Encapsulation carrier based on glass fiber-glass powder composite pressing and its preparation method

By using a glass fiber-glass powder composite pressing method, combining low-temperature glass powder with electronic glass fiber cloth to form an inorganic-inorganic composite structure, the problems of high difficulty, high cost and warpage risk in packaging substrate preparation are solved. This achieves matching of thermal expansion coefficient with silicon chip and low dielectric loss, making it suitable for high-density packaging.

CN123075801APending Publication Date: 2026-11-10SHAANXI REACTOR MICROELECTRONICS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611286195.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing methods for preparing packaging substrates suffer from problems such as high manufacturing difficulty, high mass production costs, and the risk of warping at high temperatures.

Method used

A glass fiber-glass powder composite pressing method is adopted, which combines low-temperature glass powder with electronic glass fiber cloth to form an inorganic-inorganic composite structure to prepare a substrate. The substrate is then pressed under high temperature and high pressure to form a conductive circuit layer. The low thermal expansion coefficient and low dielectric loss characteristics are utilized in combination with existing PCB pressing equipment for processing.

Benefits of technology

It reduces material costs, improves reliability, solves warpage problems, achieves thermal expansion coefficient matching with silicon chips, is compatible with existing equipment, is easy to industrialize, and meets the dielectric and thermal performance requirements of different packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075801A_ABST
    Figure CN123075801A_ABST
Patent Text Reader

Abstract

This invention discloses a packaging carrier based on glass fiber-glass powder composite pressing and its preparation method, solving the problems of high manufacturing difficulty, high mass production cost, and warping risk at high temperatures in existing packaging carrier preparation methods. The packaging carrier consists of a substrate, a filling medium, and a conductive circuit layer. The substrate is a flat layer of electronic glass fiber cloth. The filling medium is prepared by mixing low-temperature glass powder and an organic carrier, covering both sides of the electronic glass fiber cloth and filling its interior under high temperature and high pressure conditions. The conductive circuit layer is formed by hot-pressing copper foil onto both sides of the electronic glass fiber cloth containing the filling medium, followed by etching circuits on the copper foil. The conductive circuit layers located on both sides of the electronic glass fiber cloth achieve electrical connection by drilling holes in the electronic glass fiber cloth, metallizing the hole walls, and filling with conductive material. This packaging carrier has the advantages of low manufacturing cost, high reliability, excellent dimensional stability, strong process compatibility, and adjustable performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to PCB substrates for chip packaging and their preparation methods, specifically to packaging substrates based on glass fiber-glass powder composite pressing and their preparation methods. Background Technology

[0002] With the explosive growth in demand for high-performance computing such as AI chips and HBM memory, packaging substrates need to simultaneously possess low coefficient of thermal expansion (Low-CTE), low dielectric loss (Low-Df), and high structural strength. Traditional packaging substrates use organic resins as substrates (such as BT and ABF), whose dielectric parameters can be adjusted through resin modification, and whose manufacturing cost is relatively low, making it easy to achieve multi-layer, high-density, high-precision wiring. However, when applied to high-density, multi-layer stacked chip packaging, they are prone to problems such as warpage and high signal loss.

[0003] Based on this, the existing technology uses a pure glass substrate instead of an organic resin substrate. The thermal expansion coefficient of glass can be better matched with that of silicon chips, and the warpage is smaller. However, due to the high brittleness and poor impact resistance of glass, the process of preparing through holes with high aspect ratio is complicated, difficult, and has high mass production cost.

[0004] Furthermore, Chinese invention patent CN118234127A discloses an adjustable stacked packaging structure and its fabrication method. This structure utilizes PCB manufacturing technology to process a transfer printed circuit board and a lamination frame to achieve multi-layer circuit board stacking and signal connectivity. After achieving a high-density, thin embedded package, it also allows for component adjustment and replacement, ensuring optimal electrical performance. While PCB lamination technology enables component embedding, its printed substrate uses traditional resin materials (such as bonding sheets or fiberglass PCBs). The thermal expansion coefficient of these materials does not match that of silicon chips, posing a risk of warping at high temperatures. Summary of the Invention

[0005] The purpose of this invention is to solve the technical problems of existing packaging substrate preparation methods, such as high preparation difficulty, high mass production cost, and risk of warping at high temperatures, and to provide a packaging substrate based on glass fiber-glass powder composite pressing and its preparation method.

