Gas barrier film and packaging body
By stacking an aluminum oxide and/or silicon oxide with a divalent metal oxide vapor deposition layer on a plastic film, the problem of cracking in the gas barrier film during bending is solved, achieving excellent flexibility and gas barrier properties.
Patent Information
- Application Number
- CN202580026054.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-28
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-10
AI Technical Summary
Existing gas barrier membranes are prone to cracking during bending, which reduces their barrier performance.
A vapor-deposited layer of aluminum oxide and/or silicon oxide and a vapor-deposited layer of divalent metal oxide are sequentially stacked on a plastic film to form a gas barrier film.
It improves the flexibility of the gas barrier film, avoids cracking of the vapor-deposited film during bending, and maintains good gas barrier performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to a gas barrier membrane with excellent flexibility. Background Technology
[0002] For packaging materials used in the packaging of food, medicine and other products, in order to prevent the contents, flavor and efficacy from being altered by oxidation, it is required to have the ability to block oxygen and water vapor (hereinafter referred to as gas barrier). From the perspective of being inexpensive and able to impart high barrier performance, resin films with vapor-deposited films are used.
[0003] As barrier films with vapor-deposited films, for example, there are films in which aluminum oxide (AlOx) and / or silicon oxide (SiOx) are vapor-deposited on a polyethylene terephthalate film, or films in which multiple vapor-deposited films of silicon oxide are stacked (see, for example, Patent Document 1); and barrier films in which vapor-deposited materials containing metallic silicon and silicon oxide and vapor-deposited materials containing any metal or metal oxide selected from aluminum, zinc, tin, and iron are vapor-deposited on a resin substrate with an anchoring coating (see, for example, Patent Document 2).
[0004] However, in general, metal oxide vapor-deposited films have weak flexibility such as torsion and bending. Sometimes, due to bending during lamination with other films or during bag making after lamination, cracks can easily occur in a part of the vapor-deposited film, reducing its barrier performance.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: Japanese Patent Application Publication No. 2013-253319
[0008] Patent Document 2: Japanese Patent Application Publication No. 2014-069389 Summary of the Invention
[0009] The problem the invention aims to solve
[0010] The objective of this invention is to provide a gas barrier film that does not crack in a portion of the vapor-deposited film, has excellent flexibility, and possesses good gas barrier properties.
[0011] Solution for solving the problem
[0012] That is, the present invention provides a gas barrier film, wherein an aluminum oxide and / or silicon oxide vapor-deposited layer (A) and a divalent metal oxide vapor-deposited layer (B) are sequentially stacked on a plastic film.
[0013] In addition, the present invention provides a packaging body containing the gas barrier film described in one of the above claims.
[0014] The effects of the invention
[0015] According to the present invention, a gas barrier film that does not crack in a portion of the vapor-deposited film, has excellent flexibility and good gas barrier properties, and a packaging body using the gas barrier film can be provided. Detailed Implementation
[0016] (Definition of Language)
[0017] In this specification, "~" means the value above the value preceding "~" and the value below the value following "~".
[0018] (Gas barrier membrane)
[0019] The gas barrier film of the present invention is characterized in that an aluminum oxide and / or silicon oxide vapor-deposited layer (A) and a divalent metal oxide vapor-deposited layer (B) are sequentially stacked on the plastic film.
[0020] (Plastic film)
[0021] There are no particular limitations on the raw materials used in the plastic film of this invention. Plastic films used in packaging materials for food, pharmaceuticals, etc., can be used. Specifically, examples include polyethylene terephthalate (PET) film, polystyrene film, polyamide film, nylon film, polyacrylonitrile film, polyethylene film (OPE: biaxially oriented polyethylene film, LLDPE: low-density polyethylene film, HDPE: high-density polyethylene film), polypropylene film (CPP: unstretched polypropylene film, OPP: biaxially oriented polypropylene film), polyvinyl alcohol film, ethylene-vinyl alcohol copolymer film, cellophane, etc.
[0022] In the case of single-material packaging, a film formed from a thermoplastic resin with olefin-based resins as the base material can be used. Specifically, examples of olefin-based resins include: low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear (linear) low-density polyethylene, polypropylene, ethylene-propylene copolymers, α-olefin polymers, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, ethylene-acrylic acid copolymers, ethylene-methyl methacrylate copolymers, ethylene-ethyl acrylate copolymers, cyclic olefin resins, ionomer resins, polymethylpentene, and other olefin resins; modified olefin resins obtained by modifying olefin resins with acrylic acid, methacrylic acid, maleic anhydride, fumaric acid, and other unsaturated carboxylic acids.
[0023] Furthermore, as the membrane substrate, membranes formed from materials containing components derived from biomass are preferred. In addition to biomass membranes sold by various companies, sheets listed in the biomass certified product list documented by the Japan Organic Resources Association can also be used.
[0024] Specifically, well-known membranes are obtained using biomass-derived ethylene glycol as a raw material. Biomass-derived ethylene glycol is obtained from ethanol (biomass ethanol) produced from biomass. For example, biomass-derived ethylene glycol can be obtained by using conventionally known methods to produce ethylene glycol from biomass ethanol via ethylene oxide. Alternatively, commercially available biomass ethylene glycol can be used; for example, biomass ethylene glycol commercially available from India Glycols Limited is preferred.
[0025] Alternatively, membranes made from biomass feedstocks that are classified according to the biomass plasticity standards specified in ISO 16620 or ASTM D6866 are also in circulation. These membranes, with an atmospheric plasticity of 10... 12 One-third of the carbon in plant-derived resins contains radioactive carbon-14C, a proportion that remains constant in atmospheric carbon dioxide and therefore also remains constant in plants that fix carbon dioxide through photosynthesis. Therefore, plant-derived resins contain radioactive carbon-14C. In contrast, fossil fuel-derived resins contain almost no radioactive carbon-14C. Therefore, by measuring the concentration of radioactive carbon-14C in the resin using an accelerator mass spectrometer, the proportion of plant-derived resin in the resin, i.e., the biomass plasticity, can be determined. Plant-derived low-density polyethylene (LDPE), which has a biomass plasticity of 80% or more, preferably 90% or more, as specified in ISO 16620 or ASTM D6866, is suitable for use as a raw material for membranes, for example, those manufactured by Braskem under trade names such as "SBC818," "SPB608," "SBF0323HC," "STN7006," "SEB853," and "SPB681."
[0026] For example, as alternatives to conventional polyolefin membranes that use petroleum-based raw materials, biomass polyolefin membranes, such as biomass polyethylene membranes and biomass polyethylene-polypropylene membranes, are also known.
[0027] Polyethylene resins are not particularly limited except for the use of ethylene glycol from the aforementioned biomass source in part of the raw materials. Examples include homopolymers of ethylene, copolymers of ethylene and α-olefins with ethylene as the main component (ethylene-α-olefin copolymers containing more than 90% by mass of ethylene units), etc. They can be used alone or in combination of two or more.
[0028] It should be noted that the α-olefin constituting the copolymer of ethylene and α-olefin is not particularly limited, and examples include α-olefins with 4 to 8 carbon atoms such as 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene. Known polyethylene resins such as low-density polyethylene resin, medium-density polyethylene resin, and linear low-density polyethylene resin can be used.
