Preparation method of multi-matrix high thermal conductivity pads based on boron nitride film coating
By wrapping a boron nitride film around the thermally conductive foam substrate to form a multi-matrix heat dissipation channel, the problems of short circuits and low heat dissipation efficiency of carbon-based filler thermally conductive materials are solved, achieving efficient and safe heat dissipation for electronic devices.
Patent Information
- Application Number
- CN202611306301.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-10
AI Technical Summary
Existing carbon-based filler thermal conductive materials are prone to causing short-circuit faults in electronic devices, and the single bulk filler structure limits heat dissipation efficiency, making it difficult to meet the heat dissipation requirements of high-power electronic devices.
A method for preparing multi-matrix high thermal conductivity pads using boron nitride film coating is employed. By attaching a boron nitride film around a thermally conductive foam substrate, multiple heat dissipation channels are formed. Furthermore, a BN thermally conductive filler is used to replace the carbon-based filler, thus avoiding electrical conductivity and improving heat dissipation efficiency.
It achieves efficient heat dissipation without the risk of short circuits in electronic devices, meets the heat dissipation requirements of high-power electronic devices, and saves material costs, meeting the requirements of thinness and lightness.
Smart Images

Figure CN123075863A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermal conductive and heat dissipation materials for electronic devices, and in particular provides a method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating. Background Technology
[0002] In the field of heat dissipation for electronic device components, silicone pads, thermal conductive gels, and carbon-based thermal conductive foams are currently the most widely used thermal interface materials. However, the thermal conductivity of these conventional thermal conductive materials is generally low, mostly not exceeding 20W / (mK), and their heat dissipation capacity has inherent limitations.
[0003] Existing carbon-based thermal conductive materials mainly involve filling a foam matrix with carbon-based thermal conductive fillers such as graphite, carbon nanotubes, graphene, and carbon fibers. The overall thermal conductivity of the material is improved by increasing the filler content. However, carbon-based fillers themselves are conductive, resulting in the formed thermal conductive foam being conductive. If directly applied to the inside of electronic devices, this can easily cause short circuits. Therefore, current solutions typically employ insulating film coating, covering the thermal conductive foam with insulating films such as PET or PI films to achieve electrical isolation and mitigate the risk of short circuits.
[0004] The thermally conductive foams produced above mostly adopt a single large-block filling structure, which is directly sandwiched between the heat source and the heat sink. The material cannot form a thermal conductive path, and the heat transfer path is singular, which limits the overall heat dissipation efficiency and makes it difficult to meet the ever-increasing heat dissipation requirements of high-power electronic devices. Summary of the Invention
[0005] To overcome the shortcomings of the prior art, this invention discloses a method for preparing multi-matrix high thermal conductivity pads based on boron nitride film coating.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a method for preparing multi-matrix high thermal conductivity pads based on boron nitride film coating. The first step is the preparation of modified foam. 50-55 parts by weight of methyl vinyl silicone rubber (VMQ) raw rubber, 10-15 parts of fumed silica, 10-15 parts of BN thermally conductive filler, 15-20 parts of aluminum hydroxide (ATH) flame-retardant filler, 0.5-1.5 parts of DCP vulcanizing agent, 2-3 parts of AC foaming agent, 0.5-1.5 parts of foaming activator, 0.5-1 parts of silicone-based foam equalizing agent, and 0.1-0.5 parts of zinc stearate are mixed in a mixing mill and then extruded into a flat vulcanizing mold to foam and shape, thus obtaining a modified thermally conductive foam blank.
[0007] The second step is foam cutting. A segmented cutting machine is used to cut the thermally conductive foam blank into several small segments of thermally conductive foam substrate.
[0008] The third step is the separate fabrication of high thermal conductivity materials. A layer of BN film is attached to the periphery of several small sections of thermally conductive foam substrate with thermally conductive adhesive to form several separate high thermal conductivity materials.
[0009] The fourth step is the fabrication of high thermal conductivity pads. Several high thermal conductivity materials are arranged in a linear array and fixed with thermally conductive adhesive to form a high thermal conductivity pad with several heat dissipation channels.
