A semiconductor packaging substrate and its preparation method
By bonding a film onto an insulating substrate and depositing a through electrode within the via using a chemical mechanical polishing process, the problem of substrate damage caused by carrier substrate peeling is solved, achieving the formation of a gapless through electrode with low damage risk, which is suitable for high-density semiconductor packaging.
Patent Information
- Application Number
- CN202611441929.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-10
AI Technical Summary
In forming a gapless through electrode, the existing technology has problems such as substrate damage and difficulty in peeling off the carrier substrate during the peeling process, which is especially difficult to achieve when the substrate is large-scale.
A film is bonded to the first surface of an insulating substrate using a chemical mechanical polishing process, and a through electrode is deposited in the via along the direction of the film pointing to the second surface. Finally, the film is removed by a chemical mechanical polishing process, avoiding the use of a carrier substrate and reducing thermal and mechanical loads.
Forming a seamless through-hole electrode within a high aspect ratio via reduces the risk of damage to the insulating substrate, enabling low-stress, damage-free film removal. This method is suitable for uniform removal of large-area substrates, avoiding over-abrasion or residue.
Smart Images

Figure CN123076263A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor packaging technology, and in particular to a semiconductor packaging substrate and its preparation method. Background Technology
[0002] Previously, semiconductor devices were packaged individually for each semiconductor chip. However, with the increasing integration of semiconductor devices, the method of mounting multiple chips on a semiconductor packaging substrate, such as an interposer, to form a single package has gradually become mainstream. Semiconductor packaging substrates are formed by providing multiple through electrodes on an insulator such as silicon, resin, or glass. Multilayer wiring patterns (rewiring layers) connected to the through electrodes are formed on both sides of this substrate. The wiring patterns on the front side are connected to each chip, for example, via bumps, while the wiring patterns on the back side are connected to an external printed circuit board, for example, via solder balls.
[0003] The through-electrode of the semiconductor packaging substrate is formed by the following method: a through-hole is first formed on the substrate, and a seed layer is formed on the inner wall surface of the through-hole by physical vapor deposition (PVD). Then, copper or the like is plated to fill the through-hole (e.g., Patent Document 1, Patent Document 2). However, with the increasing density of wiring patterns in the redistribution layer, the through-hole becomes narrower, resulting in an increase in the length-to-diameter ratio (aspect ratio) of the through-hole to, for example, around 10. During the plating process, plating growth is easily performed near the openings at both ends of the through-hole. Therefore, for through-holes with high aspect ratios, the following problem exists: the openings are first sealed by the plating layer, and the interior is not permeated with plating solution, easily creating cavities (voids) without Cu inside the through-hole (e.g., Patent Document 1, Patent Document 2). In addition, for through holes with high aspect ratio, there are the following problems: no seed layer is formed on the inner wall surface in the center of the through hole, resulting in a cavity (void) without Cu inside the through hole.
[0004] As a countermeasure, the following method (bottom-up method) is adopted: a carrier substrate with a seed layer on its surface is bonded to one side of a substrate using a low-melting-point metal or the like, thereby sealing one opening of the through-hole. Plating solution is supplied to the inside of the through-hole, causing the plating layer to grow from the seed layer on the carrier substrate inside the through-hole (e.g., Patent Document 1, Patent Document 2, Patent Document 3). In this case, no seed layer is needed on the inner wall of the through-hole, thus reducing the risk of the plating layer sealing the opening side and minimizing the risk of voids.
[0005] Existing technical documents Patent Document 1: Japanese Patent Application Publication No. 2004-119606 Patent Document 2: Japanese Patent Application Publication No. 2016-213283 Patent Document 3: Japanese Patent Publication No. 2018-501641 However, in the bottom-up method using a carrier substrate, the carrier substrate must first be bonded using a low-melting-point metal, requiring expensive materials and equipment. Furthermore, after filling the through-holes with a plating layer, the carrier substrate needs to be peeled off. For example, when a low-melting-point metal is used as the adhesive layer, the carrier is mechanically peeled off by heating to weaken the adhesion (Patent Document 2). However, in this peeling process, there is a risk of breakage due to the application of thermal / mechanical loads to the substrate, especially when the substrate is large, making peeling difficult. Summary of the Invention
[0006] This invention provides a semiconductor packaging substrate and its preparation method to solve the problems that the peeling process easily damages the substrate and that the carrier substrate is difficult to peel off when forming a gapless through electrode.
[0007] In a first aspect, the present invention provides a method for preparing a substrate for semiconductor packaging, the method comprising: An insulating substrate is provided; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending along the thickness direction of the insulating substrate, the through hole extending from the first surface to the second surface; A diaphragm is bonded to the first surface; the diaphragm seals the opening of the through-hole on the first surface; A through electrode is formed in the through hole along the direction of the diaphragm pointing to the second surface; the through electrode protrudes from the second surface; The through electrode protruding from the second surface is removed using a chemical mechanical polishing process; The film is removed using a chemical mechanical polishing process.
[0008] Optionally, a through electrode is formed within the via along the direction of the diaphragm pointing towards the second surface, including: Using an electrolytic plating process or an electroless plating process, a through electrode is deposited and grown in the via along the direction of the film pointing to the second surface.
[0009] Optionally, before bonding the diaphragm to the first surface, the following steps are also included: An adhesion reinforcement layer is formed on the first surface; the vertical projection of the adhesion reinforcement layer on the first surface does not overlap with the vertical projection of the through hole on the first surface. A film is bonded to the first surface, including: The film is bonded to the side of the adhesion reinforcement layer away from the first surface; The chemical mechanical polishing process removes the film and also includes: The adhesion reinforcement layer is removed using the aforementioned chemical mechanical polishing process.
