Apparatus and method for continuous production of metal

By using a metal refining device and method in an atmosphere-controlled chamber, and by continuously moving a movable feed box for metal vapor separation and condensation, the problems of low productivity and high energy consumption caused by intermittent processes are solved, and efficient and low-consumption continuous metal production is achieved.

CN123076689APending Publication Date: 2026-11-10COMMONWEALTH SCI & IND RES ORG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580027215.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-26
Filing Date
2025-03-25
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing metal refining processes, such as magnesium production, typically employ intermittent processes, resulting in low productivity and high energy consumption, making it difficult to achieve continuous production under low pressure and high temperature conditions.

Method used

Design a metal refining equipment and method that utilizes a movable feed box that moves continuously within an atmosphere-controlled chamber. Through a combination of a feeding unit, a metal refining unit, and a condenser, metal vapor is separated and condensed. The process employs thermal reduction or distillation under low-pressure vacuum conditions to ensure environmental control and impurity prevention.

Benefits of technology

It enables continuous metal production, improves production efficiency, reduces energy consumption, and produces high-purity metal products while reducing the introduction of impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076689A_ABST
    Figure CN123076689A_ABST
Patent Text Reader

Abstract

A metal extraction apparatus for extracting a selected metal from a metal-containing feedstock, the apparatus comprising: a feed unit configured to feed the metal-containing feedstock onto at least one movable cartridge; a metal extraction unit connected to the feed unit, the metal extraction unit comprising a heated interior space and, in the interior space, the selected metal is separated from the metal-containing feedstock in the form of a metal vapor; at least one condenser in fluid communication with the interior space of the metal extraction unit to condense the metal vapor from the interior space to form a metal product; and a drive unit for driving the at least one movable cartridge to move through the feed unit and the metal extraction unit, wherein the feed unit, the metal extraction unit, the at least one condenser, and the movable cartridge therein are enclosed within an atmosphere-controlled chamber or a plurality of atmosphere-controlled chambers in fluid communication.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority cross-referencing

[0002] This application claims priority to Australian Provisional Patent Application No. 2024900807, filed on 26 March 2024, the contents of which are to be construed as incorporated herein by reference. Technical Field

[0003] This application discloses a novel apparatus and method for the continuous extraction of metals from metallic raw materials. This apparatus and method are particularly suitable for extracting metals such as magnesium using distillation or thermal reduction processes in a vacuum distillation tank arrangement, and will be described in this context. However, it should be understood that the system and method can be applied to any metal that can be produced similarly using thermal reduction, heat recovery, metal distillation, or equivalent metal separation processes. Background Technology

[0004] The following discussion of the background of the invention is intended to aid in understanding the invention. However, it should be understood that this discussion is not an admission or confirmation that any material mentioned has been published, is known, or is part of the general public knowledge as of the priority date of this application.

[0005] Magnesium is typically produced via a thermal reduction route known as the Pidgeon Process, in which magnesium feedstocks such as dolomite are calcined to produce magnesium oxide, which is then heated at high temperatures under vacuum with a reducing agent such as ferrosilicon, thereby thermally reducing the magnesium oxide to magnesium. Under these conditions (temperatures of at least 1200°C and high vacuum – pressures below 100 Pa), magnesium vapor is produced, which can then be cooled and condensed to form solid metallic magnesium. The overall reaction is endothermic and can therefore have high energy requirements. To maintain low reaction temperatures, the process is typically operated under high vacuum.

[0006] In many cases, the high vacuum and high temperature conditions required for the thermal reduction of magnesium must be achieved through a batch process to create those conditions in a sealed environment. However, batch production can limit the productivity of the process because the operation of the production equipment includes auxiliary steps, such as start-up, shutdown, loading, and unloading processes. Furthermore, heat losses occur during these auxiliary steps.

[0007] Similarly, the purification of metals such as magnesium, for example using metal distillation processes, also requires low-pressure and high-temperature conditions, which typically necessitates the use of batch processes to create those conditions in a sealed environment. This, too, can limit the productivity of the process.

[0008] Therefore, providing an apparatus and related continuous process for refining metals such as magnesium from metallic raw materials would have certain advantages. The apparatus and related continuous process can be configured for thermal reduction processes, metal distillation processes, etc. Summary of the Invention

[0009] This application discloses a metal refining apparatus and / or method, which can be used to refine metals from metal-containing raw materials. The method can be used to thermally reduce the metal-containing raw materials and separate the desired metal; or for temperature-based separation (such as metal distillation) to separate the desired metal from the metal-containing raw materials.

[0010] The first embodiment provides a metal refining apparatus for extracting selected metals from metallic raw materials, the apparatus comprising: A feeding unit configured to convey the metal-containing raw material to at least one movable hopper; A metal refining unit connected to the feeding unit, the metal refining unit including an internal space, the internal space being heated, and in the internal space, the selected metal being separated from the metal-containing raw material in the form of metal vapor; At least one condenser, the at least one condenser being in fluid communication with the internal space of the metal refining unit, for condensing the metal vapor from the internal space to form a metal product; and A drive unit is configured to drive the at least one movable hopper to move through the feeding unit and the metal refining unit. The feeding unit, the metal refining unit, the at least one condenser, and the movable feed box therein are enclosed in an atmosphere-controlled chamber or in multiple atmosphere-controlled chambers in fluid communication.

