A self-healing polymer-sulfide composite solid electrolyte, its preparation method and application, and an all-solid-state lithium battery.
By combining polyurethane-urea polymer with Li7P3S11 sulfide, a self-healing solid electrolyte is formed, which solves the problem of sulfide electrolytes requiring high pressure operation and achieves high conductivity, wide electrochemical window and long life, making it suitable for all-solid-state lithium batteries.
Patent Information
- Application Number
- CN202611469504.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-10
AI Technical Summary
Sulfide solid electrolytes require an external pressure of 50-100 MPa in the battery system to charge and discharge normally. Existing organic-inorganic physical blended composite electrolytes have weak interfacial bonding, non-healable interfacial damage, and poor long-term cycle stability.
A polyurethane-urea polymer containing dynamic disulfide bonds and multiple hydrogen bonds is composited with Li7P3S11 sulfide glass-ceramic particles. The network is rebuilt at room temperature through dynamic covalent bonds to achieve self-repair, and lithium salt is introduced into the polymer matrix to form a bicontinuous ion transport network.
It achieves stable cycling under normal pressure, with an ionic conductivity of 1 mS/cm, an electrochemical stability window of 5 V, good flexibility, strong self-healing ability, and is suitable for high-voltage cathodes. It also exhibits high long-term cycling stability and a simple preparation process.
Smart Images

Figure CN123073141A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of solid-state lithium battery materials technology, specifically to a self-healing polymer-sulfide composite solid electrolyte, its preparation method and application, and an all-solid-state lithium battery. Technical Background
[0002] With the increasing demands for energy density and safety from new energy vehicles and large-scale energy storage industries, all-solid-state lithium batteries, which replace flammable organic carbonate electrolytes with non-flammable solid electrolytes, are considered the core development direction of next-generation electrochemical energy storage technology. Among the mainstream solid electrolytes such as oxides, sulfides, halides, and polymers, sulfide systems are considered the most promising technology route for industrialization due to their combination of room-temperature ionic conductivity comparable to liquid electrolytes, low Young's modulus, and the ability to be cold-pressed without high-temperature sintering. Li7P3S, in particular, is a promising candidate. 11Sulfide-based glass-ceramic sulfide electrolytes, with room-temperature lithium-ion conductivity on the order of 1 mS / cm, and whose sulfide framework is inherently non-flammable, theoretically can simultaneously address both energy density and intrinsic safety issues. However, sulfide solid-state electrolytes have long faced a severe engineering bottleneck hindering their practical application: the battery must withstand extremely high external stacking pressures (reported in the literature to be on the order of 50–100 MPa) during charge-discharge cycles to maintain normal operation. This pressure requirement stems from the intrinsic defects of the solid-solid contact in sulfide electrolytes. First, sulfides are rigid, inorganic, brittle materials. Even after cold pressing, the contact between particles and between the electrolyte layer and the electrode remains primarily point-to-point, with the effective contact area far lower than the apparent area, resulting in significant interfacial resistance. Second, during charging and discharging, the active electrode material (especially the silicon-based anode) undergoes repeated volume expansion and contraction, generating cyclic alternating stress at the electrolyte / electrode interface. This leads to gradual interface peeling, contact point breakage, and a sharp increase in contact resistance. Third, once contact is lost, sulfide particles cannot flow back to fill the gap like liquid electrolyte; the interfacial damage is irreversible, and the capacity subsequently drops precipitously. Applying an external pressure of 50-100 MPa essentially forces interfacial contact through external mechanical constraints, a stopgap measure to address the symptoms rather than eliminating the root cause. At the battery and system level, the cost of this high-pressure requirement is unacceptable. First, the hydraulic or bolt-fitting clamps that provide and maintain 50-100 MPa pressure over long periods are bulky and account for a large proportion of volume and weight, severely offsetting the theoretical advantage of solid-state batteries in energy density, resulting in a decline in energy density at both the battery and system levels. Second, the high-voltage clamps are inherently incompatible with the flexible packaging form of pouch cells, making it difficult to use mature pouch stacking technology for sulfide systems. Third, maintaining long-term pressure stability under conditions such as vehicle vibration and temperature cycling is itself a complex engineering challenge; pressure relaxation will directly lead to battery failure. Therefore, how to free sulfide electrolytes from dependence on extreme external pressure and achieve stable cycling under normal pressure or even near-zero external pressure conditions is a key prerequisite for the practical application of sulfide all-solid-state lithium batteries.
[0003] To address the aforementioned problems, several improvement approaches have been developed in this field, but all have significant shortcomings. The first approach involves replacing sulfides with solid polymer electrolytes, using polyether matrices such as polyethylene oxide (PEO) and lithium salts to form a flexible electrolyte membrane. Polymer electrolytes possess good flexibility and interfacial adhesion, allowing them to maintain contact with the electrode under no or low pressure conditions. However, the high crystallinity of polyether segments at room temperature restricts segment movement, and lithium ion migration is highly dependent on the thermal motion of the segments, resulting in room temperature ionic conductivity generally around 10. -7 ~10 -5The S / cm range is two to three orders of magnitude lower than that of sulfides, meaning batteries using polyether polymers typically need to operate at 60°C or even higher. Furthermore, the oxidation initiation potential of polyether polymers is relatively low, making it difficult to match with high-voltage cathodes of 4V. Additionally, the pure polymer film itself is an organic material and flammable when exposed to open flame, negating any safety advantages. A second approach is to construct organic-inorganic composite solid electrolytes, dispersing sulfide particles within a polymer matrix to balance the high ionic conductivity of sulfides with the flexibility of polymers. However, existing composite solutions mostly employ physical blending, where pre-synthesized sulfide powder is simply mixed with polymers and lithium salts in a solvent to form a film. In this approach, the organic and inorganic phases are only bound by van der Waals forces or mechanical interlocking, lacking chemical bonding. The interfacial bonding is weak, and the interfacial compatibility is poor. Sulfide particles easily aggregate and settle, leading to uneven microstructure of the composite film. During cycling, due to the mismatch between the thermal expansion coefficients and mechanical responses of the two phases, microcracks easily initiate at the interface and gradually expand into macroscopic cracking and delamination, disrupting ion transport pathways. More importantly, conventional polymer matrices cannot self-heal once cracks form; interfacial damage is unidirectionally cumulative, making it difficult to guarantee the long-term cycling stability of the composite electrolyte. A third approach seeks breakthroughs in self-healing materials. In recent years, intrinsically self-healing polymers based on dynamic covalent bonds (such as disulfide metathesis, borate ester exchange, and Diels-Alder reversible addition) and dynamic non-covalent interactions (such as multiple hydrogen bonds, metal coordination, and ion interactions) have rapidly developed. These materials can rebuild their networks and restore their mechanical and functional integrity at room temperature after damage. However, directly using self-healing polymers in solid-state electrolytes still faces three major obstacles: First, most self-healing polymers lack continuous lithium-ion coordination sites in their molecular chains, resulting in insufficient ionic conductivity; second, the introduction of self-healing groups is often accompanied by a large number of polar groups, narrowing the electrochemical window and making it difficult to withstand high-voltage cathodes; third, there is a lack of effective interfacial coupling between self-healing polymers and the sulfide inorganic phase, and the two-phase interface remains a performance bottleneck. Therefore, simply physically mixing self-healing polymers with sulfides cannot simultaneously achieve high conductivity, a wide operating window, low-voltage operation, and long lifespan.