[0010] Optionally, an adhesion enhancement layer is formed on the first surface, comprising: An adhesion enhancement layer is formed on the first surface using a plating process or a vapor deposition process. A film is bonded to the side of the attachment reinforcement layer away from the first surface, including: By using at least one of surface activation bonding process, plasma activation bonding process, solid-liquid interdiffusion bonding process, and transient liquid phase diffusion bonding process, a membrane is bonded to the side of the adhesion reinforcement layer away from the first surface, so that the side of the adhesion reinforcement layer away from the first surface and the opening of the through hole on the first surface are provided with a membrane.
[0011] Optionally, before bonding the film to the side of the adhesion reinforcement layer away from the first surface using a surface activation bonding process, plasma activation bonding process, solid-liquid interdiffusion bonding process, or transient liquid phase diffusion bonding process, the method further includes: Provide temporary substrate; The diaphragm is attached to one side of a temporary substrate using an adhesive layer; Bonding a film to the side of the adhesion reinforcement layer away from the first surface using surface activation bonding, plasma activation bonding, solid-liquid interdiffusion bonding, or transient liquid phase diffusion bonding includes: An insulating substrate with an attachment reinforcement layer and a temporary substrate with a film are placed in a surface activation bonding apparatus, a plasma activation bonding apparatus, a solid-liquid interdiffusion bonding apparatus, or a transient liquid phase diffusion bonding apparatus, so that the film is bonded to the side of the attachment reinforcement layer away from the first surface; wherein the attachment reinforcement layer and the film are placed opposite each other. A laser is used to peel off the temporary substrate.
[0012] Optionally, after attaching the film to the side of the reinforcing layer away from the first surface, the method further includes: An insulating substrate having an adhesion reinforcement layer formed on its first surface and a film bonded to the side of the adhesion reinforcement layer away from the first surface is subjected to annealing treatment.
[0013] Optionally, the insulating substrate is subjected to annealing treatment, including: A first heating plate is disposed on the second surface, and a second heating plate is disposed on the side of the diaphragm away from the first surface; Annealing of the insulating substrate is achieved by applying a first temperature and a first pressure.
[0014] Optionally, a film is bonded to the first surface, comprising: A film with a thickness of 10um-35um is bonded to the first surface; wherein the film includes a copper film or an aluminum film; A through electrode is formed within the via along the direction of the diaphragm pointing towards the second surface, including: A through-hole copper electrode is formed in the direction of the diaphragm pointing to the second surface.
[0015] Optionally, an adhesion enhancement layer is formed on the first surface, comprising: At least one of the following is formed on the first surface: a copper layer, an indium layer, a tin layer, a silver layer, a gold layer, a tantalum-copper composite layer, and a titanium-copper composite layer.
[0016] Optionally, the insulating substrate is a glass substrate.
[0017] Optionally, when depositing and growing through electrodes in the vias along the direction of the film pointing to the second surface using an electrolytic plating process, the film is used as the cathode for electrolytic plating.
[0018] Secondly, the present invention provides a semiconductor packaging substrate, wherein the semiconductor packaging substrate is manufactured using the semiconductor packaging substrate preparation method provided in any embodiment of the present invention.
[0019] The technical solution of this invention involves bonding a film to the first surface of an insulating substrate, depositing a through-electrode in the via from bottom to top along the direction of the film pointing to the second surface, and finally removing the film using a chemical mechanical polishing (CMP) process. This invention allows for bottom-to-top deposition without using an existing carrier substrate, and creates a gapless through-electrode within the high aspect ratio via. Therefore, this invention eliminates the need for carrier substrate bonding and peeling processes. The film in this invention can be removed using CMP, which applies extremely low thermal and mechanical loads to the insulating substrate during semiconductor packaging substrate fabrication, resulting in a very low risk of damage. Furthermore, the CMP process, through the synergistic effect of chemical etching and mechanical polishing, enables low-stress, non-damaging removal of the film across the entire surface. Even on large-area insulating substrates, complete and uniform removal is easily achieved without over-polishing or residue risks.
[0020] It should be understood that the description in this section is not intended to identify key or essential features of the embodiments of the present invention, nor is it intended to limit the scope of the invention. Other features of the invention will become readily apparent from the following description. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 1 of the present invention; Figures 2-6 This is a schematic diagram of the structure corresponding to each step in the preparation method of a semiconductor packaging substrate provided in Embodiment 1 of the present invention; Figure 7 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 2 of the present invention; Figure 8 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 3 of the present invention; Figures 9-12 This is a schematic diagram of some steps in the preparation method of a semiconductor packaging substrate provided in Embodiment 3 of the present invention; Figure 13 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 4 of the present invention; Figure 14 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 5 of the present invention; Figures 15-17 This is a schematic diagram of some steps in the preparation method of a semiconductor packaging substrate provided in Embodiment 5 of the present invention; Figure 18 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment Six of the present invention; Figure 19 This is a schematic diagram of some steps in the preparation method of a semiconductor packaging substrate provided in Embodiment Six of the present invention.
[0023] Explanation of reference numerals in the attached figures 100: Substrate for semiconductor packaging; 10: Insulating substrate; 11: Through hole; 101: First surface; 102: Second surface; 20: Film; 12: Through electrode; 30: Adhesive reinforcement layer; 40: Temporary substrate; 50: Adhesive layer; 61: First heating plate; 62: Second heating plate. Detailed Implementation
[0024] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0025] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.
[0026] Example 1 Figure 1 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 1 of the present invention. Figures 2-6 This is a schematic diagram of the structure corresponding to each step in the preparation method of a semiconductor packaging substrate provided in Embodiment 1 of the present invention, as shown below. Figure 1 As shown, the preparation method includes: S100: Provide an insulating substrate; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending through the thickness direction of the insulating substrate from the first surface to the second surface.
[0027] Specifically, such as Figure 2 As shown, an insulating substrate 10 is first provided. The insulating substrate 10 may include a glass substrate, which is an insulating substrate with excellent smoothness and shape stability, such as quartz glass or alkali-free glass. After encapsulation, the glass substrate will not warp due to temperature rise during use, avoiding the risk of the substrate detaching from the connected redistribution layer. Furthermore, glass substrates are easy to form high-density redistribution layers. In some embodiments of the present invention, the insulating substrate 10 may also be formed of other insulating materials, including silicon substrates, quartz (SiO2) substrates, alumina (Al2O3) substrates, silicon carbide (SiC) substrates, or resin substrates.