[0011] Therefore, the first embodiment provides a metal refining apparatus capable of continuously producing metal from a metal-containing raw material. The raw material can be continuously moved through the metal refining unit via the drive unit on at least one movable hopper (typically a series of movable hoppers), the raw material being separated from the metal-containing raw material in the form of metal vapor in the metal refining unit for production of the desired metal via thermal reduction. This enables continuous metal production by continuously passing the raw material through the system. Furthermore, the feeding unit, the metal refining unit, and the at least one condenser are advantageously arranged within an atmosphere-controlled chamber, which provides environmental control within its interior.

[0012] The metal refining unit can be configured to heat the metal-containing raw material to generate metal vapor therein. The metal vapor can be generated by the boiling point difference between a selected metal and other components of the metal-containing raw material, or by a reaction (e.g., a reduction reaction – such as a thermal reduction reaction). Therefore, the metal refining equipment can include one or more of the following: thermal separation equipment, distillation equipment / metal distillation equipment, reduction equipment, thermal reduction equipment, etc.

[0013] In some forms, this first embodiment may include a thermal reduction apparatus capable of continuously producing metals such as magnesium from a metal-containing raw material (e.g., a magnesium oxide-containing raw material). In these forms, a metal refining unit may be configured for the thermal reduction reaction of the metal-containing raw material, which produces metal vapor. Alternatively, this first embodiment may include a distillation apparatus capable of continuously separating metals such as magnesium and lithium from the metal-containing raw material based on the differences in boiling points of its components. In these forms, a metal refining unit may be configured to separate a selected metal from the metal-containing raw material based on the boiling point of the selected metal to produce metal vapor.

[0014] Once the movable cassettes have passed through the metal refining unit, continuous production can be further achieved by returning each movable cassette to the feeding unit. In an embodiment, the at least one movable cassette can be configured to return to the feeding unit after it leaves the metal refining unit to receive the next batch of metal-containing raw material. This return can be facilitated by any suitable means; for example, an additional drive unit in the cassette return unit can be used to receive each movable cassette and transport each movable cassette from the outlet of the metal refining unit back to the feeding unit. However, the device can be configured such that the drive unit drives the at least one movable cassette to move back to the feeding unit. This can advantageously utilize the drive unit to achieve movement of the at least one movable cassette at various stages / units of the device.

[0015] The system can be completely sealed under low-pressure conditions (typically high vacuum conditions), thus enclosing the raw materials and containers within a controlled environment. In this regard, the atmosphere-controlled environment can be used to ensure that the temperature and environment throughout the entire device remain constant. It should be understood that "low pressure" and "low-pressure conditions" refer to pressures less than atmospheric pressure (i.e., less than approximately 100 Pa absolute pressure (equivalent to 0.001 bar)). In embodiments, the feed unit, the first condenser, the second condenser, and the movable feed box therein can be enclosed in one atmosphere-controlled chamber or multiple atmosphere-controlled chambers in fluid communication. In some embodiments, the drive unit can also be enclosed in an atmosphere-controlled chamber in fluid communication with the atmosphere-controlled chamber. The atmosphere in the atmosphere-controlled chamber or the atmosphere-controlled chamber in fluid communication can be controlled by an atmosphere control unit configured to maintain the desired atmospheric conditions therein. Enclosing critical units within a controlled atmosphere facilitates good process control of the thermal reduction process and controls the intrusion of impurities that might otherwise enter the device / system. For example, a controlled environment can cause any dust present to settle rapidly because there is little or no atmosphere to suspend fine particles. It should be noted that dust is an impurity that can be mixed into the metal being refined on one or more condensers. This low pressure can be generated by a powerful vacuum pump that can reduce the pressure to less than 100 Pa. An atmosphere-controlled chamber or a fluidly connected atmosphere-controlled chamber may include at least one vacuum pump capable of generating an absolute pressure of less than 50 Pa, preferably 5 Pa to 50 Pa, more preferably 10 Pa to 40 Pa, and still more preferably 10 Pa to 25 Pa. In many cases, the metal extraction process can be optimized by maintaining the pressure within the metal refining unit below 40 Pa.

[0016] The atmosphere-controlled chamber can have any suitable configuration. It can comprise a shared or common atmosphere-controlled chamber, or alternatively, multiple chambers in fluid communication. In an embodiment, the atmosphere-controlled chamber may include at least one vacuum chamber, which is divided into at least a feed unit and a metal refining unit using at least one partition or baffle. The at least one vacuum chamber may be configured with at least one sealable pressure door through which access to its interior is possible. The at least one vacuum chamber may include one or more peripheral ports through which at least one condenser is located within and extends from the vacuum chamber, and may communicate with a movable hopper refining unit (e.g., a chute described below).

[0017] The low-pressure atmosphere within the system may need to be minimized, or more typically, prevented from allowing air to seep into the metal refining unit. Therefore, the system may be fluidly sealed and may include various seals, valve seals, or similar components.

[0018] The extraction of a selected metal from the metal-containing raw material can be carried out in a single stage, or in two or more stages within the metal refining unit. In a single-stage process, the raw material can be heated in a single internal space, which is in fluid communication with a single condenser unit. When using two or more stages, the internal space of the metal refining unit can be sequentially divided into at least two heating spaces in the direction of movement of the raw material through the metal refining unit, wherein each heating space is connected to a separate condenser. For example, the at least two heating spaces may include at least a first heating space and a second heating space. The apparatus can then include two or more condensers, wherein each condenser is connected to a separate heating space. For example, a first condenser may be in fluid communication with the first heating space of the metal refining unit to condense a first metal vapor from the first heating space; and a second condenser may be in fluid communication with the second heating space of the metal refining unit to condense a second metal vapor from the second heating space. This allows the raw materials to be heated to different temperatures sequentially as they move through the metal refining unit (i.e., through the first heating space and then through the second heating space), thereby vaporizing different substances according to their boiling / vaporization points.

