Pressure-welded WS2 nanosheet-bridged silver nanowire composite transparent electrode, its preparation method and application

By combining WS2 nanosheets with AgNWs networks, Ag-S covalent bonds are formed through capillary self-assembly and mechanical pressure, solving the problems of conductivity, roughness, adhesion and stability of AgNWs electrodes, and preparing high-performance flexible transparent electrodes for application in flexible OLEDs.

CN123076112APending Publication Date: 2026-11-10TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610993612.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-06
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing silver nanowire (AgNWs) based flexible transparent conductive electrodes face numerous challenges in terms of conductivity, surface roughness, adhesion, and environmental stability, making it difficult to meet the requirements of flexible optoelectronic devices.

Method used

By employing capillary self-assembly and mechanical pressure-induced methods, WS2 nanosheets are composited with AgNWs networks to form Ag-S covalent bonds, thereby realizing a transparent composite electrode of WS2 nanosheets and silver nanowires. Combined with physical embedding and chemical welding, the electrode performance is improved.

Benefits of technology

It achieves extremely low sheet resistance, high transmittance, ultra-low surface roughness, excellent mechanical flexibility and environmental stability, making it suitable for high-performance flexible OLEDs and possessing excellent comprehensive optoelectronic performance and mechanical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076112A_ABST
    Figure CN123076112A_ABST
Patent Text Reader

Abstract

This invention discloses a pressure-welded WS2-bridged silver nanowire composite transparent electrode, its preparation method, and its application. The composite transparent electrode comprises a flexible transparent substrate, an AgNWs network embedded layer that is mechanically pressure-treated and anchored to the substrate surface, and WS2 nanosheets bridged by Ag-S covalent bonds in the nodes and gaps of the AgNWs network embedded layer through mechanical pressure induction. This invention utilizes a combination of capillary self-assembly and mechanical pressure-induced welding to enable the WS2 nanosheets to spontaneously migrate to the nodes of the AgNWs network embedded layer and form Ag-S covalent bonds under pressure, achieving a "riveting-welded" interface enhancement. This solves the problems of high node resistance, large roughness, weak adhesion, and poor stability of AgNWs electrodes, resulting in an electrode with excellent overall performance, suitable for the field of flexible optoelectronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor optoelectronic technology, and relates to a flexible transparent conductive electrode, particularly to a flexible transparent conductive electrode that achieves AgNWs and WS2 nanosheet composites through pressure-induced Ag-S bonding, its preparation method, and the application of the electrode in flexible organic light-emitting diodes. Background Technology

[0002] In recent years, the flexible electronics industry has developed rapidly. Flexible nano-optoelectronic devices, such as flexible organic light-emitting diodes, flexible solar cells, and flexible sensing and detection devices, are gradually entering the market, profoundly changing people's production and lifestyles. The ever-increasing demand for flexible electronic products continues to drive social progress.

[0003] Flexible transparent conductive electrodes (FTCEs) are a key component of flexible nano-optoelectronic devices, and their performance directly determines the overall performance of the device. Indium tin oxide (ITO) is widely used as an electrode material for optoelectronic devices due to its high light transmittance and good conductivity. However, the inherent brittleness of ITO makes it difficult to meet the bending and stretching requirements of flexible optoelectronic devices, which greatly limits the development of flexible optoelectronic devices.

[0004] To develop flexible transparent conductive electrodes that can replace ITO, researchers have conducted extensive studies and proposed various construction strategies and schemes, such as using silver nanowires (AgNWs), carbon nanotubes, and two-dimensional materials to construct high-performance flexible transparent conductive electrodes. Among these materials, AgNWs have become a highly promising candidate material for developing flexible transparent conductive electrodes due to their excellent conductivity and transmittance, good film-forming properties, and outstanding mechanical flexibility.

[0005] However, the practical application of AgNWs-based flexible transparent conductive electrodes still faces many challenges. First, the nanowires in the AgNWs network are mainly connected through point contacts rather than continuous conductive paths, resulting in high junction contact resistance and limiting the overall conductivity of the electrode. Second, the surface roughness of the AgNWs network is high due to the microscopic protrusions at the nanowire junctions, which can easily cause current leakage or short-circuit failure during subsequent device fabrication. Third, the adhesion between AgNWs and flexible substrates (such as PET and PEN) is weak, mainly maintained by van der Waals forces. When subjected to mechanical stress or undergoing solution processing, AgNWs are prone to peeling or displacement. Finally, AgNWs are susceptible to oxidation, sulfidation, or electrochemical migration when exposed to heat, moisture, or oxygen, leading to irreversible conductivity loss and device failure.

[0006] To address these challenges, researchers have developed various optimization strategies. For example, thermal annealing or chemical welding can enhance the fusion of nanowire nodes and reduce contact resistance. Tze-Bin Song et al. (Nanoscale Joule heating and electromigration enhanced ripening of silver nanowire contacts, ACS Nano , 2014, 8(3): 2804.) By precisely controlling the constant current power supply and utilizing the Joule heating effect, the contact morphology between AgNWs was improved, and the contact resistance was successfully reduced. However, this hot welding process is prone to thermal damage to the substrate when heating the electrodes, so further improvement is still needed. Mechanical pressing or polymer filling methods can effectively reduce surface roughness. Ding et al. (Pressure-induced fusion of silver nanowire networks for transparent conductive electrodes, 2014, 8(3): 2804.) International Journal of Machine Tools and Manufacture (2024, 199: 104162.) An attempt was made to use pressure to press a silver nanowire network into PMMA to achieve electrode welding, at 200 kg / cm². 2 Under pressure, the overall performance of silver nanowire networks was significantly optimized, with the sheet resistance decreasing from the original 2.6 kΩ / sq to 34.3 Ω / sq, a reduction of nearly two orders of magnitude. Simultaneously, the root mean square roughness of the surface was significantly improved from 76.1 nm to 12.6 nm. However, single methods often only solve part of the problem and frequently involve new performance trade-offs. Therefore, developing an integrated strategy that can simultaneously achieve high conductivity, high transmittance, low roughness, strong adhesion, and excellent environmental stability has become a research hotspot in this field.

[0007] In recent years, combining other conductive materials with AgNWs networks to prepare composite electrodes has become a hot research topic.

[0008] Professor Yang Xuyong's research group at Shanghai University (Cao F., et al., Multidimensional Perovskite Embedded with Silver Nanowires for Highly Efficient and Stable Flexible Light-Emitting Diodes) Nano Letters(2022, 22(10): 4246.) A multi-dimensional composite transparent electrode of 0D AgNPs / 1D AgNWs / 2D MXene / 3D PEDOT:PSS was proposed. Through the synergistic effect between the materials of each dimension, a sheet resistance of 11.9 Ω / sq was achieved, while maintaining 83.5% transmittance at a wavelength of 550 nm. When this electrode was applied to flexible perovskite light-emitting diodes (PeLEDs), the device exhibited an external quantum efficiency (EQE) of 16.3% and a transmittance of 40,100 cd / m². 2 It exhibits high brightness and retains over 90% of its initial efficiency after 1000 bends. However, the acidity and hygroscopicity of PEDOT:PSS inevitably reduce the lifespan of electrodes and devices, and to some extent sacrifice environmental stability.