[0028] A through hole 11 is formed on the provided insulating substrate 10, extending through the thickness direction of the insulating substrate 10. The through hole 11 extends from the first surface 101 of the insulating substrate 10 to the second surface 102 of the insulating substrate 10.
[0029] The method for forming the via 11 in this embodiment of the invention may include photolithography. During photolithography, a photoresist is first coated on the surface of the insulating substrate 10. Then, using an exposure device, a pattern corresponding to the top view position and shape of the via 11 is exposed onto the photoresist, followed by development and baking, thereby forming a pattern corresponding to the top view position and shape of the via 11 on the photoresist. Next, the photoresist with the above pattern is used as a mask to etch the insulating substrate 10, thereby forming the via 11. For the etching process, a wet etching process can be used when the length-to-diameter ratio of the via 11 is low, and a reactive ion etching (RIE) process is preferred when the length-to-diameter ratio of the via 11 is high.
[0030] In some embodiments of the present invention, the method for forming the through-hole 11 is not limited to photolithography. For example, when the insulating substrate 10 is a resin substrate, the through-hole 11 can be formed by drilling or other methods. When the insulating substrate 10 is a glass substrate, selective laser etching (SLE) can also be used to irradiate the area on the glass substrate where the through-hole 11 needs to be formed with a laser to modify the glass, and then etch away the modified part with hydrofluoric acid or potassium hydroxide aqueous solution to form the through-hole 11.
[0031] S110: A diaphragm is joined to the first surface; the diaphragm seals the opening of the through hole on the first surface.
[0032] Specifically, such as Figure 3 As shown, after forming the through-hole 11, a diaphragm 20 can be bonded to the first surface 101 of the insulating substrate 10 to seal the opening of the through-hole 11 on the first surface 101. For example, when bonding the diaphragm 20 to the first surface 101 of the insulating substrate 10, any existing adhesive material can be applied to the first surface 101 of the insulating substrate 10, and then the adhesiveness of the adhesive material can be used to bond the diaphragm 20 to the first surface 101 of the insulating substrate 10. The diaphragm 20 may include a copper diaphragm or an aluminum diaphragm, etc., and is not specifically limited here.
[0033] S120: A through electrode is formed in the through hole along the direction of the diaphragm pointing to the second surface; the through electrode protrudes from the second surface.
[0034] Specifically, such as Figure 4As shown, in this embodiment of the invention, a seamless conductive through-electrode 12 can be formed within the through-hole 11 using a plating process, along the direction from the diaphragm 20 toward the second surface 102. The through-electrode 12 can fill the through-hole 11 and protrude from the opening of the through-hole 11 onto the second surface 102. Preferably, the formation of the through-electrode 12 is stopped immediately after it protrudes from the second surface.
[0035] For example, the through electrode 12 can be a copper electrode. In the fabrication of the redistribution layer, as the redistribution layer becomes smaller, it mostly uses copper wiring with low resistivity. When the through electrode 12 is a copper electrode, the connectivity between the redistribution layer and the through electrode 12 can be improved. In some embodiments of the present invention, the through electrode 12 can also be any other conductive metal material such as aluminum or solder.
[0036] S130: The through electrode protruding from the second surface is removed using a chemical mechanical polishing process.
[0037] Specifically, such as Figure 5 As shown, a chemical mechanical polishing (CMP) process is used to remove the through electrode 12 protruding from the second surface 102, so that the end face of the through electrode 12 is flush with the second surface 102. The CMP process can be a method of polishing the workpiece flat by flowing a slurry containing chemicals and abrasive particles while contacting and rotating a polishing pad with the insulating substrate 10, which is the workpiece to be polished. The through electrode 12 protruding from the second surface 102 can be removed using the CMP process.
[0038] S140: Remove the film using a chemical mechanical polishing process.
[0039] Specifically, such as Figure 5 and Figure 6 As shown, after the through electrode 12 is fabricated, the film 20 can be removed using a CMP process. Using a CMP process, the film 20 bonded to the first surface 101 can be removed, so that the end face of the through electrode 12 is flush with the first surface 101, thereby forming a semiconductor packaging substrate 100.
[0040] During the CMP process to remove the membrane 20, the adhesive material used to bond the insulating substrate 10 and the membrane 20 can be removed. In some embodiments of the invention, at least a portion of the adhesive material can also be completely removed using additional cleaning steps; for example, plasma ashing removal process can be used to remove the adhesive material.
[0041] The technical solution of this invention involves bonding a film 20 to the first surface 101 of an insulating substrate 10, and depositing a through electrode 12 from bottom to top within the through hole 11 along the direction of the film 20 pointing to the second surface 102. Finally, a chemical mechanical polishing (CMP) process is used to remove the film 20. This invention allows for bottom-to-top deposition without using an existing carrier substrate. A gapless through electrode 12 can be formed within the high aspect ratio through hole. Therefore, this invention eliminates the need for carrier substrate bonding and peeling processes. The film 20 in this invention can be removed using the CMP process. During the fabrication of the semiconductor packaging substrate 100, the thermal and mechanical loads applied to the insulating substrate 10 are extremely low, resulting in a very low risk of damage to the insulating substrate 10. Furthermore, the CMP process, through the synergistic effect of chemical etching and mechanical polishing, can remove the film 20 across the entire surface with low stress and without damage. Even on a large area of the insulating substrate 10, complete and uniform removal can be easily achieved without over-polishing or residue risks.
[0042] Example 2 Optionally, based on the above embodiments, Figure 7 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 2 of the present invention, as shown below. Figure 7 As shown, the preparation method includes: S200: Provide an insulating substrate; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending through the thickness direction of the insulating substrate from the first surface to the second surface.
