer includes one or more of polypropylene glycol or polyethylene glycol; the binder includes polytetrafluoroethylene; the conductive agent includes one or more of acetylene black, Super P, carbon nanotubes, carbon fibers, Ketjen black, conductive graphite or graphene; and the electrode active material includes one or more of hard carbon, soft carbon or modified hard carbon.
[0011] Preferably, by mass percentage, the content of the electrode active material is 88.8wt%-98wt%, the content of the conductive agent is 0.2wt%-5wt%, the content of the binder is 0.2wt%-10wt%, and the content of the polyether oligomer is 1wt%-10wt%.
[0012] Secondly, the present invention provides a method for preparing a dry electrode sheet, the method comprising the following steps: Electrode active material, conductive agent, binder and polyether oligomer are mixed under solvent-free conditions and sheared to cause fibrillation of the binder, resulting in a dry powder mixture; wherein the molecular chain of the polyether oligomer contains ether oxygen groups, and the polyether oligomer is in a liquid state during shearing, acting as a processing aid to promote fibrillation of the binder; The dry powder mixture is pressed into an electrode film using a film-forming and thinning device; The electrode film is composited onto the current collector to obtain a dry electrode sheet.
[0013] Preferably, the polyether oligomer includes one or more of polypropylene glycol or polyethylene glycol; the binder includes polytetrafluoroethylene; the conductive agent includes one or more of acetylene black, Super P, carbon nanotubes, carbon fibers, Ketjen black, conductive graphite or graphene; and the electrode active material includes one or more of hard carbon, soft carbon or modified hard carbon.
[0014] Preferably, the mass ratio of the electrode active material, the conductive agent, the binder, and the polyether oligomer is 88.8-98:0.2-5:0.2-10:1-10.
[0015] Preferably, the shearing process includes two stages: low-speed mixing and high-speed shear fibrillation; the low-speed mixing speed is 1200rpm-3000rpm and the time is 5min-20min; the high-speed shear fibrillation speed is 4000rpm-8000rpm and the time is 3min-30min.
[0016] Preferably, the roller temperature of the film-forming and thinning equipment is 70℃-250℃; the thermal bonding temperature for bonding the electrode film onto the current collector is 70℃-250℃, and the pressure is 2T-30T.
[0017] Thirdly, the present invention provides a dry electrode sheet, the dry electrode sheet comprising a current collector and an electrode film disposed on the current collector; the electrode film is formed by fibrillation treatment of the dry electrode composition described in the first aspect above, or the dry electrode sheet is prepared by the preparation method described in the second aspect above.
[0018] Fourthly, the present invention provides a sodium-ion battery, the sodium-ion battery comprising a dry electrode sheet; the dry electrode sheet comprising a current collector and an electrode film formed by fibrillation treatment of the dry electrode composition described in the first aspect above, or comprising a dry electrode sheet prepared by the preparation method described in the second aspect above, or comprising a dry electrode sheet described in the third aspect above.
[0019] The present invention provides a dry electrode composition, a dry electrode sheet, a method for preparing the same, and a battery, which have the following technical effects: (1) The present invention adds polyether oligomers containing ether oxygen groups to the dry electrode composition, which transforms into a low viscosity fluid during shearing and thus is in a liquid state, providing an instantaneous liquid phase environment, realizing uniform dispersion and efficient lubrication of polyether oligomers and binders under solvent-free conditions, promoting fibrillation of PTFE, and significantly improving the processing performance and mechanical properties of dry electrode sheets, specifically manifested as a significant reduction in electrode sheet resistivity and a significant increase in electrode sheet peel strength.
[0020] (2) The polyether oligomer molecular chain in this invention contains ether oxygen groups. During the first charge and discharge process of the battery, the ether oxygen groups can participate in the solvation structure of sodium ions, preferentially reduce and decompose, and induce the formation of a dense, stable, and highly ionicly conductive solid electrolyte interface film on the negative electrode surface. This effectively inhibits the continuous decomposition of the electrolyte and the consumption of active sodium, thereby significantly reducing the electrode resistivity and improving the first coulombic efficiency and cycle life of the sodium-ion battery.