[0010] More preferably, the modified foam is obtained by mixing 50 parts by weight of methyl vinyl silicone rubber (VMQ) raw rubber, 15 parts by weight of fumed silica, 15 parts by weight of BN thermally conductive filler, 15 parts by weight of aluminum hydroxide (ATH) flame retardant filler, 1.5 parts by weight of DCP vulcanizing agent, 2 parts by weight of AC foaming agent, 0.5 parts by weight of foaming activator, 0.5 parts by weight of silicone foam leveling agent and 0.5 parts by weight of zinc stearate in a mixing mill, and then extruding and foaming the mixture in a flat vulcanizing mold.
[0011] More preferably, the high thermal conductivity material is provided in two, three, or four rows.
[0012] More preferably, the overall thickness of the high thermal conductivity material component is 2.05 mm.
[0013] More preferably, the thickness of the boron nitride film is 0.05-0.5 mm.
[0014] More preferably, the resistivity of the boron nitride film is >10. 14 Ω.cm.
[0015] More preferably, the thermal conductivity of the boron nitride film is 200-600 W / (mK).
[0016] A further preferred embodiment is that a portion of the BN film around each high thermal conductivity material component is coated with thermally conductive adhesive and fixed to the other high thermal conductivity material components.
[0017] More preferably, the thermally conductive adhesive is an organosilicon adhesive.
[0018] The present invention achieves the following beneficial effects:
[0019] 1. The modified thermally conductive foam produced in this application replaces the traditional thermally conductive material with carbon-based filler by adding BN thermally conductive filler, thus avoiding the thermal conductivity of the molded thermally conductive foam body. When directly applied inside electronic devices, it will not cause short circuit faults.
[0020] 2. The high thermal conductivity pad made in this application can form multiple heat dissipation channels by separately pasting several high thermal conductivity materials in an array. Compared with a single large block filling structure, it improves the overall heat dissipation efficiency and can meet the continuously increasing heat dissipation requirements of high power electronic devices.
[0021] 3. The high thermal conductivity material split produced in this application can reduce the overall thickness by wrapping a boron nitride film around the thermally conductive foam substrate, which not only saves material costs but also meets the development requirements of thinner and lighter materials.
[0022] Other features and advantages of the invention will be set forth in the following description and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention can be realized and obtained by means of the structures pointed out in the description and the drawings. Attached Figure Description
[0023] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the disclosure of this invention and, together with the description, serve to explain the principles of this disclosure.
[0024] Figure 1 This is a schematic diagram of the overall structure disclosed in this invention;
[0025] Figure 2 This is a schematic diagram of the split structure of the high thermal conductivity material disclosed in this invention;
[0026] In the diagram: 10, high thermal conductivity material; 11, thermally conductive foam; 12, boron nitride film; 20, thermally conductive adhesive; 30, heat dissipation channel. Detailed Implementation
[0027] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0028] In the description of this invention, it should be understood that the terms "opening", "upper", "lower", "thickness", "top", "middle", "length", "inner", "around", etc., which indicate orientation or positional relationship, are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the components or elements referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as limiting this invention.
[0029] Example
[0030] To address the following shortcomings of thermally conductive foams made using existing technologies:
[0031] First, carbon-based filler thermal conductive materials mainly involve filling the foam matrix with carbon-based thermal conductive fillers such as graphite, carbon nanotubes, graphene, and carbon fibers. The overall thermal conductivity of the material is improved by increasing the filling ratio of the filler. However, carbon-based fillers themselves have electrical conductivity, which causes the molded thermal conductive foam body 11 to be conductive. If it is directly applied to the inside of electronic devices, it is very easy to cause short circuit faults.
[0032] Secondly, the overall structure adopts a single large-block filling structure, which is directly sandwiched between the heat source and the heat sink. The material cannot form a heat conduction path, and the heat transfer path is singular, which limits the overall heat dissipation efficiency and makes it difficult to meet the ever-increasing heat dissipation requirements of high-power electronic devices.