[0043] S210: A diaphragm is joined to the first surface; the diaphragm seals the opening of the through hole on the first surface.
[0044] S220: Using an electrolytic plating process or an electroless plating process, a through electrode is deposited and grown in the through hole along the direction of the film pointing to the second surface; the through electrode protrudes from the second surface.
[0045] Specifically, such as Figure 4 As shown, in this embodiment of the invention, a plating layer can be formed in the through hole 11 by plating process on the basis of the diaphragm 20 along the direction of the diaphragm 20 pointing to the second surface 102. The plating layer can fill the through hole 11 and protrude from the opening of the through hole 11 at the second surface 102, thereby forming a through electrode 12 with no gaps protruding from the second surface 102.
[0046] The plating process can include electroplating or electroless plating. In the electroplating process, the film 20 is conductive and can serve as a cathode. Metal ions in the electroplating solution can migrate to the surface of the film 20, be reduced to metal atoms, and deposit on the surface of the film 20. This allows metal to be electroplated and grown within the through-hole 11 along the direction of the film 20 towards the second surface 102, thereby forming the through electrode 12. This process facilitates the management of the growth of the through electrode 12. Furthermore, plating can be stopped immediately after the through electrode 12 protrudes from the second surface 102, thus suppressing the amount of material removed by chemical mechanical polishing.
[0047] In this embodiment of the invention, an electroless plating process can be used when the aspect ratio of the through hole 11 is low. For the electroless plating process, the membrane 20 may include a catalytically active material, which itself acts as an activation source. Metal ions in the chemical plating solution are reduced and deposited on the surface of the membrane 20, growing from the membrane 20 and along the direction of the membrane 20 toward the second surface 102, thereby growing metal in the through hole 11 to form the through electrode 12.
[0048] S230: The through electrode protruding from the second surface is removed using a chemical mechanical polishing process.
[0049] S240: Using chemical mechanical polishing process, the film is removed to form a substrate for semiconductor packaging.
[0050] Through the above processes, one end face of the through electrode 12 is flush with the first surface 101, and the other end face is flush with the second surface 102. Both end faces of the through electrode 12 are exposed, forming a semiconductor packaging substrate 100. Through the two-step CMP process (S230 and S240), the first surface 101 and the second surface 102 of the insulating substrate 10 can achieve good flatness and smoothness. Therefore, fine redistribution patterns can be formed on both sides of the insulating substrate 10, enabling the fabrication of a semiconductor packaging substrate 100 suitable for high-density mounting.
[0051] Example 3 Optionally, based on the above embodiments, Figure 8 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 3 of the present invention. Figures 9-12 This is a schematic diagram of some steps in the preparation method of a semiconductor packaging substrate provided in Embodiment 3 of the present invention, as shown in the diagram. Figure 8 As shown, the preparation method includes: S300: Provide an insulating substrate; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending through the thickness direction of the insulating substrate from the first surface to the second surface.
[0052] S310: An adhesion reinforcement layer is formed on the first surface; the vertical projection of the adhesion reinforcement layer on the first surface does not overlap with the vertical projection of the through hole on the first surface.
[0053] Specifically, such as Figure 9 As shown, after forming the through-hole 11, in order to improve the adhesion between the subsequent diaphragm 20 and the insulating substrate 10, an adhesion reinforcement layer 30 is first formed on the first surface 101 of the insulating substrate 10. The adhesion reinforcement layer 30 does not cover the opening of the through-hole 11 on the first surface 101. For example, the material of the adhesion reinforcement layer 30 can be the same metal material as the diaphragm 20, or it can be a low-melting-point metal material or an easily manufactured metal material. The material of the adhesion reinforcement layer 30 can also be an alloy material; no specific limitations are made here. The process of forming the adhesion reinforcement layer 30 on the first surface 101 can include processes such as plating or vapor deposition.
[0054] S320: A diaphragm is bonded on the side of the attachment reinforcement layer away from the first surface, and the diaphragm seals the opening of the through hole on the first surface.
[0055] Specifically, such as Figure 10 As shown, a diaphragm 20 is joined to the side of the adhesion reinforcement layer 30 away from the first surface 101 and to the opening of the through hole 11 on the first surface 101, thereby sealing the opening of the through hole 11 on the first surface 101 by the diaphragm 20. Exemplarily, embodiments of the present invention can utilize processes such as surface activation bonding, plasma activation bonding, solid-liquid interdiffusion bonding, and transient liquid phase diffusion bonding to join the diaphragm 20 to the side of the adhesion reinforcement layer 30 away from the first surface 101.
[0056] S330: Using an electrolytic plating process or an electroless plating process, a through electrode is deposited and grown in the through hole along the direction of the film pointing to the second surface; the through electrode protrudes from the second surface.
[0057] Specifically, such as Figure 11 As shown, in this embodiment of the invention, a through electrode 12 can be formed in the through hole 11 using a plating process, along the direction from the diaphragm 20 to the second surface 102. In this case, the through electrode 12 protrudes from both the first surface 101 and the second surface 102.
[0058] S340: The through electrode protruding from the second surface is removed using a chemical mechanical polishing process.
[0059] Specifically, such as Figure 12 As shown, the through electrode 12 protruding from the second surface 102 is removed by CMP process, so that the end face of the through electrode 12 is flush with the second surface 102.
[0060] S350: Uses chemical mechanical polishing to remove the film and the attached reinforcement layer.
[0061] Specifically, such as Figure 12 and Figure 6 As shown, in this embodiment of the invention, the film 20, the attached reinforcement layer 30, and the through electrode 12 protruding from the first surface 101 can be removed using the CMP process. One end face of the through electrode 12 is flush with the first surface 101, and the other end face is flush with the second surface 102. At the same time, both end faces of the through electrode 12 are exposed, thereby forming a semiconductor packaging substrate 100.