[0004] In summary, there is an urgent need in the field for a solid electrolyte and its preparation method that can simultaneously meet the following requirements: an ionic conductivity on the order of 1 mS / cm at room temperature; an electrochemical stability window on the order of 5 V to match a high-voltage cathode; sufficient flexibility to maintain close contact with the electrode under no external pressure or low pressure conditions; intrinsic self-healing ability to heal interface damage caused by electrode volume changes during cycling; and a simple, scalable preparation process that is compatible with existing battery manufacturing processes. Summary of the Invention
[0005] The primary objective of this application is to provide a method for preparing a self-healing polymer-sulfide composite solid electrolyte to solve the problem that sulfide solid electrolytes require an external pressure of 50-100 MPa in the battery system to charge and discharge normally, thus making it difficult to expand to practical applications. At the same time, it solves the problems of weak interfacial bonding, non-healing interfacial damage, and poor long-term cycle stability of existing organic-inorganic physical blend composite electrolytes.
[0006] Another object of the present invention is to provide a self-healing polymer-sulfide composite solid electrolyte.
[0007] Another object of the present invention is to provide the application of the above-mentioned self-healing polymer-sulfide composite solid electrolyte.
[0008] Another object of the present invention is to provide an all-solid-state lithium battery comprising the above-mentioned composite solid-state electrolyte.
[0009] To achieve the above objectives, this application adopts the following technical solution:
[0010] A method for preparing a self-healing polymer-sulfide composite solid electrolyte includes the following steps:
[0011] (1) Under an inert atmosphere, polyisocyanate, 2,2-dimethyl-1,3-propanediol, diethylene glycol dimethyl ether and dried polyethylene glycol are mixed and reacted to obtain polyurethane prepolymer;
[0012] (2) Add disulfide bond chain extender, 2,2-dimethyl-1,3-propanediol, and diethylene glycol dimethyl ether to the reaction system and stir to obtain a polyurethane-urea polymer solution containing disulfide bonds;
[0013] (3) Add sulfide glass ceramic particles and lithium salt to the polyurethane-urea polymer solution containing disulfide bonds obtained in step (2), stir and mix to obtain a slurry;
[0014] (4) The slurry obtained in step (3) is dripped into a mold and dried to obtain the self-healing polymer-sulfide composite solid electrolyte.
[0015] Preferably, the polyethylene glycol in step (1) has a molecular weight of 1000~4000, and the drying treatment is a vacuum drying treatment, which is carried out by stirring at 100~150 ℃ for 1~12 h.
[0016] Preferably, the temperature of the reaction in step (1) is 60~90℃ and the reaction time is 1~4h;
[0017] The polyisocyanate is hexamethylene diisocyanate, diphenylmethane diisocyanate, or terephthalic diisocyanate. The molar ratio of the isocyanate groups of the polyisocyanate to the total hydroxyl groups in the polyethylene glycol and 2,2-dimethyl-1,3-propanediol is 1.5:1 to 2.5:1. The amount of 2,2-dimethyl-1,3-propanediol used is 0.1% to 0.5% of the mass of polyethylene glycol. The inert atmosphere is argon.
[0018] Preferably, the disulfide chain extender in step (2) is 4,4'-dithiodiphenylamine, the molar ratio of the disulfide chain extender to 2,2-dimethyl-1,3-propanediol is 3:7 to 7:3, the molar ratio of the disulfide chain extender to polyisocyanate is 0.1 to 0.3:1, the reaction temperature is 30 to 50 °C, and the reaction time is 5 to 10 h.
[0019] Preferably, step (3) is carried out in an inert atmosphere glove box, wherein the water content and oxygen content of the inert atmosphere glove box are both less than 1 ppm;
[0020] The sulfide glass-ceramic is Li7P3S. 11 The average particle size is 0.5~5 μm, and the lithium salt is one or more of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, or lithium perchlorate.
[0021] The mass of the added sulfide glass-ceramic particles is 10% to 60% of the total mass of the polymer matrix and the sulfide glass-ceramic; the molar ratio of the ether oxygen unit to the lithium salt in the polyethylene glycol segment is 5:1 to 20:1.
[0022] Preferably, the drying in step (4) is vacuum drying, with a temperature of 50~70 ℃ and a time of 36~60 h.
[0023] Preferably, the mold in step (4) is a polytetrafluoroethylene mold.
[0024] A self-healing polymer-sulfide composite solid electrolyte is prepared by the above-described preparation method.
[0025] Preferably, the composite solid electrolyte comprises a polyurethane-urea polymer matrix containing disulfide bonds and Li7P3S dispersed in the polymer matrix. 11 Sulfide particles and lithium salts;
[0026] The composite solid electrolyte has an ionic conductivity ≥1.0 mS / cm, a lithium-ion transference number ≥0.80, and an electrochemical stability window ≥5.0 V at 25 °C.
[0027] An all-solid-state lithium battery includes a positive electrode, a negative electrode, and a solid electrolyte between the positive and negative electrodes, wherein the solid electrolyte is the composite solid electrolyte as described in claim 7 or 8; the negative electrode is a silicon-carbon negative electrode, and the active material of the positive electrode is a layered nickel-manganese-cobalt oxide; the all-solid-state lithium battery operates under an applied stacking pressure not exceeding 5 MPa.
[0028] Preferably, the silicon-carbon anode has a silicon content of 40% by mass, an initial reversible capacity of 1500-1600 mAh / g at a current density of 1 A / g, and a capacity retention rate of ≥70% after 100 cycles; the positive electrode active material is LiNi. 0.6 Mn 0.2 Co 0.2 O2 has a reversible capacity of 145~160 mAh / g within a voltage window of 2.8~4.3 V, a capacity retention of ≥65% after 300 cycles, and an average coulombic efficiency of ≥98.5%.
[0029] The design basis and technical content of each step proposed in this application are detailed below.
