Isocyanate compositions, methods for storing the same, and non-foamed polyurethanes comprising the same with optical lenses

By using a combination of specific nitrile-containing compounds and diisocyanate compounds, the problems of discoloration and turbidity of isocyanate compounds have been solved, achieving high stability and low defect rate of optical lenses while maintaining excellent optical properties and blue light blocking effect.

CN123076584APending Publication Date: 2026-11-10HANWHA SOLUTIONS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580026919.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-09
Filing Date
2025-04-08
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Isocyanate compounds are prone to oxidation or self-polymerization during storage and use, leading to discoloration and cloudiness, which affects the clarity and quality of optical lenses. Using UV blockers will increase the defect rate and reduce optical properties.

Method used

An isocyanate composition containing a diisocyanate compound and a nitrile compound is used, the content of the nitrile compound is controlled within a specific range, and it is stored under a nitrogen-purged atmosphere to reduce or eliminate the use of UV blockers.

Benefits of technology

It improves the storage stability of isocyanate compounds, reduces the defect rate of optical lenses, maintains excellent optical properties and blue light blocking effect, and reduces the use of UV blockers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to: an optical lens, wherein, at the time of manufacturing the optical lens, no or a significantly reduced amount of a UV blocker for blocking blue light is used; a non-foamed polyurethane for manufacturing the optical lens; an isocyanate composition for synthesizing the non-foamed polyurethane; and a method for storing the isocyanate composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to: an optical lens wherein, in manufacturing the optical lens, a UV blocker for blocking blue light is not used or its usage is significantly reduced; a non-foamed polyurethane for manufacturing the optical lens; an isocyanate composition for synthesizing the non-foamed polyurethane; and a method for storing the isocyanate composition. Background Technology

[0002] Isocyanate compounds are raw materials for polyurethanes and are used in a wide variety of applications such as coatings, tackifiers / adhesives, paints, foams, and optical materials. In fields requiring excellent appearance properties, especially in the case of polyurethanes used in optical applications where transparency is required, minimal discoloration is desirable. Therefore, it is important not only that discoloration does not occur during the polyurethane formation reaction, but also that the isocyanate compound used as a raw material, particularly polyvalent isocyanates with two or more functionalities, does not itself discolor.

[0003] However, due to the high reactivity of isocyanate compounds, they are easily oxidized by oxygen in the air or form self-polymers during storage, resulting in deterioration or fading. Furthermore, they can cause discoloration or clouding in optical products that use them, such as urethane lenses.

[0004] In this regard, various methods have been studied and proposed to suppress discoloration in isocyanate compounds and products made using isocyanate compounds, such as sealing with nitrogen to block air and storing under refrigeration, and adding additives such as ultraviolet absorbers for storage.

[0005] However, in order to use isocyanate compounds, they need to be moved from their storage location to the atmospheric environment. During this process, the isocyanate compounds may become discolored or cloudy depending on the moisture content of the atmosphere or changes in atmospheric temperature. If optical lenses or other components are manufactured using isocyanate compounds that have become discolored or cloudy, there will be problems with reduced clarity and deterioration in quality.

[0006] Furthermore, it is difficult to ensure the long-term storage stability of isocyanate compounds.

[0007] In addition, UV blockers are used to block blue light when manufacturing optical lenses, but there are problems: when UV blockers are used in the composition used to manufacture optical lenses, the defect rate of optical lenses increases or the optical properties decrease. Summary of the Invention

[0008] Technical issues This invention addresses the aforementioned problems. UV blockers can increase the defect rate and / or degrade the physical properties of optical lenses. Various studies and attempts have been made to reduce or eliminate the use of UV blockers. It has been found that when an appropriate amount of a specific compound is included in the isocyanate compound composition used to synthesize the non-foamed polyurethane for manufacturing optical lenses, the amount of UV blocker used in the polyurethane for manufacturing optical lenses can be reduced. Alternatively, even without using UV blockers, optical lenses with appropriate blue light blocking rates can be manufactured without adversely affecting the optical lenses. In other words, this invention aims to provide an isocyanate composition, a non-foamed polyurethane comprising the isocyanate, and an optical lens manufactured using the isocyanate.

[0009] Furthermore, the present invention aims to provide a method for storing isocyanate compositions.

[0010] Technical solution To address the above-mentioned problems, the isocyanate composition of the present invention comprises: a diisocyanate compound; and a nitrile-containing compound, the nitrile-containing compound comprising one or more compounds selected from those represented by Chemical Formula 1 and those represented by Chemical Formula 2.