[0006] To achieve the above objectives, the technical solution provided by this invention is as follows:

[0007] A packaging substrate based on glass fiber-glass powder composite pressing is characterized by being composed of a substrate, a filling medium, and a conductive circuit layer.

[0008] The substrate is a single layer of electronic fiberglass cloth laid flat.

[0009] The filling medium is prepared by low-temperature glass powder and organic carrier, and covers both sides of the electronic fiberglass cloth and fills the interior of the electronic fiberglass cloth under high temperature and high pressure conditions.

[0010] The conductive circuit layer is formed by hot-pressing copper foil onto both sides of an electronic fiberglass cloth with a filling medium, and then etching circuits on the copper foil.

[0011] The conductive circuit layers located on both sides of the electronic fiberglass cloth achieve electrical connection by drilling holes in the electronic fiberglass cloth, metallizing the hole walls, and filling them with conductive material.

[0012] Furthermore, the electronic fiberglass cloth is a low coefficient of thermal expansion fiberglass cloth, with a coefficient of thermal expansion ≤10 ppm / ℃;

[0013] Alternatively, the electronic fiberglass cloth may be a quartz electronic cloth.

[0014] Furthermore, the softening point of the low-temperature glass powder is 300°C~600°C, the dielectric constant is ≤8.0, and the dielectric loss is ≤0.01; the organic carrier is prepared by dissolving the binder in an organic solvent.

[0015] Meanwhile, the present invention also provides a method for preparing the above-mentioned encapsulation carrier based on glass fiber-glass powder composite pressing, which is characterized by including the following steps:

[0016] Step 1: Mix low-temperature glass powder with an organic carrier to prepare a glass powder slurry;

[0017] Step 2: First, coat the glass powder slurry onto both sides of the pre-prepared electronic fiberglass cloth, and then place the copper foil on both sides of the electronic fiberglass cloth to obtain the composite substrate blank.

[0018] Step 3: Place the composite substrate blank into a hot press and press it under high temperature and high pressure conditions, then cool it to room temperature to obtain a glass-fiberglass composite substrate.

[0019] Step 4: According to the preset process requirements, drill holes, electroplat, and etch on the glass-glass fiber composite substrate to form a conductive circuit layer, thereby obtaining a packaging carrier based on glass fiber-glass powder composite pressing.

[0020] Furthermore, step 2 also includes the step of coating the glass powder slurry onto both sides of the pre-prepared electronic fiberglass cloth and then baking and shaping it.

[0021] In step 3, the high temperature is 400°C~600°C, and the high pressure is 10 MPa~30 MPa;

[0022] The pressing is carried out in a low-pressure or vacuum environment, and the pressing process adopts a gradient heating and gradient pressurization process. During the gradient heating process, the organic carrier is fully volatilized and decomposed before the low-temperature glass powder softens.

[0023] Step 4 also includes the step of preparing a polyimide or silica buffer layer on the inner wall of the through hole after drilling.

[0024] In addition, the present invention also provides another encapsulation carrier based on glass fiber-glass powder composite pressing, which is characterized in that it is composed of a substrate, a filling medium and a conductive circuit layer.

[0025] The substrate comprises N layers of electronic fiberglass cloth stacked sequentially, where N≥2;

[0026] The filling medium is prepared by low-temperature glass powder and organic carrier. Under high temperature and high pressure conditions, it covers both sides of each layer of electronic glass fiber cloth and fills the interior of the corresponding electronic glass fiber cloth. The softening point of the filling medium corresponding to each layer of electronic glass fiber cloth decreases from bottom to top.

[0027] The conductive circuit layer is formed by hot-pressing copper foil between adjacent electronic fiberglass cloths with a filling medium and the outer surface of the outermost electronic fiberglass cloth, and then etching circuits on the copper foil.

[0028] The conductive circuit layers are electrically connected by drilling holes in the electronic fiberglass cloth, metallizing the hole walls, and filling them with conductive material.