[0030] Step (1): Polyethylene glycol (PEG) serves as the source of soft segments in the polymer matrix. The ether oxygen (—C—O—C—) units on its molecular chain are coordination sites for lithium ions. Lithium ions migrate along the chain segments through coordination-discoordination between adjacent ether oxygen sites. Therefore, PEG is a key component determining the ionic conductivity of the composite electrolyte. PEG is also a highly hygroscopic material. The adsorbed water will react with isocyanate groups in subsequent steps to form urea bonds and release carbon dioxide. This consumes isocyanate, disrupts the stoichiometric ratio, and creates bubble defects within the membrane. Therefore, it must be completely removed before prepolymerization. Setting the drying temperature to 100~150 ℃ and the time to 1~12 h provides a window that balances dehydration efficiency and PEG thermal stability: below 100 ℃, water removal is slow and incomplete; above 150 ℃, the polyether segments are at risk of oxidative degradation and chain breakage under prolonged heating, and high temperatures exacerbate PEG volatilization losses. Vacuum conditions lower the boiling point of water and accelerate the diffusion and escape of water molecules from viscous melts. Cooling to 75°C after drying before adding isocyanate ensures that polyethylene glycol (PEG) is in a molten, low-viscosity state, facilitating uniform mixing with the isocyanate. This also avoids the volatilization loss of isocyanate and the exacerbation of side reactions (such as the trimerization of isocyanate into isocyanurate) that would occur with high-temperature addition. The selection of PEG molecular weight between 1000 and 4000 is based on the following: If the molecular weight is too low, the polyether soft segments are too short, resulting in insufficient mechanical strength and film-forming properties of the polymer. Furthermore, the high density of terminal hydroxyl groups per unit mass of chain segments leads to excessive crosslinking density and restricted chain movement. If the molecular weight is too high, PEG is prone to crystallization, reducing chain mobility at room temperature and weakening lithium-ion migration. Additionally, excessively high melt viscosity is detrimental to mass transfer and subsequent compounding. A molecular weight of approximately 2000 strikes a balance between soft segment length, chain mobility, and film-forming properties, making it the optimal choice.
[0031] Hexamethylene diisocyanate (HDI), an aliphatic diisocyanate, has two -NCO groups that react with the terminal hydroxyl groups of polyethylene glycol (PEG) to form urethane bonds (-NH-CO-O-). Coupling the two PEG segments while retaining the unreacted -NCO groups at both ends yields a polyurethane prepolymer with terminal isocyanate groups. The reason for choosing aliphatic hexamethylene diisocyanate over aromatic diisocyanate is that in the urethane bonds formed by aliphatic isocyanates, the lone pair electrons on the nitrogen atom are not conjugated with the aromatic ring, resulting in significantly better oxidative stability than aromatic systems, which is beneficial for broadening the electrochemical stability window of the composite electrolyte. Simultaneously, the flexible methylene sequence of hexamethylene can inhibit excessive aggregation of hard segments, maintaining good flexibility in the polymer matrix, thus ensuring close adhesion to the electrode even under low-pressure conditions. The reasons for choosing diethylene glycol dimethyl ether as the organic solvent are as follows: its molecule contains an ether oxygen structure, which provides excellent solubility for polyethylene glycol, isocyanates, and subsequently added chain extenders and lithium salts; its high boiling point allows for prolonged reflux at a prepolymerization temperature of 75 °C without significant volatilization; and it is an aprotic polar solvent, free of active hydrogen, and will not compete with isocyanate groups for reaction. The reaction is carried out under an argon atmosphere to isolate moisture from the air, at a temperature of 75 °C for 2 hours, ensuring sufficient prepolymerization without triggering significant side reactions. 2,2-Dimethyl-1,3-propanediol (neopentyl glycol) is introduced in this step as a small-molecule diol regulator. Its two primary hydroxyl groups can participate in prepolymerization, and its geminal dimethyl structure can introduce side groups between the polyether soft segments, disrupting the regular stacking of the chain, inhibiting crystallization, and thus improving the room-temperature chain segment mobility.
[0032] Step (2): The chain extension reaction is the core step in constructing the polyurethane-urea backbone and introducing self-healing functional groups. The chain extender solution is added dropwise after the system is cooled to 40 °C. The reason for this is that the chain extender 4,4'-dithiodiphenylamine is an aromatic primary diamine. Its reaction rate with isocyanate groups to form urea bonds (—NH—CO—NH—) is much higher than the reaction rate between alcohol hydroxyl groups and isocyanates. If it is added rapidly at 75 °C, the reaction will be exothermic and the local concentration will be too high, which will easily cause burst polymerization, gelation or even uncontrolled crosslinking, resulting in a very wide molecular weight distribution and deterioration of film-forming properties. Cooling to 40 °C and adding it dropwise can make the chain extension reaction proceed uniformly at a controllable rate, and obtain a linear polyurethane-urea with a narrow molecular weight distribution. The aromatic disulfide bonds (Ar—S—S—Ar) in the 4,4'-dithiodiphenylamine molecule are the chemical basis for the self-healing function of this composite electrolyte. The disulfide bonds have low bond energies, allowing for reversible metathesis exchange reactions at room temperature. When microcracks appear in the composite membrane due to volume changes in the silicon-carbon anode or external stress, the disulfide bonds on both sides of the crack can recombine across the crack surface through exchange reactions, healing the crack and rebuilding the network, thereby restoring the membrane's integrity and ion transport pathways. Simultaneously, disulfide bond exchange is a dynamic covalent process, and its reversibility allows the polymer network to release stress through chain rearrangement under stress, endowing the membrane with excellent stress buffering capabilities. In this step, 2,2-dimethyl-1,3-propanediol is added as a co-chain extender. Combined with the diamine chain extender, it can control the regularity and hydrogen bond density of the hard segments: the urea bonds introduced by the diamine chain extender provide bidentate hydrogen bonds, forming strong physical crosslinking points; the urethane bonds introduced by the glycol chain extender provide relatively weaker hydrogen bonds. The ratio of the two determines the cohesive energy of the hard segments and the mechanical response of the material. The reaction time was 8 h, and the infrared spectrum at 2270 cm⁻¹ was used as the reference value. - The complete disappearance of the characteristic absorption peak of -NCO at ¹ is used as the reaction endpoint criterion to ensure that the isocyanate groups are completely consumed, thus avoiding uncontrollable side reactions when the residual highly active -NCO comes into contact with lithium salts or sulfides in the future.
[0033] Step (3): Li7P3S 11 Sulfide glass-ceramic particles and lithium salts are introduced into a polyurethane-urea polymer solution to form a functional filler and ion source for a composite electrolyte. Li7P3S 11 The introduction of sulfides serves three functions: First, as fast ion conductors, they provide ion transport pathways in the composite membrane that are far superior to those of the polymer phase, thereby increasing the room-temperature ionic conductivity of the composite electrolyte to 10. -Firstly, its particle surface is rich in sulfur vacancies and unsaturated coordinated phosphorus sites, which can strongly adsorb lithium salt anions, promote lithium salt dissociation, increase the concentration of free lithium ions, and thus enhance the lithium ion transport number. Secondly, its surface can undergo nucleophilic addition and coordination with nitrogen-containing active sites such as amino and urea groups on the polyurethane-urea molecular chain, forming chemical bonds between inorganic particles and the organic matrix rather than simple mechanical mixing. This fundamentally eliminates interfacial voids, inhibits particle aggregation, and obtains a uniform bicontinuous ion transport network. Li7P3S 11 The mass fraction of sulfides is expressed as a percentage of the polymer matrix and Li7P3S. 11 The total mass fraction of sulfides is preferably 50%, which is the optimal value for considering both ionic conductivity and mechanical properties. If the mass fraction is too low, the inorganic fast ionic phase is insufficient to form interconnected pathways, resulting in limited improvement in conductivity. If the mass fraction is too high, the continuity of the polymer phase is disrupted, leading to film embrittlement and decreased flexibility, which in turn weakens interfacial contact and self-healing capabilities under low-pressure conditions. Lithium bis(fluorosulfonyl)imide (LiFSI) is chosen as the lithium salt because its anionic charge is highly delocalized, its association energy with lithium ions is low, its dissociation degree is high, and its film-forming properties and electrochemical stability are superior to conventional lithium salts such as lithium hexafluorophosphate. The molar ratio of ether oxygen units to lithium salt is set at 10:1, representing a balance between the number of ion carriers and the chain segment mobility. If the lithium salt ratio is too low, the carrier concentration is insufficient; if the lithium salt ratio is too high, excess lithium ions will coordinate and crosslink with the ether oxygen, which will restrict chain segment mobility, reduce conductivity, and narrow the electrochemical window due to anion enrichment. The necessity of performing the composite in an inert atmosphere glove box with both water and oxygen content below 1 ppm lies in: Li7P3S 11 Sulfides are extremely sensitive to trace amounts of water, hydrolyzing upon contact with water to release hydrogen sulfide and generate oxygen-containing impurities, leading to a sharp decrease in ionic conductivity; lithium salt LiFSI also exhibits strong hygroscopicity. Thorough stirring for 24 hours allows for the full dispersion of sulfide particles and the complete dissolution of lithium salt in the high-viscosity system, facilitating interaction with the polymer chains and resulting in a macroscopically uniform and microscopically stable slurry.