[0011] In a preferred embodiment of the present invention, the additive may include a compound represented by the following chemical formula 1, a compound represented by the following chemical formula 2, and a compound represented by the following chemical formula 3.

[0012] [Chemical Formula 1]

[0013] [Chemical Formula 2]

[0014] In chemical formulas 1 and 2 above, R 1 and R 2 Each can be independently -CH2-, -CH2CH2-, or -CH2CH2CH2-, R 3 It can be a hydrogen atom, a C1 to C3 straight-chain alkyl group, a C3 to C5 branched alkyl group, or a metal salt, where a is an integer from 0 to 3, b is an integer from 0 to 5, and n is 1 or 2.

[0015] In a preferred embodiment of the invention, the content of the nitrile compound may be 700 ppm or less, based on the total weight of the isocyanate composition.

[0016] In a preferred embodiment of the present invention, the isocyanate composition may satisfy the following formula 1.

[0017] [Formula 1] 0.50 ≤ B / (A+B) ≤ 0.80 In Formula 1, A is the content (ppm) of the compound represented by the above chemical formula 1 based on the total weight of the isocyanate composition, and B is the content (ppm) of the compound represented by the above chemical formula 2 based on the total weight of the isocyanate composition.

[0018] In a preferred embodiment of the present invention, the isocyanate composition of the present invention may further include metal elements, measured by inductively coupled plasma atomic emission spectrometry (ICP-AES), including 1 ppm to 10 ppm of aluminum (Al) and 1 ppm to 20 ppm of calcium (Ca).

[0019] In a preferred embodiment of the present invention, the content of one or more metallic elements selected from tin (Sn), iron (Fe), titanium (Ti), chromium (Cr), nickel (Ni), manganese (Mn) and magnesium (Mg) may be 2.0 ppm or less.

[0020] In a preferred embodiment of the present invention, the diisocyanate compound may include one or more selected from 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, isophthalimethylene diisocyanate, terephthalimethylene diisocyanate, and orthophthalimethylene diisocyanate.

[0021] In a preferred embodiment of the present invention, the diisocyanate compound may include isophthalimide diisocyanate.

[0022] In a preferred embodiment of the invention, in chemical formula 1 and / or chemical formula 2, R 1 and R 2 They can each be independently -CH2- or -CH2CH2-, R 3 It can be a hydrogen atom or a metal salt, a can be an integer from 0 to 2, b can be an integer from 0 to 3, and n can be 1.

[0023] In a preferred embodiment of the present invention, the isocyanate composition may satisfy the following condition (1).

[0024] (1) 0.001% ≤ H b -H a ≤ 4.0% Under the above condition (1), H a H represents the haze value of the isocyanate composition.b The haze value represents the haze value measured after the isocyanate composition has been stored at a temperature of 20°C or lower and a relative humidity of 1% or lower for 70 to 110 days.

[0025] Meanwhile, the method for storing the isocyanate composition according to the present invention can store the isocyanate composition under a nitrogen-purified atmosphere at a temperature of 20°C or lower and a relative humidity of 1% or lower.

[0026] Furthermore, the polyurethane of the present invention is a non-foamed polyurethane used as an optical resin, and is synthesized using the above-described isocyanate composition.

[0027] Furthermore, the optical lens of the present invention may include non-foamed polyurethane.

[0028] In a preferred embodiment of the present invention, the optical lens of the present invention may have a yellowness index (YI) of 5.0 or less.

[0029] In a preferred embodiment of the present invention, the absorbance of the optical lens of the present invention at a wavelength of 415 nm can be 0.30% or less, preferably 0.15% to 0.30%, even without the use of additional UV blocking agents.

[0030] Beneficial effects The isocyanate composition of the present invention and the method for storing the isocyanate composition using the isocyanate composition can have excellent storage stability.

[0031] Furthermore, when optical lenses are manufactured from polyurethane synthesized using the above-mentioned isocyanate composition, the amount of UV blocker used can be significantly reduced or eliminated, thereby reducing the defect rate during the manufacture of optical lenses and enabling the manufacture of transparent optical materials (e.g., optical lenses) with excellent optical properties, low blue light absorption, and improved yellowness index (YI). Detailed Implementation

[0032] The invention will be described in more detail below.

[0033] Various methods have been studied and proposed for suppressing discoloration in conventional isocyanate compounds and products made using these compounds, such as sealing with nitrogen to prevent air exposure and storing under refrigeration, and adding additives such as UV absorbers for storage. However, in order to use the isocyanate compound, it is moved from its storage location to the atmospheric environment. During this process, the isocyanate compound may discolor or become cloudy depending on the moisture content of the atmosphere or changes in atmospheric temperature. If isocyanate compounds that have discolored or become cloudy are used to manufacture optical lenses, etc., there will be problems of reduced clarity and deterioration in quality. Furthermore, it is difficult to ensure the long-term storage stability of isocyanate compounds.