[0021] (3) In this invention, the polyether oligomer is in a liquid state during shearing, which can uniformly encapsulate the active material particles, physically block the migration of electrons to PTFE, inhibit the reduction and decomposition of PTFE, and further improve the structural stability and electrochemical stability of the electrode.
[0022] (4) This invention introduces a single polyether oligomer into the dry electrode composition, which simultaneously functions as a processing aid, an electronic barrier, and an SEI film-forming additive: during the preparation process, it acts as a processing aid to promote fibrillation of the binder and improve the processing performance of the electrode; within the electrode, it acts as a physical barrier layer to inhibit the reduction and decomposition of PTFE, thereby enhancing the structural stability of the electrode; during the first charge and discharge process of the battery, it preferentially reduces and decomposes, and induces the formation of a dense and stable SEI film, thus improving interfacial stability. This fundamentally solves the technical problem of balancing processing performance and interfacial stability in existing dry electrode processes.
[0023] (5) The preparation method provided by the present invention does not add organic solvents throughout the process, is suitable for solvent-free dry electrode process system, and has the advantages of short process, low energy consumption, low cost and easy industrial production. Attached Figure Description
[0024] Figure 1 A flowchart illustrating the method for preparing a dry electrode sheet according to an embodiment of the present invention. Detailed Implementation
[0025] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0027] This invention provides a composition for dry electrode fabrication, the composition comprising an electrode active material, a conductive agent, a binder, and a polyether oligomer.
[0028] Among them, polyether oligomers contain etheroxy groups on their molecular chains. Polyether oligomers are in a liquid state during the dry electrode preparation process, which allows them to act as processing aids to promote the fibrillation of the binder; and polyether oligomers induce the formation of a solid electrolyte interface film on the negative electrode surface during battery charging and discharging.
[0029] The polyether oligomers have a molecular weight of 400-2000 and include one or more of polypropylene glycol or polyethylene glycol. The binder includes polytetrafluoroethylene. The conductive agent includes one or more of acetylene black, Super P, carbon nanotubes, carbon fibers, Ketjen black, conductive graphite, or graphene. The electrode active material includes one or more of hard carbon, soft carbon, or modified hard carbon.
[0030] By mass percentage, the content of electrode active material is 88.8wt%-98wt%, the content of conductive agent is 0.2wt%-5wt%, the content of binder is 0.2wt%-10wt%, and the content of polyether oligomer is 1wt%-10wt%.
[0031] This invention adds polyether oligomers to the dry electrode composition. These oligomers, containing ether oxygen groups on their molecular chains, transform into low-viscosity fluids during shearing, thus remaining in a liquid state and providing a transient liquid environment. This enables uniform dispersion and efficient lubrication of the polyether oligomers and binders under solvent-free conditions, promoting the fibrillation of PTFE and significantly improving the processing and mechanical properties of the dry electrode. Simultaneously, the polyether oligomers can participate in the solvation structure of sodium ions during battery charging and discharging, preferentially reducing and decomposing them to induce the formation of a dense and stable solid electrolyte interface film on the negative electrode surface, thereby improving the interface stability and cycle life of the sodium-ion battery.
[0032] In addition, embodiments of the present invention also provide a method for preparing a dry electrode, the main steps of which are as follows: Figure 1 As shown, it includes the following steps: Step 110: The electrode active material, conductive agent, binder, and polyether oligomer are mixed under solvent-free conditions and subjected to shearing treatment to induce fibrillation of the binder, resulting in a dry powder mixture. The polyether oligomer contains ether oxygen groups on its molecular chain. During shearing, the polyether oligomer is in a liquid state, acting as a processing aid to promote fibrillation of the binder.
[0033] The polyether oligomers have a molecular weight of 400-2000 and include one or more of polypropylene glycol or polyethylene glycol. The binder includes polytetrafluoroethylene. The conductive agent includes one or more of acetylene black, Super P, carbon nanotubes, carbon fibers, Ketjen black, conductive graphite, or graphene. The electrode active material includes one or more of hard carbon, soft carbon, or modified hard carbon.