[0034] Step (4): The solution casting method in a polytetrafluoroethylene (PTFE) mold is chosen based on the simplicity and scalability of the process. PTFE has extremely low surface energy, and the dried film can be completely self-peeled, avoiding contamination from the release agent. The drop casting method does not require hot pressing or rolling equipment and can be completed directly in an inert atmosphere, making it compatible with existing electrode coating processes and easy to scale up to continuous coating. The drying temperature is set at 60 ℃ and the time is set at 48 h, which is a balance between the thoroughness of solvent removal and the integrity of the film structure. Diethylene glycol dimethyl ether has a high boiling point. If the drying temperature is too low or the time is too short, the residual solvent will plasticize the polymer segments and participate in the side reactions at the electrode interface, and the residual solvent itself poses a safety hazard. If the drying temperature is too high, the solvent will boil violently, forming pores and pinhole defects in the film, and the high temperature may cause premature exchange of disulfide bonds and thermal oxidation of the polymer. Long-term vacuum drying at 60 °C allows the solvent to be removed gradually and evenly, resulting in a dense, defect-free self-supporting composite electrolyte membrane. The membrane thickness is preferably controlled between 20 and 100 μm, balancing ion transport distance and mechanical strength.
[0035] Compared with the prior art, the beneficial effects of this application include:
[0036] First, this application introduces a polyurethane-urea polymer containing dynamic disulfide bonds and multiple hydrogen bonds into the sulfide electrolyte, enabling the composite electrolyte to cycle stably under normal pressure, fundamentally eliminating the dependence of the sulfide system on external pressures in the 50-100 MPa range. The mechanism is as follows: the polyurethane-urea elastic matrix deforms under normal pressure and fills the microscopic undulations on the electrode surface, transforming solid-solid point contact into surface contact, significantly reducing interfacial impedance; when the silicon-carbon anode undergoes volume expansion and contraction during charging and discharging, generating cyclic alternating stress at the interface, the elastic deformation of the polymer network absorbs and buffers this stress, preventing interfacial delamination; even if microcracks initiate due to stress concentration, the room-temperature metathesis exchange of disulfide bonds and the reversible reconstruction of hydrogen bonds allow the cracks to self-heal during the cycle intervals, preventing unidirectional accumulation of interfacial damage. This is the core technical effect that distinguishes this application from existing technologies.
[0037] Second, this application introduces Li7P3S into the polyurethane-urea network. 11 The sulfide glass-ceramic particles enable the composite electrolyte to achieve an ionic conductivity of 1.24 mS / cm at room temperature, reaching 10. -3 The S / cm ratio is on the order of magnitude, more than two orders of magnitude higher than that of pure polymer electrolytes. Li7P3S 11The fast ion conduction characteristics of sulfides and the segment migration of polyether soft segments form a dual continuous transport network, enabling lithium ions to migrate synergistically along multiple channels from the polymer phase to the sulfide phase to the two-phase interface. The lithium ion transference number of the composite electrolyte reaches 0.84, which is much higher than that of conventional polymer electrolytes, indicating that anion migration is effectively suppressed, which is beneficial to reducing concentration polarization and improving rate performance.
[0038] Third, this application uses aliphatic hexamethylene diisocyanate to construct the polyurethane-urea backbone, enabling the composite electrolyte to achieve an electrochemical stability window of 5.1 V, which is compatible with high-voltage layered oxide cathodes such as NMC622. The aliphatic carbamate and urea bonds do not contain easily oxidized aromatic conjugated structures, and their highest occupied molecular orbital energy levels are relatively low, resulting in strong oxidation resistance; simultaneously, Li7P3S... 11 The strong adsorption of FSI⁻ anions on the surface of sulfide particles reduces the oxidative decomposition of free anions at the positive electrode interface. The synergy between the two enables the composite electrolyte to remain stable in a potential range of 2.8~4.3 V and even wider.
[0039] Fourth, the composite electrolyte of this application exhibits excellent compatibility with silicon-carbon anodes. In a half-cell assembled with a silicon-carbon anode containing 40% silicon, the initial capacity reaches 1600 mAh / g at room temperature and pressure and a current density of 1 A / g. After 100 cycles, the capacity still remains at 1200 mAh / g, with a capacity retention of 75%. This effect is attributed to the synergistic effect of the flexible buffering and self-healing capabilities of the polymer matrix: the silicon-carbon anode undergoes a huge volume expansion during lithium intercalation, and the polymer network can deform accordingly without breaking. The dynamic characteristics of disulfide bonds and hydrogen bonds allow the network to recover its integrity after repeated deformation, thereby maintaining the long-lasting contact and continuous ion / electrolyte pathways at the electrode / electrolyte interface.
[0040] Fifth, the composite electrolyte of this application can be simultaneously matched with a high-voltage ternary cathode and achieve long-term cycling. In a full cell with NMC622 as the cathode, the reversible capacity reaches 156 mAh / g at room temperature and pressure and a voltage window of 2.8~4.3 V. After 300 cycles, the capacity retention rate is 75%, and the average coulombic efficiency is 99.2%, indicating that the interface between the composite electrolyte and the cathode remains stable during long-term cycling and side reactions are effectively suppressed.
[0041] Sixth, the composite electrolyte of this application has a high proportion of inorganic sulfide phase and a correspondingly lower proportion of organic combustible components. Furthermore, the inorganic phase and the polymer matrix form a dense structure through chemical bonding, which makes the flammability of the membrane material significantly lower than that of a pure polymer electrolyte membrane. Combined with the fact that the solid system itself does not have free-flowing organic liquid, the intrinsic safety of the battery is improved.