[0034] In addition, there is a problem that using UV blockers to block blue light during the manufacture of optical lenses can increase the defect rate of optical lenses and reduce their optical properties.

[0035] Therefore, the present invention provides an isocyanate composition comprising a diisocyanate compound and a nitrile-containing compound. When the specific compound contained in the isocyanate composition used in polyurethane synthesis is a nitrile-containing compound, the specific compound is retained in the polyurethane, and the nitrile-containing compound acts as a UV blocker, resulting in excellent blue light blocking effects for optical articles such as optical lenses made of polyurethane. In other words, by significantly reducing or eliminating the use of UV blockers in polyurethane, the increased defect rate and deterioration of optical properties of optical articles due to the use of UV blockers can be prevented.

[0036] In the isocyanate compositions of the present invention, the diisocyanate compound may include one or more selected from 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-cyclohexene diisocyanate, 1,4-cyclohexene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, isophthalimethylene diisocyanate, terephthalimethylene diisocyanate, and orthophthalimethylene diisocyanate, and may preferably include isophthalimethylene diisocyanate.

[0037] In addition, in the isocyanate composition of the present invention, the nitrile-containing compound includes one or more compounds selected from those represented by the following chemical formula 1 and those represented by the following chemical formula 2.

[0038] [Chemical Formula 1]

[0039] [Chemical Formula 2]

[0040] In the above chemical formulas 1 and 2, R 1 and R 2 Each is independently -CH2-, -CH2CH2- or -CH2CH2CH2-, preferably -CH2- or -CH2CH2-, more preferably -CH2-.

[0041] In addition, the above R 3 It is a hydrogen atom, a C1 to C3 straight-chain alkyl group, a C3 to C5 branched alkyl group, or a metal salt, preferably a hydrogen atom or a metal salt, more preferably a hydrogen atom. In this case, the metal salt is Na. + K + Monovalent cation metal salts.

[0042] Furthermore, 'a' is an integer from 0 to 3, preferably an integer from 0 to 2, and more preferably 0 or 1. Additionally, 'b' is an integer from 0 to 5, preferably an integer from 0 to 3, and more preferably an integer from 0 to 2.

[0043] In addition, n can be 1 or 2, preferably 1.

[0044] The nitrile-containing compound can be a byproduct and / or compound generated during the synthesis of the diisocyanate compound, and is typically removed during the purification step of the diisocyanate compound synthesis process. In this invention, the amount of nitrile-containing compound removed in the purification step is controlled such that it is contained in the isocyanate compound within a specific content range. When using the composition to synthesize polyurethane and manufacturing optical lenses from the synthesized polyurethane, to reduce defect rates and improve optical properties, the content of the nitrile-containing compound in the isocyanate composition is 700 ppm or less, preferably 30 ppm to 700 ppm, more preferably 50 ppm to 500 ppm, even more preferably 60 ppm to 480 ppm, and even more preferably 350 ppm to 450 ppm, based on the total weight of the isocyanate composition. A purification step is performed such that the nitrile-containing compound is contained within this content range. If, after the purification step, the content of the nitrile-containing compound in the isocyanate composition is below the listed range, these compounds may optionally be added to prepare the isocyanate composition.

[0045] Furthermore, the nitrile-containing compound may include either the nitrile-containing compound represented by Chemical Formula 1 above or the nitrile-containing compound represented by Chemical Formula 2 above. Preferably, including both the nitrile-containing compound represented by Chemical Formula 1 above and the nitrile-containing compound represented by Chemical Formula 2 above is advantageous in terms of UV blocking effect and low yellowness index of the optical lens, and more preferably, the nitrile-containing compound is included within the range satisfying the following Formula 1.

[0046] [Formula 1] 0.50 ≤ B / (A+B) ≤ 0.80, preferably 0.55 ≤ B / (A+B) ≤ 0.80, more preferably 0.60 ≤ B / (A+B) ≤ 0.75 In Formula 1, A is the content (ppm) of the compound represented by the above chemical formula 1 based on the total weight of the isocyanate composition, and B is the content (ppm) of the compound represented by the above chemical formula 2 based on the total weight of the isocyanate composition.