[0034] Preferably, the mass ratio of electrode active material, conductive agent, binder, and polyether oligomer is 88.8-98:0.2-5:0.2-10:1-10. If the amount of polyether oligomer is too low, it will not provide enough liquid phase medium after liquefaction, resulting in insufficient shear force transmission efficiency, incomplete fibrillation of the binder, and limited improvement in the mechanical properties of the electrode. If the amount of polyether oligomer is too high, the excessive amount of polyether oligomer may affect the electronic conductivity and compaction density of the electrode, and increase the cost.
[0035] The shearing process includes two stages: low-speed mixing and high-speed shear fibrillation. The mixing speed is 1200rpm-3000rpm, and the time is 5min-20min. The purpose of low-speed mixing is to initially disperse the components evenly and avoid excessively high local concentrations.
[0036] The high-speed shear fibrillation process involves rotation speeds of 4000-8000 rpm and durations of 3-30 minutes. The purpose of high-speed shearing is to keep the polyether oligomers in a liquid state and induce fibrillation of the binder through strong shear force, forming a three-dimensional fibrous network structure. Specifically, this involves two aspects: firstly, increasing the material temperature to liquefy the polyether oligomers, transforming them from a solid waxy substance into a low-viscosity fluid; or secondly, increasing the material temperature to further transform the polyether oligomers from a high-viscosity liquid at room temperature into a low-viscosity fluid; and thirdly, using strong shear force to induce fibrillation of the binder, forming a three-dimensional fibrous network structure.
[0037] Step 120: Press the dry powder mixture into an electrode film using a film-forming and thinning device.
[0038] The roller temperature of the film-forming and thinning equipment is 70℃-250℃. By controlling the roller temperature, the electrode film maintains good plasticity and film-forming properties during the pressing process. If the temperature is too low, the flowability of the dry powder mixture is insufficient, making it difficult to form a continuous and uniform film; if the temperature is too high, it may cause thermal decomposition of the binder or polyether oligomers, affecting the electrode performance.
[0039] Step 130: Composite the electrode film onto the current collector to obtain a dry electrode sheet.
[0040] The thermal bonding temperature for attaching the electrode diaphragm to the current collector is 70℃-250℃, and the pressure is 2T-30T. The purpose of thermal bonding is to tightly bond the electrode diaphragm to the current collector, forming a dry electrode sheet with good interfacial bonding strength.
[0041] In this invention, polyether oligomers act as additives, and their mechanism of action includes at least the following aspects: First, as a processing aid.
[0042] In the dry electrode fabrication process, polyether oligomers transform into low-viscosity fluids under shear heating conditions, thus entering a liquid state and providing an instantaneous liquid environment. Upon cooling, they become fixed on the particle surface. The liquid polyether oligomers are uniformly dispersed in the powder mixture, providing a lubricating medium between the active material particles and the binder particles, reducing the friction coefficient between particles, and enabling shear force to be transferred more efficiently to the PTFE particle surface. This promotes the stretching and orientation of PTFE along the shear direction, forming a three-dimensional fiber network structure. Simultaneously, the low viscosity of the polyether oligomers allows for uniform wetting of the surfaces of each component particle, avoiding uneven dispersion caused by particle agglomeration during dry powder mixing. Therefore, the mechanical integrity of the electrode film and the continuity of the electron conduction network are significantly improved.
[0043] Second, it serves as an electronic barrier.
[0044] Polyether oligomers are in a liquid state during shearing and can uniformly coat the surface of active material particles and PTFE particles to form an in-situ coated isolation layer. This isolation layer can block the migration path of electrons to PTFE and inhibit the reduction and decomposition of PTFE, thereby improving the structural stability and electrochemical stability of the electrode.
[0045] Third, it can be used as an SEI film-forming additive.