[0009] Professor Cheolmin Park (Jiang W., et al.) of Yonsei University, South Korea, MXene-Silver Nanowire Hybrid Transparent Electrodes for High-Performance Flexible Quantum DotLight-Emitting Diodes. ACS Nano (2022, 14(12): 38021.) proposed a composite transparent electrode called MXAg (PET / PMMA / MXene+AgNWs). By mixing a highly conductive AgNWs network with solution-treated MXene nanosheets, and effectively welding AgNWs nodes using MXene nanosheets, an electrode with a low sheet resistance of 13.9 Ω / sq and a high transmittance of 83.8% was obtained. By introducing a PMMA polymer buffer layer, the surface roughness of the electrode was improved while enhancing the bending stability of the film. The work function of this composite electrode can also be adjusted by controlling the amount of MXene. A fully solution-treated quantum dot light-emitting diode (QLED) prepared with this composite electrode as the anode achieved a maximum external quantum efficiency of 9.88% and a current efficiency of 25.8 cd / A. However, the synthesis process of MXene is cumbersome and requires harsh conditions, which to some extent limits the industrial application of this composite electrode.

[0010] Among two-dimensional materials, tungsten disulfide (WS2) has attracted much attention due to its high carrier mobility, good chemical inertness, and thermal stability. Studies have shown that exposed sulfur atoms at the edges of WS2 nanosheets can form strong coordination bonds (Ag-S bonds) with silver atoms, with bond energies significantly higher than intermolecular van der Waals forces, providing an ideal platform for constructing stable heterointerfaces. Furthermore, WS2 monolayers possess a direct band gap in the visible to near-infrared spectral range, combining high transparency with mechanical flexibility, making them an ideal component for transparent electrodes in optoelectronic devices. (Myja H et al. [Silver nanowire electrodes for transparent light emitting devices based on WS2 monolayers]). Nanotechnology (2023, 34(28): 285201.) Using MOCVD-grown WS2 monolayers as active light-emitting materials, embedded in a scalable vertical device structure and combined with AgNWs transparent top electrodes, a vertically structured transparent light-emitting diode device was successfully fabricated, achieving an average transmittance of over 60% in the visible light range and a turn-on voltage of approximately 3V. However, how to effectively integrate WS2 nanosheets into AgNWs networks and fully utilize their interfacial bonding potential to simultaneously address the comprehensive issues of AgNWs electrodes in terms of conductivity, roughness, adhesion, and environmental stability has not yet been systematically reported. Summary of the Invention

[0011] The purpose of this invention is to provide a pressure-welded WS2 nanosheet-bridged silver nanowire composite transparent electrode with extremely low sheet resistance, high transmittance, ultra-low surface roughness, excellent mechanical flexibility and environmental stability, and to provide a simple and controllable preparation method for it and its application in high-performance flexible OLEDs.

[0012] To achieve the aforementioned objectives, this invention employs a process combining "capillary self-assembly" and "mechanical pressure-induced welding" to composite two-dimensional WS2 nanosheets with a one-dimensional AgNWs network. First, solvent evaporation generates capillary forces that drive the spontaneous migration of WS2 nanosheets and their encapsulation of AgNWs nodes. Subsequently, mechanical pressure treatment densifies the AgNWs network and partially embeds it into a flexible substrate. More importantly, under pressure, sulfur atoms exposed at the edges of the WS2 nanosheets form strong Ag-S covalent bonds with silver atoms on the AgNWs surface, achieving a "riveting-welded" type of interface enhancement.

[0013] Therefore, the present invention specifically provides a pressure-welded WS2-bridged silver nanowire composite transparent electrode, wherein the composite transparent electrode consists of a flexible transparent substrate, an AgNWs network embedded layer formed by mechanical pressure treatment and embedded and anchored on the surface of the flexible transparent substrate, and WS2 nanosheets bridged in the nodes and gaps of the AgNWs network embedded layer by Ag-S covalent bonds under mechanical pressure.

[0014] Specifically, the flexible transparent substrate of the present invention can be any of the flexible transparent polymer films conventional in the art, including but not limited to any one of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyimide (PI), and polycarbonate (PC). Preferably, the flexible transparent substrate is a PET film.

[0015] More specifically, the WS2 nanosheets of the present invention are preferably few-layer (1 to 10 layers) nanosheets prepared by liquid phase exfoliation, with their lateral dimensions mainly distributed in the range of 200 to 600 nm, so as to facilitate their filling into the gaps of the AgNWs network.

[0016] Furthermore, the present invention also provides a method for preparing the pressure-welded WS2-bridged silver nanowire composite transparent electrode, comprising the following steps: S1: An AgNWs network is formed on the surface of a flexible transparent substrate; S2: Coat the surface of the AgNWs network with WS2 nanosheet dispersion, and use the capillary force generated by solvent evaporation to cause the WS2 nanosheets to self-assemble to the nodes of the AgNWs network to form a composite film; S3: Apply mechanical pressure to the composite film to embed and anchor the AgNWs network on the surface of the flexible transparent substrate to form an AgNWs network embedding layer, and induce Ag atoms on the surface of AgNWs to form Ag-S covalent bonds with S atoms on the edge of WS2 nanosheets to form the pressure-welded WS2 bridging silver nanowire composite transparent electrode.

[0017] More preferably, the preparation method of the pressure-welded WS2-bridged silver nanowire composite transparent electrode of the present invention further includes first performing a surface hydrophilic treatment on the flexible transparent substrate to enhance its wettability to the AgNWs dispersion and the WS2 nanosheet dispersion.

[0018] Furthermore, the surface hydrophilization treatment is specifically ultraviolet-ozone treatment or oxygen plasma treatment.

[0019] More specifically, the UV-ozone treatment time is preferably 5 to 15 minutes.

[0020] The coating of the AgNWs dispersion and WS2 nanosheet dispersion described in this invention can be performed using solution film formation methods, including but not limited to spin coating, drop coating, spray coating, blade coating, or slot coating.

[0021] Specifically, the present invention preferably employs spin coating to coat the dispersion. More specifically, the preferred spin coating speed is 1500–3500 rpm. It should be understood that the choice of the above coating method does not affect the essence of the technical solution of the present invention, and those skilled in the art can select an appropriate coating method based on the substrate size, dispersion properties, and mass production requirements.

[0022] Specifically, the AgNWs dispersion can be obtained by dispersing water, isopropanol, ethanol or a mixture thereof as a dispersion medium, and the concentration of the dispersion is preferably 1.0 to 2.0 mg / mL.

[0023] More specifically, the silver nanowires used to prepare the AgNWs dispersion preferably have a diameter of 20–50 nm and a length of 10–40 μm.