[0047] Furthermore, the isocyanate compositions of the present invention may contain metal elements as byproducts generated during the synthesis process. Metal elements in isocyanate compositions typically degrade the optical properties of optical lenses. However, in the presence of nitrile-containing compounds, certain metal elements can have a synergistic effect in UV blocking. Such metal elements include aluminum (Al) and / or calcium (Ca), and for this effect, the isocyanate compositions of the present invention may include 1 ppm to 15 ppm of aluminum (Al) and 1 ppm to 20 ppm of calcium (Ca), preferably 1.2 ppm to 10.0 ppm of aluminum (Al) and 3.0 ppm to 17.0 ppm of calcium (Ca), and more preferably 1.2 ppm to 6.0 ppm of aluminum (Al) and 3.0 ppm to 15.0 ppm of calcium (Ca).

[0048] For the purpose of preventing the degradation of the optical properties of polyurethane and optical lenses made therefrom, it is advantageous that the compositions of the present invention do not contain any metal elements other than Al and Ca. Therefore, the isocyanate compositions of the present invention may contain metal elements other than Al and Ca in an amount of 2.0 ppm or less, preferably 1.0 ppm or less, more preferably 0.5 ppm or less, or such metal elements may be absent. In this case, the metal elements other than Al and Ca may include one or more selected from tin (Sn), iron (Fe), titanium (Ti), chromium (Cr), nickel (Ni), manganese (Mn), and magnesium (Mg).

[0049] The isocyanate composition of the present invention has excellent long-term storage stability and can meet the following conditions (1).

[0050] (1) 0.001% ≤ H b -H a ≤ 4.0%, preferably 0.001% ≤ H b -H a ≤ 3.0%, more preferably 0.003% ≤H b -H a ≤2.0%, or more preferably 0.005% ≤ H b -Ha ≤1.0%, or even more preferably 0.005% ≤ H b -H a ≤ 0.5% In the above condition (1), H a H represents the haze value of the isocyanate composition. b The haze value represents the haze measured after the isocyanate composition has been stored at 20°C or lower and 1% or lower relative humidity for 70 to 110 days.

[0051] Furthermore, in the method for storing the isocyanate composition of the present invention, the composition is preferably stored in a nitrogen-padded atmosphere at a temperature of 20°C or lower and a relative humidity of 1% or lower, more preferably in a nitrogen-padded atmosphere at a temperature of 0°C to 20°C and a relative humidity of 0.001% to 1%, and even more preferably in a nitrogen-padded atmosphere at a temperature of 5°C to 15°C and a relative humidity of 0.001% to 0.1%. In this case, if the storage temperature is greater than 20°C, not only will the storage stability decrease, but there may also be problems such as the optical lenses manufactured therefrom becoming opaque due to increased haze and / or the inability to manufacture optical lenses therefrom. Similarly, if the relative humidity is greater than 1%, not only will the storage stability decrease, but there may also be problems such as the optical lenses manufactured therefrom becoming opaque due to increased haze.

[0052] [Methods for preparing the composition] The method for preparing the isocyanate composition of the present invention described above is as follows.

[0053] Isocyanate compositions are synthesized by reacting amine compounds with phosgene in a solvent.

[0054] As solvents used in the phosgenation reaction, aromatic hydrocarbon solvents such as benzene, toluene, xylene, or ethylbenzene; chlorinated aromatic hydrocarbon solvents such as monochlorobenzene, 1,2-dichlorobenzene, or 1,4-dichlorobenzene; or chlorinated hydrocarbon solvents such as dichloromethane, chloroform, or carbon tetrachloride can be used, and two or more of them can be used in combination.

[0055] The amine compound used in the phosgenation reaction can be, for example, an amine compound obtained by hydrogenating a nitro compound or its hydrochloride salt. Specifically, the amine compound can be one or more selected from the group consisting of 1,4-tetramethylenediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,3-cyclohexylenediamine, 1,4-cyclohexylenediamine, isophoronediamine, diamine, methylenediphenylamine, methylenedicyclohexylenediamine, toluenediamine, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine and their salts, and preferably m-phenylenediamine, p-phenylenediamine, o-phenylenediamine or their salts.

[0056] Based on 100 parts by weight of solvent, the amine compound may be contained in an amount of 1 to 20 parts by weight. If the content of the amine compound is greater than 20 parts by weight, a large amount of the amine compound may precipitate out. It may preferably be contained in an amount of 1 to 15 parts by weight or 3 to 10 parts by weight.

[0057] Specifically, the phosgenation reaction can be carried out by the following methods: a direct phosgenation method in which an amine compound reacts directly with phosgene (Method 1); a method in which an amine compound reacts with anhydrous hydrogen chloride to form an amine-hydrochloride compound, and then the formed salt is reacted with phosgene (Method 2); or a method in which an amine compound reacts with carbonic acid to form an aliphatic amine-carbonate compound, and then the formed salt is reacted with phosgene (Method 3).