[0046] Polyether oligomers contain etheroxy groups (-O-) on their molecular chains. During the initial charge-discharge cycle of the battery, these etheroxy groups can participate in the solvation structure of sodium ions, entering the solvation sheath layer and partially replacing the original solvent molecules, thereby regulating the solvation environment of sodium ions. The regulated solvation structure preferentially undergoes reductive decomposition over the electrolyte solvent at low negative electrode potentials. Its decomposition products serve as nucleation sites, participating in the construction of the SEI film and inducing the formation of a dense and stable SEI film. This SEI film effectively passivates the negative electrode interface, inhibiting the continuous decomposition of the electrolyte and the continuous consumption of active sodium, thus significantly improving the initial coulombic efficiency and cycle life of sodium-ion batteries.
[0047] In summary, by introducing a single polyether oligomer, this invention simultaneously achieves the triple functions of processing aid, electron barrier, and SEI film-forming additive in the dry electrode preparation process, thereby synergistically improving the overall performance of the dry electrode from both the perspectives of processing performance and interfacial stability.
[0048] The preparation method provided by this invention does not involve the addition of any organic solvents throughout the entire process, and is fully compatible with the solvent-free process system of dry electrode. It has the advantages of short process, low energy consumption, low cost, and easy industrial production.
[0049] To better understand the technical solutions provided by this invention, the following examples illustrate the dry electrode composition, dry electrode sheet and its preparation method, and the characteristics of the battery.
[0050] Example 1 This embodiment 1 provides a method for preparing a dry electrode sheet, specifically including the following steps: (1) Mixing and shearing treatment of dry electrode composition: Commercially available hard carbon anode material, Super P conductive agent, PTFE binder and polypropylene glycol with a molecular weight of 2000 were mixed in a mass ratio of 94.5:1.5:2:2 and mixed and sheared in a dry mixing mixer under solvent-free conditions. First, the mixture was mixed at a low speed of 2250 rpm for 5 min to make the components initially dispersed evenly; then, it was sheared at a high speed of 4500 rpm for 10 min to make the PTFE fibrillated and form a dry powder mixture with a three-dimensional fiber network structure.
[0051] (2) Pressing into a film: The dry powder mixture is pressed into an electrode film using a film-forming and thinning equipment at a roller temperature of 100°C and a pressure of 5T. The designed film surface density is 9.5 mg / cm³. 2 .
[0052] (3) Thermal bonding: The electrode film is thermally bonded to both sides of the carbon-coated aluminum foil at a temperature of 100℃ and a pressure of 5T. After winding, the negative electrode sheet is rolled to achieve a compaction density of 0.98 g / cm³.3 The areal density of the electrode on both sides is 19 mg / cm³. 2 Dry electrode sheets are obtained.
[0053] The methods for testing areal density and compacted density in this application are as follows: Areal density test: Using an area of S (cm) 2 Dry-process electrode sheets, after being punched and rolled using a punching die, are weighed using an analytical balance with an accuracy of 0.0001g and recorded as m1 (g). Carbon-coated aluminum foil of the same size is punched using a punching die of the same area, and its mass is recorded as m0 (g). The areal density is calculated using the following formula: areal density (g / cm³) 2 ) = (m1-m0) / S Where S is the area of the stamping die. At least three different locations are randomly selected from each electrode sheet for sampling and testing, and the arithmetic mean is taken as the areal density value of the electrode sheet.
[0054] Compacted density: Take the dry-process electrode sheet after roller pressing, and use a micrometer to measure the total thickness of the electrode sheet at at least 10 points evenly selected on the sheet. Subtract the known current collector thickness to obtain the electrode film thickness T (cm). Measure the surface density of the electrode film using the surface density test method described above. The compacted density is calculated using the following formula: Compacted density (g / cm³) 3 = Surface density (g / cm³) 2 ) / membrane thickness (cm).
[0055] Example 2 This embodiment 2 provides a method for preparing a dry electrode sheet, the difference from embodiment 1 being that polypropylene glycol with a molecular weight of 400 is used instead of polypropylene glycol with a molecular weight of 2000. Specifically, it includes the following steps: (1) Mixing and shearing treatment of dry electrode composition: Commercially available hard carbon anode material, Super P conductive agent, PTFE binder and polypropylene glycol with a molecular weight of 400 were mixed in a mass ratio of 94.5:1.5:2:2 and mixed and sheared in a dry mixing mixer under solvent-free conditions. First, the mixture was mixed at a low speed of 2250 rpm for 5 min to make the components initially dispersed evenly; then, it was sheared at a high speed of 4500 rpm for 10 min to make the PTFE fibrillated and form a dry powder mixture with a three-dimensional network structure.