[0062] The technical solution of this invention first forms an adhesion reinforcement layer 30 on the first surface 101 of the insulating substrate 10 through processes such as plating or deposition. Then, the diaphragm 20 can be bonded to the side of the adhesion reinforcement layer 30 away from the first surface 101 using processes such as surface activation bonding, plasma activation bonding, solid-liquid interdiffusion bonding, and transient liquid phase diffusion bonding. This invention allows the bonding of the diaphragm 20 to be performed at low temperature and low pressure. Therefore, the bonding of the diaphragm 20 can be reliably performed without applying large thermal or mechanical loads to the insulating substrate 10, thereby effectively avoiding damage to the insulating substrate 10.
[0063] Example 4 Optionally, based on the above embodiments, Figure 13 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 4 of the present invention, as shown below. Figure 13 As shown, the preparation method includes: S400: Provides an insulating substrate; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending through the thickness direction of the insulating substrate from the first surface to the second surface.
[0064] S410: An adhesion reinforcement layer is formed on the first surface using a plating process or a vapor deposition process; the vertical projection of the adhesion reinforcement layer on the first surface does not overlap with the vertical projection of the through hole on the first surface.
[0065] Specifically, such as Figure 9 As shown, in order to improve the adhesion between the subsequent film 20 and the insulating substrate 10, an adhesion enhancement layer 30 is first formed on the first surface 101 of the insulating substrate 10. The process of forming the adhesion enhancement layer 30 on the first surface 101 may include processes such as plating and vapor deposition.
[0066] S420: Using at least one of surface activation bonding process, plasma activation bonding process, solid-liquid interdiffusion bonding process, and transient liquid phase diffusion bonding process, a diaphragm is bonded to the side of the adhesion reinforcement layer away from the first surface, and the diaphragm seals the opening of the through hole on the first surface, so that the side of the adhesion reinforcement layer away from the first surface and the opening of the through hole on the first surface are provided with a diaphragm.
[0067] Specifically, such as Figure 10 As shown, the material of the attachment reinforcement layer 30 can be the same metal material as the membrane 20 or an easily fabricated metal material. In this case, the thickness of the metal material serving as the attachment reinforcement layer 30 can be arbitrarily set, as long as it meets the requirements for subsequent surface activation bonding or plasma activation bonding with the membrane 20. Alternatively, the material of the attachment reinforcement layer 30 can be an alloy material. In this case, the thickness of the single-layer metal in the alloy material that needs to be subsequently bonded to the membrane 20 can be arbitrarily set, as long as it meets the requirements for subsequent surface activation bonding or plasma activation bonding with the membrane 20. For example, the thickness of the metal layer in the attachment reinforcement layer 30 that needs to be surface activated bonding or plasma activation bonding with the membrane 20 can be 0.1µm-3µm.
[0068] The technical solution of this invention can utilize surface activated bonding (SAB) or plasma activated bonding (PAB) processes to bond the diaphragm 20 to the side of the adhesion reinforcement layer 30 away from the first surface 101. Both surface activated bonding and plasma activated bonding processes involve surface treatment of the bonding surface in a vacuum to activate it, thereby bonding the bonding surfaces without applying adhesives, high temperatures, or high pressures. This invention can utilize surface activated bonding or plasma activated bonding processes to bond the diaphragm 20 to the side of the adhesion reinforcement layer 30 away from the first surface 101 without applying adhesives, high temperatures, or high pressures.
[0069] The material of the attachment reinforcement layer 30 may also include a low-melting-point metal material. For example, the material of the attachment reinforcement layer 30 may include metal materials such as indium and tin. In this case, embodiments of the present invention can utilize solid-liquid inter-diffusion (SLID) bonding and transient liquid phase (TILP) bonding processes to bond the film 20 to the side of the attachment reinforcement layer 30 away from the first surface 101. During the bonding process, the temperature can be raised above the melting point of the attachment reinforcement layer 30 by heating, causing the metal to become a liquid phase, thereby bonding the film 20.
[0070] The technical solution of this invention first forms an adhesion reinforcement layer 30 on the first surface 101 of the insulating substrate 10 through processes such as plating or deposition. Then, the diaphragm 20 can be bonded to the side of the adhesion reinforcement layer 30 away from the first surface 101 using processes such as surface activation bonding, plasma activation bonding, solid-liquid interdiffusion bonding, and transient liquid phase diffusion bonding. This invention allows the bonding of the diaphragm 20 to be performed at low temperature and low pressure. Therefore, the bonding of the diaphragm 20 can be reliably performed without applying large thermal or mechanical loads to the insulating substrate 10, thereby effectively avoiding damage to the insulating substrate 10.
[0071] S430: Using an electrolytic plating process or an electroless plating process, a through electrode is deposited and grown in the through hole along the direction of the film pointing to the second surface; the through electrode protrudes from the second surface.
[0072] S440: The through electrode protruding from the second surface is removed using a chemical mechanical polishing process.
[0073] S450: Uses chemical mechanical polishing to remove the film and the attached reinforcement layer.
[0074] Example 5 Optionally, based on the above embodiments, Figure 14 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment 5 of the present invention. Figures 15-17 This is a schematic diagram of some steps in the method for preparing a semiconductor packaging substrate provided in Embodiment 5 of the present invention, as shown in the diagram. Figure 14 As shown, the preparation method includes: S500: Provides an insulating substrate; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending through the thickness direction of the insulating substrate from the first surface to the second surface.
[0075] S510: An adhesion reinforcement layer is formed on the first surface; the vertical projection of the adhesion reinforcement layer on the first surface does not overlap with the vertical projection of the through hole on the first surface.
[0076] S520: Provide a temporary substrate; attach the film to one side of the temporary substrate via an adhesive layer.
[0077] Specifically, such as Figure 15 As shown, in the process of bonding the film 20 and the reinforcement layer 30 using surface activation bonding, plasma activation bonding, solid-liquid interdiffusion bonding, or transient liquid phase diffusion bonding, the film 20 can first be attached to the temporary substrate 40 via the adhesive layer 50. For example, the temporary substrate 40 may include a glass substrate, etc., and the adhesive layer 50 may include a polyimide layer, etc.