[0058] The direct phosgenation method described in Method 1 above can be carried out by reacting an amine compound with phosgene in an organic solvent. In this case, the phosgene can be added all at once at the beginning of the reaction, or a portion can be added at the beginning of the reaction, and the remaining portion can be added in batches during the reaction.

[0059] Meanwhile, Method 1 above can be carried out through the following steps: a first step of dissolving a portion of phosgene in a solvent and then adding an amine compound; and a second step of adding the remaining portion of phosgene after the addition of the amine compound and allowing the reaction to proceed. In this case, the first step is preferably carried out at a temperature of -15°C to -10°C to prevent leakage of the highly toxic phosgene and to prevent rapid heating during the addition of the amine compound. Furthermore, the phosgenation reaction in the second step can be controlled at 120°C to 140°C, allowing the reaction to proceed at an appropriate rate without concern about the decomposition of the amine compound.

[0060] In the case of method 2 above, it can be carried out by the following steps: reacting the amine compound with hydrochloric acid in an organic solvent to form an amine-hydrochloride compound, and then adding phosgene to allow the reaction to proceed. The formation of the amine-hydrochloride compound can be carried out at a temperature of 30°C or lower, preferably at a temperature of about 23±5°C, and the reaction can be controlled to 120°C to 140°C after the addition of phosgene. When carried out under such temperature conditions, the solubility of the amine-hydrochloride compound increases, and the thermal decomposition of the isocyanate is prevented, allowing for the preparation of high-purity isocyanate compounds in high yield.

[0061] In the case of method 3 above, it can be carried out by the following steps: reacting the amine compound with carbonic acid in a solvent to form an amine-carbonate compound, and then adding phosgene to allow the reaction to proceed. In this case, the formation of the amine-carbonate compound can be carried out at a temperature of 30°C or lower, preferably at a temperature of about 23±5°C, and the reaction can be controlled to 80°C to 180°C after the addition of phosgene. Preferably, the reaction can be controlled to a range of 100°C or higher, or 120°C or higher, and 150°C or lower, or 140°C or lower. When carried out under such temperature conditions, the solubility of the amine-carbonate compound increases, and thermal decomposition of the isocyanate is prevented, allowing for the preparation of high-purity isocyanate compounds in high yield.

[0062] After the reaction with phosgene is completed according to the various methods, optional further steps for the removal of unreacted phosgene and hydrogen chloride gas may be carried out, such as nitrogen bubbling and solvent removal steps by distillation, which can be performed according to conventional methods.

[0063] In addition, after completing the reaction with phosgene according to each method and / or after performing the solvent removal step, a purification step is performed to remove organic impurities and inorganic impurities such as metal elements from the prepared isocyanate compound. Preferably, the purification step is carried out using a thin-film evaporator (or system, TFE) under specific conditions, thereby allowing control over the content of specific nitrile-containing compounds and specific metal elements in the isocyanate compound.

[0064] As a preferred example of the conditions for the purification step using TFE, the purification step is carried out under the following conditions: the feed temperature of the isocyanate compound is 75°C to 150°C, the feed rate is 8 mL / min to 35 mL / min, the TFE distillation temperature is 130°C to 170°C, and the vacuum degree is 0.1 Torr to 4.0 Torr; preferably, the feed temperature is 88°C to 145°C, the feed rate is 9 mL / min to 32 mL / min, the TFE temperature is 135°C to 165°C, and the vacuum degree is 0.2 Torr to 3.2 Torr; more preferably, the feed temperature is 90°C to 142°C, the feed rate is 9.5 mL / min to 31.0 mL / min, the TFE temperature is 138°C to 162°C, and the vacuum degree is 0.3 Torr to 3.0 Torr. In this case, the purification step under the above conditions is preferred in terms of the following effects: the nitrile-containing compounds represented by chemical formula 1 and / or chemical formula 2 are not completely removed, but are retained in the synthesized isocyanate compounds at a certain concentration; Al and Ca are retained within an appropriate range; and other metal elements are sufficiently removed.

[0065] The polyurethane of the present invention is a non-foamed polyurethane synthesized using the above-described isocyanate composition.

[0066] In addition, non-foamed polyurethane can be used for one or more applications selected from automotive, marine, coating, adhesive, sealant and elastomer.

[0067] In addition, non-foamed polyurethane can be used as a transparent optical material. When used as a material for optical lenses, the amount of UV blocker used to impart blue light blocking effect can be minimized, or UV blocker can be omitted altogether.