[0019] It should be understood that the internal space can be divided into separate heating spaces, and each heating space is connected to a separate condenser. For example, if the internal space is sequentially divided into at least three spaces in the direction of movement of the raw material through the metal refining unit, each of the three spaces can be connected to a separate condenser.

[0020] For example, a first heating space can be configured to heat the raw material to a temperature at which a first component or substance (such as an impurity) from the raw material is sufficiently vaporized, and a second heating space can be configured to heat the raw material to a temperature at which a selected metal in the raw material is sufficiently vaporized. These temperature ranges may vary depending on the metal being refined. For example, for the thermal reduction of magnesium oxide-rich raw materials, the first heating space can be configured to enclose the metal-containing raw material therein and heat it to 200°C to 1150°C, preferably 700°C to 1150°C, more preferably 800°C to 1100°C. Similarly, the second heating space can be configured to enclose the metal-containing raw material therein and heat it to 1100°C to 1300°C, preferably greater than 1150°C, more preferably at least 1200°C. This temperature difference can be achieved using two different heating zones with two different setpoint temperatures. However, even when using a single heat source (e.g., a high-temperature furnace), it should be understood that the metal-containing feedstock entering the heating zone of the metal refining unit will be gradually heated from the feed temperature (typically below 100°C) to at least 1200°C, and the different heating zones can be distinguished using this gradual heating profile. The movement of the metal-containing feedstock through the internal space of the metal refining unit and within its heating zones allows the feedstock to gradually move from a first heating space to a second heating space, while being gradually heated to at least 1200°C. Therefore, the size of the first heating space can be configured to include the metal-containing feedstock at, for example, 200°C to 1150°C during the heating process. Using two strategically positioned condensers in such a configuration allows for the production of high-purity metals, such as Mg, without the need for refining. An example of a high-purity metal is one with a purity greater than 99%, more specifically greater than 99.5%, and more specifically greater than 99.7%. This purity can be collected from the second condenser, while impurities from the feedstock can be extracted and collected from the first condenser before the feedstock enters the second internal space.

[0021] The internal space of the metal refining unit can be sequentially divided into at least two heating spaces by at least one baffle in the direction in which the raw material moves through the metal refining unit. The internal space may include at least two baffles positioned at or near the ends of the internal space. These baffles can be used to retain internal gas / vapor flow within the internal space. When the internal space is divided into at least two distinct heating spaces (e.g., a first heating space and a second heating space), those heating spaces can be separated by any number of baffles. When a first heating space and a second heating space are provided, the at least one baffle may include a first baffle, a second baffle, and a third baffle, the first baffle and the third baffle being positioned at or near the ends of the internal space, and the second baffle being positioned between the first baffle and the third baffle to divide the internal space into the first heating space and the second heating space. The first baffle, the second baffle, and the third baffle may be spaced apart along the direction of material movement. The first baffle and the third baffle may be positioned at or near the ends of the internal space (i.e., the beginning and end of the internal space in the direction of material movement). Each baffle may comprise a sheet, plate, or membrane. The baffle may be configured to direct vapors generated from heating the feed product within an adjacent internal space to a corresponding fluidly connected condenser. Furthermore, each baffle may include a guide configured to space the baffle from at least one movable hopper. The guide ensures that the baffle does not jam the hopper as it moves through the metal refining unit.

[0022] As described above, the first heating space can be configured to heat the feedstock to a temperature at which a first component or substance (such as an impurity) from the feedstock is sufficiently vaporized, and the second heating space can be configured to heat the feedstock to a temperature at which a selected metal in the feedstock is sufficiently vaporized. In this configuration, the function of the second baffle can be to direct the first component or substance—such as impurities from the feedstock—e.g., Na, K, Cl, H2O, and CO2 during the production of Mg from a MgO-rich feedstock—towards the first condenser, thereby enabling the second condenser to collect a metal of higher purity (e.g., Mg metal). If this higher purity metal is collected with sufficient purity (i.e., substantially free of the impurities collected in the first condenser), the metal may not require refining. An example of a high-purity metal is greater than 99%, more specifically greater than 99.5%, and more specifically greater than 99.7%. The amount of metal collected on the first condenser will be less because the first heating space is designed such that the feedstock moving through the metal refining unit may just reach the temperature at which metal vapor is formed before passing through the second baffle. Impurities are released at temperatures lower than metal vapor. The metal from the first condenser may require refining, depending on the impurity content. As described below, the condenser is controlled at approximately 400°C. At this temperature, impurities may not settle on the heated surfaces; instead, they are more likely to travel into impurity collection units, such as water-cooled waste tanks.