[0042] Seventh, the preparation method of this application is completed entirely in a solution system, without the need for high-temperature sintering, high-pressure molding equipment, or ball milling. The process steps are simple and the conditions are mild. The drop casting film formation method is easy to scale up to continuous coating and roll-to-roll processes. It is compatible with existing lithium-ion battery manufacturing equipment and has good prospects for industrialization. Attached Figure Description
[0043] Figure 1 Example 1 of this application shows the FTIR curves of a self-healing polymer-LPS sulfide composite solid electrolyte and the polymer electrolyte and LPS sulfide electrolyte.
[0044] Figure 2 The electrochemical performance of the electrolyte prepared in Example 1 of this application in a silicon-carbon anode is shown.
[0045] Figure 3 The electrochemical performance of the electrolyte prepared in Example 1 of this application in the NMC622 cathode is shown. Detailed Implementation
[0046] The implementation schemes of this application will be described in detail below with reference to specific embodiments. However, those skilled in the art will understand that the following embodiments are only for illustrating this application and should not be regarded as limiting the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments used that do not specify the manufacturer are all conventional products that can be purchased commercially.
[0047] In the examples, polyethylene glycol (molecular weight 1000~4000), hexamethylene diisocyanate, 2,2-dimethyl-1,3-propanediol, 4,4'-dithiodiphenylamine, diethylene glycol dimethyl ether (purity ≥99%, dehydrated by molecular sieve, water content less than 50 ppm), lithium bis(fluorosulfonyl)imide (LiFSI, purity ≥99.5%), and Li7P3S were used. 11 Sulfide glass-ceramic powder (self-made, average particle size approximately 2 μm). All operations involving sulfides and lithium salts were performed in a high-purity argon glove box with water and oxygen content both below 1 ppm.
[0048] Example 1
[0049] This embodiment provides a preferred preparation method for a self-healing polymer-sulfide composite solid electrolyte, the preparation method of which is as follows.
[0050] 4.0 g (approximately 2.0 mmol) of polyethylene glycol (PEG, molecular weight approximately 2000) was placed in a dry three-necked flask and connected to a vacuum-argon double-row tube. The flask was magnetically stirred and dried at approximately 10 Pa and 120 °C for 4 h to completely remove the adsorbed moisture from the polyethylene glycol. After drying, stirring was maintained, and the system temperature was lowered to 75 °C. Under argon protection, 0.66 g of hexamethylene diisocyanate (HDI) and 4 mg of 2,2-dimethyl-1,3-propanediol (NPG) (0.1% of the polyethylene glycol mass) were added to the flask, along with 30 mL of dehydrated diethylene glycol dimethyl ether. The mixture was stirred and reacted at 75 °C under positive argon pressure for 2 h to obtain a polyurethane prepolymer solution with terminal isocyanate groups. The three-necked flask reactor was then cooled to 40 °C. 10 mL of a pre-prepared chain extender solution, consisting of diethylene glycol dimethyl ether containing 0.7 mmol (approximately 0.174 g) of 4,4'-dithiodiphenylamine (DTDA) and 0.3 mmol (approximately 0.031 g) of 2,2-dimethyl-1,3-propanediol (NPG), was added dropwise to the reactor over approximately 30 min using a constant-pressure dropping funnel. After the addition was complete, the reactor was stirred at 40 °C for 8 h. Samples were taken every 2 h during the reaction for Fourier transform infrared spectroscopy (FTIR) up to 2270 cm⁻¹. - The reaction was stopped when the characteristic absorption peak of the isocyanate group (-NCO) at ¹ completely disappeared, yielding a diethylene glycol dimethyl ether solution of a polyurethane-urea polymer (denoted as PUU-SS) containing disulfide bonds. The theoretical yield of the polymer matrix was approximately 4.87 g.
[0051] The polymer solution was transferred to an argon glove box with both water and oxygen content below 1 ppm, and Li7P3S was added to it. 11 4.87 g of sulfide glass-ceramic particles (based on their proportion in the polymer matrix and Li7P3S) 11A 50% sulfide by mass fraction and 1.70 g of lithium difluorosulfonyl imide (LiFSI) (calculated based on a 10:1 molar ratio of ether oxygen units to lithium salt in polyethylene glycol segments [EO]:[LiFSI], 2.0 mmol of polyethylene glycol contains approximately 90.8 mmol of ether oxygen units, corresponding to approximately 9.08 mmol of LiFSI) were magnetically stirred in a glove box at room temperature for 24 h to obtain a uniformly dispersed grayish-white slurry. The obtained slurry was drop-cast into a clean polytetrafluoroethylene mold, allowed to stand horizontally for 30 min to level the slurry and release air bubbles, and then transferred to a vacuum drying oven and dried at 60 ℃ under vacuum for 48 h to completely remove diethylene glycol dimethyl ether. After drying, the mold was allowed to cool to room temperature, and the membrane was completely peeled off from the polytetrafluoroethylene mold to obtain a self-supporting polymer-sulfide composite solid electrolyte membrane with a thickness of approximately 40 μm, denoted as PUU-SS-50%LPS. The infrared spectrum is shown in [reference needed]. Figure 1 .
[0052] The obtained composite electrolyte membrane was systematically characterized and subjected to electrochemical tests. AC impedance spectroscopy (stainless steel blocking electrode, frequency range 10) was used. 6 ~10 -1 The ionic conductivity at 25 °C was measured to be 1.24 mS / cm (Hz, amplitude 10 mV). Using DC polarization (lithium / electrolyte / lithium symmetric cell, polarization potential 18 mV) combined with impedance calculations before and after polarization, the lithium-ion transference number was determined to be 0.84. The electrochemical stability window reached 5.1 V using linear scanning voltammetry (stainless steel working electrode, lithium counter electrode, scan rate 1 mV / s). A silicon-carbon anode half-cell was assembled using the obtained composite electrolyte membrane: the anode used a silicon-carbon composite material with a silicon content of 40% (silicon-carbon active material, conductive agent, and binder were coated on copper foil in a mass ratio of 8:1:1, with an areal loading of approximately 1.5 mg / cm²). 2 The counter electrode is a lithium metal sheet, and a PUU-SS-50%LPS film is sandwiched between the two electrodes. The coin cell is assembled under ambient temperature and pressure conditions without applying additional stacking pressure. At a current density of 1 A / g, the initial reversible capacity of this battery is 1600 mAh / g, and after 100 cycles, the capacity is retained at 1200 mAh / g, representing a capacity retention of 75%. (See attached image.) Figure 2 A ternary cathode full cell was assembled using the obtained composite electrolyte membrane: the cathode active material was LNMC622, and NMC622, conductive carbon black, and polyvinylidene fluoride were coated on aluminum foil at a mass ratio of 94:3:3, with an areal loading of approximately 8 mg / cm³. 2 The negative electrode is the same as above. Tested at room temperature and pressure within a voltage window of 2.8–4.3 V, the battery's reversible capacity reaches 156 mAh / g, with a capacity retention of 75% after 300 cycles and an average coulombic efficiency of 99.2%. (See attached image.) Figure 3 .