[0033] refer to Figure 1 and Figure 2 As shown, this application provides a method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film 12 coating. The first step is the preparation of modified foam. 50-55 parts by weight of methyl vinyl silicone rubber (VMQ) raw rubber, 10-15 parts of fumed silica, 10-15 parts of BN thermally conductive filler, 15-20 parts of aluminum hydroxide (ATH) flame-retardant filler, 0.5-1.5 parts of DCP vulcanizing agent, 2-3 parts of AC foaming agent, 0.5-1.5 parts of foaming activator, 0.5-1 parts of silicone-based foam equalizing agent, and 0.1-0.5 parts of zinc stearate are mixed in a mixer and then extruded into a mold on a flat vulcanizing machine for foaming and shaping to obtain a modified thermally conductive foam blank. This step, by adding BN thermally conductive filler instead of the traditional method of adding carbon-based filler, avoids the thermally conductive foam body 11 becoming conductive, thus preventing short-circuit faults when directly applied inside electronic devices.
[0034] The second step is foam cutting. A segmented cutting machine is used to cut the thermally conductive foam blank into several small segments of thermally conductive foam substrate.
[0035] The third step involves fabricating the high thermal conductivity material components 10. A layer of boron nitride (BN) film is attached to the periphery of several small sections of the thermally conductive foam substrate using silicone adhesive, forming several high thermal conductivity material components 10 with a thickness of 2.05 mm. In specific implementations, the thickness of the boron nitride film 12 is preferably 0.05-0.5 mm; more preferably, the thickness of the boron nitride film 12 is 0.05 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.5 mm, or 0.8 mm. This step, by wrapping the thermally conductive foam substrate with a boron nitride film 12, reduces the overall thickness, saving material costs and meeting the requirements for thinner and lighter designs.
[0036] The resistivity of boron nitride film 12 is >10. 14 The thermal conductivity of boron nitride film 12 is 200-600 W / (mK).
[0037] The fourth step is the fabrication of a high thermal conductivity pad. Several high thermal conductivity material components 10 are arranged in a linear array and fixed with silicone adhesive to form a high thermal conductivity pad with several heat dissipation channels 30. This step, by attaching several high thermal conductivity material components 10 in an array, can form multiple heat dissipation channels 30. Compared with a single large-block filling structure, this improves the overall heat dissipation efficiency and can meet the continuously increasing heat dissipation requirements of high-power electronic devices.
[0038] The following is a specific preparation process for a modified foam provided in this application. The modified foam is prepared by mixing 50 parts by weight of methyl vinyl silicone rubber (VMQ) raw rubber, 15 parts by weight of fumed silica, 15 parts by weight of BN thermally conductive filler, 15 parts by weight of aluminum hydroxide (ATH) flame retardant filler, 1.5 parts by weight of DCP vulcanizing agent, 2 parts by weight of AC foaming agent, 0.5 parts by weight of foaming activator, 0.5 parts by weight of silicone foam leveling agent, and 0.5 parts by weight of zinc stearate in a mixing mill, followed by extrusion and foaming and shaping in a flat vulcanizing mold. The specific preparation process is as follows:
[0039] S100: 50 parts of methyl vinyl silicone rubber VMQ raw rubber, 15 parts of fumed silica, 15 parts of BN thermally conductive filler, 15 parts of aluminum hydroxide ATH flame retardant filler, 1.5 parts of DCP vulcanizing agent, 2 parts of AC foaming agent, 0.5 parts of foaming activator, 0.5 parts of silicone foam leveling agent and 0.5 parts of zinc stearate are sequentially poured into a mixer and mixed at 4000 rpm for 10 minutes to obtain a mixture.
[0040] S200: The mixture is added to a twin-screw extruder, melt-blended at 150°C, extruded, cooled, and pelletized to obtain composite foaming masterbatch;
[0041] S300 involves placing the composite foaming masterbatch into a preheated flat vulcanizing mold for foaming and shaping to obtain a thermally conductive foam blank.