[0024] Furthermore, after the AgNWs dispersion is uniformly coated onto the surface of a flexible transparent substrate, it is annealed to evaporate the solvent and form an AgNWs network. The annealing temperature is preferably 100–150°C, and the time is 5–20 min.

[0025] Specifically, the WS2 nanosheet dispersion preferably uses water or an alcohol-water mixture as the dispersion medium, and the dispersion concentration is preferably 0.4 to 0.8 mg / mL.

[0026] Furthermore, after coating the AgNWs network surface with a WS2 nanosheet dispersion, an annealing treatment is performed to evaporate the solvent and form a composite film. The preferred annealing temperature is 80–120°C, and the time is 5–20 min.

[0027] Specifically, the mechanical pressure treatment applies a pressure of 10–50 MPa, preferably 20 MPa, and holds the pressure for 5–30 seconds, preferably 15 seconds. This pressure allows for the physical compaction and embedding of the AgNWs network without damaging the structure of the WS2 nanosheets.

[0028] The mechanical pressure treatment can be carried out using a hydraulic press, pneumatic press, or precision tablet press, etc. The surface of the press plate is mirror polished to avoid introducing additional roughness.

[0029] The pressure-welded WS2-bridged silver nanowire composite transparent electrode prepared by the above method of the present invention has excellent comprehensive performance, with a sheet resistance of less than 20 Ω / sq, a transmittance of more than 92% at 550 nm, a quality factor (FOM) of more than 230, and a surface roughness (RMS) of less than 8 nm.

[0030] Meanwhile, this composite transparent electrode also exhibits excellent mechanical flexibility and environmental stability. After 1000 bending cycles with a 4mm bending radius, the resistance change rate (R / R0) is less than 1.1; after heating at 180℃ for 2.5 hours, the R / R0 is less than 1.3; after being placed at room temperature for 40 days, the R / R0 is less than 1.2; after 30 peels with 3M tape, the R / R0 is less than 1.5; and after ultrasonic treatment with ethanol for 40 minutes, the R / R0 is less than 2.0. These properties are significantly superior to those of pure AgNW electrodes and AgNWs / WS2 composite electrodes that have not undergone mechanical pressure treatment.

[0031] Furthermore, the present invention also provides the application of the pressure-welded WS2-bridged silver nanowire composite transparent electrode in the fabrication of flexible optoelectronic devices, particularly as an anode in the fabrication of high-performance flexible organic light-emitting diodes.

[0032] In application, a flexible OLED device can be obtained by sequentially depositing a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a cathode on the surface of the composite transparent electrode described in this invention as the anode.

[0033] The flexible OLED device constructed with the composite transparent electrode of this invention also possesses excellent comprehensive optoelectronic performance and mechanical stability. Compared with traditional transparent electrode-based devices, the external quantum efficiency and current efficiency of the flexible OLED device of this invention are significantly improved, and the device has a lower turn-on voltage. At the same time, the device has excellent mechanical flexibility, with outstanding resistance to bending, and minimal brightness decay after repeated bending.

[0034] The composite transparent electrode of the present invention can be adapted to various phosphorescent emission systems such as green light and red light, and has a wide range of applications.

[0035] Compared with the prior art, the present invention has the following outstanding advantages:

[0036] 1) In this invention, Ag-S covalent bonds are formed in the AgNW / WS2 composite system by mechanical pressure induction, which combines physical "rivet" embedding with chemical "welding", fundamentally solving the problems of high electrode junction resistance and weak interfacial interaction in traditional AgNWs, while making WS2 nanosheets firmly anchored to the AgNWs network.

[0037] 2) The composite transparent electrode prepared by this invention simultaneously achieves ultra-low sheet resistance, high transmittance, high FOM value and extremely low roughness. Compared with commercial ITO electrodes and AgNWs-based composite electrodes reported in related articles, its comprehensive photoelectric performance has obvious advantages.

[0038] 3) WS2 nanosheets not only act as conductive bridges to reduce junction resistance, but their excellent chemical inertness and thermal stability also protect AgNWs from oxidation and sulfidation. Mechanical pressure treatment further enhances the physical anchoring of AgNWs to the substrate, resulting in good stability. In harsh bending cycles, high-temperature heating, long-term storage, tape peeling and solvent ultrasonic treatment tests, they all showed stability far exceeding that of the control group, effectively overcoming the key bottleneck in the practical application of AgNWs electrodes.

[0039] 4) The composite transparent electrode of the present invention was applied to flexible phosphorescent OLED, which achieved extremely high external quantum efficiency (23.84% for green light and 24.68% for red light) and exhibited extremely low efficiency roll-off and excellent bending durability.

[0040] 5) This invention mainly adopts solution spin coating and mechanical pressing processes, which do not require complex high temperature or vacuum equipment. The main raw materials WS2 and AgNWs can be obtained through commercial means or easily prepared. The process conditions are mild, making it easy to achieve large-area, mass production, and is compatible with the roll-to-roll process of the flexible electronics industry. Attached Figure Description

[0041] Figure 1 This is a schematic diagram of the process flow for pressure welding of WS2 nanosheets to bridge silver nanowire composite transparent electrodes according to the present invention.

[0042] Figure 2 These are the performance characterization results of the WS2 nanosheets prepared in this invention.

[0043] Figure 3 These are the surface morphology characterization results of electrodes AgNWs, AgNWs / WS2, and P-AgNWs / WS2.

[0044] Figure 4 These are the results of interfacial chemical analysis between WS2 and electrodes AgNWs, AgNWs / WS2, and P-AgNWs / WS2.

[0045] Figure 5 This is a comparison of the photoelectric properties of electrodes ITO, AgNWs, P-AgNWs, AgNWs / WS2, and P-AgNWs / WS2.

[0046] Figure 6 These are the bending stability test results of different electrodes of this invention.

[0047] Figure 7 These are the test results of the thermal stability and air stability of different electrodes of this invention.

[0048] Figure 8 These are the adhesion stability test results of different electrodes of this invention.

[0049] Figure 9 This invention relates to the photoelectric luminescence performance of the green flexible OLED device.

[0050] Figure 10 This invention relates to the photoelectric luminescence performance of the red flexible OLED device.

[0051] Figure 11 These are the test results of the light emission uniformity of the large-area flexible OLED device of this invention.

[0052] Figure 12 These are the bending stability test results of different flexible OLED devices of this invention. Implementation

[0053] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings and specific examples. It should be noted that the embodiments are merely illustrative and are intended to provide a thorough understanding of the technical solutions of the present invention and to provide guidance for those skilled in the art to implement and apply the present invention. It should be understood that these descriptions do not constitute any limitation on the scope of protection of the present invention.

[0054] Unless otherwise expressly stated, the production processes, experiments, tests or analysis methods involved in the embodiments of the present invention are all considered to be conventional methods known to those skilled in the art, and only need to be implemented in accordance with conventional conditions or relevant product instructions. The steps and names involved are also generally clear and unambiguous in the art.