[0023] The metal refining unit can be configured as a vacuum distillation tank arrangement, wherein a metal-containing feedstock is vaporized and flows through a cooler vapor collection conduit or pipe, wherein the metal vapor is condensed into solid metal on a condenser located therein or in fluid communication with it. In these embodiments, the metal refining unit includes at least one vapor collection conduit that fluidly communicates the internal space with a corresponding condenser. Each of the condensers can be located within or in fluid communication with the vapor collection conduit. When the internal space is divided into two or more heating spaces, each heating space can have a vapor collection conduit fluidly connected to a corresponding condenser. For example, in the presence of two heating spaces, each of the first and second heating spaces has a vapor collection conduit fluidly connected to a corresponding condenser. Each vapor collection conduit can have any suitable configuration. For example, each vapor collection conduit can contain a pipe.

[0024] Corresponding vapor collection conduits can be positioned to selectively collect different vapor components generated within the metal refining unit. In an embodiment, a first heating space can be connected to a first condenser using a first vapor collection conduit positioned to collect vapor from a container moving through the metal refining unit, in which the raw material is heated to 200°C to 1150°C, preferably 700°C to 1150°C, more preferably 800°C to 1100°C. Similarly, a second heating space can be connected to a second condenser using a second vapor collection conduit positioned to collect vapor from a container moving through the metal refining unit, in which the raw material is heated to 1100°C to 1300°C, preferably greater than 1150°C, more preferably at least 1200°C.

[0025] The metal refining unit may have a heating shell or may be located within a heating shell. The heating shell may comprise any suitable high-temperature enclosure, such as a furnace or similar vessel. In some embodiments, the heating shell may be configured to create at least two distinct heating zones within the internal space of the metal refining unit. These distinct heating zones may have different temperatures, as discussed above for the first and second heating spaces. These distinct heating zones (and therefore temperature zones) allow for differentiated extraction of different portions of the metal-containing feedstock. For example, one heating zone may be used to preferentially remove impurities, while the second heating zone may be used to extract selected metals as metal vapor, thereby producing high-purity metal vapor, which can be refined at high purity on a corresponding condenser. An example of high-purity metal is greater than 99% purity, more specifically greater than 99.5% purity, and more specifically greater than 99.7% purity. As mentioned above, the heating zones can be created by gradually heating the feedstock from the feed temperature (typically below 100°C) to the temperature within the heating zone, and the gradual heating profile is used to distinguish the different heating zones. The movement of the metal-containing raw material through the internal space of the metal refining unit and its heating zones allows the raw material to gradually move through the first heating space and into the second heating space, while simultaneously heating it progressively. Alternatively, each heating zone (e.g., the first and second heating spaces) can have different or separate heat sources, which can be controlled to produce different temperatures within the different heating zones.

[0026] The vapor collection conduit may be cooler than the internal space within the metal refining unit to allow the vapor to cool before condensation. In some embodiments, the vapor collection conduit may extend outside the heating zone of the metal refining unit and include at least one heating unit for heating the material therein. For example, the material in the vapor collection conduit may be kept above 900°C by using an additional heat source, such as an electric / ceramic pipe heater.

[0027] The metal-containing raw material can comprise any suitable raw material that can be deposited onto a movable container. For example, the metal-containing raw material can comprise granular material or briquettes. In embodiments, the granular raw material can comprise any suitable particulate material, such as powder, pellets, fine particles, beads, pills, etc. Therefore, the granular raw material at 25°C can comprise powdered or pelleted raw material. In some embodiments, the granular raw material at 25°C (i.e., at or near ambient temperature) can comprise a mixed powder.

[0028] Selected metals extracted from metallic raw materials may include a variety of target metals. Examples of selected metals include at least one of the following: lithium, calcium, magnesium, titanium, silicon, or rare earth metals.

[0029] In some embodiments, the metal-containing feedstock may include metals containing impurities that need to be refined to increase their purity. For example, the metal-containing feedstock may contain magnesium with a purity of less than 95 wt%, and it is desirable to refine the magnesium to a purity greater than 99 wt%, such as greater than 99.5%, and more specifically greater than 99.7%. Other metals that can benefit from purification by distillation may include titanium, calcium, and silicon.

[0030] In some embodiments, the metal-containing raw material may comprise a metal precursor material, which can be thermally reduced to form the desired metal. The metal precursor may comprise any suitable metal salt or compound. For example, the metal precursor may comprise a metal oxide. One example is magnesium production, where the metal precursor may comprise magnesium oxide.

[0031] A first embodiment may provide a thermal reduction apparatus for producing magnesium in certain forms or embodiments. Here, the raw material may comprise a magnesium oxide-rich mixture mixed with a reducing agent, and the metallic product primarily comprises magnesium. Any suitable reducing agent can be used; for example, the reducing agent may comprise aluminum, carbon, or at least one silicon, such as ferrosilicon. In some instances, calcium fluoride may be added as a catalyst for reduction. Similarly, the composition of the MgO-rich mixture may comprise any suitable MgO-containing mixture, and the composition generally depends on the source material used to produce MgO. In some embodiments, the MgO mixture may be formed from calcined dolomite. Dolomite typically contains 60% calcium carbonate and 40% magnesium carbonate, as well as trace impurities Na, K, and Cl. These trace impurities remain in the MgO-rich mixture and are preferably removed during the process to collect pure Mg metallic product. In other embodiments, the MgO-rich mixture may be derived from other sources (mined magnesite (MgCO3), or magnesium chloride hydrolyzed into hydroxide), and may also include these and other impurities, which are preferably removed during the Mg production process. In magnesium production, the residue formed after separating metallic magnesium from the metal-containing raw material can have a Portland cement-type composition. In this respect, the chemical composition of the MgO-rich mixture, particularly when derived from dolomite, can be supplemented with calcium-containing materials (such as lime (CaO)) to generate a residue composed of Portland cement. Therefore, the residue (typically comprising about 80% of the mass of the metal-containing raw material) can provide secondary commercial products derived from said raw material.