[0029] Furthermore, the electronic fiberglass cloth is a low coefficient of thermal expansion fiberglass cloth, with a coefficient of thermal expansion ≤10 ppm / ℃;

[0030] Alternatively, the electronic fiberglass cloth may be a quartz electronic cloth.

[0031] Furthermore, the softening point of the low-temperature glass powder is 300°C~600°C, the dielectric constant is ≤8.0, and the dielectric loss is ≤0.01.

[0032] The organic carrier is prepared by dissolving the binder in an organic solvent.

[0033] Meanwhile, this invention also provides another method for preparing the encapsulation carrier plate based on glass fiber-glass powder composite pressing, which is characterized by including the following steps:

[0034] Step 1: Mix low-temperature glass powder with different softening points with an organic carrier to prepare N types of glass powder slurries with successively decreasing softening points;

[0035] Step 2: Apply the glass powder slurry with the highest softening point from Step 1 to both sides of the prepared bottom layer of electronic fiberglass cloth, then place copper foil on both sides of the electronic fiberglass cloth, then place the whole into a hot press and press it under high temperature and high pressure conditions, and then cool it to room temperature to obtain the first composite substrate blank.

[0036] Step 3: Drilling, electroplating, and etching are performed on the first composite substrate blank according to the preset process requirements to form a conductive circuit layer, thereby obtaining a glass-fiberglass composite substrate.

[0037] Step 4: Apply the glass powder slurry with the second highest softening point from Step 1 to both sides of the pre-prepared second layer of electronic fiberglass cloth. Then place the second layer of electronic fiberglass cloth on the top side of the first layer of glass-fiberglass composite substrate. Next, place the copper foil on the top side of the second layer of electronic fiberglass cloth and place the whole thing into a hot press. Press it under high temperature and high pressure conditions, and then cool it to room temperature to obtain the second composite substrate blank.

[0038] Step 5: Using the method in Step 3, a two-layer stacked glass-fiberglass composite substrate is obtained;

[0039] Step 6: Following the methods in Steps 4 to 5, until an N-layer stacked glass-fiber composite substrate is obtained, the N-layer stacked glass-fiber composite substrate is then placed in an oven or tunnel heating furnace for annealing treatment, thereby obtaining an N-layer encapsulation carrier based on glass fiber-glass powder composite pressing.

[0040] Furthermore, in step 1, the temperature difference between the two adjacent softening points of the glass powder slurry is 3~20℃;

[0041] Steps 2 and 4 also include the step of coating the glass powder slurry onto both sides of the pre-prepared electronic fiberglass cloth and then baking the electronic fiberglass cloth to set the glass powder slurry.

[0042] In step 2, the high temperature is 400°C to 600°C, and the high pressure is 10 MPa to 30 MPa;

[0043] The pressing is carried out in a low-pressure or vacuum environment, and the pressing process adopts a gradient heating and gradient pressurization process. During the gradient heating process, the organic carrier is fully volatilized and decomposed before the low-temperature glass powder softens.

[0044] Step 3 also includes the step of preparing a polyimide or silica buffer layer on the inner wall of the through hole after drilling;

[0045] In step 6, the annealing process specifically involves slowly heating the N-layer stacked glass-fiber composite substrate to near the lowest softening point of the low-temperature glass powder and holding it at that temperature, then cooling it to room temperature. The annealing process takes 20 to 300 minutes, which further releases the stress on the glass-fiber composite substrate.

[0046] The beneficial effects of this invention are as follows:

[0047] 1. The present invention provides a packaging substrate based on glass fiber-glass powder composite pressing. The overall structure is simple and uses low-temperature glass powder as the main functional material, which greatly reduces the material cost. At the same time, the low-temperature glass powder and electronic glass fiber cloth form an inorganic-inorganic composite structure at high temperature, which avoids the problem of aging and decomposition of packaging substrates with organic resin as substrate at high temperature, and has higher reliability.

[0048] 2. The present invention provides a method for preparing a packaging substrate based on glass fiber-glass powder composite pressing. During the preparation process, the composition of the low-temperature glass powder and the type of electronic glass fiber cloth can be adjusted, so that the coefficient of thermal expansion (CTE) of the packaging substrate can be precisely controlled at 2~6 ppm / ℃ according to actual needs, so as to perfectly match it with the silicon chip and fundamentally solve the warpage problem.