[0055] The instruments, equipment, raw materials, reagents, or samples used in the embodiments are not subject to any special restrictions on their source. They are all conventional products that can be purchased through regular commercial channels or prepared by known methods, and their source does not have a substantial impact on the implementation results of the present invention.

[0056] Unless otherwise expressly defined, the scientific and technical terms used in this invention have the meanings commonly understood by one of ordinary skill in the art. In case of any conflict, the definitions in this specification shall prevail.

[0057] The terms “comprising,” “including,” “having,” etc., used in this invention should be understood as open-ended, meaning “including but not limited to.” The term “and / or” includes any and all combinations of one or more of the associated listed items. Quantitative terms such as “a,” “one,” etc., do not exclude multiples; “multiple” or “a variety” refers to quantities greater than or equal to two.

[0058] This invention relates to the description of numerical parameters (such as quantity, concentration, temperature, time, etc.), and it should be understood that reasonable deviations naturally exist due to measuring instruments, operational errors, statistical fluctuations, etc. The range of such deviations should be within limits acceptable to those skilled in the art based on common sense.

[0059] The following specific embodiments of the present invention are in accordance with Figure 1 The process flow shown is used to prepare the pressure-welded WS2 nanosheet-bridged silver nanowire composite transparent electrode, which includes three main steps: AgNW spin coating, WS2 self-assembly, and mechanical pressure welding.

[0060] The pressure-welded WS2-bridged silver nanowire composite transparent electrode described in the following embodiments of the present invention is prepared according to the following steps:

[0061] S1: The flexible transparent substrate is treated with ultraviolet-ozone to enhance its wettability to AgNWs dispersion and WS2 nanosheet dispersion through surface hydrophilization treatment.

[0062] S2: AgNWs dispersion is uniformly coated onto the surface of a flexible transparent substrate using a solution film-forming method, and then annealing is performed to form an AgNWs network on the surface of the flexible transparent substrate.

[0063] S3: WS2 nanosheet dispersion is uniformly coated on the surface of the formed AgNWs network. During the solvent evaporation process of annealing, the WS2 nanosheets self-assemble to the AgNWs nodes through capillary force, forming a composite film containing AgNWs network and WS2 nanosheets on a flexible transparent substrate.

[0064] S4: The composite film is subjected to mechanical pressure treatment to densify the AgNWs network and partially embed it into the flexible transparent substrate. At the same time, the Ag atoms on the surface of AgNWs and the S atoms on the edge of WS2 are induced to undergo interfacial bonding reaction to form Ag-S covalent bonds, thus obtaining the pressure-welded WS2-bridged silver nanowire composite transparent electrode.

[0065] More specifically, the UV-ozone treatment time is preferably 5 to 15 minutes.

[0066] More specifically, the preferred spin coating speed is 1500 to 3500 rpm, more preferably 2500 rpm.

[0067] Specifically, the concentration of the AgNWs dispersion is preferably 1.0–2.0 mg / mL, more preferably 1.6 mg / mL. The annealing temperature is preferably 100–150 °C, and the time is 5–20 min.

[0068] Specifically, the concentration of the WS2 nanosheet dispersion is preferably 0.4–0.8 mg / mL, more preferably 0.6 mg / mL. The annealing temperature is preferably 80–120 °C, and the time is preferably 5–20 min.

[0069] Specifically, the mechanical pressure treatment applies a pressure of 10–50 MPa, preferably 20 MPa, and holds the pressure for 5–30 seconds, preferably 15 seconds. Example

[0070] Example 1

[0071] Weigh 35 mg of WS2 powder (purity 99.9%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and disperse it in 250 mL of ethanol / water mixed solvent (volume ratio of ethanol to water is 35:65) to obtain a dispersion.

[0072] The dispersion was placed in a cell disruptor and sonicated in an ice-water bath at 500W for 7 hours. Then it was centrifuged at 5000rpm for 5 minutes to remove large particles and aggregates that had not been separated, and the supernatant was collected.

[0073] The solvent in the supernatant was removed by rotary evaporation, and the supernatant was washed three times with deionized water to remove residual ethanol. The supernatant was then dried under vacuum at 60°C for 24 hours. WS2 nanosheet powder was prepared by liquid phase exfoliation.

[0074] Figure 2 The properties of the prepared WS2 nanosheets and its raw material WS2 powder were characterized. Figure 2 (a) The Raman spectrum shows that the bulk WS2 is located at 420.8 cm⁻¹. -1 Compared to the A1g peak, the A1g peak of WS2 nanosheets redshifts to 418.8 cm⁻¹. -1 This indicates that the interlayer coupling is weakened, and few-layer nanosheets were successfully obtained. Figure 2 The XRD pattern in (b) shows that, compared with the bulk WS2, the relative intensity of the (002) peak of the exfoliated nanosheets is significantly enhanced, while the other characteristic peaks are weakened, which confirms the preferred orientation and few-layer structure of the WS2 nanosheets along the c-axis. Figure 2 (c) is a low-magnification TEM image showing that the WS2 nanosheets are veil-like with clear edges and a lateral dimension of approximately 300–500 nm; while Figure 2 (d) The high-resolution TEM image shows clear lattice fringes with a lattice constant of 0.274 nm. The selected area electron diffraction (SAED) pattern in the inset shows clear hexagonal symmetric diffraction points, which together prove its good crystallinity. Finally, the morphology of the sample was characterized by scanning electron microscopy. Figure 2 (e) The WS2 mass exhibits as irregular, large-particle aggregates at the micrometer scale. After exfoliation, Figure 2 (f) The product is transformed into a nanosheet structure with obvious thin-layer characteristics, and the nanosheets are evenly distributed with no significant large-size bulk residues.

[0075] Example 2

[0076] A PET film (0.125 mm thick, purchased from Shenzhen Lelin Technology Co., Ltd.) was cut into 2 cm × 2 cm pieces and ultrasonically cleaned sequentially in deionized water, acetone, and isopropanol for 15 minutes each to remove organic and inorganic contaminants from the surface. Afterward, it was dried with nitrogen and then dried in a 60°C constant temperature drying oven. The dried PET substrate was then placed in a UV ozone cleaner and irradiated with UV light for 10 minutes to further remove residual organic matter from the substrate surface and improve the wettability of the substrate. After the above treatment, the water contact angle of the PET substrate decreased from 61.5° to 35.5°.

[0077] A commercial AgNWs isopropanol dispersion (30 nm diameter, 25 μm length, purchased from Beijing Bailingwei Technology Co., Ltd.) was diluted to a concentration of 1.6 mg / mL with isopropanol. 100 μL of the diluted dispersion was spin-coated onto a treated PET substrate at 2500 rpm for 60 s. The coated PET substrate was then placed on a 120°C hot plate and annealed for 10 min to allow complete solvent evaporation, resulting in a uniform AgNWs network film.