[0032] The feeding unit can comprise any suitable particulate feeding arrangement for dispensing metal-containing raw materials. In embodiments where the metal-containing raw material comprises particulate materials such as powder or pellets, the feeding unit can include a feed hopper configured to feed the metal-containing raw material into at least one movable hopper. The feed hopper preferably has a low-pressure atmosphere maintained by an atmosphere control unit. Therefore, the feed hopper can also be part of or within the atmosphere-controlled chamber. The flow rate of the metal-containing raw material dispensed from the feed hopper can be controlled using various powder feeding arrangements. For example, various valves, trough feeding arrangements, etc., can be used. In some embodiments, the feed hopper includes a screw feeder for controlling the flow rate of the raw material on at least one movable hopper. The screw feeder can be driven by a variable-speed motor to control the flow rate / feed speed. After the metal-containing raw material is dispensed into the container, the material can optionally be uniformly distributed using a rake, plate comb, etc., to achieve a uniform thickness.

[0033] The movable cassette can have any suitable form to facilitate the movement of the metal-containing raw material through the metal refining unit. The at least one movable cassette may comprise at least one concave body, such as a receiving element, and preferably a shallow-walled receiving element, such as a tray. The receiving element may include a walled cavity configured to receive the metal-containing raw material therein. For continuous metal production, multiple movable cassettes are typically required, onto which the metal-containing raw material can be continuously fed and then moved into and through the metal refining unit. Here, the at least one movable cassette may comprise at least one of the following driven by a drive unit: a series of individual trays, a connected tray chain, a continuous chain or belt including recesses (e.g., tray recesses), or a screw conveyor or screw feeder. This chain / belt of trays or recesses can circulate through the metal refining unit and return to the feeding unit to be refilled with the metal-containing raw material.

[0034] The at least one movable container can be formed from any suitable high-temperature metal or alloy, or ceramic, preferably a Ni / Cr or austenitic steel with a chromium content of at least 18%. Of course, the choice of material needs to be adapted to the temperature required to generate metal vapor within the metal refining unit. However, in several embodiments, the at least one movable container can be constructed from a high-temperature metal or ceramic. In some embodiments, the at least one movable container is formed from a Ni / Cr alloy.

[0035] Depending on the configuration of the at least one movable cassette, the drive unit can take many different forms. For example, the drive unit may include a motor configured to drive the rotation of a screw conveyor or screw feeder, drive wheel, or conveyor belt. In some forms, the drive unit may include at least one drive wheel configured to drive the at least one movable cassette to move through the feeding unit and the metal refining unit. When the at least one movable cassette comprises a series of individual trays or a chain of connected trays, the drive unit may include a drive unit that engages the trays and pushes the trays through the feeding unit and the metal refining unit. The drive wheel may include at least one rib, plate, or blade configured to contact and drive the at least one movable cassette. More specifically, the drive wheel may include at least two blades configured to hold at least one movable cassette therebetween. The drive wheel can be configured to rotate to push each movable cassette along a surface through the feeding unit and the metal refining unit. Alternatively, in cases where the continuous chain or belt includes recesses (such as tray recesses), the continuous chain or belt is driven by the drive wheel. The speed of the drive wheel can be adjusted using a variable frequency drive. The rotational speed of the drive wheel determines the residence time of the material within the metal refining unit. For example, the drive unit can be configured to move at least one movable cassette through the metal refining unit at a speed of 0.5 m / h to 2 m / h, preferably 0.8 m / h to 1.5 m / h, more preferably about 1 m / h. It should be understood that the drive unit is typically located outside the heating zone of the thermal reduction equipment, for example, in the cold zone where the temperature of the equipment is less than 100°C.

[0036] The feeding unit and the metal refining unit may include at least one air inlet to generate an airflow through the respective unit, and at least one air inlet in the metal refining unit is located upstream of the internal space. This air inlet may be located upstream of the heated internal space of the reduction unit to create an airflow in the direction of movement of the feedstock through the metal refining unit, thereby helping to retain the metal vapor in the hot zone of the metal refining unit. However, other suitable locations may be used depending on the overall equipment and atmosphere-controlled chamber configuration. Any metal vapor outside the metal refining unit is treated as metal on the cooler parts of the equipment.

[0037] The temperature of the condenser itself is below, typically well below, the melting point of the metal to be condensed. This temperature can be controlled to ensure preferential extraction of metal from the vapor generated from the feedstock. For example, the condenser can be controlled at a temperature of at least 300°C, preferably 300°C to 600°C, more preferably about 400°C. At this temperature, impurities are less likely to deposit on the heated surfaces of the condenser; instead, they travel into a fluid-communication impurity collection unit, such as a water-cooled waste container. Each condenser may include a scraper arrangement configured to remove, preferably break off, metal deposits formed on the condenser. In an embodiment, the metal deposits are removed using a scraper unit attached to a pneumatic push rod with a flexible metal seal. The removed metal deposits fall into a collection tank with a valve interlock for online collection.