[0053] Example 2
[0054] This embodiment provides a method for preparing a self-healing polymer-sulfide composite solid electrolyte to investigate its applicability under conditions of low molecular weight polyethylene glycol and low sulfide content. The preparation method is as follows: 4.0 g of polyethylene glycol (molecular weight approximately 1000) was placed in a three-necked flask and dried magnetically at 100 °C and a vacuum of approximately 10 Pa for 12 h. The temperature was then lowered to 75 °C. 0.66 g of hexamethylene diisocyanate, 4 mg of 2,2-dimethyl-1,3-propanediol, and 30 mL of diethylene glycol dimethyl ether were added. The mixture was reacted at 75 °C for 2 h under argon protection to obtain a polyurethane prepolymer. The temperature was then lowered to 40 °C, and 10 mL of a diethylene glycol dimethyl ether solution containing 0.7 mmol of 4,4'-dithiodiphenylamine and 0.3 mmol of 2,2-dimethyl-1,3-propanediol was added dropwise. The mixture was stirred at 40 °C for 8 h until the solution reached 2270 cm⁻¹. - The NCO peak disappears at position ¹. Li7P3S is added to the polymer solution in a glove box. 11 Sulfide particles (based on their proportion in the polymer matrix and Li7P3S) 11 The total mass fraction of sulfides was 40%, and the amount added was adjusted accordingly. LiFSI was stirred for 24 h and then drop-cast into a polytetrafluoroethylene mold. The mixture was then vacuum dried at 60 °C for 48 h to obtain a composite electrolyte membrane.
[0055] Test results show that the membrane has an ionic conductivity of 0.96 mS / cm at 25 °C, a lithium-ion transference number of 0.79, and an electrochemical window of 4.9 V. When matched with a silicon-carbon anode with 40% silicon content, the initial capacity is 1520 mAh / g at room temperature and pressure, and 1 A / g, with a capacity retention of 1080 mAh / g after 100 cycles, representing 71% of the capacity. When matched with an NMC622 cathode, the capacity is 148 mAh / g within the 2.8–4.3 V window, with a capacity retention of 68% after 300 cycles and an average coulombic efficiency of 98.6%. The performance is somewhat lower than in Example 1 because the soft segments formed by the low molecular weight polyethylene glycol are shorter, the density of ether oxygen coordination sites per unit volume deviates from the optimal value for chain segment mobility, and the reduced sulfide content decreases the connectivity of the inorganic fast ion phase. This example demonstrates that even under conditions of lower molecular weight and lower sulfide content, the method of this application can still obtain a composite electrolyte with good overall performance.
[0056] Example 3
[0057] This embodiment provides a method for preparing a self-healing polymer-sulfide composite solid electrolyte to investigate its applicability under conditions of high molecular weight polyethylene glycol and high sulfide content. The preparation method is as follows: 4.0 g of polyethylene glycol (molecular weight approximately 4000) was dried magnetically at 150 °C under vacuum for 1 h, and then cooled to 75 °C. 0.66 g of hexamethylene diisocyanate, 4 mg of 2,2-dimethyl-1,3-propanediol, and 30 mL of diethylene glycol dimethyl ether were added. The mixture was reacted at 75 °C for 2 h under argon protection to obtain a polyurethane prepolymer. The mixture was then cooled to 40 °C, and 10 mL of a diethylene glycol dimethyl ether solution containing 0.7 mmol of 4,4'-dithiodiphenylamine and 0.3 mmol of 2,2-dimethyl-1,3-propanediol was added dropwise. The mixture was stirred at 40 °C for 8 h until the -NCO peak disappeared. Li7P3S was added to the polymer solution in a glove box. 11 Sulfide particles (60% by mass) and LiFSI ([EO]:[LiFSI]=10:1) were stirred for 24 h and then drop-cast into a polytetrafluoroethylene mold. The mixture was then vacuum dried at 60 °C for 48 h to obtain a composite electrolyte membrane.
[0058] Test results show that the membrane has an ionic conductivity of 1.12 mS / cm at 25 °C, a lithium-ion transference number of 0.81, and an electrochemical window of 5.0 V. When matched with a silicon-carbon anode with 40% silicon content, the initial capacity is 1580 mAh / g at room temperature and pressure, and 1 A / g, with a capacity retention of 1150 mAh / g after 100 cycles, representing 72.8% of the capacity. When matched with an NMC622 cathode, the capacity is 154 mAh / g, with a capacity retention of 71% after 300 cycles and an average coulombic efficiency of 98.9%. Although the ionic conductivity of this embodiment is higher than that of Example 1, the cycle retention is slightly lower. This is because when the sulfide content is increased to 60%, the polymer continuous phase is diluted, the membrane's elongation at break and flexibility decrease, and the stress buffering and self-healing capabilities are correspondingly weakened, leading to gradual interface deterioration during long cycles. This embodiment confirms that there is an optimal range for sulfide content, and higher is not necessarily better.
[0059] Example 4
[0060] This embodiment provides a method for preparing a self-healing polymer-sulfide composite solid electrolyte to investigate its applicability under conditions with a high lithium salt ratio. The preparation method is as follows: 4.0 g of polyethylene glycol (molecular weight approximately 2000) was dried magnetically at 120 °C under vacuum for 4 h, and then cooled to 75 °C. 0.66 g of hexamethylene diisocyanate, 4 mg of 2,2-dimethyl-1,3-propanediol, and 30 mL of diethylene glycol dimethyl ether were added. The mixture was reacted at 75 °C for 2 h under argon protection to obtain a polyurethane prepolymer. The temperature was lowered to 40 °C, and 10 mL of a diethylene glycol dimethyl ether solution containing 0.7 mmol of 4,4'-dithiodiphenylamine and 0.3 mmol of 2,2-dimethyl-1,3-propanediol was added dropwise. The mixture was stirred at 40 °C for 12 h until the -NCO peak disappeared. Li7P3S was added to the polymer solution in a glove box. 11 Sulfide particles (50% by mass) and LiFSI ([EO]:[LiFSI]=8:1) were stirred for 24 h and then drop-cast into a polytetrafluoroethylene mold. The mixture was then vacuum dried at 60 °C for 48 h to obtain a composite electrolyte membrane.
[0061] Test results show that the membrane has an ionic conductivity of 1.33 mS / cm at 25 °C, a lithium-ion transference number of 0.80, and an electrochemical window of 4.8 V. When matched with a silicon-carbon anode with 40% silicon content, the initial capacity is 1560 mAh / g at room temperature and pressure, and 1 A / g, with a capacity of 1120 mAh / g after 100 cycles and a retention rate of 71.8%. When matched with an NMC622 cathode, the capacity is 152 mAh / g, with a capacity retention rate of 70% after 300 cycles and an average coulombic efficiency of 98.8%. Compared with Example 1, increasing the lithium salt ratio increases the carrier concentration and slightly improves the conductivity, but the excessive lithium ions' coordination crosslinking of ether oxygen restricts chain movement, resulting in a decrease in the lithium-ion transference number. Simultaneously, the increased free anion concentration advances the oxidation decomposition initiation potential, narrowing the electrochemical window to 4.8 V. This example demonstrates that [EO]:[LiFSI]=10:1 is the optimal overall value.