[0029] From the viewpoint that even if the membranes rub against each other, they are less prone to damage such as openings and cracks, linear low-density polyethylene resin (LLDPE) (a copolymer of ethylene and 1-hexene, or a copolymer of ethylene and 1-octene) is preferred, and a density of 0.910~0.925 g / cm³ is even more preferred. 3 Linear low-density polyethylene resin.
[0030] Biomass membranes can be stacked with multiple biomass membranes, or they can be stacked with traditional petroleum-based membranes and biomass membranes.
[0031] To improve the adhesion of the vapor-deposited layer (A) described later, the substrate may be a substrate that has undergone a certain surface treatment, such as physical treatment (e.g., corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen or nitrogen, glow discharge treatment, flame treatment, etc.), chemical treatment (e.g., oxidation treatment using chemicals), or other treatments. Alternatively, it may have a coating such as an anchoring agent to improve adhesion.
[0032] The aforementioned substrate can be manufactured by using conventionally known film-making methods such as extrusion, casting, T-die forming, cutting, and blow molding of the aforementioned resin. It can be an unstretched film, and from the viewpoint of the strength, dimensional stability, and heat resistance of the film (1), it can also be a film stretched in a uniaxial or biaxial direction using a tenter frame or tubular method.
[0033] The aforementioned substrate may also contain additives as needed. Specifically, for the purpose of improving or modifying processability, heat resistance, weather resistance, mechanical properties, dimensional stability, oxidation resistance, slip properties, mold release properties, flame retardancy, mildew resistance, electrical properties, strength, etc., elastomers, lubricants, crosslinking agents, antioxidants, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and other plastic compounding agents and additives may be added. The amount of additives added shall be adjusted within the range that does not affect other properties or recyclability.
[0034] The film thickness of the aforementioned substrate is not particularly limited; from the viewpoint of formability and transparency, it can be appropriately selected within the range of 0.1 to 300 μm. A range of 0.3 to 100 μm is preferred. If the thickness is below 0.1 μm, the strength is insufficient; if it exceeds 300 μm, the rigidity becomes too high, and processing may become difficult.
[0035] From a recycling perspective, the preferred layer structure should be as simple as possible; however, from the perspective of the circulation of packaging materials, printing is often required to display the contents of the packaging material, product descriptions, and names. This printing is mostly done on the aforementioned substrate.
[0036] (Printed layer)
[0037] The printed layer is a layer on which text, graphics, symbols, and other desired patterns are printed. There are no particular limitations on the printing method or ink; any known printing method or ink can be used. Films used as the aforementioned substrate often employ printing inks produced using gravure printing, flexographic printing, offset lithography, inkjet printing, etc. Additionally, printing inks combining these printing methods with methods that utilize active energy rays such as ultraviolet (UV), LEDs, or electron beams (EB) for curing, or methods that utilize heat for curing, can also be used. Furthermore, depending on the solvent used, these are sometimes referred to as water-based inks or organic solvent-based inks.
[0038] Specifically, examples include gravure printing inks, flexographic printing inks (depending on the industry, gravure printing inks and flexographic printing inks are sometimes referred to as liquid inks), UV-curable inks for offset lithography, electron beam-curable inks for offset lithography, UV-curable inks for inkjet recording printing, and electron beam-curable inks for inkjet recording printing.
[0039] The location of the printing layer printed using these inks is arbitrary. It can be located on the first substrate mentioned above, or on a separate substrate where the printing layer is also provided, which can also be one of the components of the laminate of the present invention, and its location is arbitrary. In addition, the ink can be an ink containing resin, colorant, and solvent as essential components, or it can be a so-called transparent ink containing resin and solvent but substantially not containing colorant.
[0040] The following section explains the most commonly used liquid inks for printing on films.
[0041] The resin used in liquid inks is not particularly limited, and examples include acrylic resins, polyester resins, styrene resins, styrene-maleic acid resins, maleic acid resins, polyamide resins, polyurethane resins, vinyl chloride-vinyl acetate copolymer resins, vinyl chloride-acrylic acid copolymer resins, ethylene-vinyl acetate copolymer resins, vinyl acetate resins, polyvinyl chloride resins, chlorinated polypropylene resins, cellulose resins, epoxy resins, alkyd resins, rosin resins, rosin-modified maleic acid resins, ketone resins, cyclized rubbers, chlorinated rubbers, butyral, and petroleum resins. One or more of these resins may be used. Preferably, at least one or more resins selected from polyurethane resins, vinyl chloride-vinyl acetate copolymer resins, and cellulose resins are used.
[0042] Examples of colorants used in liquid inks include inorganic pigments such as titanium dioxide, iron oxide red, antimony red, cadmium red, cadmium yellow, cobalt blue, Prussian blue, ultramarine, carbon black, and graphite; organic pigments such as soluble azo pigments, insoluble azo pigments, azo lake pigments, condensed azo pigments, copper phthalocyanine pigments, and fused polycyclic pigments; and extender pigments such as calcium carbonate, kaolin, barium sulfate, aluminum hydroxide, and talc.
[0043] Most liquid inks used in film printing are organic solvent-based inks. Preferably, the organic solvent used is free of aromatic hydrocarbons. More specifically, examples include: alcohol-based organic solvents such as methanol, ethanol, n-propanol, isopropanol, and butanol; ketone-based organic solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester-based organic solvents such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; aliphatic hydrocarbon-based organic solvents such as n-hexane, n-heptane, and n-octane; and alicyclic hydrocarbon-based organic solvents such as cyclohexane, methylcyclohexane, ethylcyclohexane, cycloheptane, and cyclooctane. One or more of these solvents can be used in combination.
[0044] (A vapor-deposited layer of aluminum oxide and / or silicon oxide)
[0045] The gas barrier film of the present invention has an aluminum oxide (sometimes also called aluminum oxide, aluminum oxide or AlOx, which are various aluminum oxides such as AlO, Al2O3 or mixtures thereof) and / or silicon oxide (sometimes also called silicon oxide, silicon oxide or SiOx, which are various silicon oxides such as SiO, SiO2 or mixtures thereof) vapor-deposited layer (A) on the above-mentioned plastic film.
[0046] The vapor-deposited layer (A) is preferably formed by a vapor-phase film formation method. As a vapor-phase film formation method for forming the vapor-deposited layer (A) in this invention, there are physical deposition methods (hereinafter referred to as PVD methods) such as vacuum evaporation, sputtering, and ion plating, and chemical deposition methods (hereinafter referred to as CVD methods). Any method can be used within the scope of achieving the effects of this invention. As described above, the vapor-phase film formation method used in this invention is not particularly limited. From the perspective of easily forming a stable thin film, it is preferred to use PVD methods such as vacuum evaporation, sputtering, and ion plating, and most preferably, vacuum evaporation is used for thin film formation.
[0047] The vapor deposition process used in the aforementioned PVD method employs the following method: A metal, metal oxide, metal hydroxide, or resin (hereinafter, these vapor deposition materials are sometimes collectively referred to as the target) is heated using various heat sources to evaporate, and then precipitated on the substrate surface at a lower temperature as an amorphous or crystalline film. This method can be used in both intermittent processes that treat the entire surface at once, and continuous processes that treat different surfaces by moving the substrate or reaction tank.