[0038] The use of residue collection units further facilitates continuous metal production by enabling the continuous collection of product metals and the disposal of any residues. In this regard, the apparatus may further include at least one metal collection unit located near the at least one condenser for collecting metal deposits removed from each collector. The metal collection unit may include a metal collection box. The metal collection unit may be located within a low-pressure atmosphere in an atmosphere-controlled chamber. Similarly, the apparatus may further include at least one residue collection unit located after the metal refining unit for collecting the raw material remaining in the at least one movable container, as well as any other residual material after leaving the metal refining unit. For example, for the production of magnesium by thermal reduction of magnesium oxide, the goal is to keep the amount of Mg in the residue less than 4%. If the Mg content is higher than 4%, the residence time in the metal refining unit can be reduced to achieve higher conversion, for example, by slowing down the travel speed of the movable container through the metal refining unit. The residue collection unit may include at least one vessel or container comprising a collection space therein for residual material and remaining raw material. The residue collection unit can be maintained in a low-pressure atmosphere within an atmosphere-controlled chamber.

[0039] The device and its units can be made of any suitable material. In an embodiment, the metal refining unit is formed of a high-temperature material, such as a high-temperature metal or alloy, a refractory-lined container, ceramic, or a combination thereof. For example, the metal refining unit can be constructed of Ni / Cr. The metal refining unit can be constructed of Ni / Cr 150NB tubes with a wall thickness of 40 or 80 and reinforcing rings to help resist collapse under extreme high vacuum and high temperature conditions. The length of the tube can be 2.5 to 5 meters and can be inclined at an angle of 5 to 20°, for example, inclined downwards at a 14° angle, to assist in the movement of the tray through the metal refining unit.

[0040] Advantageously, the high-temperature zone within the metal refining unit has no moving parts other than a movable hopper that progressively moves the raw material through a first space and then through a second space of the metal refining unit. Material can be fed into the unit via a hopper and discharged from the condenser and residue section. Furthermore, loading the raw material into at least one movable hopper can be performed within an atmosphere-controlled section of the system / equipment. The operator only needs to fill the hopper and replace the residue and metal collection boxes. The raw material moving through the hot zone of the metal refining unit is unlikely to be disturbed.

[0041] The second embodiment provides a method for extracting selected metals from metal-containing raw materials, the method comprising: Feed the metal-containing raw material into at least one movable material box; The metal-containing raw material is moved into and through the metal refining unit using the at least one movable container. The selected metal is separated from the metal-containing raw material in the form of metal vapor under low-pressure conditions in the metal refining unit; and The metal vapor is cooled and condensed into a solid product. The feeding, moving, and separating steps are performed in an atmosphere-controlled chamber or multiple atmosphere-controlled chambers in fluid communication.

[0042] This second embodiment relates to a continuous method for refining selected metals from a metallic feedstock. Similar to the first embodiment, the feeding, moving, and separating steps can be performed in an atmosphere-controlled chamber or a fluidly connected atmosphere-controlled chamber. In this respect, the atmosphere-controlled environment can be used to ensure that the temperature and environment throughout the entire apparatus remain substantially constant. Furthermore, enclosing key process units (feed unit, metal refining unit, and at least one condenser) within a controlled atmosphere facilitates good process control of the thermal reduction process and controls the intrusion of impurities that might otherwise enter the apparatus / system. It should also be understood that "low pressure" and "low-pressure conditions" refer to a pressure less than atmospheric pressure (i.e., less than approximately 100 kPa absolute pressure (equivalent to 1 bar)). This low pressure can be generated by a powerful vacuum pump, which can be used to reduce the pressure to less than 100 Pa. For example, the low pressure can come from an absolute pressure of less than 50 Pa, preferably 5 Pa to 50 Pa, more preferably 20 Pa to 40 Pa, and still more preferably 25 Pa to 35 Pa. In some embodiments, the metal extraction process can be kept in optimal condition by maintaining the pressure below 40 Pa.

[0043] The metal refining process can be facilitated by moving the at least one movable container through a feeding step, a thermal reduction step, and then back to its original position to receive additional metal-containing raw materials. This allows the metal-containing raw materials to be continuously fed through the system for the separation and refining of selected metals.

[0044] In the separation step, metal vapor is generated within the metal refining unit. The metal vapor can be generated by the boiling point difference between a selected metal and other components of the metal-containing raw material, or it can be generated as a result of a reaction (e.g., a reduction reaction – such as a thermal reduction reaction). Therefore, the process can include one or more of the following: thermal separation process, metal distillation process, reduction process, thermal reduction process, etc.

[0045] In some forms, this second embodiment may include a thermal reduction process capable of continuously producing a metal such as magnesium from a metal-containing feedstock (e.g., a feedstock containing magnesium oxide). In these forms, the separation step includes thermally reducing the metal-containing feedstock under low-pressure conditions in the metal refining unit to produce metal vapor containing the selected metal. Alternatively, this second embodiment may include a distillation process capable of continuously separating a selected metal, such as magnesium or lithium, from the metal-containing feedstock based on the boiling point differences of its components. In these forms, the separation step includes separating the selected metal from the metal-containing feedstock based on its boiling point to produce the metal vapor.