[0062] Example 5
[0063] This embodiment provides a method for preparing a self-healing polymer-sulfide composite solid electrolyte to investigate its applicability under conditions of lower lithium salt ratio and extended film-forming drying time. The preparation method is as follows: 4.0 g of polyethylene glycol (molecular weight approximately 2000) was magnetically stirred and dried at 130 °C under vacuum for 3 h, then cooled to 75 °C. 0.66 g of hexamethylene diisocyanate, 4 mg of 2,2-dimethyl-1,3-propanediol, and 30 mL of diethylene glycol dimethyl ether were added. The mixture was reacted at 75 °C for 2 h under argon protection to obtain a polyurethane prepolymer. The temperature was lowered to 40 °C, and 10 mL of a diethylene glycol dimethyl ether solution containing 0.7 mmol of 4,4'-dithiodiphenylamine and 0.3 mmol of 2,2-dimethyl-1,3-propanediol was added dropwise. The mixture was stirred at 40 °C for 8 h until the -NCO peak disappeared. Li7P3S was added to the polymer solution in a glove box. 11 Sulfide particles (55% by mass) and LiFSI ([EO]:[LiFSI]=15:1) were stirred for 24 h and then drop-cast into a polytetrafluoroethylene mold. The mixture was then vacuum-dried at 60 ℃ for 72 h to obtain a composite electrolyte membrane. Test results showed that the membrane had an ionic conductivity of 1.15 mS / cm at 25 ℃, a lithium-ion transference number of 0.82, and an electrochemical window of 5.05 V. When matched with a silicon-carbon anode with 40% silicon content, the initial capacity was 1590 mAh / g at room temperature and pressure, and 1 A / g. After 100 cycles, the capacity was 1180 mAh / g, with a retention rate of 74.2%. When matched with an NMC622 cathode, the capacity was 155 mAh / g, with a capacity retention rate of 73% after 300 cycles and an average coulombic efficiency of 99.0%. The performance of this embodiment is close to that of Example 1 but slightly lower. The lower lithium salt ratio results in insufficient carrier concentration and decreased conductivity. Although extending the drying time to 72 h further reduces the residual solvent, the marginal benefit is limited, indicating that 60 ℃ for 48 h is sufficient to achieve complete solvent removal. The following comparative examples 1 to 4 verify the irreplaceability of each key technical feature in this application. Except for explicitly stated differences, the operating conditions (glove box water and oxygen content, raw material batch, equipment model, electrode formulation, and testing conditions) of each comparative example are strictly consistent with those of Example 1 to eliminate interference from non-target variables.
[0064] Comparative Example 1
[0065] This comparative example is used to verify the necessity of introducing a disulfide-bonded polyurethane-urea polymer into a sulfide electrolyte to eliminate dependence on high applied pressure. This comparative example does not introduce any polymer or lithium salt; it directly incorporates Li7P3S... 11Sulfide glass-ceramic powder was uniaxially cold-pressed into sheets at 360 MPa to obtain pure sulfide electrolyte sheets. Using these sheets as the electrolyte, a battery was assembled with the same silicon-carbon anode (40% silicon content) and lithium metal counter electrode as in Example 1. The battery was tested at 1 A / g under ambient temperature and pressure with only a stacking pressure of approximately 0.5 MPa. The results showed that the battery's initial discharge capacity was only 420 mAh / g, and the capacity rapidly decreased to below 80 mAh / g within 20 cycles. The coulombic efficiency fluctuated drastically between 85% and 95%, failing to maintain stable cycling. AC impedance spectroscopy showed that the interfacial impedance increased rapidly with cycling, indicating that the electrolyte / electrode interface continuously degraded and failed under the influence of the silicon-carbon anode's volume change. As a control, when an external pressure of 50 MPa was applied to this battery, its initial capacity recovered to approximately 1450 mAh / g and could maintain several dozen cycles, but the capacity immediately decreased again once the external pressure was removed. This comparative example confirms the rigid dependence of pure sulfide electrolytes on external pressures in the range of 50-100 MPa. It also demonstrates that the technical effect of achieving stable cycling under normal pressure by introducing a self-healing polymer matrix is not inherent to the sulfide itself, but rather is imparted by the composite structure of this application.
[0066] Comparative Example 2
[0067] This comparative example was used to verify the necessity of introducing the disulfide bond-containing chain extender 4,4'-dithiodiphenylamine and constructing dynamic disulfide bonds in the polymer network. Except for completely replacing 0.7 mmol of the chain extender 4,4'-dithiodiphenylamine with an equivalent amount of 2,2-dimethyl-1,3-propanediol (i.e., adjusting the total amount of co-chain extender to 1.0 mmol, resulting in a polymer network free of disulfide bonds), the raw materials, proportions, process steps, and post-treatment conditions were completely consistent with Example 1. The resulting composite electrolyte membrane was designated PUU-50%LPS. Test results showed that the membrane had an ionic conductivity of 1.18 mS / cm at 25 °C, a lithium-ion transference number of 0.83, and an electrochemical window of 5.0 V. These three intrinsic parameters were close to those of Example 1, indicating that the introduction of disulfide bonds did not impair ion conduction or electrochemical stability. However, significant differences exist in battery performance: When matched with a silicon-carbon anode containing 40% silicon, the initial capacity at room temperature and pressure (1 A / g) was 1590 mAh / g, but after 100 cycles, the capacity was only 890 mAh / g, with a retention rate of 56%, significantly lower than the 75% in Example 1; when matched with an NMC622 cathode, the capacity was 154 mAh / g, but after 300 cycles, the capacity retention rate was only 58%, with an average coulombic efficiency of 97.5%. Disassembly of the cycled battery revealed obvious microcracks and localized delamination at the interface between the composite film and the silicon-carbon anode. This comparative example demonstrates that the composite electrolyte continuously generates interfacial damage during long-term cycling due to repeated volume changes in the silicon-carbon anode. Without dynamic disulfide bonds, this damage cannot heal itself and can only accumulate unidirectionally, ultimately leading to interfacial failure and rapid capacity decay. This confirms the irreplaceable core role of the disulfide bond chain extender in this application.
[0068] Comparative Example 3
[0069] This comparative example is used to verify the introduction of Li7P3S. 11 The necessity of the inorganic fast ionic phase of sulfides. Except for the absence of Li7P3S. 11 Aside from the sulfide particles, the remaining steps were completely consistent with Example 1, yielding a pure polyurethane-urea polymer electrolyte membrane (PUU-SS-LiFSI). Test results showed that the membrane's ionic conductivity at 25 °C was only 0.021 mS / cm, approximately two orders of magnitude lower than that of Example 1, with a lithium-ion transference number of 0.71 and an electrochemical window of 4.6 V. When matched with a silicon-carbon anode containing 40% silicon, the initial capacity at room temperature and pressure (1 A / g) was only 780 mAh / g, decreasing to 320 mAh / g after 100 cycles, with a retention rate of 41%. This comparative example demonstrates that relying solely on the chain segment movement of the polyether soft segments to conduct lithium ions is insufficient to support the operation of high-rate and high-capacity silicon-carbon anodes. (Li7P3S) 11 The inorganic fast ion pathway provided by sulfides and their adsorption and dissociation of lithium salt anions are key factors in obtaining a composite electrolyte with 10... -3The key to high conductivity in the S / cm range and high lithium-ion transference number.