[0048] The vapor deposition process of this invention can be carried out under pressure, atmospheric pressure, reduced pressure, vacuum, or fluctuations thereof, in any atmosphere, including the atmosphere and in a non-reactive gas. By performing the process under reduced pressure or vacuum, the evaporation rate can be increased and the evaporation temperature can be lowered, while pressurization can promote the precipitation of the evaporated material. Furthermore, by setting the atmosphere to vacuum or a non-reactive atmosphere, the oxidation of the aforementioned metals, metal oxides, metal hydroxides, and the carrier can be controlled. Moreover, considering cost factors, the process can also be carried out in an atmospheric atmosphere if oxidation during the vapor deposition process can be controlled and tolerated.
[0049] In this invention, by adjusting the vapor deposition conditions, a preferred thin film can be obtained according to the desired effect. To control the chemical structure of the target vapor-deposited material, the aforementioned conditions include the pressure within the chamber, the molecules present in the target vapor and atmosphere, and the contact time with the substrate surface. By controlling this time, the composition of the vapor-deposited thin film can be controlled. Alternatively, the surface structure of the thin film can be controlled by contacting the film with oxygen or water vapor after film formation.
[0050] The so-called control of the chemical structure of the target vapor-deposited material refers to, for example, obtaining a compound with hydroxyl and oxygen added to the target metal as a vapor-deposited layer by adding water vapor or oxygen during vapor deposition, and studying appropriate vapor deposition conditions according to the desired vapor-deposited film.
[0051] The sputtering method used in this invention is not particularly limited within the scope of achieving the effects of this invention, and can be selected from DC sputtering, RF sputtering, magnetron sputtering, ion beam sputtering, RF magnetron sputtering, etc. From the perspective of being able to perform sputtering with high efficiency, magnetron sputtering and RF magnetron sputtering methods are preferred. Magnetron sputtering is expected to reduce the pressure to, for example, 1×10⁻⁶. -4 The process is carried out in a processing space such as a chamber containing an inert gas (e.g., argon) at a pressure below Pa. Within this processing space, a target, which is to be used as the raw material for the thin film, is positioned opposite a substrate. A permanent magnet and, if necessary, a holding member for holding the target are disposed on the back side of the target.
[0052] The magnetic field of the permanent magnet can confine the helical orbits of electrons within the processing space, generating a high-density plasma region. This high-density plasma region promotes the ionization of inactive gases, and the collisions of these ions with the target generate target particles. These particles then adhere to the substrate to form a thin film.
[0053] There are no particular limitations on the high-frequency output during RF magnetron sputtering; it can be adjusted to achieve an appropriate film deposition rate. Furthermore, the temperature of the substrate during film deposition is preferably controlled between room temperature and approximately 100°C.
[0054] The thickness of the aforementioned vapor-deposited layer (A), measured in terms of the thickness of the layer exhibiting gas barrier properties, is preferably 10 nm or more and 500 nm or less. If the layer thickness is less than 10 nm, areas where gas barrier properties cannot be adequately guaranteed may occur, resulting in problems such as uneven gas barrier properties within the substrate surface. If the layer thickness is more than 500 nm, the stress remaining within the vapor-deposited layer (A) increases, thus causing cracks in the vapor-deposited layer (A) under high temperature and high humidity conditions, sometimes leading to a decrease in gas barrier properties. From the viewpoint of ensuring flexibility, the lower limit is more preferably 20 nm or more, and the upper limit is more preferably 300 nm or less. The thickness of the vapor-deposited layer (A) can usually be measured by cross-sectional observation using a transmission electron microscope (TEM).
[0055] The aforementioned vapor-deposited layer (A) can be a mixture of aluminum oxide and silicon oxide. More preferably, it is a composite oxide of aluminum oxide and silicon oxide. That is, in this composite oxide, the mixing ratio of aluminum oxide and silicon oxide, expressed as a mass ratio converted from metal atoms, preferably has an Al content of 20% by mass or more and 70% by mass or less. If it is 20% by mass or more, the gas barrier properties are excellent. If it is 70% by mass or less, it prevents the vapor-deposited layer (A) from becoming too hard.
[0056] (Vapor-deposited layer (B))
[0057] A vapor-deposited layer (B) of a divalent metal oxide (B) is formed on the aforementioned vapor-deposited layer (A). The divalent metal oxide (B) is preferably selected from one or more of zinc oxide, magnesium oxide, calcium oxide, manganese oxide, iron oxide, cobalt oxide, nickel oxide, and copper oxide; more preferably from one or more of zinc oxide, magnesium oxide, and calcium oxide; and particularly preferably zinc oxide. These metal compounds can be used alone or in combination of two or more. The vapor-deposited layer (B), like the vapor-deposited layer (A), is preferably formed by a vapor-phase film formation method.
[0058] The thickness of the vapor-deposited layer (B) is not particularly limited within the range that allows the effects of the present invention to be obtained, as long as it falls within that range. As for the thickness of the vapor-deposited layer (B), there is no particular limitation as described above, but from the viewpoint of obtaining sufficient protective effect of the vapor-deposited layer (A), 1 to 200 nm is preferred, and from the viewpoint of ensuring the overall plasticity of the laminate, 3 to 150 nm is more preferred, and particularly preferred is 5 to 100 nm.
[0059] The vapor deposition process used in the aforementioned PVD method employs the following method: A metal, metal oxide, metal hydroxide, or resin (hereinafter, these vapor deposition materials are sometimes collectively referred to as the target) is heated using various heat sources to evaporate, and then precipitated on the substrate surface at a lower temperature as an amorphous or crystalline film. This method can be used in both intermittent processes that treat the entire surface at once, and continuous processes that treat different surfaces by moving the substrate or reaction tank.
[0060] The vapor deposition process of this invention can be carried out under pressure, atmospheric pressure, reduced pressure, vacuum, or fluctuations thereof, in any atmosphere, including the atmosphere and in a non-reactive gas. By performing the process under reduced pressure or vacuum, the evaporation rate can be increased and the evaporation temperature can be lowered, while pressurization can promote the precipitation of the evaporated material. Furthermore, by setting the atmosphere to vacuum or a non-reactive atmosphere, the oxidation of the aforementioned metals, metal oxides, metal hydroxides, and the carrier can be controlled. Moreover, considering cost factors, the process can also be carried out in an atmospheric atmosphere if oxidation during the vapor deposition process can be controlled and tolerated.
[0061] In this invention, by adjusting the vapor deposition conditions, a preferred thin film can be obtained according to the desired effect. To control the chemical structure of the target vapor-deposited material, the aforementioned conditions include the pressure within the chamber, the molecules present in the target vapor and atmosphere, and the contact time with the substrate surface. By controlling this time, the composition of the vapor-deposited thin film can be controlled. Alternatively, the surface structure of the thin film can be controlled by contacting the film with oxygen or water vapor after film formation.
[0062] The so-called control of the chemical structure of the target vapor-deposited material refers to, for example, obtaining a compound with hydroxyl and oxygen added to the target metal as a vapor-deposited layer by adding water vapor or oxygen during vapor deposition, and appropriately studying the vapor deposition conditions according to the desired vapor-deposited film.