[0046] Separating a selected metal from a metal-containing feedstock typically involves heating the metal-containing material to a selected temperature. The process may include heating the metal-containing material to a selected temperature, or it may include two or more different temperatures. These different temperatures allow for differentiated extraction of different portions of the metal-containing feedstock. For example, one temperature may be used to preferentially remove impurities, and a second temperature may be used to extract the selected metal as metal vapor, thereby producing high-purity metal vapor, which can be refined at high purity on a corresponding condenser. An example of a high-purity metal is greater than 99% purity, more specifically greater than 99.5% purity, and more specifically greater than 99.7% purity. In this regard, the separation of the selected metal as metal vapor from the metal-containing feedstock can be carried out in a single stage or in two or more stages within the metal refining unit. In embodiments, the selected metal can be separated from the metal-containing feedstock in at least two stages, the at least two stages comprising at least two different temperatures. For example, the metal-containing feedstock can be heated in at least two stages within the metal refining unit, comprising: The metal-containing raw material is heated to 200°C to 1150°C, preferably 700°C to 1150°C, more preferably 800°C to 1100°C, to generate a first vapor, the first vapor mainly containing any impurities in the raw material, and the first vapor is cooled and condensed into a first solid product; and The metal-containing raw material is heated to 1100°C to 1300°C, preferably greater than 1150°C, more preferably at least 1200°C, to generate a second vapor, the second vapor mainly containing metal vapor, and the first vapor is cooled and condensed into a second solid product.

[0047] The metal-containing raw material can comprise any suitable raw material that can be deposited onto a movable container. For example, the metal-containing raw material can comprise granular material or briquettes. In embodiments, the granular raw material can comprise any suitable particulate material, such as powder, pellets, fine particles, beads, pills, etc. Therefore, the granular raw material at 25°C can comprise powdered or pelleted raw material. In some embodiments, the granular raw material at 25°C (i.e., at or near ambient temperature) can comprise a mixed powder.

[0048] Selected metals extracted from metallic raw materials may include a variety of target metals. Examples of selected metals include at least one of the following: lithium, calcium, magnesium, titanium, silicon, or rare earth metals.

[0049] In some embodiments, the metal-containing feedstock may include metals containing impurities that need to be refined to improve their purity. For example, the metal-containing feedstock may contain magnesium with a purity of less than 95 wt%, and it is desirable to refine the magnesium to a purity greater than 99 wt%. Other metals that can benefit from purification by distillation may include titanium, calcium, and silicon.

[0050] In some embodiments, the metal-containing raw material may comprise a metal precursor material, which can be thermally reduced to form the desired metal. The metal precursor may comprise any suitable metal salt or compound. For example, the metal precursor may comprise a metal oxide. One example is magnesium production, where the metal precursor may comprise magnesium oxide.

[0051] Specific embodiments provide a thermal reduction apparatus for producing magnesium. Here, the feedstock may comprise a magnesium oxide-rich mixture mixed with a reducing agent, and the metallic product primarily comprises magnesium. Any suitable reducing agent can be used; for example, the reducing agent may comprise aluminum, carbon, or at least one silicon, such as ferrosilicon. In some instances, calcium fluoride may be added as a catalyst for reduction. Similarly, the composition of the MgO-rich mixture may comprise any suitable MgO-containing mixture, and the composition typically depends on the source material used to produce MgO. In embodiments, the MgO mixture may be formed from calcined dolomite. Dolomite typically contains 60% calcium carbonate and 40% magnesium carbonate, as well as trace impurities Na, K, and Cl. These trace impurities remain in the MgO-rich mixture and are preferably removed during the process to collect a pure Mg metallic product. In other embodiments, the MgO-rich mixture may be derived from other sources (mined magnesite (MgCO3), or magnesium chloride hydrolyzed into hydroxide), and may also include these and other impurities, which are preferably removed during the Mg production process.

[0052] The movable cassette can have any suitable form to facilitate the movement of the metal-containing raw material through the metal refining unit. The at least one movable cassette may comprise at least one concave body, such as a receiving element, and preferably a shallow-walled receiving element, such as a tray. The receiving element may include a walled cavity configured to receive the metal-containing raw material therein. For continuous metal production, multiple movable cassettes are typically required, onto which the metal-containing raw material can be continuously fed and then moved into and through the metal refining unit. Here, the at least one movable cassette may comprise at least one of the following driven by a drive unit: a series of individual trays, a connected tray chain, a continuous chain or belt including recesses (e.g., tray recesses), or a screw conveyor or screw feeder. This chain / belt of trays or recesses can circulate through the metal refining unit and return to the feeding unit to be refilled with the metal-containing raw material. Moving the at least one movable container may involve operating at least one drive wheel operatively connected to the at least one movable container to push, pull, or otherwise translate the at least one movable container through the metal refining unit. The at least one movable container can move through the metal refining unit at any suitable speed to achieve the desired conversion and metal production. In an embodiment, the at least one movable container moves through the metal refining unit at a speed of 0.5 m / h to 2 m / h, preferably 0.8 m / h to 1.5 m / h, more preferably about 1 m / h.

[0053] The cooling and condensation steps are preferably performed at a temperature of at least 300°C, preferably 300°C to 600°C, and more preferably about 400°C. As described with respect to the first embodiment, at this temperature, impurities are unlikely to deposit on the heated surface; instead, the impurities travel into the impurity collection unit, such as a water-cooled waste container.

[0054] The method may further include the step of collecting solids generated by the cooling and condensation steps in at least one metal collection unit located near the at least one condenser. The metal collection unit may include a metal collection box. The metal collection unit may be located within a low-pressure atmosphere maintained in the atmosphere-controlled chamber. The method may further include the step of collecting residual raw materials discharged from the reduction unit in at least one residue collection unit.