[0056] Steps (2)-(3) are the same as in Example 1.
[0057] Comparative Example 1 Comparative Example 1 provides a method for preparing a dry electrode sheet, which differs from Example 1 in that it does not add polypropylene glycol with a molecular weight of 2000. The method specifically includes the following steps: (1) Mixing and shearing treatment: Commercially available hard carbon anode material, Super P conductive agent and PTFE binder are mixed in a mass ratio of 96:2.5:1.5. Under solvent-free conditions, a dry mixing mixer is used to mix the mixture at a speed of 2250 rpm for 5 min, and then shears it at a speed of 4500 rpm for 10 min to obtain a dry powder mixture.
[0058] Steps (2)-(3) are the same as in Example 1.
[0059] Comparative Example 2 Comparative Example 2 provides a method for preparing a dry electrode sheet, which differs from Example 1 in that zinc stearate is used as an additive to replace polypropylene glycol with a molecular weight of 2000. The method specifically includes the following steps: Hard carbon anode material, Super P conductive agent, PTFE binder and zinc stearate were mixed in a mass ratio of 94.5:1.5:2:2. The mixture was first mixed at 2250 rpm for 5 minutes under solvent-free conditions using a dry mixing mixer, and then sheared at 4500 rpm for 10 minutes. The material temperature was about 95℃, resulting in a dry powder mixture.
[0060] Steps (2)-(3) are the same as in Example 1.
[0061] The performance of the dry-process electrode sheets prepared in Examples 1-2 and Comparative Examples 1-2 was tested. The test results are recorded in Table 1. The specific test methods are as follows: Resistivity test: The resistivity of the electrode was tested using the two-probe method. A 10cm circular sample after rolling was taken. 2 For the electrode, place the sample to be tested on the lower metal terminal of the resistivity meter, click to start the resistivity test, apply a pressure of 5MPa to both sides of the sample on the upper metal terminal, hold the pressure for 5s, collect 6 points for each electrode, and take the average value as the resistivity value of the electrode.
[0062] Peel strength test: Referring to GB / T 2792-2014 standard, the peel strength of the electrode sheet was tested using the 180° peel method. The prepared electrode sheet was cut into 15mm × 150mm samples. A thin steel plate with a length of 17cm and a width of 5cm was prepared. A strip of double-sided tape was attached to the center of the steel plate, ensuring that the length of the tape was greater than the test length of the sample and the same width as the electrode sheet. The tape was then flattened using a roller. The prepared electrode sheet was attached to the double-sided tape and flattened again using a roller. The steel plate with the attached electrode sheet was inserted into the lower clamp and fixed horizontally. The electrode sheet without tape was inserted into the upper clamp and fixed at a 90° angle to the electrode sheet in the lower clamp. The peel length and width, test force value, and peel speed were input to start the test, obtaining the peel strength curve and peel strength value. The test force value was 50N, and the peel speed was 25cm / min.
[0063] Electrochemical performance testing The dry-process electrode sheets prepared in Examples 1-2 and Comparative Examples 1-2 were die-cut and welded with tabs. A 9μm thick ceramic-coated polyethylene separator was used to assemble the positive electrode sheet, separator, and negative electrode sheet into a sandwich structure to form a pouch cell, which was then placed in an aluminum-plastic film casing. Electrolyte at a rate of 2 g / Ah was injected into the cell, followed by vacuum sealing. The sealed cell was then placed in an inert atmosphere glove box for 48 hours to allow the electrolyte to fully wet the electrodes and separator. After the standing period, the cell underwent formation, followed by vacuum degassing, ultimately yielding a sodium-ion pouch full battery.
[0064] First Coulomb efficiency test: The assembled sodium-ion pouch cell was placed on a charge-discharge tester and charged at a constant current rate of 0.1C to 2.5V at 25℃±2℃. The initial charge capacity was recorded. After resting for 5 minutes, it was discharged at a constant current rate of 0.1C to 0V, and the initial discharge capacity was recorded. The initial coulombic efficiency was calculated using the following formula: First coulombic efficiency (%) = First discharge capacity (mAh) / First charge capacity (mAh) × 100%.