[0049] 3. The present invention provides a method for preparing a packaging substrate based on glass fiber-glass powder composite pressing, which is compatible with existing PCB lamination equipment and does not require additional investment in expensive glass substrate processing equipment (such as laser drilling and plasma etching). It has strong process compatibility and is easy to industrialize.

[0050] 4. Another method for preparing a packaging carrier based on glass fiber-glass powder composite pressing provided by the present invention is used to prepare N layers of electronic glass fiber cloth (N≥2) stacked in sequence, thereby meeting different packaging requirements.

[0051] 5. This invention allows for flexible customization of the dielectric properties, thermal properties, and mechanical strength of the packaging substrate by selecting electronic fiberglass cloths with different properties (such as low CTE cloth and low Df cloth) and adjusting the ratio of low-temperature glass powder, thereby meeting the needs of different packaging scenarios (such as AI servers and optical modules). Attached Figure Description

[0052] Figure 1 This is a schematic diagram of the structure of the encapsulation carrier plate based on glass fiber-glass powder composite pressing according to the present invention;

[0053] Figure 2 This is a schematic diagram of the second embodiment of the encapsulation carrier plate based on glass fiber-glass powder composite pressing of the present invention;

[0054] Figure 3This is a schematic flowchart of Example 2 of the preparation method of the encapsulation carrier plate based on glass fiber-glass powder composite pressing according to the present invention.

[0055] The attached figures are labeled as follows:

[0056] 1-Substrate, 2-Filling medium, 3-Conductive circuit layer. Detailed Implementation

[0057] To make the objectives, advantages, and features of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. Those skilled in the art should understand that these embodiments are merely used to explain the technical principles of the present invention and are not intended to limit the scope of protection of the present invention.

[0058] Example 1

[0059] like Figure 1 As shown, this embodiment provides a packaging carrier based on glass fiber-glass powder composite pressing, which consists of a substrate 1, a filling medium 2 and a conductive circuit layer 3.

[0060] Substrate 1 is a flat layer of electronic fiberglass cloth, which can be low-CTE fiberglass cloth, ordinary E-glass fiber cloth (a fabric woven from continuous E-glass fiber yarn), or T-Glass (a type of fiberglass cloth with a low coefficient of thermal expansion (Low-CTE)). The coefficient of thermal expansion of this type of fiberglass cloth is ≤10 ppm / ℃, ensuring the mechanical strength and dimensional stability of the substrate, thus effectively solving the problem of substrate warpage in advanced packaging. Alternatively, quartz electronic cloth (CTE≈0.54 ppm / ℃) can be selected according to actual needs to further reduce the overall coefficient of thermal expansion of the carrier board.

[0061] The filling medium 2 is prepared by mixing low-temperature glass powder with an organic carrier. Under high temperature and high pressure conditions, it covers both sides of the electronic fiberglass cloth and fills the interior of the electronic fiberglass cloth. The softening point of the low-temperature glass powder is generally between 300°C and 600°C, which is lower than the melting point of PCB copper foil. The dielectric constant of the low-temperature glass powder is ≤8.0, the dielectric loss is ≤0.01, and its coefficient of thermal expansion matches that of silicon chips (approximately 3 ppm / °C).

[0062] The conductive circuit layer 3 is formed by hot-pressing copper foil onto both sides of an electronic fiberglass cloth containing a filling medium 2, and then etching circuits onto the copper foil. The conductive circuit layer 3 is mainly used for signal transmission, and the conductive circuit layers located on both sides of the electronic fiberglass cloth are electrically connected by drilling holes in the electronic fiberglass cloth, metallizing the hole walls, and filling them with conductive material.

[0063] This embodiment also provides a method for preparing a packaging carrier based on glass fiber-glass powder composite pressing, including the following steps:

[0064] Step 1: Mix low-temperature glass powder with an organic carrier to make a glass powder slurry.