[0063] The sputtering method used in this invention is not particularly limited within the scope of achieving the effects of this invention, and can be selected from DC sputtering, RF sputtering, magnetron sputtering, ion beam sputtering, RF magnetron sputtering, etc. From the perspective of being able to perform sputtering with high efficiency, magnetron sputtering and RF magnetron sputtering methods are preferred. Magnetron sputtering is expected to reduce the pressure to, for example, 1×10⁻⁶. -4 The process is carried out in a processing space such as a chamber containing an inert gas (e.g., argon) at a pressure below Pa. Within this processing space, a target, which is to be used as the raw material for the thin film, is positioned opposite a substrate. A permanent magnet and, if necessary, a holding member for holding the target are disposed on the back side of the target.
[0064] The magnetic field of the permanent magnet can confine the helical orbits of electrons within the processing space, generating a high-density plasma region. This high-density plasma region promotes the ionization of inactive gases, and the collisions of these ions with the target generate target particles. These particles then adhere to the substrate to form a thin film.
[0065] There are no particular limitations on the high-frequency output during RF magnetron sputtering; it can be adjusted to achieve an appropriate film deposition rate. Furthermore, the temperature of the substrate during film deposition is preferably controlled between room temperature and approximately 100°C.
[0066] In the gas barrier film of the present invention, the metal ratio of the vapor-deposited layer (B) to the vapor-deposited layer (A), based on the fluorescence X-ray intensity, is preferably in the range of 0.5:100 to 90:100, more preferably in the range of 2:100 to 50:100. Within this range, excellent bending resistance is achieved.
[0067] In this invention, the intensity of fluorescent X-rays is measured using a handheld fluorescent X-ray measuring device (device name X-MET8000, manufactured by Horiba, Ltd.). The ratio of the metal in the vapor-deposited layer (A) to the metal in the vapor-deposited layer (B) on the film surface is calculated from the measured intensity (metal in vapor-deposited layer (B) / metal in vapor-deposited layer (A)).
[0068] (coating)
[0069] The gas barrier film of the present invention can be coated with a coating agent on the surface of layer (B) or the back of the plastic film after layering layer (A) and layer (B). In the present invention, there are no particular limitations on the coating method, and commonly known coating methods such as roller coating, spray coating, spin coating, doctor blade coating, dip coating, screen printing, inkjet printing, doctor blade coating, doctor blade coating, curtain coating, slot coating, and dispensing can be used.
[0070] Examples of coatings include hard coatings coated with a hard coating agent intended to protect the gas barrier film of the present invention, coatings with various functionalities, and heat-resistant coatings coated with a heat-resistant coating agent described later.
[0071] The gas barrier film of the present invention exhibits excellent flexibility. Specifically, the ring stiffness value a (g / cm) calculated by formula (1) described later is preferably in the range of +1.0% to +30.0%. If it is below +1.0%, there is a tendency to make it difficult to obtain the protective effect of the vapor-deposited layer (A) when bent, and if it is above +30.0%, there is a tendency for the film to harden and the vapor-deposited layer (B) to easily crack.
[0072] It should be noted that, in this invention, the ring stiffness value a (g / cm) is a parameter representing the stiffness of films such as stretched plastic films. Besides single-layer films such as stretched plastic films, multilayer films such as vapor-deposited films and laminated films can also be evaluated.
[0073] One method for measuring ring stiffness is as follows: the membrane is cut into strips to form a ring, which is then mounted on a device, and the force required to crush the ring at a constant distance under a constant load is read. In this invention, the value is evaluated using a ring stiffness meter manufactured by Toyo Seiki Co., Ltd. (registered trademark).
[0074] It should be noted that the formal determination of the ring stiffness value a (g / cm) depends on the thickness of each raw material. Therefore, in order to evaluate the change caused by vapor deposition, the ring stiffness value a1 of the film with only vapor deposition layer (A) and the ring stiffness value a2 of the film with vapor deposition layer (B) deposited on vapor deposition layer (A) are measured and evaluated using the change rate (%) calculated by the following formula (1).
[0075] Equation (1) (a2-a1) / (a1)×100(%)
[0076] (Second layer)
[0077] The gas-barrier film of the present invention can also be bonded to other plastic films using an adhesive. Alternatively, other plastic layers (hereinafter referred to as the second layer) can be formed on the gas-barrier film by extrusion.
[0078] The second layer can be a layer of the same resin material as the aforementioned plastic film, or it can be a layer of a different resin material. When applying the gas-barrier film of the present invention to packaging materials, it is conceivable to use the second layer as a sealing layer, selecting a polyolefin resin with heat-sealing adaptability. Examples include: polyethylene resins such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (VLDPE), polypropylene (CPP), ethylene-propylene copolymer, and polymethylpentene; ethylene copolymers such as ethylene-vinyl acetate copolymer (EVA), ethylene-methyl methacrylate copolymer (EMMA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl acrylate (EMA), ethylene-ethyl acrylate-maleic anhydride copolymer (E-EA-MAH), ethylene-acrylic acid copolymer (EAA), and ethylene-methacrylic acid copolymer (EMAA); and ionomers of ethylene-acrylic acid copolymers and ionomers of ethylene-methacrylic acid copolymers, etc., which can be used alone or in combination of two or more.
[0079] When the second layer is set as a heat-sealing layer, its film thickness can be adjusted appropriately according to the purpose. From the viewpoint of aroma retention and heat sealing, for example, it is 1μm to 10μm, and more preferably 3μm to 10μm.
[0080] (Adhesive)
[0081] As the adhesive used when bonding the second layer to the gas barrier film of the present invention, any adhesive that can be used in a general lamination method is acceptable. Examples of lamination methods include dry lamination, wet lamination, solvent-free lamination, and extrusion lamination. The adhesive becomes the adhesive layer after curing or drying.
[0082] As for the adhesive used in the above-mentioned dry lamination, for example, one-component or two-component cured or non-curing adhesives such as vinyl-based, (meth)acrylic-based, polyamide-based, polyester-based, polyether-based, polyurethane-based, epoxy-based, rubber-based, and others, solvent-based, water-based, or emulsion-based adhesives can be used. As for two-component cured adhesives, two-component cured adhesives of polyols and isocyanate compounds can be used. As for the coating method of the above-mentioned adhesive for lamination, for example, it can be coated by direct gravure roller coating, gravure offset roller coating, coincidence coating, reverse roller coating, ink fountain roller coating, transfer roller coating, and other methods. For example, the DICDRY series manufactured by DIC Corporation can be preferred.
[0083] Alternatively, various adhesives can be used, with pressure-sensitive adhesives being preferred. Examples of pressure-sensitive adhesives include: polyisobutylene rubber, butyl rubber, and rubber-based adhesives obtained by dissolving mixtures thereof in organic solvents such as benzene, toluene, xylene, and hexane; or adhesives obtained by adding thickeners such as abietic rosin ester, terpene-phenol copolymer, and terpene-indene copolymer to these rubber-based adhesives; or acrylic adhesives obtained by dissolving acrylic copolymers with a glass transition temperature of -20°C or below, such as 2-ethylhexyl acrylate-n-butyl acrylate copolymer and 2-ethylhexyl acrylate-ethyl acrylate-methyl methacrylate copolymer, in organic solvents.