[0070] Comparative Example 4
[0071] This comparative example is used to verify the necessity of replacing the conventional polyether matrix (physical blend) with a disulfide-bonded polyurethane-urea matrix constructed by in-situ stepwise polymerization. The polymer matrix was replaced by an equal mass of commercially available polyethylene oxide (PEO, molecular weight approximately 6 × 10⁻⁶). 5 ), and directly combine PEO, LiFSI and Li7P3S 11 Sulfide particles (50% by mass, in polymer matrix with Li7P3S) 11 In addition to the physical blending of the sulfide (by total mass) in diethylene glycol dimethyl ether to form a film, the ratio of the remaining lithium salts ([EO]:[LiFSI]=10:1), stirring time, drop casting and drying conditions were the same as in Example 1, resulting in a PEO-50%LPS physical blend film.
[0072] Test results show that the membrane has an ionic conductivity of 0.88 mS / cm at 25 ℃, a lithium-ion transference number of only 0.62, and an electrochemical window of 4.5 V. When matched with a silicon-carbon anode with 40% silicon content, the initial capacity is 1430 mAh / g at room temperature and pressure, and 885 mAh / g after 100 cycles, with a capacity retention of 62%. When matched with an NMC622 cathode, the capacity is 141 mAh / g, with a capacity retention of 55% after 300 cycles and an average coulombic efficiency of 97.8%. However, the membrane exhibits visible particle aggregation and localized phase separation after drying, and it is prone to cracking upon bending, with the cracks being non-healable. This comparative example illustrates that, lacking the multiple hydrogen bonds and chemical bonding sites provided by the urea bonds and urethane bonds on the polyurethane-urea molecular chain, there is only a weak physical interaction between the inorganic sulfide and the organic matrix. As a result, the interfacial compatibility is poor, the anion migration is not inhibited, and the damage cannot be self-healed. The overall performance is inferior to that of this application, thus confirming the irreplaceability of the technical solution of constructing a polyurethane-urea matrix containing disulfide bonds in situ in this application.
[0073] The results of the examples and comparative examples are summarized and compared as follows.
[0074] Table 1
[0075]
[0076] The corresponding positive electrode matching performance is summarized in the table below.
[0077] Table 2
[0078]
[0079] It should be noted that the embodiments described herein are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
Claims
1. A method for preparing a self-healing polymer-sulfide composite solid electrolyte, characterized in that, Includes the following steps: (1) Under an inert atmosphere, polyisocyanate, 2,2-dimethyl-1,3-propanediol, diethylene glycol dimethyl ether and dried polyethylene glycol are mixed and reacted to obtain polyurethane prepolymer; (2) Add the disulfide bond chain extender, 2,2-dimethyl-1,3-propanediol, and diethylene glycol dimethyl ether to the reaction system and stir to obtain a polyurethane-urea polymer solution containing disulfide bonds; (3) Add sulfide glass ceramic particles and lithium salt to the polyurethane-urea polymer solution containing disulfide bonds obtained in step (2), stir and mix to obtain a slurry; (4) The slurry obtained in step (3) is dripped into a mold and dried to obtain the self-healing polymer-sulfide composite solid electrolyte.
2. The method for preparing the self-healing polymer-sulfide composite solid electrolyte according to claim 1, characterized in that, The polyethylene glycol in step (1) has a molecular weight of 1000~4000, and the drying process is a vacuum drying process, which involves stirring and drying at 100~150 ℃ for 1~12 h.
3. The method for preparing the self-healing polymer-sulfide composite solid electrolyte according to claim 1, characterized in that, The reaction temperature in step (1) is 60~90℃, and the reaction time is 1~4h; The polyisocyanate is hexamethylene diisocyanate, diphenylmethane diisocyanate, or terephthalic diisocyanate. The molar ratio of the isocyanate groups of the polyisocyanate to the total hydroxyl groups in the polyethylene glycol and 2,2-dimethyl-1,3-propanediol is 1.5:1 to 2.5:
1. The amount of 2,2-dimethyl-1,3-propanediol used is 0.1% to 0.5% of the mass of polyethylene glycol. The inert atmosphere is argon.
4. The method for preparing the self-healing polymer-sulfide composite solid electrolyte according to claim 1, characterized in that, The disulfide chain extender in step (2) is 4,4'-dithiodiphenylamine, and the molar ratio of the disulfide chain extender to 2,2-dimethyl-1,3-propanediol is 3:7 to 7:3; the molar ratio of the disulfide chain extender to polyisocyanate is 0.1 to 0.3:1; the reaction temperature is 30 to 50 °C, and the reaction time is 5 to 10 h.
5. The method for preparing the self-healing polymer-sulfide composite solid electrolyte according to claim 1, characterized in that, Step (3) is carried out in an inert atmosphere glove box, wherein the water content and oxygen content of the inert atmosphere glove box are both less than 1 ppm; The sulfide glass-ceramic is Li7P3S. 11 The average particle size is 0.5~5 μm, and the lithium salt is one or more of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, or lithium perchlorate. The mass of the added sulfide glass-ceramic particles is 10% to 60% of the total mass of the polymer matrix and the sulfide glass-ceramic; the molar ratio of the ether oxygen unit to the lithium salt in the polyethylene glycol segment is 5:1 to 20:
1.
6. The method for preparing the self-healing polymer-sulfide composite solid electrolyte according to claim 1, characterized in that, The drying process described in step (4) is vacuum drying, with a temperature of 50~70 ℃ and a time of 36~60 h.
7. A self-healing polymer-sulfide composite solid electrolyte, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 6.
8. The self-healing polymer-sulfide composite solid electrolyte according to claim 7, characterized in that, The composite solid electrolyte comprises a polyurethane-urea polymer matrix containing disulfide bonds and Li7P3S dispersed in the polymer matrix. 11 Sulfide particles and lithium salts; The composite solid electrolyte has an ionic conductivity ≥1.0 mS / cm, a lithium-ion transference number ≥0.80, and an electrochemical stability window ≥5.0 V at 25 °C.
9. An all-solid-state lithium battery, comprising a positive electrode, a negative electrode, and a solid electrolyte between the positive and negative electrodes, characterized in that, The solid electrolyte is the composite solid electrolyte as described in claim 7 or 8; the negative electrode is a silicon-carbon negative electrode, and the active material of the positive electrode is a layered nickel-manganese-cobalt oxide; the all-solid-state lithium battery operates under an applied stacking pressure not exceeding 5 MPa.
10. The all-solid-state lithium battery according to claim 9, characterized in that, The silicon-carbon anode contains 40% silicon by mass, and its initial reversible capacity at a current density of 1 A / g is 1500~1600 mAh / g, with a capacity retention of ≥70% after 100 cycles; the positive electrode active material is LiNi. 0.6 Mn 0.2 Co 0.2 O2 has a reversible capacity of 145~160 mAh / g within a voltage window of 2.8~4.3 V, a capacity retention of ≥65% after 300 cycles, and an average coulombic efficiency of ≥98.5%.