[0078] The WS2 nanosheet powder prepared in Example 1 was dispersed in deionized water to prepare a dispersion of 0.6 mg / mL, and ultrasonically dispersed for 30 min to ensure uniform dispersion. 100 μL of this dispersion was spin-coated onto the surface of the AgNWs network film at 2000 rpm for 60 s. After spin-coating, the film was allowed to stand at room temperature to allow the solvent to evaporate naturally. During evaporation, the WS2 nanosheets spontaneously migrated and self-assembled at the nodes of the AgNWs network under capillary force. The film was then annealed at 120°C for 10 min to ensure complete evaporation of moisture, resulting in the AgNWs / WS2 composite film.

[0079] The AgNWs / WS2 composite film was placed between two mirror-polished 304 stainless steel plates and then placed into a hydraulic press. A pressure of 20 MPa was applied and held for 15 seconds. After depressurization, the composite film was removed, thus obtaining the pressure-welded WS2 nanosheet-bridged silver nanowire composite transparent electrode film of the present invention, denoted as P-AgNWs / WS2.

[0080] The surface morphology, structure, and elemental distribution of the AgNWs, AgNWs / WS2, and P-AgNWs / WS2 films prepared in each of the above steps were characterized by atomic force microscopy (AFM), scanning electron microscopy (SEM), and energy dispersive spectroscopy (EDS), respectively. The results are as follows: Figure 3 As shown.

[0081] SEM images of thin films at different stages, Figure 3 (a) Pure AgNWs network thin film nanowires are randomly stacked to form a network structure, with obvious protrusions visible at the nodes, and the nanowires are in point contact with each other; Figure 3 (b) After WS₂ deposition, it can be seen that WS₂ nanosheets mainly cover the junctions of AgNWs, forming a bridging structure; Figure 3 (c) After mechanical pressure treatment, the AgNWs network becomes more compact, part of the nanowires are embedded in the PET substrate, the WS₂ nanosheets tightly wrap the junctions, and the entire thin film surface is smoother.

[0082] AFM images and roughness analysis further quantified the surface morphology changes. Figure 3 (d) The root mean square roughness (RMS) of the pure AgNWs network is as high as 26.6 nm, which mainly originates from the protrusions at the nanowire junctions; Figure 3 (e) After depositing WS₂ nanosheets, the RMS drops to 22.5 nm, indicating that WS₂ has a certain filling effect on the junction protrusions; Figure 3 (f) After mechanical pressure treatment, the RMS is greatly reduced to 7.1 nm, with a reduction of 73%. Meanwhile, the figure shows that the average height of the nanowires also decreases from 106.4 nm (AgNWs) and 84.9 nm (AgNWs / WS₂) to 36.3 nm (P-AgNWs / WS₂), which proves that the mechanical pressure effectively embeds the nanowires into the substrate and achieves surface planarization. The above roughness and average height values are all obtained by statistical analysis of the scanned images using the image analysis software matched with AFM.

[0083] Figure 3 The EDS element mapping images of (g-i) show that the Ag (green) and S (cyan) signals highly overlap at the junctions, confirming that WS₂ nanosheets selectively cover the AgNWs junctions rather than being uniformly distributed on the entire thin film surface, which provides a structural basis for junction welding.

[0084] Figure 4 X-ray photoelectron spectroscopy (XPS) was further used to analyze the interfacial chemical states of the thin films at the different stages described above.

[0085] Figure 4 In the XPS survey spectra of the WS₂, AgNWs, AgNWs / WS₂ and P-AgNWs / WS₂ thin films in (a), characteristic element peaks of all samples are clearly displayed, and no impurity peaks appear.

[0086] Figure 4 In the Ag 3d high-resolution XPS spectrum of (b), the Ag 3d of the pure AgNWs network 5 / 2 and Ag 3d 3 / 2The characteristic peaks are located at 367.9 and 373.9 eV, respectively; these two peaks in AgNWs / WS2 shift to 368.2 and 374.2 eV, respectively; and in P-AgNWs / WS2, they further shift to 368.4 eV and 374.4 eV. This positive shift indicates a decrease in the electron density around the Ag atom, with electrons transferring from Ag to S, proving the formation of the Ag-S bond.

[0087] Figure 4 In the high-resolution XPS spectrum of S 2p in (c), the S 2p of pure WS2... 3 / 2 and S 2p 1 / 2 The characteristic peaks are located at 162.3 and 163.4 eV, respectively; in AgNWs / WS2, these two peaks shift to 162.1 and 163.1 eV, respectively; while in P-AgNWs / WS2, in addition to the above two peaks, a new characteristic peak appears at 161.1 eV, which belongs to the S 2p signal in the Ag-S bond. This result directly proves that mechanical pressure treatment promotes the formation of Ag-S covalent bonds.

[0088] The characterization results above demonstrate that the sulfur atoms exposed at the edges of the WS2 nanosheets have unsaturated coordination and can form strong coordination bonds with silver atoms on the surface of AgNWs. This chemical anchoring effect is much stronger than the traditional van der Waals forces, providing a molecular basis for the excellent mechanical and environmental stability of the electrode.

[0089] Comparative Example 1

[0090] The AgNWs network film prepared in Example 2 was placed directly between 304 stainless steel plates without WS2 nanosheet deposition. After being held under pressure of 20 MPa for 15 seconds in a hydraulic press, the pressure was released and the film was removed to obtain a pressure-welded silver nanowire transparent electrode film, denoted as P-AgNWs.

[0091] Comparative Example 2

[0092] The AgNWs / WS2 composite film prepared in Example 2 was not subjected to mechanical pressure treatment. Instead, it was directly used as a transparent electrode film for WS2 nanosheet bridging silver nanowire composite, denoted as AgNWs / WS2.

[0093] Application Example 1

[0094] Using commercial flexible ITO as a control, the photoelectric properties of pure AgNWs, P-AgNWs, AgNWs / WS2, and P-AgNWs / WS2 films were tested. The sheet resistance of the films was measured using a four-probe tester. R S The transmittance of the thin film at a wavelength of 550 nm was recorded using a UV-Vis spectrophotometer. T And according to the formula FOM=188.5 / Rs ( T -1 / 2 -1) Calculate the film's quality factor (FOM) value, the result is as follows: Figure 5 As shown.

[0095] in, Figure 5 (a) shows the full-band transmittance spectra of various thin films. It can be seen that pure AgNWs and AgNWs / WS2 have the best transmittance, with transmittances of 94.9% and 94.1% at 550 nm, respectively; the transmittances of P-AgNWs and P-AgNWs / WS2 are 92.8% and 92.0%, respectively; while the transmittance of commercial ITO at 550 nm is 95.3%.