[0068] In addition, the yellowness index (YI) of the optical lens can be 5.0 or less, preferably 0.1 to 4.5, and more preferably 0.5 to 4.0.

[0069] In addition, the absorbance of the optical lens of the present invention at a wavelength of 415 nm can be 0.30% or less, preferably 0.15% to 0.30%, even without the use of additional UV blocking agents.

[0070] The invention will be described in more detail below by way of examples. However, the following examples do not limit the scope of the invention and should be construed as being provided to aid in understanding the invention.

[0071] [Example] Example 1-1: Preparation of isocyanate composition 471 g of 1,2-dichlorobenzene and 32.5 g of m-XDA (m-xylenediamine) with a purity of 99.4% were placed in a flask, and anhydrous hydrogen chloride was fed at a rate of 20 g / hr with stirring at room temperature (23±5℃). Due to the feeding of anhydrous hydrogen chloride, the temperature rose to 50℃.

[0072] Four hours after feeding, the formed salt was cooled to room temperature, and 43 mL of liquid phosgene was introduced into the reactor. The reactor temperature was then heated to 130°C. From the time the phosgene was added until the reaction was complete, a dry ice-acetone condenser was used to prevent phosgene leakage to the outside. After the reactor temperature reached 130°C, it was maintained between 125°C and 135°C for 2 hours until the reaction solution became clear. After the reaction solution became clear, the inside of the reactor was cooled to 80°C while purging with nitrogen to obtain a reaction solution in which phosgene had been removed.

[0073] Next, the solvent was removed from the reaction solution where phosgene had been removed by vacuum distillation, and the product was purified using a thin-film evaporator (TFE) to obtain an isocyanate-based composition including m-XDI (m-xDI, m-xylene diisocyanate). In this case, the TFE purification conditions were: feed temperature 80°C, TFE temperature 160°C, vacuum 3 Torr, and feed rate 30 mL / min.

[0074] The isocyanate composition contains 2 ppm of a nitrile-containing compound represented by the following chemical formula 1-1 and 49 ppm of a nitrile-containing compound represented by the following chemical formula 2-1.

[0075] [Chemical Formula 1-1]

[0076] In the above chemical formula 1-1, R 1 The expression is -CH2-, a is 1, b is 0, and n is 1.

[0077] [Chemical Formula 2-1]

[0078] In the above chemical formula 2-1, R 2 For -CH2-, R 3 For each hydrogen atom, a is 1, b is 0, and n is 1.

[0079] Comparative Example 1-1 A reaction solution in which phosgene has been removed was obtained using the same composition and method as in Example 1. The solvent was then removed by vacuum distillation, a conventional purification method, and the solution was subjected to reduced pressure treatment at a bottom temperature of 148°C and a pressure of 0.6 mbar to prepare an isocyanate-based composition containing m-XDI (yield: 65%).

[0080] Examples 1-2 to 1-5 and Comparative Examples 1-2 to 1-5 Isocyanate-based compositions containing m-XDI were prepared using the same composition and method as in Example 1, except that the purification step conditions were changed as shown in Table 1 below, thereby performing Examples 1-2 to Examples 1-5 and Comparative Examples 1-2 to Comparative Examples 1-5 respectively.

[0081] [Table 1]

[0082] Experimental Example 1: Measurement of the content of nitrile-containing compounds and metal elements For each isocyanate-based composition prepared in Examples 1-1 to 1-5 and Comparative Examples 1-1 to 1-5 above, the content of nitrile-containing compounds represented by chemical formula 1-1 and / or chemical formula 2-1 and the content of metal elements were measured, and the results are shown in Tables 2 and 3 below.

[0083] [Table 2]

[0084] [Table 3]

[0085] Referring to Tables 2 and 3 above, compared with other examples, in the case of Comparative Example 1-1, which was prepared by purification using conventional purification steps, the content of nitrile-containing compounds was relatively very high, especially the content of Al and Na among the metal elements. Furthermore, Comparative Examples 1-2 and 1-3 had a Ca content exceeding 20 ppm and a high Mg residue, and Comparative Example 1-2 contained residual Sn.

[0086] Furthermore, compared to the examples, Comparative Examples 1-4 showed relatively high contents of nitrile compounds, as well as high Al and high Ca contents.

[0087] Experimental Example 1: Measurement of APHA color and haze According to the method of ASTM E313, the APHA color and haze of each isocyanate composition prepared in Examples 1-1 to Examples 1-5 and Comparative Examples 1-1 to Comparative Examples 1-4 were measured using Ultrascan Pro from HunterLab (light source: C / 2), and the results are shown in Table 4 below.