[0065] The low-temperature glass powder comprises silicon dioxide (SiO2), boron oxide (B2O3), aluminum oxide (Al2O3), and alkaline earth metal oxides. The organic carrier is prepared by dissolving the binder in an organic solvent, and the specific content of each component is determined according to the actual functional requirements. Alternatively, the low-temperature glass powder with the corresponding components can be selected according to the proportions disclosed in Chinese invention patent CN120841842A, and the corresponding glass powder slurry can be prepared.

[0066] Step 2: First, the glass powder slurry is coated on both sides of the pre-prepared electronic fiberglass cloth and baked to set it, so that some of the organic carrier evaporates and the adhesive in the organic carrier can stably bond the low-temperature glass powder to the electronic fiberglass cloth; then, copper foil is placed on both sides of the electronic fiberglass cloth to obtain the composite substrate blank.

[0067] Step 3: The composite substrate blank is placed in a hot press and pressed under high temperature (400°C~600°C) and high pressure (10MPa~30MPa). During this process, the low temperature glass powder melts and flows, fully wetting and covering the electronic glass fiber cloth. At the same time, the copper foil and the electronic glass fiber cloth are bonded together. Then, it is slowly cooled to room temperature to eliminate internal stress and obtain a dense glass-glass fiber composite substrate.

[0068] It should be noted that the pressing process employs a gradient heating and gradient pressurization technique. The gradient heating process allows the organic carrier to fully volatilize and decompose before the low-temperature glass powder melts, while simultaneously preventing the rapid flow of the low-temperature glass powder from causing displacement of the electronic fiberglass cloth and ensuring that there are no internal air bubbles. Furthermore, the pressing process can also be carried out under low pressure or vacuum conditions to further ensure that there are no air bubbles inside the electronic fiberglass cloth.

[0069] Step 4: According to the preset process requirements, drilling, electroplating, and etching are performed on the glass-glass fiber composite substrate to form conductive circuit layer 3, thereby obtaining the encapsulation carrier board based on glass fiber-glass powder composite pressing.

[0070] In this embodiment, drilling, electroplating, and etching can be performed using existing conventional processes, or, depending on the requirements, the methods disclosed in documents such as CN115295502A and CN104112673A can be used for processing.

[0071] In addition, after drilling, a polyimide or silicon dioxide buffer layer can be prepared on the inner wall of the obtained through hole to relieve the thermal stress between the glass and copper and prevent warping.

[0072] This invention uses low-temperature glass powder instead of traditional resin as a binder and presses it with electronic fiberglass cloth at high temperature. This method not only takes advantage of the low thermal expansion coefficient and low dielectric loss of glass, but also retains the low cost and high efficiency of PCB pressing process, making it easy to industrialize.

[0073] Example 2

[0074] like Figure 2 As shown, this embodiment provides a packaging carrier based on glass fiber-glass powder composite pressing. Compared with Embodiment 1, the substrate 1 in this packaging carrier includes N layers of electronic glass fiber cloth stacked sequentially, where N≥2. The filling medium 2 is prepared by low-temperature glass powder and organic carrier, and covers both sides of each layer of electronic glass fiber cloth under high temperature and high pressure conditions and fills the interior of the corresponding electronic glass fiber cloth. The softening point of the filling medium 2 corresponding to each layer of electronic glass fiber cloth is different.

[0075] The conductive circuit layer 3 is formed by hot-pressing copper foil between adjacent electronic fiberglass cloths containing the filling medium 2 and on the outer surface of the outermost electronic fiberglass cloth, and then etching circuits on the copper foil. Simultaneously, electrical connections are achieved between adjacent conductive circuit layers 3 or between conductive circuit layers 3 spanning multiple layers by drilling holes in the electronic fiberglass cloth, metallizing the hole walls, and filling them with conductive material, facilitating signal transmission.

[0076] Combination Figure 3 Taking the fabrication of a four-layer encapsulation substrate as an example, the fabrication method includes the following steps:

[0077] Step 1: Mix four types of low-temperature glass powder with an organic carrier to make four glass powder slurries with successively decreasing softening points. The temperature difference between two adjacent glass powder slurries with different softening points is 3~20℃. For example, the softening point of the glass powder slurry used for the bottom layer of electronic fiberglass cloth can be set at 450℃, and the softening temperatures of the glass powder slurries for the second, third, and fourth layers can be 440℃, 430℃, and 420℃, respectively.