[0096] Figure 5 (b) A summary of the 550nm transmittance and sheet resistance of various thin films. R S The sheet resistance (FROM) values ​​are as follows: ITO: 45.2 Ω / sq, FROM 171.18; pure AgNWs: 36.8 Ω / sq, FROM 193.16; P-AgNWs: 26.8 Ω / sq, FROM 184.76; unpressurized AgNWs / WS2: 22.2 Ω / sq, FROM 275.03; and pressure-bonded P-AgNWs / WS2: 19.2 Ω / sq, FROM 230.61.

[0097] Compared with commercial ITO and various control films, P-AgNWs / WS2 has a further reduced sheet resistance. Although the light transmittance decreased slightly, resulting in a slight reduction in FOM, the overall optoelectronic performance was significantly improved. The reduction in light transmittance and FOM is still within an acceptable range.

[0098] Figure 5 (c) The sheet resistance thermodynamic distribution of pure AgNWs and P-AgNWs / WS2 over a large area of ​​5cm×5cm was further compared using a four-probe multi-point test. The results showed that the sheet resistance of the P-AgNWs / WS2 film was 19.6±3.2Ω / sq, and the overall resistance fluctuation was significantly better than that of the pure AgNWs film (35.7±8.4Ω / sq), indicating that the film formation process has excellent uniformity and is suitable for large-scale preparation.

[0099] Application Example 2

[0100] The overall stability of the P-AgNWs / WS2 electrode prepared in Example 2 was systematically tested, with pure AgNWs electrode, P-AgNWs electrode, AgNWs / WS2 electrode and commercial ITO electrode as controls.

[0101] Bending stability test:

[0102] To evaluate the mechanical flexibility of the electrodes, various electrodes were fixed on a self-made bending test platform and subjected to repeated bending cycle tests. Bending stability was evaluated in two ways: 1) The bending radius of the test platform was fixed at 4 mm and repeated bending cycle tests were performed. After each certain number of bends, the sheet resistance change of the electrode was measured, and the resistance change rate was characterized by R / R0; 2) Different bending radii from 2 to 10 mm were set, and the sheet resistance change was measured after each bending radius was continuously bent for 5 minutes to examine the change in resistance with the degree of bending.

[0103] Figure 6 In (a), the pure AgNWs electrode has a resistance change of about 1.25 after 1000 bends, while the P-AgNWs, AgNWs / WS2 and P-AgNWs / WS2 electrodes all show good bending stability. The resistance change of the AgNWs / WS2 electrode is about 1.15, the resistance change of the P-AgNWs / WS2 electrode is about 1.15, and the resistance change of the P-AgNWs / WS2 electrode is the smallest, with a resistance change of only 1.09 after 1000 bends.

[0104] Figure 6 (b) shows the resistance change after continuous bending for 5 minutes at different bending radii. The P-AgNWs / WS2 electrode maintained the lowest resistance change rate at all test radii, with R / R0 being only 1.07 even at an extreme bending radius of 2 mm.

[0105] Thermal stability and air stability tests:

[0106] Various electrodes were placed on a 180°C hot plate and heated, and the sheet resistance change was measured at regular intervals. Figure 7 In (a), the resistance of the pure AgNWs electrode increased sharply after heating for 1.5 h, while the P-AgNWs electrode performed slightly better but still deteriorated significantly after 2 h, with R / R0 exceeding 2.0. The AgNWs / WS2 and P-AgNWs / WS2 electrodes, on the other hand, exhibited excellent thermal stability. The R / R0 of the AgNWs / WS2 electrode was 1.54 after 2 h, while the resistance of the P-AgNWs / WS2 electrode remained almost unchanged within 2.5 h, with R / R0 remaining below 1.3. Further verification using SEM images showed that the pure AgNWs and P-AgNWs electrodes exhibited significant nanowire melting and spheroidization after heating, while the nanowire network of the P-AgNWs / WS2 electrode remained intact. This is attributed to the protective effect of WS2 and the stabilizing effect of the Ag-S bonds.

[0107] Then, various electrodes were stored in a room-temperature atmospheric environment, and the sheet resistance change was measured periodically. For example... Figure 7As shown in (b), the resistance of the pure AgNWs electrode began to increase significantly after 20 days, and the R / R0 approached 3.0 after 40 days; the performance of the P-AgNWs electrode improved slightly but was still not ideal, with the R / R0 exceeding 2.0 after 40 days; the AgNWs / WS2 and P-AgNWs / WS2 electrodes maintained good conductivity after 40 days, with the R / R0 of the P-AgNWs / WS2 electrode being only 1.498, indicating that the WS2 coating effectively prevented the oxidation and sulfidation of AgNWs.

[0108] Adhesion test:

[0109] Apply 3M tape to the electrode surface, apply uniform pressure, and then peel it off. Repeat this operation a certain number of times, and then measure the sheet resistance change. Figure 8 As shown in (a), the pure AgNWs electrode and the AgNWs / WS2 electrode exhibit similar behavior, with the resistance increasing sharply after one peel, indicating that both AgNWs and AgNWs / WS2 have extremely poor adhesion to the PET substrate. The P-AgNWs electrode shows a significant improvement in adhesion due to the partial embedding of nanowires into the substrate by mechanical pressing, with an R / R0 of approximately 1.79 after 30 peels. The P-AgNWs / WS2 electrode shows the best adhesion, with an R / R0 of only 1.45 after 30 peels. This is attributed to the possible interaction between the underlying WS2 and the PET substrate through hydrogen bonds, as well as the additional anchoring provided by the Ag-S bonds.

[0110] Then, the various electrodes were subjected to ultrasonic treatment in anhydrous ethanol, and the sheet resistance changes were measured at regular intervals. Figure 8 In (b), the pure AgNWs electrode was completely peeled off from the substrate within 5 min; the P-AgNWs electrode, due to the nanowire embedding, had significantly improved ultrasonic resistance and was still partially retained after 30 min; the P-AgNWs / WS2 electrode showed the best ultrasonic resistance, with an R / R0 of only 3.43 after 40 min, and its AgNWs network remained intact as shown by SEM images.

[0111] The above stability test results fully demonstrate that the present invention significantly improves the overall stability of AgNWs-based transparent electrodes through the synergistic strategy of WS2 bridging and mechanical pressure welding, laying a solid foundation for their practical application in harsh environments.

[0112] Application Example 3

[0113] Flexible phosphorescent OLED devices were fabricated using the P-AgNWs / WS2 composite transparent electrode prepared in Example 2 as the anode, and the device performance of different anodes was tested with commercial flexible ITO electrodes and P-AgNWs electrodes as controls.

[0114] Device structure: PET / anode (ITO, P-AgNWs or P-AgNWs / WS2) / MoO3 (3nm) / TAPC (100nm) / TCTA:Bepp2 (1:1, 20nm) : 6wt% Ir(ppy)3 (green light) or 4wt% Ir-RD (red light) / TPBi (45nm) / LiF (1nm) / Al (100nm).