[0088] In addition, after storing the various isocyanate compositions prepared in the Examples and Comparative Examples at a temperature of 15°C and a humidity of 0.1%RH under a nitrogen-placing atmosphere for 90 days, the APHA color and haze of the stored isocyanate compositions were measured (light source: C / 2), and the results are shown in Table 4 below.

[0089] APHA (Hazen color number) measurement is performed according to the method of color difference analysis at room temperature according to ASTM D1003, and the Hazen color number is measured using a xenon lamp source from the Ultrascan instrument from Hunterlab.

[0090] [Table 4]

[0091] Table 4 confirms that the isocyanate compositions prepared in Examples 1 to 4 have low haze values ​​and low APHA color values ​​even after 90 days of storage.

[0092] In addition, it was confirmed that the isocyanate compositions prepared in Examples 1-1 to 1-5 exhibited increased haze and APHA color values ​​after 90 days of storage.

[0093] In contrast, the isocyanate compositions of Comparative Examples 1-1 to 1-4, which have high metal content, exhibit significantly high APHA color values ​​compared to the examples, making them unsuitable for use as transparent optical materials or exhibiting relatively poor storage stability.

[0094] Manufacturing Example 1: Manufacturing of Optical Lenses 20.8 g of the isocyanate composition prepared in Examples 1-1, 0.04 g of ZELEC® UN (manufactured by Stepan) as an internal release agent, and 0.04 g of Biosorb® 583 (manufactured by Sakai Chemical Industry Co., Ltd) as a UV absorber were stirred and mixed at room temperature (23°C to 25°C) for 20 minutes to prepare a mixture. 0.002 g of DBTC (dibutyltin dichloride) was added to the prepared mixture and stirred for 10 minutes. Then, 19.2 g of 2,3-bis(2-thioethylthio)propane-1-thiol was added, and the mixture was stirred for 1 hour while defoaming at 5 mbar to prepare a composition for polyisocyanate polymerization.

[0095] The composition for polyisocyanate polymerization was prepared by filtering through a 1 μm PTFE filter and then fed into a mold consisting of a glass mold and adhesive tape. The mold was then placed in an oven, and polymerization was carried out for 20 hours while the temperature was gradually increased from 10 °C to 120 °C. After polymerization, the mold was removed from the oven and demolded to obtain individual plastic optical lenses. The obtained optical lenses were annealed at 120 °C for 6 hours to prepare optical lenses with a thickness of 9 mm.

[0096] Manufacturing Examples 2 to 6 and Comparative Manufacturing Examples 1 to 3 Except for the isocyanate composition used in Example 1-1, an optical lens was prepared with the same composition and method as in Manufacturing Example 1, except that, as shown in Table 5 below, additional nitrile-containing compounds represented by Chemical Formula 1-1 and Chemical Formula 2-1 were added to the isocyanate composition to increase the total amount of nitrile-containing compounds, and the content of nitrile-containing compounds was adjusted to satisfy Formula 1.

[0097] [Formula 1] 0.50 ≤ B / (A+B) ≤ 0.80 In Formula 1, A is the content (ppm) of the compound represented by Formula 1-1 in Example 1-1 based on the total weight of the isocyanate composition, and B is the content (ppm) of the compound represented by Formula 2-1 in Example 1-1 based on the total weight of the isocyanate composition.

[0098] [Table 5]

[0099] Experiment Example 2: Measurement of the physical properties of optical lenses The yellowness index (YI) of each optical lens manufactured in Manufacturing Examples 1 to 5 and Comparative Manufacturing Examples 1 to 3 was measured using Ultrascan Pro from HunterLab according to the method of ASTM D1209. The results are shown in Table 6.

[0100] In addition, transparency was evaluated by visually observing the degree of turbidity under various light source conditions, according to the following evaluation criteria. The evaluation was conducted as follows, and the results are shown in Table 6 below.

[0101] <Transparency Evaluation Criteria> C (Clear): Transparent under both fluorescent and zirconium lamps. SH (Slight Lamp Haze): Transparent under fluorescent light, but some cloudiness is observed under zirconium lamp. LH (Luminous Haze): Transparent under fluorescent light, but appears cloudy under zirconium lamp. VH (Visual Haze): Turbidity was observed under both fluorescent and zirconium lamps. In addition, according to the method of ASTM D1209, the absorbance of blue light (wavelength 415nm) was calculated using Ultrascan Pro from HunterLab by the following formula 1.

[0102] [Formula 1] Absorbance (A) = 2 - log(T) In Formula 1, T represents the transmittance at a wavelength of 415 nm.