[0078] The composition of the low-temperature glass powder and the glass powder slurry can be determined according to actual needs, or the low-temperature glass powder with the corresponding composition can be selected according to the proportion disclosed in Chinese invention patent with publication number CN120841842A, and a glass powder slurry with the corresponding softening point can be prepared.

[0079] Step 2: Apply the glass powder slurry with the highest softening point from Step 1 to both sides of the pre-prepared bottom layer of electronic fiberglass cloth. Ordinary E-fiberglass cloth is used for the electronic fiberglass cloth. Then place copper foil on both sides of the electronic fiberglass cloth. After that, put the whole thing into a hot press and press it at a temperature of 480°C and a pressure of 20MPa. The pressing process can also be carried out in a low-pressure or vacuum environment. The pressing process adopts a gradient heating and gradient pressurization process to ensure that the organic carrier is fully volatilized and decomposed before the low-temperature glass powder melts. Then slowly cool to room temperature to obtain the first composite substrate blank.

[0080] To improve preparation efficiency, the glass powder slurry can be coated onto both sides of the corresponding layer of electronic fiberglass cloth, and then the electronic fiberglass cloth can be baked to set the glass powder slurry, so as to save the coating time of the glass powder slurry in subsequent layered preparation.

[0081] Step 3: Drilling, electroplating, and etching are performed on the first composite substrate blank according to the preset process requirements to form a conductive circuit layer 3, thereby obtaining a glass-fiberglass composite substrate. Similar to Example 1, a polyimide or silicon dioxide buffer layer can be prepared on the inner wall of the through-holes obtained by drilling to alleviate thermal stress.

[0082] Step 4: Coat the glass powder slurry with the second highest softening point from Step 1 onto both sides of the pre-prepared second layer of electronic fiberglass cloth. Then place the second layer of electronic fiberglass cloth on the upper side of a glass-fiberglass composite substrate. Next, place copper foil on the upper side of the second layer of electronic fiberglass cloth and place the whole thing into a hot press. Press it at a temperature of 480°C and a pressure of 20MPa. Then cool it to room temperature to obtain the second composite substrate blank.

[0083] Step 5: Using the method in Step 3, a two-layer stacked glass-fiberglass composite substrate is obtained.

[0084] Step 6: Following the methods in steps 4 and 5, three-layer and four-layer glass-fiber composite substrates are obtained sequentially. The four-layer glass-fiber composite substrates are then placed in an oven or tunnel furnace and slowly heated to near the lowest softening point of the low-temperature glass powder and held at that temperature. Then, they are slowly cooled to room temperature. The entire annealing process takes 20 to 300 minutes, which further releases the stress in each layer of the glass-fiber composite substrate, thereby obtaining a four-layer encapsulation carrier based on glass fiber-glass powder composite pressing.

[0085] In this embodiment, the four-layer encapsulation substrate employs a step-by-step lamination method. The softening point of the low-temperature glass powder decreases progressively from bottom to top, ensuring that the copper foil pattern will not deform due to the softening of the already cured substrate before further lamination. Testing revealed that this four-layer encapsulation substrate has a coefficient of thermal expansion of 5.2 ppm / ℃, a dielectric loss of 0.005, and low signal loss.

[0086] Example 3

[0087] Compared with Example 2, this example is used to prepare a six-layer encapsulation carrier. The electronic fiberglass cloth is Low-CTE fiberglass cloth (CTE≤3.0 ppm / ℃) produced by Honghe Technology and low-temperature glass powder with a maximum softening point of 400℃. The pressing temperature is 420℃ and the pressure is 25MPa. The remaining steps are the same as in Example 2, thereby obtaining a six-layer encapsulation carrier based on fiberglass-glass powder composite pressing.

[0088] Tests showed that the six-layer encapsulation substrate has a coefficient of thermal expansion of 2.8 ppm / ℃ and a dielectric loss of 0.002, meeting the requirements of HBM encapsulation.