[0115] A patterned anode substrate with an effective luminescent area of ​​3mm × 3mm was sequentially ultrasonically cleaned with deionized water, acetone, and isopropanol, dried with nitrogen, and then treated with UVO for 10 minutes. It was then transferred to a vacuum evaporation chamber and allowed to evaporate until the chamber vacuum level was below 5 × 10⁻⁶ mm. -4 At Pa, each functional layer is sequentially thermally vaporized, with the vaporization rate controlled as follows: organic material 1 Å / s, LiF 0.1 Å / s, MoO3 0.5 Å / s, Al 3~6 Å / s. The thickness of each layer is monitored online by a quartz crystal oscillator.

[0116] The current density-voltage-luminance (JVL) characteristics of the device were measured using a Keithley 2400 digital source meter and a BM-7A photometer; the electroluminescence spectrum of the device was measured using a PR655 spectroradiometer; the external quantum efficiency (EQE) was calculated from the JVL and spectral data.

[0117] Photoelectric luminescence performance of green flexible OLED devices:

[0118] Figure 9 The photoelectric performance of the green flexible OLED device was characterized, including EQE-brightness curves, normalized EL emission spectra, CIE color coordinates, and physical images of the green device emitting light.

[0119] The green phosphorescent flexible OLED fabricated using P-AgNWs / WS2 composite film as the anode material exhibits excellent luminescent performance. Figure 9 (a) The device exhibits a maximum external quantum efficiency (EQE) of 23.84%, a peak current efficiency of 83.7 cd / A, and a low turn-on voltage of 2.7 V. In contrast, conventional ITO-based green light devices have a maximum EQE of only 20.82%, a peak current efficiency of 73.3 cd / A, and a turn-on voltage of 3.0 V. Furthermore, the photoelectric performance of pure P-AgNWs devices without WS2 modification is further degraded, with a maximum EQE of only 16.72% and a current efficiency of only 58.7 cd / A. Figure 9 (b) The EL spectrum and color coordinate results prove that the composite anode material does not change the intrinsic emission wavelength and color purity of the green light-emitting layer, and the device has good light emission uniformity.

[0120] Photoelectric luminescence performance of red flexible OLED devices:

[0121] Figure 10 The photoelectric performance of the red flexible OLED device was characterized, including EQE-brightness variation curves, normalized EL spectra, CIE chromaticity diagrams, and real-world images of the red device's emission.

[0122] Figure 10 In (a), the red phosphorescent flexible OLED using P-AgNWs / WS2 anode has a peak EQE of 24.68%, a maximum current efficiency of 28.4 cd / A, and a turn-on voltage of only 2.8V. The performance of the two control devices is significantly different: the ITO-based red OLED has a maximum EQE of 18.15% and a current efficiency of 20.1 cd / A; while the pure P-AgNWs anode device has a peak EQE of only 14.43% and a current efficiency of only 17.1 cd / A. Figure 10 (b) Spectral testing confirms that the composite transparent electrode of the present invention is compatible with the red phosphorescence system, with no additional impurity peaks and stable luminescence color.

[0123] Light emission uniformity of large-area flexible OLED devices:

[0124] Figure 11 Photographs of a large-area P-AgNWs / WS2-based flexible OLED device with dimensions of 25mm×25mm are provided, showing its light emission in both flat and bent states.

[0125] As can be seen from the figure, the large-area device can achieve green or red light output with no dark spots and uniform brightness under both flat and curved conditions, which proves that the composite transparent electrode can be adapted to the fabrication of large-size flexible light-emitting panels and has the potential for large-scale production and practical application.

[0126] Bending mechanical stability:

[0127] Application Example 2 only conducted bending reliability tests on the P-AgNWs / WS2 composite transparent electrode film. For flexible OLED devices that include all organic functional layers and metal cathodes, the electrodes, multilayer organic films, and cathode films are simultaneously subjected to tensile / compressive stress during bending, which poses multiple failure risks such as multi-interface delamination and multilayer film cracking. This is more in line with the actual usage conditions of flexible display terminal products.

[0128] Figure 12 Bending performance tests were conducted on the green flexible OLED device (a) and the red flexible OLED device (b) respectively. The test conditions were uniform: bending radius of 4mm, no encapsulation treatment, and 1000 cycles of reciprocating bending.

[0129] After 1000 bending cycles, the relative brightness of the P-AgNWs / WS2 anode device remained at 79% for the green light device; while the ITO anode device experienced a precipitous decrease in brightness and failed after only 500 bending cycles. Under the same bending conditions, the brightness retention rate of the P-AgNWs / WS2-based red light device reached 81% after 1000 cycles.

[0130] Comparing the two control samples, the brightness decay of the pure P-AgNWs device after bending was significantly higher than that of the P-AgNWs / WS2 system, proving that the WS2 interlayer can simultaneously improve the mechanical stability of the AgNWs electrode and buffer the stress at the organic / electrode interface, thus greatly improving the bending life of the entire light-emitting device.

[0131] Application Example 4

[0132] To visually demonstrate the performance advantages of the P-AgNWs / WS2 composite transparent electrode of this invention as the anode of OLED devices, relevant literature on flexible OLEDs published in recent years has been collected, and the electrode materials and performance parameters of various devices are summarized in Table 1.

[0133] As can be seen from the comparison in Table 1, whether it is a green or red phosphorescent flexible OLED, the device of the present invention has better external quantum efficiency and current efficiency than most reported flexible light-emitting devices.

[0134] Meanwhile, most reported high-performance systems are small-sized devices with few bending cycles, and some high-performance devices cannot achieve flexible bending. This invention achieves both higher photoelectric efficiency and excellent unencapsulated bending stability in a large-area device of 25mm×25mm, and its overall performance is at the leading level among similar flexible phosphorescent OLEDs.

[0135]

[0136] 1. A. Kim, G. Huseynova, J. Lee, and JH Lee, "Enhancement of out-Coupling Efficiency of Flexible Organic Light-Emitting Diodes Fabricated onan MLA-Patterned Parylene Substrate," Organic Electronics 71 (2019): 246-250, https: / / dx.doi.org / 10.1016 / j.orgel.2019.05.025

[0137] 2、X. Feng, L. Wang, Y.Y.S. Huang, et al., "Cost-Effective Fabricationof Uniformly Aligned Silver Nanowire Microgrid-Based Transparent Electrodeswith Higher Than 99% Transmittance," Acs Applied Materials & Interfaces 14(2022): 39199-39210, https: / / dx.doi.org / 10.1021 / acsami.2c09672

[0138] 3、Z. Wu, Z. Niu, Y. Wang, et al., "Flexible OLED PerformanceEnhancement: The Impact of Ag NWs: Ag NPs Electrode-Integrated MoO X QDs Hole-Injection Layer," Acs Applied Materials & Interfaces 17 (2025): 10898-10906,https: / / dx.doi.org / 10.1021 / acsami.4c20334

[0139] 4、Y. Bai, Y. Chuai, Y. Wang, and Y. Wang, "Ultra-Smooth and EfficientNiO / Ag / NiO Transparent Electrodes for Flexible Organic Light-EmittingDevices," Micromachines 13 (2022): 1511, https: / / dx.doi.org / 10.3390 / mi13091511