[0078] S530: An insulating substrate with an attachment reinforcement layer and a temporary substrate with a diaphragm are placed in a surface activation bonding apparatus, a plasma activation bonding apparatus, a solid-liquid interdiffusion bonding apparatus, or a transient liquid phase diffusion bonding apparatus, so that the diaphragm is bonded to the side of the attachment reinforcement layer away from the first surface; the diaphragm seals the opening of the through hole on the first surface.
[0079] Specifically, such as Figure 15 and Figure 16 As shown, the insulating substrate 10 with the attachment reinforcement layer 30 and the temporary substrate 40 with the diaphragm 20 can then be placed in a vacuum chamber of a surface activation bonding apparatus (not shown) or a plasma activation bonding apparatus (not shown), and the surfaces of the diaphragm 20 and the attachment reinforcement layer 30 are arranged in a two-sided facing state. In this state, while activating the surfaces of the diaphragm 20 and the attachment reinforcement layer 30 by atomic beam bombardment, ion beam bombardment, or plasma treatment, the surfaces of the diaphragm 20 and the attachment reinforcement layer 30 are brought into contact, thereby bonding the surfaces of the diaphragm 20 and the attachment reinforcement layer 30.
[0080] In this embodiment of the invention, the insulating substrate 10 with the attachment reinforcement layer 30 and the temporary substrate 40 with the film 20 can also be placed in a solid-liquid interdiffusion bonding device (not shown in the figure) or a transient liquid phase diffusion bonding device (not shown in the figure), and the surface of the film 20 and the surface of the attachment reinforcement layer 30 can be bonded by the solid-liquid interdiffusion bonding process or the transient liquid phase diffusion bonding process.
[0081] S540: Uses a laser to peel off the temporary substrate.
[0082] Specifically, such as Figure 17 As shown, after bonding the surface of the diaphragm 20 and the surface of the attached reinforcing layer 30, the... Figure 16 The completed structure shown is placed in a laser stripping device. The laser breaks the adhesive layer 50 between the temporary substrate 40 and the diaphragm 20, thereby separating the insulating substrate 10 with the diaphragm 20 attached from the temporary substrate 40, thus achieving the bonding of the diaphragm 20 to the side of the attachment reinforcement layer 30 away from the first surface 101.
[0083] The technical solution of this invention uses a surface activation bonding process, a plasma activation bonding process, a solid-liquid interdiffusion bonding process, or a transient liquid phase diffusion bonding process to bond the film 20 to the side of the attachment reinforcement layer 30 away from the first surface 101, and uses a laser peeling process to peel off the temporary substrate 40. This process is low temperature and low pressure, and does not apply a large thermal load or mechanical load to the insulating substrate 10, so it will not damage the film 20 and the insulating substrate 10, and can safely bond the film 20 to the side of the attachment reinforcement layer 30 away from the first surface 101.
[0084] S550: Using an electrolytic plating process or an electroless plating process, a through electrode is deposited and grown in the through hole along the direction of the film pointing to the second surface; the through electrode protrudes from the second surface.
[0085] S560: The through electrode protruding from the second surface is removed using a chemical mechanical polishing process.
[0086] S570: Uses chemical mechanical polishing to remove the film and the attached reinforcement layer.
[0087] Example 6 Optionally, based on the above embodiments, Figure 18 This is a flowchart of a method for preparing a semiconductor packaging substrate according to Embodiment Six of the present invention. Figure 19 This is a schematic diagram of some steps in the method for preparing a semiconductor packaging substrate provided in Embodiment Six of the present invention, as shown below. Figure 18 As shown, the preparation method includes: S600: Provides an insulating substrate; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending through the thickness direction of the insulating substrate from the first surface to the second surface.
[0088] S610: An adhesion reinforcement layer is formed on the first surface; the vertical projection of the adhesion reinforcement layer on the first surface does not overlap with the vertical projection of the through hole on the first surface.
[0089] S620: A diaphragm is bonded on the side of the attachment reinforcement layer away from the first surface, and the diaphragm seals the opening of the through hole on the first surface.
[0090] S630: An insulating substrate having an adhesion reinforcement layer formed on its first surface and a film bonded to the side of the adhesion reinforcement layer away from the first surface is subjected to an annealing process.
[0091] Specifically, such as Figure 19 As shown, a diaphragm 20 is joined to the side of the adhesion reinforcement layer 30 away from the first surface 101 and to the opening of the through hole 11 on the first surface 101, thereby sealing the opening of the through hole 11 on the first surface 101. Exemplarily, embodiments of the present invention can utilize processes such as surface activation bonding, plasma activation bonding, solid-liquid interdiffusion bonding, and transient liquid phase diffusion bonding to join the diaphragm 20 to the side of the adhesion reinforcement layer 30 away from the first surface 101. Then, the insulating substrate 10 on which the adhesion reinforcement layer 30 and the diaphragm 20 are disposed is annealed to improve the bonding strength between the diaphragm 20 and the adhesion reinforcement layer 30.
[0092] For example, annealing the insulating substrate 10 can be achieved by providing a first heating plate 61 on the second surface 102 and a second heating plate 62 on the side of the diaphragm 20 away from the first surface 101; annealing is then performed by applying a first pressure at a first temperature. In other words, in this embodiment of the invention, the insulating substrate 10, on which the attachment reinforcement layer 30 and the diaphragm 20 are provided, can be sandwiched between the first heating plate 61 and the second heating plate 62, and low pressure can be applied at a temperature of 250°C-450°C. The first heating plate 61 and the second heating plate 62 can be stainless steel or ceramic heating plates with built-in electric heaters. The first temperature can be 250°C-450°C, which will not cause thermal damage to the insulating substrate 10.