[0103] [Table 6]

[0104] Referring to Table 6, the optical lenses of Manufacturing Examples 1 to 6 exhibited particularly low yellowness indices while possessing excellent transparency. In particular, they showed high blue light blocking rates even without the use of UV blockers during manufacturing, which is a result of low blue light absorption. However, compared to Manufacturing Examples 2 to 6, Manufacturing Example 1, with a nitrile compound content of approximately 51 ppm, showed a relatively slightly higher blue light absorption.

[0105] In addition, in the case of Comparative Manufacturing Example 1, the optical film was manufactured from the isocyanate composition of Comparative Example 1-1, which has a high metal element content and a nitrile compound content of 700 ppm or more. This optical film has low blue light absorption but a relatively high yellowness index and poor transparency.

[0106] Furthermore, in Comparative Manufacturing Example 2, where the value of Formula 1 exceeds 0.75, and in Comparative Manufacturing Example 3, where the value of Formula 1 is less than 0.50, the absorption of blue light is low.

[0107] The specific embodiments have been illustrated and described above. However, the present invention is not limited to the above embodiments, and those skilled in the art can make various modifications without departing from the spirit and intent of the invention as set forth in the appended claims.

Claims

1. An isocyanate composition comprising: Diisocyanate compounds; and A nitrile-containing compound, said nitrile-containing compound comprising one or more compounds selected from those represented by Chemical Formula 1 and those represented by Chemical Formula 2: [Chemical Formula 1] [Chemical Formula 2] In chemical formulas 1 and 2 above, R 1 and R 2 Each can be independently -CH2-, -CH2CH2-, or -CH2CH2CH2-, R 3 It can be a hydrogen atom, a C1 to C3 straight-chain alkyl group, a C3 to C5 branched alkyl group, or a metal salt, where a is an integer from 0 to 3, b is an integer from 0 to 5, and n is 1 or 2.

2. The isocyanate composition according to claim 1, wherein the nitrile-containing compound is contained in an amount of 700 ppm or less based on the total weight of the isocyanate composition.

3. The isocyanate composition according to claim 2, wherein the isocyanate composition satisfies the following formula 1: [Formula 1] 0.50 ≤ B / (A+B) ≤ 0.80 In Formula 1, A is the content (ppm) of the compound represented by Formula 1 above, based on the total weight of the isocyanate composition, and B is the content (ppm) of the compound represented by Formula 2 above, based on the total weight of the isocyanate composition.

4. The isocyanate composition according to claim 1, comprising a metal element measured by inductively coupled plasma atomic emission spectrometry (ICP-AES), wherein the metal element comprises 1 ppm to 15 ppm of aluminum (Al) and 1 ppm to 20 ppm of calcium (Ca).

5. The isocyanate composition according to claim 1, wherein, The content of one or more metallic elements selected from tin (Sn), iron (Fe), titanium (Ti), chromium (Cr), nickel (Ni), manganese (Mn) and magnesium (Mg) is 2.0 ppm or less.

6. The isocyanate composition according to claim 1, wherein the diisocyanate compound comprises one or more selected from 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, isophthalimethylene diisocyanate, terephthalimethylene diisocyanate, and orthophthalimethylene diisocyanate.

7. The isocyanate composition according to claim 1, wherein the diisocyanate compound is isophthalimide diisocyanate.

8. The isocyanate composition according to claim 1, wherein R 1 and R 2 Each is independently -CH2- or -CH2CH2-, R 3 is a hydrogen atom or a metal salt, a is an integer from 0 to 2, b is an integer from 0 to 3, and n is 1.

9. The isocyanate composition according to claim 1, wherein the isocyanate composition satisfies the following condition (1): (1) 0.001% ≤ H b -H a ≤ 4.0% in, Under the above condition (1), H a H represents the haze value of the isocyanate composition. b The haze value represents the haze measured after the isocyanate composition has been stored at 20°C or lower and 1% or lower relative humidity for 70 to 110 days.

10. A method for storing an isocyanate composition, comprising storing the isocyanate composition according to any one of claims 1 to 9 in a nitrogen-purified atmosphere at a temperature of 20°C or lower and a relative humidity of 1% or lower.

11. A non-foamed polyurethane, synthesized using an isocyanate composition according to any one of claims 1 to 9.

12. An optical lens comprising the non-foamed polyurethane according to claim 11.

13. The optical lens according to claim 11, characterized in that, The optical lens has a yellowness index (YI) of 5.0 or less.

14. The optical lens according to claim 11, characterized in that, The optical lens has an absorbance of 0.15% to 0.30% at a wavelength of 415 nm.