[0065] Capacity retention rate: The assembled pouch cells were placed in a charge-discharge tester and subjected to constant current charge-discharge tests at 0.5C / 0.5C rates. The discharge capacity of each cycle was recorded, and the capacity retention rate was calculated. The test temperature was 25℃±2℃, and the voltage window was 0V-2.5V. The 200-cycle capacity retention rate (%) was calculated using the following formula: 200-week capacity retention (%) = discharge capacity in week 200 / discharge capacity in week 1 × 100%.
[0066] Table 1 As can be seen from the data in Table 1, there are significant differences between Examples 1-2 and Comparative Examples 1-2 in terms of compaction density, resistivity, peel strength, initial coulombic efficiency, and 200-week capacity retention.
[0067] The compaction densities of Examples 1 and 2 were higher than those of Comparative Examples 1 and 2, indicating that the addition of polyether oligomers helps to improve the compaction density of the electrodes. This may be due to the lubricating effect of polyether oligomers during the shearing process, which makes the PTFE fibrillation more complete and the particles more compact.
[0068] In terms of resistivity, Examples 1 and 2 were significantly lower than Comparative Examples 1 and 2, indicating that the polyether oligomers improved the continuity of the electronic conduction network inside the electrode and reduced the contact resistance.
[0069] Peel strength is a key indicator for evaluating the mechanical properties of electrode sheets. Examples 1 and 2 are significantly higher than Comparative Examples 1 and 2, indicating that the introduction of polyether oligomers effectively promotes the fibrillation of PTFE and enhances the mechanical properties of the electrode sheets.
[0070] In terms of electrochemical performance, the initial coulombic efficiency of Examples 1 and 2 was significantly higher than that of Comparative Examples 1 and 2. This is because the ether oxygen groups on the polyether oligomer molecular chains can participate in the solvation structure of sodium ions during the first charge-discharge process of the battery, preferentially undergoing reduction and decomposition before the electrolyte solvent, inducing the formation of a dense and stable SEI film on the negative electrode surface, thereby effectively reducing irreversible capacity loss. Regarding the 200-cycle capacity retention, Examples 1 and 2 were also significantly better than Comparative Examples 1 and 2. This indicates that the polyether oligomer not only plays a film-forming role in the first cycle, but the stable SEI film induced in the first cycle can continuously inhibit the decomposition of the electrolyte and the consumption of active sodium during long-term cycling, delaying capacity decay. Simultaneously, the physical barrier layer formed by the polyether oligomer uniformly coating the particle surface during shearing continuously inhibits the reduction and decomposition of PTFE during long-term cycling, maintaining the integrity of the electrode structure and the stability of the conductive network. These synergistic effects result in the significantly better cycle stability of Examples 1-2 compared to Comparative Examples 1-2.
[0071] Comparing Examples 1 and 2, it is evident that polypropylene glycol with a molecular weight of 2000 outperforms polypropylene glycol with a molecular weight of 400 in terms of compaction density, resistivity, peel strength, initial coulombic efficiency, and 200-cycle capacity retention. This is likely because higher molecular weight polypropylene glycol exhibits higher viscosity and better lubrication after shear heating, enabling more uniform coating of the particle surface, more effectively promoting the fibrillation of PTFE, and forming a more stable SEI film in subsequent electrochemical processes.
[0072] Comparative Example 2 used zinc stearate as an additive. Although it improved powder flowability to some extent, zinc stearate is an electrochemically inert substance. It cannot provide a liquid-phase lubrication environment during shearing to promote PTFE fibrillation, nor can it form an electron-barrier layer on the particle surface to inhibit the reductive decomposition of PTFE, and it cannot participate in the formation of the SEI film. Therefore, its performance is significantly inferior to that of Examples 1-2. In contrast, the polyether oligomer used in this invention has the triple functions of processing aid, electron barrier, and SEI film-forming additive, fundamentally solving the technical problem of balancing processing performance and interface stability in existing dry electrode processes.