[0084] Among the adhesives described above, functional adhesives can also be used. For example, as an adhesive with gas barrier properties, the PASLIM series of oxygen barrier adhesives manufactured by DIC Corporation, which are two-component reactive adhesives of polyester polyols and isocyanate compounds, can be used. The gas barrier adhesive becomes a gas barrier adhesive layer after curing or drying. Using a gas barrier adhesive can further improve the gas barrier properties of the laminate of the present invention, which is preferable.
[0085] When the adhesive is solvent-based, the adhesive is applied to a substrate using a roller such as a gravure roller. After the organic solvent evaporates by heating in an oven or similar source, the substrate is then bonded together to obtain the laminate of the present invention. It is preferable to perform an aging treatment after lamination. The aging temperature is preferably room temperature to 80°C, and the aging time is preferably 12 to 240 hours.
[0086] When the adhesive is solvent-free, the laminate of the present invention is obtained by applying a preheated, aroma-retaining adhesive (approximately 40°C to 100°C) to one substrate using a gravure roller or similar roller, and then immediately bonding it to another substrate. It is preferable to perform an aging treatment after lamination. The aging temperature is preferably room temperature to 70°C, and the aging time is preferably 6 to 240 hours.
[0087] The application amount of the adhesive should be adjusted appropriately. In the case of a solvent-based adhesive, for example, the solid content should be 1 g / m³. 2 Above and 10g / m 2 The following is preferred: 1g / m 2 Above and 5g / m 2 The following adjustments are made. For example, in the case of a solvent-free adhesive, the application rate is 1 g / m². 2 Above and 10g / m 2 The following, preferably 1g / m 2 Above and 5g / m 2 the following.
[0088] (Heat-resistant resin layer)
[0089] The gas barrier membrane of the present invention can have a heat-resistant coating. The heat-resistant coating is a coating layer with a heat-resistant coating agent (hereinafter sometimes simply referred to as heat-resistant coating agent).
[0090] Commercially available products can be used as heat-resistant coating agents. Examples of commercially available products include SUNSYS FS241 manufactured by SUN CHEMICAL, DH-S004 / DH-HARDENER P-60 manufactured by DIC, and ThermaGloss (registered trademark) 463 manufactured by Michelman.
[0091] Furthermore, heat-resistant coating agents containing compounds having a glass transition temperature (hereinafter sometimes referred to as Tg) of 100°C or higher, and having a cellulose backbone, a benzene ring backbone, an isocyanurate ring backbone, or an alicyclic backbone, are preferred, for example. Specifically, examples include: cellulose derivatives such as nitrocellulose, cellulose acetate, cellulose propionate, and cellulose butyrate; polyester resins having a benzene ring and / or an alicyclic backbone such as cyclopentane glycol and dihydroxymethyltricyclodecane, such as phthalic acid, naphthalene dicarboxylic acid, bisphenol A, ethylene oxide (hereinafter sometimes referred to as EO) adducts; aromatic isocyanates such as diphenylmethane diisocyanate, toluene diisocyanate, phenyl dimethylene diisocyanate, and naphthalene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate and norbornene diisocyanate; and / or polyurethane resins formed by combining isocyanurate triisocyanate with polyols and / or tris(2-hydroxyethyl) isocyanurate. Alternatively, polyisocyanates containing the aforementioned isocyanates can be used as curing agents. Furthermore, free radical copolymers of compounds having benzene rings and unsaturated double bonds, such as styrene and phenoxydiethylene glycol acrylate, and / or compounds having alicyclic structures and unsaturated double bonds, such as isobornyl acrylate and dicyclopentyl acrylate, as well as (meth)acrylates, are preferred. Additionally, considering the adhesion to olefin films, resins with low Tg can also be used in combination.
[0092] The total mass of the cellulose backbone, benzene ring backbone, isocyanurate ring backbone, and alicyclic backbone of the above-mentioned compounds is preferably 20 to 99% by mass in the solid composition of the above-mentioned heat-resistant coating (A). A more desirable mass is 30 to 95% by mass.
[0093] Furthermore, the aforementioned heat-resistant coating agent can also be colored. There are no particular limitations on the colorant; examples include inorganic pigments, organic pigments, and dyes commonly used in inks, coatings, and recording agents used in the printing layer (E) described later. Pigments are preferred. Examples of organic pigments include soluble azo, insoluble azo, azo-based, phthalocyanine, halogenated phthalocyanine, anthraquinone, anthraquinone-anthraquinone, dianthraquinone, anthraquinone, perylene, perylene ketone, quinacridone, thioindole, dioxazine, isoindolineone, quinoline ketone, azomethylazo, flavanone, diketopyrrolopyrrole, isoindoline, indanone, and carbon black pigments. Other examples include Carmine 6B, Lake Red C, Permanent Red 2B, Diazo Yellow, Pyrazolone Orange, Carmine FB, Gormley Yellow, Gormley Red, Phthalocyanine Blue, Phthalocyanine Green, Dioxazine Violet, Quinacridone Fuchsin, Quinacridone Red, Indanthrene Blue, Pyrimidine Yellow, Thioindigo, Thioindigo Fuchsin, Perylene Red, Perylene Orange, Isoindolone Yellow, Aniline Black, Diketopyrrolopyrrole Red, and daylight fluorescent pigments. Additionally, either untreated or acid-treated pigments can be used.
[0094] Examples of inorganic pigments include titanium dioxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, silicon dioxide, zinc barium white, antimony white, and gypsum. Among inorganic pigments, titanium dioxide is particularly preferred. Titanium dioxide is white and is preferred from the viewpoints of tinting strength, hiding power, chemical resistance, and weather resistance. From the viewpoint of printability, titanium dioxide obtained by treating with silicon dioxide and / or aluminum oxide is preferred.
[0095] As inorganic pigments other than white, examples include aluminum particles, mica, bronze powder, chrome vermilion, chrome yellow, cadmium yellow, cadmium red, ultramarine, Prussian blue, iron oxide red, iron oxide yellow, iron black, and zircon. Aluminum is available in powder or paste form. Considering processability and safety, it is preferred to use it in paste form. Considering brightness and concentration, it is appropriate to choose whether to use a suspended or non-suspended type.
[0096] Furthermore, when the aforementioned heat-resistant coating agent uses inorganic microparticles such as alumina, magnesium oxide, titanium dioxide, zirconium oxide, and silicon dioxide (quartz, fumed silica, precipitated silica, silicic anhydride, fused silica, crystalline silica, ultrafine amorphous silica, etc.) as aggregates, it exhibits excellent heat resistance and is therefore preferred. Alternatively, boron nitride, aluminum nitride, alumina, titanium oxide, magnesium oxide, zinc oxide, and silicon dioxide are preferred due to their excellent thermal conductivity. Inorganic microparticles can be used alone or in combination.
[0097] There are no particular limitations on the shape of the silica particles; spherical, hollow, porous, rod-shaped, plate-shaped, fibrous, or irregularly shaped silica particles can be used. For example, commercially available hollow silica particles can be SiliNax manufactured by Nippon Steel Mining Co., Ltd.
[0098] The primary particle size of the aforementioned inorganic particles is preferably in the range of 5 nm to 100 μm. If it is 1 nm or larger, the inorganic particles in the dispersion become well dispersed; if the diameter is within 100 μm, the strength of the cured material becomes good. More preferably, it is 10 nm to 20 μm.