[0093] By applying low pressure at a temperature of 250℃-450℃ and maintaining it for a first duration, atoms at the interface between the diaphragm 20 and the attachment reinforcement layer 30 diffuse into each other, thereby improving the bonding strength of the interface. During the annealing process, no bonding occurs at the contact surfaces of the diaphragm 20 and the second heating plate 62, or between the second surface 102 and the first heating plate 61. This embodiment of the invention can strengthen the bonding between the diaphragm 20 and the attachment reinforcement layer 30 without performing a peeling process between the first heating plate 61 and the second heating plate 62. The method of sandwiching the insulating substrate 10, on which the attachment reinforcement layer 30 and the diaphragm 20 are provided, between the first heating plate 61 and the second heating plate 62, facilitates bonding strengthening by applying a certain surface pressure to the interface between the attachment reinforcement layer 30 and the diaphragm 20. The first duration in this embodiment of the invention can be arbitrarily set according to actual needs, which can improve the bonding strength between the diaphragm 20 and the attachment reinforcement layer 30 without causing thermal damage to the insulating substrate 10, the diaphragm 20, and the attachment reinforcement layer 30.
[0094] In this embodiment of the invention, annealing the insulating substrate 10 can also be achieved by placing the insulating substrate 10, which is provided with the attached reinforcing layer 30 and the film 20, in a high-temperature oven and heating it to achieve the annealing process.
[0095] The technical solution of this invention improves the bonding strength by annealing the insulating substrate 10, thereby deepening the diffusion at the interface between the film 20 and the attachment reinforcement layer 30.
[0096] S640: Using an electrolytic plating process or an electroless plating process, a through electrode is deposited and grown in the through hole along the direction of the film pointing to the second surface; the through electrode protrudes from the second surface.
[0097] S650: The through electrode protruding from the second surface is removed using a chemical mechanical polishing process.
[0098] S660: Uses chemical mechanical polishing to remove the film and the attached reinforcement layer.
[0099] Optionally, based on the above embodiments, refer to... Figures 3-5 The diaphragm 20 may include a copper diaphragm, which may be an electrolytic copper foil or a rolled copper foil. The through electrode 12 in the insulating substrate 10 is typically made of copper, while the diaphragm 20 may be made of the same copper material as the through electrode 12. This ensures that during the electroplating process where the diaphragm 20 acts as a cathode to form the through electrode 12, the lattice constants of the through electrode 12 and the diaphragm 20 are identical. The deposited copper atoms can directly continue the epitaxial growth of the diaphragm 20, eliminating lattice mismatch stress between materials and resulting in superior adhesion compared to electroplating with different materials. Furthermore, the through electrode 12 and the diaphragm 20 have the same coefficient of thermal expansion, preventing delamination or cracking due to thermal mismatch, thus ensuring extremely high reliability. The composition of the cathode consumed is consistent with that of the anode replenished, preventing the introduction of foreign metal impurities into the plating solution. This ensures long-term stability of the plating solution composition, facilitating process maintenance and quality control.
[0100] In some embodiments of the present invention, the diaphragm 20 may also include an aluminum diaphragm, and the material of the diaphragm 20 may also be any other material that can be electroplated or electroless plated, without specific limitations.
[0101] The thickness of the membrane 20 can be arbitrarily set according to actual conditions. For example, the thickness of the membrane 20 can be 10um-35um. At this thickness, when the membrane 20 is used as a cathode for electroplating, a sufficient current supply can be ensured. At the same time, the membrane 20 can also be effectively removed in a short time using the CMP process.
[0102] Optionally, based on the above embodiments, such as Figures 9-12 As shown, the adhesion reinforcement layer 30 may include at least one of the following: copper layer, indium layer, tin layer, silver layer, gold layer, tantalum copper composite layer, and titanium copper composite layer.
[0103] In this embodiment of the invention, the material of the attachment reinforcement layer 30 can be the same as the material of the membrane 20. For example, both the attachment reinforcement layer 30 and the membrane 20 can be made of copper, and the thickness of the attachment reinforcement layer 30 can be arbitrarily set, as long as it meets the thickness required for subsequent bonding with the membrane 20. For example, the thickness of the attachment reinforcement layer 30 can be 0.1µm-3µm. When bonding the membrane 20 and the attachment reinforcement layer 30 using processes such as surface activation bonding, plasma activation bonding, solid-liquid interdiffusion bonding, and transient liquid phase diffusion bonding, the bonding performance of the membrane 20 and the attachment reinforcement layer 30 made of the same material is better. In some embodiments of the invention, the material of the attachment reinforcement layer 30 can also be different from the material of the membrane 20. The material of the attachment reinforcement layer 30 can be a material that is easily bonded to the membrane 20. For example, the material of the attachment reinforcement layer 30 can be indium, tin, silver, or gold. In this case, the thickness of the attachment reinforcement layer 30 can be arbitrarily set, as long as it meets the thickness required for subsequent bonding with the membrane 20. For example, the thickness of the attachment reinforcement layer 30 can be 0.1µm-3µm.
[0104] When bonding the film 20 to the attachment reinforcement layer 30 using processes such as solid-liquid interdiffusion bonding or transient liquid phase diffusion bonding, the material of the attachment reinforcement layer 30 can be a low-melting-point metal material, such as indium or tin.
[0105] In some embodiments of the present invention, the material of the attachment reinforcement layer 30 may also be a tantalum-copper alloy or a titanium-copper alloy. For example, a tantalum or titanium layer may first be formed on the first surface 101 of the insulating substrate 10, and then a copper layer may be formed on the side of the tantalum or titanium layer away from the first surface 101. Tantalum and titanium can effectively improve the adhesion between the copper layer and the insulating substrate 10. The thickness of the tantalum or titanium layer can be arbitrarily set, and the thickness of the copper layer can also be arbitrarily set, but it must meet the thickness required for subsequent bonding with the film 20. For example, the thickness of the tantalum or titanium layer may be 20nm-50nm, and the thickness of the copper layer may be 0.1µm-3µm.