[0073] In summary, by adding polyether oligomers to the dry electrode composition, this invention improves the processing and mechanical properties of the electrode, resulting in significantly higher compaction density and peel strength compared to the comparative example. On the other hand, it reduces the electrode resistivity and simultaneously significantly improves the initial coulombic efficiency and cycle stability of the sodium-ion battery.
[0074] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A composition for dry electrode fabrication, characterized in that, The composition includes an electrode active material, a conductive agent, a binder, and a polyether oligomer; The polyether oligomer contains ether oxygen groups on its molecular chain; the polyether oligomer is in a liquid state during the dry electrode preparation process, so that the polyether oligomer acts as a processing aid to promote the fibrillation of the binder during the dry electrode preparation process; and the polyether oligomer induces the formation of a solid electrolyte interface film on the negative electrode surface during battery charging and discharging.
2. The composition for dry electrode according to claim 1, characterized in that, The polyether oligomers include one or more of polypropylene glycol or polyethylene glycol; The adhesive includes: polytetrafluoroethylene; The conductive agent includes one or more of the following: acetylene black, Super P, carbon nanotubes, carbon fibers, Ketjen black, conductive graphite, or graphene. The electrode active material includes one or more of hard carbon, soft carbon, or modified hard carbon.
3. The composition for dry electrode according to claim 1, characterized in that, The electrode active material comprises 88.8 wt%-98 wt% by mass percentage, the conductive agent comprises 0.2 wt%-5 wt%, the binder comprises 0.2 wt%-10 wt%, and the polyether oligomer comprises 1 wt%-10 wt%.
4. A method for preparing a dry electrode sheet, characterized in that, The preparation method includes the following steps: Electrode active material, conductive agent, binder and polyether oligomer are mixed under solvent-free conditions and sheared to cause fibrillation of the binder, resulting in a dry powder mixture; wherein the molecular chain of the polyether oligomer contains ether oxygen groups, and the polyether oligomer is in a liquid state during shearing, acting as a processing aid to promote fibrillation of the binder; The dry powder mixture is pressed into an electrode film using a film-forming and thinning device; The electrode film is composited onto the current collector to obtain a dry electrode sheet.
5. The preparation method according to claim 4, characterized in that, The polyether oligomers include one or more of polypropylene glycol or polyethylene glycol; The adhesive includes: polytetrafluoroethylene; The conductive agent includes one or more of the following: acetylene black, Super P, carbon nanotubes, carbon fibers, Ketjen black, conductive graphite, or graphene. The electrode active material includes one or more of hard carbon, soft carbon, or modified hard carbon.
6. The preparation method according to claim 4, characterized in that, The mass ratio of the electrode active material, the conductive agent, the binder, and the polyether oligomer is 88.8-98:0.2-5:0.2-10:1-10.
7. The preparation method according to claim 4, characterized in that, The shearing process includes two stages: low-speed mixing and high-speed shear fibrillation. The low-speed mixing speed is 1200rpm-3000rpm, and the time is 5min-20min; The high-speed shear fibrillation rotation speed is 4000rpm-8000rpm, and the time is 3min-30min.
8. The preparation method according to claim 4, characterized in that, The temperature of the rollers in the film thinning equipment is 70℃-250℃; The thermal bonding temperature for bonding the electrode diaphragm to the current collector is 70℃-250℃, and the pressure is 2T-30T.
9. A dry-process electrode sheet, characterized in that, The dry electrode sheet includes a current collector and an electrode film disposed on the current collector; The electrode film is formed by fibrillation treatment of the dry electrode composition according to claims 1-3, or the dry electrode sheet is prepared by any of the preparation methods according to claims 4-8.
10. A sodium-ion battery, characterized in that, The sodium-ion battery includes a dry electrode sheet; the dry electrode sheet includes a current collector and an electrode film formed by fibrillation treatment of the dry electrode composition of claims 1-3, or includes a dry electrode sheet prepared by any of the preparation methods of claims 4-8, or includes the dry electrode sheet of claim 9.