[0099] The aforementioned inorganic microparticles can be mixed in a ratio of 5 to 90% by weight relative to the total solid content of the aforementioned heat-resistant coating agent and the aforementioned inorganic microparticles. The mixing ratio can be adjusted as needed according to the purpose. Preferably, it is 20% by weight or more.
[0100] In the aforementioned heat-resistant coating agents, to prevent damage to the coating film, prevent adhesion during the formation of the laminate, and impart processability to the bag-making process after the laminate is made, waxes, silicone additives, and organic microspheres can be used. Specifically, amide waxes, polypropylene waxes, polyethylene waxes, paraffin waxes, carnauba waxes, rice bran waxes, ethylene oxide (EO) adducts of dimethylsiloxane, silicone additives modified with silicone, and organic microspheres composed of acrylic, nylon, polyurethane, or epoxy resins can be added.
[0101] There are no particular limitations on the solvents used in the aforementioned heat-resistant coatings. Examples include aromatic hydrocarbon organic solvents such as water, toluene, xylene, Solvesso #100, and Solvesso #150; aliphatic hydrocarbon organic solvents such as hexane, methylcyclohexane, heptane, octane, and decane; and various ester-based organic solvents such as methyl acetate, ethyl acetate, isopropyl acetate, n-propyl acetate, butyl acetate, amyl acetate, ethyl formate, and butyl propionate. In addition, examples of water-mixable organic solvents include alcohols such as methanol, ethanol, propanol, butanol, and isopropanol; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; and various glycol ethers such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and dipropylene glycol monomethyl ether. These can be used alone or in mixtures of two or more. Furthermore, defoamers and leveling agents can also be used to achieve more effective coating.
[0102] The coating amount of the heat-resistant resin layer is selected appropriately according to its application. The preferred coating amount after drying is 0.01~100 g / m². 2 More preferably, it is 0.1~50 g / m 2 The preferred concentration is 0.5~3g / m 2 .
[0103] (Layered structure)
[0104] Here is one example of a specific embodiment of the gas barrier membrane of the present invention. Of course, the laminate of the present invention is not limited to this embodiment.
[0105] Plastic film / vapor deposition layer (A) / vapor deposition layer (B) / gas barrier adhesive layer / second layer
[0106] Plastic film / Printed layer / Evaporated layer (A) / Evaporated layer (B) / Gas barrier adhesive layer / Second layer
[0107] Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Gas barrier adhesive layer / Second layer
[0108] Plastic film / vapor deposition layer (A) / vapor deposition layer (B) / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0109] Plastic film / Printed layer / Evaporated layer (A) / Evaporated layer (B) / Gas barrier adhesive layer / Substrate used as intermediate layer / Adhesive layer / Second layer
[0110] Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Gas barrier adhesive layer / Substrate used as intermediate layer / Adhesive layer / Second layer
[0111] Plastic film / vapor deposition layer (A) / vapor deposition layer (B) / vapor deposition protective coating / gas barrier adhesive layer / second layer
[0112] Plastic film / Printed layer / Evaporated layer (A) / Evaporated layer (B) / Evaporated protective coating / Gas barrier adhesive layer / Second layer
[0113] Plastic film / vapor deposition layer (A) / vapor deposition layer (B) / vapor deposition protective coating / printed layer / gas barrier adhesive layer / second layer
[0114] Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Evaporated protective coating / Gas barrier adhesive layer / Second layer
[0115] Plastic film / vapor deposition layer (A) / vapor deposition layer (B) / vapor deposition protective coating / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0116] Plastic film / Printed layer / Evaporated layer (A) / Evaporated layer (B) / Evaporated protective coating / Gas barrier adhesive layer / Substrate used as intermediate layer / Adhesive layer / Second layer
[0117] Plastic film / vapor deposition layer (A) / vapor deposition layer (B) / vapor deposition protective coating / printed layer / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0118] Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Evaporated protective coating / Gas barrier adhesive layer / Substrate used as intermediate layer / Adhesive layer / Second layer
[0119] Heat-resistant resin layer / plastic film / vapor deposition layer (A) / vapor deposition layer (B) / gas barrier adhesive layer / second layer
[0120] Heat-resistant resin layer / plastic film / printed layer / vapor deposition layer (A) / vapor deposition layer (B) / gas barrier adhesive layer / second layer
[0121] Heat-resistant resin layer / Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Gas barrier adhesive layer / Second layer
[0122] Heat-resistant resin layer / plastic film / vapor deposition layer (A) / vapor deposition layer (B) / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0123] Heat-resistant resin layer / plastic film / printed layer / vapor deposition layer (A) / vapor deposition layer (B) / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0124] Heat-resistant resin layer / Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Gas barrier adhesive layer / Substrate used as intermediate layer / Adhesive layer / Second layer
[0125] Heat-resistant resin layer / plastic film / vapor deposition layer (A) / vapor deposition layer (B) / vapor deposition protective coating / gas barrier adhesive layer / second layer
[0126] Heat-resistant resin layer / plastic film / printed layer / vapor deposition layer (A) / vapor deposition layer (B) / vapor deposition protective coating / gas barrier adhesive layer / second layer
[0127] Heat-resistant resin layer / plastic film / vapor deposition layer (A) / vapor deposition layer (B) / vapor deposition protective coating / printed layer / gas barrier adhesive layer / second layer
[0128] Heat-resistant resin layer / Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Evaporated protective coating / Gas barrier adhesive layer / Second layer
[0129] Heat-resistant resin layer / plastic film / vapor-deposited layer (A) / vapor-deposited layer (B) / vapor-deposited protective coating / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0130] Heat-resistant resin layer / plastic film / printed layer / vapor-deposited layer (A) / vapor-deposited layer (B) / vapor-deposited protective coating / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0131] Heat-resistant resin layer / plastic film / vapor-deposited layer (A) / vapor-deposited layer (B) / vapor-deposited protective coating / printed layer / gas barrier adhesive layer / substrate used as intermediate layer / adhesive layer / second layer
[0132] Heat-resistant resin layer / Printed layer / Plastic film / Evaporated layer (A) / Evaporated layer (B) / Evaporated protective coating / Gas barrier adhesive layer / Substrate used as intermediate layer / Adhesive layer / Second layer
[0133] Heat-resistant resin layer / plastic film / gas barrier adhesive layer / second layer
[0134] Heat-resistant resin layer / plastic film / printed layer / gas barrier adhesive layer / second layer
[0135] Heat-resistant resin layer / Printed layer / Plastic film / Gas barrier adhesive layer / Second layer
[0136] In addition, coatings that impart functions such as release properties and antistatic properties can also be applied to plastic films.
[0137] (Packaging materials)
[0138] The laminated body of the present invention can be used as a multi-layer packaging material for the purpose of protecting food, pharmaceuticals, etc. When used as a multi-layer packaging material, its layer composition can be varied according to the contents, the usage environment, and the usage pattern. In addition, easy-opening and resealing mechanisms can be appropriately provided on the packaging body of the present invention.