[0089] Example 4

[0090] Compared with Example 2, this example is used to prepare an eight-layer encapsulation carrier. The electronic fiberglass cloth is made of quartz electronic cloth (Q cloth) produced by Feilihua and low-temperature glass powder with a maximum softening point of 550°C. The pressing temperature is 580°C and the pressure is 30MPa. The remaining steps are the same as in Example 2, thereby obtaining an eight-layer encapsulation carrier based on fiberglass-glass powder composite pressing.

[0091] Tests showed that the eight-layer encapsulation substrate has a coefficient of thermal expansion of 1.2 ppm / ℃ and a dielectric loss of 0.0005, making it suitable for encapsulating 1.6T optical modules.

[0092] In addition, in some embodiments, the multilayer packaging substrate can be prepared by stacking from top to bottom or from the middle to both sides, and is not limited to the preparation method of stacking from bottom to top as described in the above embodiments.

[0093] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, and such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the present invention.

Claims

1. A packaging carrier based on glass fiber-glass powder composite pressing, characterized in that, It consists of a substrate (1), a filling medium (2), and a conductive circuit layer (3); The substrate (1) is a flat layer of electronic fiberglass cloth; The filling medium (2) is prepared by low-temperature glass powder and organic carrier, and covers both sides of the electronic fiberglass cloth and fills the interior of the electronic fiberglass cloth under high temperature and high pressure conditions; The conductive circuit layer (3) is formed by hot pressing copper foil onto both sides of an electronic fiberglass cloth with a filling medium (2), and then etching circuits on the copper foil. The conductive circuit layer (3) located on both sides of the electronic fiberglass cloth achieves electrical connection by drilling holes in the electronic fiberglass cloth and metallizing the hole walls and filling them with conductive materials.

2. The encapsulation carrier plate based on glass fiber-glass powder composite pressing according to claim 1, characterized in that: The electronic fiberglass cloth is a low coefficient of thermal expansion fiberglass cloth, with a coefficient of thermal expansion ≤10 ppm / ℃; Alternatively, the electronic fiberglass cloth may be a quartz electronic cloth.

3. The encapsulation carrier plate based on glass fiber-glass powder composite pressing according to claim 1, characterized in that: The softening point of the low-temperature glass powder is 300°C~600°C, the dielectric constant is ≤8.0, and the dielectric loss is ≤0.

01. The organic carrier is prepared by dissolving the binder in an organic solvent.

4. A method for preparing a packaging carrier plate based on glass fiber-glass powder composite pressing as described in any one of claims 1 to 3, characterized in that, Includes the following steps: Step 1: Mix low-temperature glass powder with an organic carrier to prepare a glass powder slurry; Step 2: First, coat the glass powder slurry onto both sides of the pre-prepared electronic fiberglass cloth, and then place the copper foil on both sides of the electronic fiberglass cloth to obtain the composite substrate blank. Step 3: Place the composite substrate blank into a hot press and press it under high temperature and high pressure conditions, then cool it to room temperature to obtain a glass-fiberglass composite substrate. Step 4: According to the preset process requirements, drill holes, electroplat, and etch on the glass-glass fiber composite substrate to form a conductive circuit layer (3), thereby obtaining a packaging carrier based on glass fiber-glass powder composite pressing.

5. The method for preparing the encapsulation carrier plate based on glass fiber-glass powder composite pressing according to claim 4, characterized in that: Step 2 also includes the step of coating the glass powder slurry onto both sides of the pre-prepared electronic fiberglass cloth and then baking and shaping it. In step 3, the high temperature is 400°C~600°C, and the high pressure is 10 MPa~30 MPa; The pressing is carried out in a low-pressure or vacuum environment, and the pressing process adopts a gradient heating and gradient pressurization process. Step 4 also includes the step of preparing a polyimide or silica buffer layer on the inner wall of the through hole after drilling.

6. A packaging carrier based on glass fiber-glass powder composite pressing, characterized in that: It consists of a substrate (1), a filling medium (2), and a conductive circuit layer (3); The substrate (1) comprises N layers of electronic fiberglass cloth stacked sequentially, where N≥2; The filling medium (2) is prepared by low temperature glass powder and organic carrier. Under high temperature and high pressure conditions, it covers both sides of each layer of electronic glass fiber cloth and fills the interior of the corresponding electronic glass fiber cloth. The softening point of the filling medium (2) corresponding to each layer of electronic glass fiber cloth decreases from bottom to top. The conductive circuit layer (3) is formed by hot pressing copper foil between adjacent electronic fiber cloths with filling medium (2) and the outer surface of the outermost electronic fiber cloth, and then etching circuits on the copper foil. The conductive circuit layers (3) are electrically connected by drilling holes in the electronic fiberglass cloth, metallizing the hole walls, and filling them with conductive material.