[0042] The molding procedure for the flat vulcanizing machine mold in step S300 above is as follows:
[0043] Step 1, plasticization: hot press at 150℃ and 10MPa pressure for 5 minutes to completely melt the material and fill the cavity;
[0044] The second step is foaming: quickly adjust the temperature and pressure to the foaming temperature of 165℃ and release the pressure to 2MPa. Maintain this condition for 8-10 minutes, and the material will expand and fill the mold cavity.
[0045] The third step is shaping: cool the mold with water to 65°C, then open the mold and remove the product.
[0046] In a preferred embodiment, depending on the size of the heat source, the high thermal conductivity material split 10 of this application is provided with two, three or four rows. When multiple high thermal conductivity material splits 10 are arranged in an array and adhered together by thermally conductive adhesive 20, high thermal conductivity pads of different area sizes can be formed.
[0047] In one specific embodiment, a portion of silicone adhesive is coated on the BN film around each high thermal conductivity material component 10 to fix it to other high thermal conductivity material components 10. Only in this way can the BN films around the two high thermal conductivity material components 10 be prevented from completely adhering, thereby forming a heat dissipation channel 30.
[0048] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0049] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent transformations or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating, characterized in that, The first step is the production of modified foam. 50-55 parts by weight of methyl vinyl silicone rubber (VMQ) raw rubber, 10-15 parts of fumed silica, 10-15 parts of BN thermally conductive filler, 15-20 parts of aluminum hydroxide (ATH) flame-retardant filler, 0.5-1.5 parts of DCP vulcanizing agent, 2-3 parts of AC foaming agent, 0.5-1.5 parts of foaming activator, 0.5-1 parts of silicone-based foam leveling agent, and 0.1-0.5 parts of zinc stearate are mixed in a mixer and then extruded into a flat vulcanizing mold to foam and shape, thus obtaining the modified thermally conductive foam blank. The second step is foam cutting. A segmented cutting machine is used to cut the thermally conductive foam blank into several small segments of thermally conductive foam substrate. The third step is the separate fabrication of high thermal conductivity materials. A layer of BN film is attached to the periphery of several small sections of thermally conductive foam substrate with thermally conductive adhesive to form several separate high thermal conductivity materials. The fourth step is the fabrication of high thermal conductivity pads. Several high thermal conductivity materials are arranged in a linear array and fixed with thermally conductive adhesive to form a high thermal conductivity pad with several heat dissipation channels.
2. The method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating according to claim 1, characterized in that, The modified foam is obtained by mixing 50 parts by weight of methyl vinyl silicone rubber (VMQ) raw rubber, 15 parts by weight of fumed silica, 15 parts by weight of BN thermally conductive filler, 15 parts by weight of aluminum hydroxide (ATH) flame retardant filler, 1.5 parts by weight of DCP vulcanizing agent, 2 parts by weight of AC foaming agent, 0.5 parts by weight of foaming activator, 0.5 parts by weight of silicone foam leveling agent and 0.5 parts by weight of zinc stearate in a mixing mill, and then extruding and foaming the mixture in a flat vulcanizing mold.
3. The method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating according to claim 1, characterized in that, The high thermal conductivity material is divided into two, three, or four rows.
4. The method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating according to claim 1, characterized in that, The overall thickness of the high thermal conductivity material component is 2.05 mm.
5. The method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating according to claim 1, characterized in that, The thickness of the boron nitride film is 0.05-0.5 mm.
6. The method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating according to claim 1, characterized in that, The resistivity of the boron nitride film is >10. 14 Ω.cm.
7. The method for preparing a multi-matrix high thermal conductivity pad based on boron nitride film coating according to claim 1, characterized in that, The thermal conductivity of the boron nitride film is 200-600 W / (mK).
8. The method for preparing a multi-matrix high-density heat pad based on boron nitride film coating according to claim 1, characterized in that, Each high thermal conductivity material component has a portion of thermally conductive adhesive coated on the BN film around its perimeter to fix it in place with the other high thermal conductivity material components.