[0139] As a packaging material of the present invention, for example, a laminate with a sealing layer is formed by overlapping the sealing layers of the laminate face to face and then heat-sealing its peripheral ends to form a bag. As a bag-making method, the laminate of the present invention can be bent or overlapped so that the inner layers (the sealing layers) face each other, and its peripheral ends are heat-sealed using methods such as side sealing, two-sided sealing, three-sided sealing, four-sided sealing, envelope sealing, folded sealing, flat-bottom sealing, corner-bottom sealing, insert sealing, and other heat-sealing methods. The packaging material of the present invention can take various forms depending on the contents, the usage environment, and the usage pattern. It can also be a self-standing packaging material (stand-up pouch). As a heat-sealing method, known methods such as rod sealing, rotary roller sealing, band sealing, pulse sealing, high-frequency sealing, and ultrasonic sealing can be used.
[0140] If the plastic film and the second substrate of the laminate of the present invention do not function as a sealing layer for heat-sealing during the formation of packaging material, a further sealing layer may be added. As a sealing layer, the additional substrate can be bonded with the adhesive of the present invention, or it can be an adhesive layer formed by the adhesive of the present invention.
[0141] In the packaging material of the present invention, after filling the contents through its opening, the opening is heat-sealed to manufacture an article using the packaging material of the present invention. Examples of the contents to be filled, for example, are food products: rice crackers, bean-based snacks, nuts, biscuits / cookies, wafers, fruit gummies, pies, semi-baked cakes, candies, snacks, bread, snack noodles, instant noodles, dried noodles, pasta, aseptically packaged rice, mixed porridge, porridge, packaged sticky rice cakes, cereal products, etc.; pickled vegetables, boiled beans, natto, miso, frozen tofu, tofu, chestnut mushrooms, konjac, processed wild vegetables, jams, peanut butter, salads, frozen vegetables, processed potato products, etc.; ham, cured meat, sausages, processed chicken products, corned beef, etc. Animal products such as processed meats, fish, ham / sausages, aquatic porridge products, fish cakes, seaweed, sweet seafood, dried bonito, salted fish, smoked salmon, spicy mentaiko and other processed aquatic products, fruits and meats such as peaches, citrus fruits, pineapples, apples, pears, cherries, corn, asparagus, mushrooms, onions, carrots, radishes, potatoes and other vegetables, frozen home-cooked dishes such as hamburger patties, meatballs, fried seafood, dumplings, croquettes and other cooked foods, dairy products such as butter, margarine, cheese, cream, instant cream powder, infant formula and other food products, liquid seasonings, steamed curry, pet food and other food products.
[0142] In addition, as a non-food product, it can be used as packaging material for various products such as cigarettes, disposable hand warmers, infusion bags and other pharmaceuticals, liquid detergents for washing, liquid detergents for kitchen use, liquid detergents for bathing, liquid soaps for bathing, liquid shampoos, liquid conditioners, lotions and other cosmetics, vacuum insulation materials, and batteries.
[0143] In particular, the packaging material of the present invention has excellent hydrogen sulfide adsorption capacity, thus its performance can be achieved even when the contents contain sulfur. For example, it is suitable as a packaging material for reheated foods because it reduces the cooking odor generated during cooking. In addition, because it can adsorb hydrogen sulfide generated by moisture intrusion, it is also suitable as an outer packaging material for all-solid-state lithium-ion batteries.
[0144] (Recycled plastics)
[0145] The laminate and packaging material of the present invention can also be directly processed using various known recycling plastic processing methods to manufacture recycled plastics. As a specific example, recycled plastics can be obtained by a manufacturing method having the following steps: a step of separating the laminate of the present invention into recycled materials of individual substrates, or a step of crushing the laminate and packaging material of the present invention; a step of melting and mixing the crushed film; and a step of granulating the melt-mixed mixture.
[0146] The crusher used for crushing (pulverizing) can be any known crusher; there are no special restrictions.
[0147] The pulverized film is physically mixed through processes such as melt mixing, solvent casting, latex mixing, and polymer compounding. Melt mixing is particularly common. Examples of equipment used for this mixing process include rotary drum mixers, Henschel mixers, rotary mixers, high-speed mixers, ribbon mixers, and V-type mixers. After melt mixing using such equipment, the film is granulated. Melt-mixed granulation typically uses single-screw or multi-screw extruders, which can either directly feed the film or compress it under heated or unheated conditions before feeding. Furthermore, in addition to these extruders, Banbury mixers, roller mixers, co-kneaders, jet mills, and Brabender rheometers can also be used, operating intermittently or continuously. Alternatively, the resin can be used as a molding resin without melt mixing, and melt mixing can be performed within the heating cylinder of a molding machine.
[0148] Example
[0149] The present invention will be described in more detail below with specific examples of synthesis and embodiments, but the present invention is not limited to these embodiments. It should be noted that, in the following examples, unless otherwise stated, "parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0150] (Examples 1-7)
[0151] In a vacuum evaporation apparatus (ULVACTECHNO, Ltd. VPC-1100) capable of both EB heating and resistance heating, zinc as a target is placed in a crucible, and the vacuum is reduced to 3.0 × 10⁻⁶. -3 Pa, while using a quartz oscillator to determine the film-forming speed, is heated to enable film formation in the range of 10 Å / s to 500 Å / s.
[0152] Oxygen is introduced as the process gas, and a zinc oxide (hereinafter referred to as ZnO) film is fabricated on a membrane (hereinafter referred to as AlOxOPP membrane) with a total light transmittance of over 90%. The aforementioned AlOxOPP membrane is a membrane on which 20 nm of aluminum oxide (hereinafter referred to as AlOx) is deposited on a biaxially stretched polypropylene membrane (hereinafter referred to as OPP membrane).
[0153] By controlling the conveying speed of the AlOxOPP membrane to control the film-forming time, gas barrier membranes of Examples 1-7 with varying ZnO membrane thickness were obtained.
[0154] (Example 8)
[0155] In a vacuum evaporation apparatus (ULVACTECHNO, Ltd. VPC-1100) capable of both EB heating and resistance heating, magnesium as a target is placed in a crucible, and the vacuum is reduced to 3.0 × 10⁻⁶. -3 Pa, while using a quartz oscillator to determine the film-forming speed, is heated to enable film formation in the range of 10 Å / s to 500 Å / s.
[0156] Oxygen was introduced as the process gas, and a magnesium oxide (hereinafter referred to as MgO) film was fabricated on an AlOxOPP film with a total light transmittance of over 90% as the indicator, resulting in the gas barrier film of Example 8.
[0157] (Example 9)
[0158] In a vacuum evaporation apparatus (ULVACTECHNO, Ltd. VPC-1100) capable of both EB heating and resistance heating, zinc as a target is placed in a crucible, and the vacuum is reduced to 3.0 × 10⁻⁶. -3 Pa, while using a quartz oscillator to determine the film-forming speed, is heated to enable film formation in the range of 10 Å / s to 500 Å / s.
[0159] Oxygen was introduced as the process gas, and a ZnO film was fabricated on a membrane (hereinafter referred to as AlOxPET membrane) with a total light transmittance of 90% or more. The AlOxPET membrane was a membrane with 20 nm of AlOx deposited on a polyethylene terephthalate membrane (hereinafter referred to as PET membrane), and the gas barrier membrane of Example 9 was obtained.
[0160] (Example 10)
[0161] In a vacuum evaporation apparatus (ULVACTECHNO, Ltd. VPC-1100) capable of both EB heating and resistance heating, zinc as a target is placed in a crucible, and the vacuum is reduced to 3.0 × 10⁻⁶. -3 Pa, while using a quartz oscillator to determine the film-forming speed, is heated to enable film formation in the range of 10 Å / s to 500 Å / s.