7. The encapsulation carrier plate based on glass fiber-glass powder composite pressing according to claim 6, characterized in that: The electronic fiberglass cloth is a low coefficient of thermal expansion fiberglass cloth, with a coefficient of thermal expansion ≤10 ppm / ℃; Alternatively, the electronic fiberglass cloth may be a quartz electronic cloth.

8. The encapsulation carrier plate based on glass fiber-glass powder composite pressing according to claim 6, characterized in that: The softening point of the low-temperature glass powder is 300°C~600°C, the dielectric constant is ≤8.0, and the dielectric loss is ≤0.

01. The organic carrier is prepared by dissolving the binder in an organic solvent.

9. A method for preparing a packaging carrier plate based on glass fiber-glass powder composite pressing as described in any one of claims 6 to 8, characterized in that, Includes the following steps: Step 1: Mix low-temperature glass powder with different softening points with an organic carrier to prepare N types of glass powder slurries with successively decreasing softening points; Step 2: Apply the glass powder slurry with the highest softening point from Step 1 to both sides of the prepared bottom layer of electronic fiberglass cloth, then place copper foil on both sides of the electronic fiberglass cloth, then place the whole into a hot press and press it under high temperature and high pressure conditions, and then cool it to room temperature to obtain the first composite substrate blank. Step 3: Drilling, electroplating and etching are performed on the first composite substrate blank according to the preset process requirements to form a conductive circuit layer (3), thereby obtaining a glass-fiberglass composite substrate. Step 4: Apply the glass powder slurry with the second highest softening point from Step 1 to both sides of the pre-prepared second layer of electronic fiberglass cloth. Then place the second layer of electronic fiberglass cloth on the top side of the first layer of glass-fiberglass composite substrate. Next, place the copper foil on the top side of the second layer of electronic fiberglass cloth and place the whole thing into a hot press. Press it under high temperature and high pressure conditions, and then cool it to room temperature to obtain the second composite substrate blank. Step 5: Using the method in Step 3, a two-layer stacked glass-fiberglass composite substrate is obtained; Step 6: Following the methods in Steps 4 to 5, until an N-layer stacked glass-fiber composite substrate is obtained, the N-layer stacked glass-fiber composite substrate is then placed in an oven or tunnel heating furnace for annealing treatment, thereby obtaining an N-layer encapsulation carrier based on glass fiber-glass powder composite pressing.

10. The method for preparing the encapsulation carrier plate based on glass fiber-glass powder composite pressing according to claim 9, characterized in that: In step 1, the temperature difference between the two adjacent softening points of glass powder slurry is 3~20℃; Steps 2 and 4 also include the step of coating the glass powder slurry onto both sides of the pre-prepared electronic fiberglass cloth and then baking the electronic fiberglass cloth to set the glass powder slurry. In step 2, the high temperature is 400°C to 600°C, and the high pressure is 10 MPa to 30 MPa; The pressing is carried out in a low-pressure or vacuum environment, and the pressing process adopts a gradient heating and gradient pressurization process. Step 3 also includes the step of preparing a polyimide or silica buffer layer on the inner wall of the through hole after drilling; In step 6, the annealing process specifically involves slowly heating the N-layer stacked glass-fiber composite substrate to near the lowest softening point of the low-temperature glass powder and holding it at that temperature, then cooling it to room temperature; the annealing process takes 20 to 300 minutes.

Citation Information

Patent Citations

  • Chip packaging base board and manufacturing method thereof

    CN104112673A

  • Three-dimensional packaging structure and manufacturing method thereof

    CN115295502A

  • Adjustable package-on-package structure and preparation method thereof

    CN118234127A

  • Glass slurry as well as preparation method and application thereof

    CN120841842A