[0106] Figure 6 This is a schematic diagram of the structure of a semiconductor packaging substrate provided in an embodiment of the present invention, as shown below. Figure 6 As shown, the semiconductor packaging substrate 100 is a substrate for packaging with a through electrode 12 extending along the thickness direction on an insulating substrate 10. The semiconductor packaging substrate 100 can be manufactured by the semiconductor packaging substrate manufacturing method provided in any of the above embodiments of the present invention, and has the beneficial effects of the semiconductor packaging substrate manufacturing method provided in any of the above embodiments of the present invention.
[0107] It should be understood that the various forms of processes shown above can be used, with steps reordered, added, or deleted. For example, the steps described in this invention can be executed in parallel, sequentially, or in different orders, as long as the desired result of the technical solution of this invention can be achieved, and this is not limited herein.
[0108] The specific embodiments described above do not constitute a limitation on the scope of protection of this invention. Those skilled in the art should understand that various modifications, combinations, sub-combinations, and substitutions can be made according to design requirements and other factors. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.
Claims
1. A method for preparing a substrate for semiconductor packaging, characterized in that, include: An insulating substrate is provided; the insulating substrate includes a first surface and a second surface, and the insulating substrate further includes at least one through hole extending along the thickness direction of the insulating substrate, the through hole extending from the first surface to the second surface; A diaphragm is bonded to the first surface; the diaphragm seals the opening of the through-hole on the first surface; A through electrode is formed within the through hole along the direction of the diaphragm pointing toward the second surface; the through electrode protrudes from the second surface. The through electrode protruding from the second surface is removed using a chemical mechanical polishing process; The film is removed using a chemical mechanical polishing process.
2. The method for preparing a semiconductor packaging substrate according to claim 1, characterized in that, A through electrode is formed within the through hole along the direction of the diaphragm pointing towards the second surface, comprising: The through electrode is deposited and grown in the through hole using an electrolytic plating process or an electroless plating process, along the direction of the film pointing to the second surface.
3. The method for preparing a semiconductor packaging substrate according to claim 1, characterized in that, Prior to the first surface bonding film, the following is also included: An adhesion enhancement layer is formed on the first surface; the vertical projection of the adhesion enhancement layer on the first surface does not overlap with the vertical projection of the through hole on the first surface. The film is bonded to the first surface, including: The membrane is bonded to the side of the adhesion enhancement layer away from the first surface; The process of removing the film using chemical mechanical polishing also includes: The adhesion reinforcement layer is removed using the chemical mechanical polishing process described above.
4. The method for preparing a semiconductor packaging substrate according to claim 3, characterized in that, An adhesion enhancement layer is formed on the first surface, comprising: The adhesion enhancement layer is formed on the first surface using a plating process or a vapor deposition process; The film is bonded to the side of the adhesion enhancement layer away from the first surface, including: The film is bonded to the side of the adhesion enhancement layer away from the first surface using at least one of surface activation bonding process, plasma activation bonding process, solid-liquid interdiffusion bonding process, and transient liquid phase diffusion bonding process.
5. The method for preparing a semiconductor packaging substrate according to claim 4, characterized in that, Before bonding the film to the side of the adhesion enhancement layer away from the first surface using a surface activation bonding process, plasma activation bonding process, solid-liquid interdiffusion bonding process, or transient liquid phase diffusion bonding process, the method further includes: Provide temporary substrate; The diaphragm is attached to one side of the temporary substrate using an adhesive layer; The film is bonded to the side of the adhesion enhancement layer away from the first surface using a surface activation bonding process, a plasma activation bonding process, a solid-liquid interdiffusion bonding process, or a transient liquid phase diffusion bonding process, including: The insulating substrate with the attachment reinforcement layer and the temporary substrate with the film are placed in a surface activation bonding apparatus, a plasma activation bonding apparatus, a solid-liquid interdiffusion bonding apparatus, or a transient liquid phase diffusion bonding apparatus, so that the film is bonded to the side of the attachment reinforcement layer away from the first surface. The temporary substrate is peeled off using a laser.
6. The method for preparing a semiconductor packaging substrate according to claim 3, characterized in that, After the film is bonded to the side of the adhesion enhancement layer away from the first surface, the process further includes: The insulating substrate having the adhesion enhancement layer formed on its first surface and a film bonded to the side of the adhesion enhancement layer away from the first surface is subjected to annealing.
7. The method for preparing a semiconductor packaging substrate according to claim 6, characterized in that, Annealing the insulating substrate includes: A first heating plate is disposed on the second surface, and a second heating plate is disposed on the side of the diaphragm away from the first surface; Annealing of the insulating substrate is performed at a first temperature and under a first pressure.
8. The method for preparing a semiconductor packaging substrate according to claim 1, characterized in that, The film is bonded to the first surface, including: A film with a thickness of 10µm-35µm is bonded to the first surface; wherein the film includes a copper film or an aluminum film; A through electrode is formed within the through hole along the direction of the diaphragm pointing towards the second surface, comprising: A through-hole copper electrode is formed in the direction of the diaphragm pointing toward the second surface.
9. The method for preparing a semiconductor packaging substrate according to claim 3, characterized in that, An adhesion enhancement layer is formed on the first surface, comprising: At least one of the following is formed on the first surface: a copper layer, an indium layer, a tin layer, a silver layer, a gold layer, a tantalum-copper composite layer, and a titanium-copper composite layer.
10. The method for preparing a semiconductor packaging substrate according to claim 1, characterized in that, The insulating substrate is a glass substrate.
11. The method for preparing a semiconductor packaging substrate according to claim 2, characterized in that, When the through electrode is grown in the through hole using an electrolytic plating process along the direction of the film pointing to the second surface, the film is used as the cathode for electrolytic plating.
12. A substrate for semiconductor packaging, characterized in that, The semiconductor packaging substrate is manufactured using the semiconductor packaging substrate preparation method according to any one of claims 1-11.
Citation Information
Patent Citations
Semiconductor substrate and method for filling through-hole thereof
JP2004119606A
Manufacturing method and wiring board with through electrode
JP2016213283A
Bottom-up electroplating method