[0162] Oxygen was introduced as the process gas, and a ZnO film was fabricated on a membrane (hereinafter referred to as SiOxPET membrane) with a total transmittance of 90% or more as the indicator. The SiOxPET membrane is a membrane on which 30 nm of silicon oxide (hereinafter referred to as SiOx) is deposited by vapor deposition on a PET membrane, and the gas barrier membrane of Example 10 is obtained.
[0163] (Comparative Example 1)
[0164] An AlOxOPP film with 20 nm of AlOx deposited on a biaxially stretched polypropylene film (hereinafter referred to as OPP film) without ZnO was used.
[0165] (Comparative Example 2)
[0166] An AlOxPET film without ZnO deposition was used (thickness: 12 μm, AlOx film thickness: 20 nm).
[0167] (Comparative Example 3)
[0168] The evaluation was carried out using a SiOxPET film without ZnO deposition (thickness: 12 μm, SiOx film thickness: 30 nm), following the same steps as in the examples.
[0169] (Comparative Example 4)
[0170] In a vacuum evaporation apparatus (ULVACTECHNO, Ltd. VPC-1100) capable of both EB heating and resistance heating, zinc as a target is placed in a crucible, and the vacuum is reduced to 3.0 × 10⁻⁶. -3 Pa, while using a quartz oscillator to determine the film-forming speed, is heated to enable film formation in the range of 10 Å / s to 500 Å / s.
[0171] Oxygen was introduced as the process gas, and a ZnO film (20 nm thick) was fabricated on an OPP film with a total transmittance of 90% or more as the target. Next, aluminum was placed in a crucible as a target, and an AlOx film (40 nm thick) was fabricated on the previously fabricated ZnO vapor-deposited film using the same method, resulting in the film of Comparative Example 4.
[0172] (Evaluation of membrane fabrication)
[0173] The evaluation membrane used was membrane 1, which was directly used with the membranes of the examples and comparative examples, and laminated membrane 2, which was formed by bonding the membranes of the examples and comparative examples with unstretched polypropylene membrane (hereinafter referred to as CPP membrane) using an adhesive.
[0174] (Manufacturing method of laminate 2)
[0175] The films from the examples and comparative examples were mixed with DICDRY LX-830 and KW-75 (both manufactured by DIC) at a mixing ratio of 10 / 1.5. A reactive adhesive, obtained by mixing ethyl acetate with a non-volatile component of 25%, was coated onto the vapor-deposited layer (B) with a dried film thickness of 2.5 μm. After the diluted solvent was evaporated using a dryer set to 50°C, the film was laminated with a CPP film (P1128, manufactured by Toyobo). The film was aged at 40°C for 3 days to obtain laminate 2.
[0176] (Manufacturing method of laminate 3)
[0177] The laminate 2 was adjusted to a size of 30cm × 20cm. According to ASTM F392, a bending test was conducted using a Gelbo Flex Tester (manufactured by TESTER Industrial Co., Ltd.) under the conditions of 440° / 90mm linear motion for 65mm and bending 30 times at 23°C to obtain the laminate 3.
[0178] (Evaluation Method)
[0179] <Fluorescent X-rays>
[0180] The fluorescence X-ray intensity was measured on film 1. It was measured using a handheld fluorescence X-ray measuring device (X-MET8000, manufactured by Horiba, Ltd.), and the ratio of the metal of the vapor-deposited layer (B) to the metal of the vapor-deposited layer (A) on the film surface was calculated from the measured intensity.
[0181] Total transmittance
[0182] The total transmittance was measured for film 1. Based on JIS K7361 (1997), it was measured using a haze meter NDH7000 (manufactured by Nippon Denshoku Kogyo Co., Ltd.). Three gas barrier films, cut to dimensions of 10cm x 10cm, were measured. Each film was measured five times, and the average of the total 15 measurements was taken as the total transmittance.
[0183] <Ring Stiffness Test>
[0184] The ring stiffness value a (g / cm) was measured for membrane 1. A ring stiffness tester (manufactured by Toyo Seiki Co., Ltd.) was used. Under the conditions of a sample width of 25 mm, a ring length of 80 mm, and a compression distance of 10 mm, the force was read after 2 minutes of compression.
[0185] The ring stiffness value a1 of the film with only vapor deposition layer (A) and the ring stiffness value a2 of the film with vapor deposition layer (B) deposited on vapor deposition layer (A) are measured and evaluated using the rate of change (%) calculated by the following formula (1).
[0186] Equation (1) (a2-a1) / (a1)×100(%)
[0187] <Evaluation of gas barrier properties: Oxygen permeability>
[0188] Oxygen permeation rate (OTR) was measured on membranes 1, 2, and 3. Following JIS-K7126 (isobaric method), an OTR measuring apparatus (OX-TRAN2 / 22) from MOCON was used, under conditions of 23°C and 0%RH, and also under conditions of 23°C and 90%RH. RH represents relative humidity. It should be noted that the unit of OTR is cc / day·atm·m. 2 .
[0189] <Evaluation of air barrier properties: Water vapor transmission rate>
[0190] Water vapor transmission rate (MVTR) was measured on membranes 1, 2, and 3. The measurement was performed according to JIS-K7129 using an Illinois Water Vapor Transmission Rate Measuring Apparatus 7001, under conditions of 40°C and 90% RH. It should be noted that the unit for oxygen transmission rate is g / m³. 2 ·day.
[0191] Evaluation of hydrogen sulfide adsorption capacity
[0192] The hydrogen sulfide adsorption capacity was assessed using laminate 2. The laminate was adjusted to a size of 5cm x 5cm, placed in an odor bag, and heat-sealed. 3L of air was introduced to achieve a hydrogen sulfide gas concentration of 20ppm. The bag was allowed to stand for several hours (10 minutes, 1 hour, 3 hours, 6 hours, and 24 hours), after which the gas concentration inside the bag was measured using a gas detection tube.
[0193] Using the undeposited film as a control, the observed decrease in hydrogen sulfide gas concentration was judged as indicating the presence of hydrogen sulfide adsorption capacity.
[0194] The membrane composition and evaluation results of the embodiments are shown in Table 1, and the membrane composition and evaluation results of the comparative examples are shown in Table 2.
[0195] [Table 1]
[0196]
[0197] [Table 2]
[0198]
Claims
1. A gas barrier membrane, characterized in that, A vapor-deposited layer (A) of aluminum oxide and / or silicon oxide and a vapor-deposited layer (B) of divalent metal oxide are sequentially stacked on a plastic film.
2. The gas barrier membrane according to claim 1, wherein, The divalent metal oxide (B) is zinc oxide, magnesium oxide, and / or calcium oxide.
3. The gas barrier membrane according to claim 1, wherein, The thickness of the vapor-deposited layer (B) is in the range of 1~200 nm.
4. The gas barrier membrane according to claim 1, wherein, The ratio of metal in vapor-deposited layer (B) to metal in vapor-deposited layer (A) based on fluorescence X-ray intensity is in the range of 0.5:100 to 90:
100.
5. A packaging body comprising the gas barrier film according to any one of claims 1 to 4.
Citation Information
Patent Citations
Gas barrier film and method for producing the same
JP2013253319A
Gass barrier laminate film
JP2014069389A