[0140] 5、L.L. Chen, H. Yu, M. Dirican, et al., "Highly Transparent andColorless Nanocellulose / Polyimide Substrates with Enhanced Thermal andMechanical Properties for Flexible OLED Displays," Advanced Materials Interfaces7 (2020): 2000928, https: / / dx.doi.org / 10.1002 / admi.202000928

[0141] 6、D.J. Lee, I.S. Yoon, C.H. Park, et al., "Extraction of Light UsingRandom Nanocone on Poly(Vinyl-Butyral) for Flexible Oleds," Scientific Reports 9 (2019): 12312, https: / / dx.doi.org / 10.1038 / s41598-019-48808-8

[0142] 7、L. Wang, Y. Luo, X.M. Feng, et al., "Efficiency Enhancement ofFlexible OLEDs by Using Nano-Corrugated Substrates and Conformal AgTransparent Anodes," Aip Advances 8 (2018): https: / / dx.doi.org / 10.1063 / 1.5034484

[0143] 8、J. Lee, K. An, P. Won, et al., "A Dual-Scale Metal Nanowire NetworkTransparent Conductor for Highly Efficient and Flexible Organic LightEmitting Diodes," Nanoscale 9 (2017): 1978-1985, https: / / dx.doi.org / 10.1039 / c6nr09902e

[0144] 9、Y.N. Lai, C.H. Chang, P.C. Wang, and Y.H. Chu, "Highly EfficientFlexible Organic Light-Emitting Diodes Based on a High-Temperature DurableMica Substrate," Organic Electronics75 (2019): 105442, https: / / dx.doi.org / 10.1016 / j.orgel.2019.105442

[0145] 10、C. Xue, N. He, X. Zhao, et al., "Submicron-Thickness UltraflexibleOrganic Light-Emitting Diodes Via a Photoregulated Stripping Strategy," Acs Applied Materials & Interfaces 16 (2024): 14015-14025, https: / / dx.doi.org / 10.1021 / acsami.3c17782

[0146] 11、M.Y. Du, Z. Yang, Y.Q. Miao, et al., "Facile Nanowelding Processfor Silver Nanowire Electrodes toward High-Performance Large-Area FlexibleOrganic Light-Emitting Diodes," Advanced Functional Materials 34 (2024):2404567, https: / / dx.doi.org / 10.1002 / adfm.202404567

[0147] 12、Z. Yang, Y. Guo, W. Guo, et al., "MXene / AgNWs / MXene Sandwich-Structured Transparent Electrode for High-Performance Flexible OLEDs," Small 21 (2025): e2409621, https: / / dx.doi.org / 10.1002 / smll.202409621

[0148] 13、H.G. Kim, M. Kim, S.S. Kim, S.H. Paek, and Y.C. Kim, "SilverNanowire / PEDOT:PSS Hybrid Electrode for Flexible Organic Light-EmittingDiodes," Journal of Science-Advanced Materials and Devices 6 (2021): 372-378, https: / / dx.doi.org / 10.1016 / j.jsamd.2021.03.004

[0149] 14. L. Lian, D. Dong, S. Yang, B. Wei, and G. He, "Highly Conductiveand Uniform Alginate / Silver Nanowire Composite Transparent Electrode by RoomTemperature Solution Processing for Organic Light Emitting Diode," Acs Applied Materials & Interfaces 9 (2017): 11811-11818, https: / / dx.doi.org / 10.1021 / acsami.7b01159

[0150] 15. W. Cho, G. Sarada, H. Lee, et al., "Highly Efficient, Conventionaland Flexible Deep-Red Phosphorescent OLEDs Using Ambipolar Thiophene / Selenophene-Phenylquinoline Ligand-Based Ir(III) Complexes," Dyes and Pigments 136 (2017): 390-397, https: / / dx.doi.org / 10.1016 / j.dyepig.2016.08.060.

[0151] The above embodiments of the present invention do not describe all details exhaustively, nor do they limit the present invention to the embodiments described above. Various changes, modifications, substitutions, and variations made by those skilled in the art to these embodiments without departing from the principles and spirit of the present invention should be included within the scope of protection of the present invention.

Claims

1. A pressure-welded WS2-bridged silver nanowire composite transparent electrode, comprising a flexible transparent substrate, an AgNWs network embedded layer formed by mechanical pressure treatment and anchored on the surface of the flexible transparent substrate, and WS2 nanosheets bridged in the nodes and gaps of the AgNWs network embedded layer by Ag-S covalent bonds under mechanical pressure.

2. The pressure-welded WS2-bridged silver nanowire composite transparent electrode according to claim 1, characterized in that... The flexible transparent substrate is any one of polyethylene terephthalate, polyethylene naphthalate, polyimide, or polycarbonate.

3. The pressure-welded WS2-bridged silver nanowire composite transparent electrode according to claim 1, characterized in that... The WS2 nanosheets are few-layer nanosheets with 1 to 10 layers and a lateral dimension of 200 to 600 nm.

4. The method for preparing the pressure-welded WS2-bridged silver nanowire composite transparent electrode according to claim 1, comprising: S1: An AgNWs network is formed on the surface of a flexible transparent substrate; S2: Coat the surface of the AgNWs network with WS2 nanosheet dispersion, and use the capillary force generated by solvent evaporation to cause the WS2 nanosheets to self-assemble to the nodes of the AgNWs network to form a composite film; S3: Apply mechanical pressure to the composite film to embed and anchor the AgNWs network on the surface of the flexible transparent substrate to form an AgNWs network embedding layer, and induce Ag atoms on the surface of AgNWs to form Ag-S covalent bonds with S atoms on the edge of WS2 nanosheets to form the pressure-welded WS2 bridging silver nanowire composite transparent electrode.

5. The preparation method according to claim 4, characterized in that: AgNWs dispersions were uniformly coated onto the surface of a flexible transparent substrate using a solution film-forming method, and then annealed to evaporate the solvent and form an AgNWs network.

6. The preparation method according to claim 4, characterized in that: A WS2 nanosheet dispersion was uniformly coated onto the surface of an AgNWs network using a solution film-forming method, followed by annealing to evaporate the solvent and form a composite film.

7. The preparation method according to claim 4, characterized in that: The mechanical pressure is 10–50 MPa, and the pressure holding time is 5–30 seconds.

8. The preparation method according to claim 4, characterized in that: It also includes a step of hydrophilicating the surface of a flexible transparent substrate, wherein the hydrophilic treatment is ultraviolet-ozone treatment or oxygen plasma treatment.

9. The application of the pressure-welded WS2-bridged silver nanowire composite transparent electrode as described in claim 1 in the fabrication of flexible organic light-emitting diodes.

10. The application according to claim 9, characterized in that it is... The pressure-welded WS2 bridged silver nanowire composite transparent electrode serves as the anode, and a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a cathode are sequentially deposited on its surface.