[0055] The third embodiment provides a metal produced using the method according to the second embodiment. In this embodiment, the metal produced by this method may contain magnesium. It should be understood that the features described above with respect to the first and second embodiments are also applicable to this third embodiment.

[0056] The fourth embodiment provides the method of the second embodiment, which can be implemented using the metal refining equipment according to the first embodiment. It should be understood that the features described above with respect to the first and second embodiments are also applicable to this fourth embodiment. Attached Figure Description

[0057] The invention will now be described with reference to the accompanying drawings, which illustrate specific examples, wherein: Figure 1 A process flow diagram of an example metal refining method according to the present invention is provided.

[0058] Figure 2 A schematic diagram is provided illustrating a first example of an apparatus and continuous process configured to produce magnesium using the Pidgeon process according to the present invention.

[0059] Figure 3 Provided shows that it can be used Figure 2 The diagram shows an example of a condenser and metal collection system in a continuous process. Detailed Implementation

[0060] An apparatus and method are disclosed that allow for the continuous extraction of metals from metal-containing feedstocks. Specifically, the apparatus and method are configured as a high-temperature and low-pressure (near-vacuum) metal refining process. In this sense, the disclosed apparatus and method can be configured to produce various metals using a thermal reduction route, or to purify or refine selected metals via a metal distillation process.

[0061] Figure 1 An example of an overall process flow diagram of a process system according to this disclosure is provided. The process following this process flow diagram is as follows: (A) Metal-containing raw material 16 is fed into or otherwise loaded into a feeding unit 10, which is configured to feed the metal-containing raw material 16 into a movable hopper (not shown) for conveying the raw material through a subsequent metal refining unit 30. As previously mentioned, the feeding unit may include various feeding configurations depending on the nature of the metal-containing raw material. Similarly, the movable hopper may take many forms, such as one or more pallets, conveyor belts, screw conveyors, or screw feeders as previously described. The metal-containing raw material 16 is conveyed from the feeding unit 10 to the metal refining unit 30. The movement of the movable hopper is driven by a drive unit (not shown). Specific embodiments of the drive unit will be described in more detail below.

[0062] (B) The metal refining unit 30 is connected to the feed unit 110 and typically includes a heated vacuum distillation vessel arrangement in which a selected metal is separated from the metal-containing feedstock 16. This separation may be the result of a thermal reduction reaction or alternatively as part of a metal distillation process (see below). Figure 2 and Figure 3 (The example device shown is described in more detail). The metal refining unit 30 includes a heat source, such as a furnace or similar device, which heats the internal space therein. The internal space is under low pressure (near vacuum) to promote the generation of vapor.

[0063] (C) At least one condenser 40 is in fluid communication with the internal space of the metal refining unit 30 and condenses the metal vapor from the internal space to form a metal product thereon. Metal 44 is extracted as a product from the process. Impurities 43 or other substances precipitated from the metal-containing raw material 16 in the internal space of the metal refining unit 30 can also be captured and / or refined by one or more condensers 40.

[0064] (D) After the selected metal is separated from the metal-containing raw material 16, the remaining residue is removed (or otherwise removed) from the movable hopper in the residue collection unit 69. The movable hopper is then returned to the feed unit 10 via the movable hopper return arrangement 68 to receive the metal-containing raw material 16 ready to enter the metal refining unit 30.

[0065] As shown by the dashed boxes enclosing each process unit, the feed unit, metal refining unit, condenser 40, drive unit, and residue collection section are all housed within an atmosphere-controlled chamber 74. The atmosphere-controlled chamber 74 is sealed within a low-pressure atmosphere generated by a vacuum pump (described in detail below), thereby ensuring a controlled low-pressure atmosphere in those critical units of this process and equipment.

[0066] Available for Figure 1 The specific selection of equipment in the process shown depends on the feed composition and the conditions used to extract the selected metal from the metal-containing raw material within the metal refining unit 30.

[0067] Figure 1 An example application of the process shown is a thermal reduction process, such as the Pidgeon process for producing magnesium. It should be understood that the Pidgeon process typically involves two steps: Step 1: MgO Production Magnesium oxide can be obtained by hydrolyzing magnesium chloride in seawater or lake water to form hydroxide. In most cases, the magnesium feedstock is calcined to produce magnesium oxide-rich precursor materials. For example, in the calcination of dolomite—which typically contains about 60% calcium carbonate and about 40% magnesium: Another option is to use mined magnesite (MgCO3) and calcine it into magnesium oxide by removing carbon dioxide.

[0068] Step 2: Vacuum thermal reduction: The magnesium oxide-rich precursor material is then thermally reduced under vacuum (low pressure conditions) to produce magnesium vapor, which is then condensed into a metal. While various reducing agents can be used, ferrosilicon mixtures are most commonly used due to their lower cost and greater availability compared to silicon. Iron from the alloy is a byproduct of the reaction. The Pidgeon process is an endothermic reaction (ΔH° is approximately 183.0 kJ / mol Si). By conducting the reaction at lower pressures, the reaction is placed in a more favorable thermodynamic position (i.e., lower temperature / energy requirements), thus vacuum reduction is used in magnesium production.

[0069] This system provides a thermal reduction apparatus for the second step of the process, in which a magnesium oxide-rich precursor material is thermally reduced under vacuum (low pressure conditions) to produce magnesium vapor, which is then condensed into a metal.

[0070] Figure 2 A schematic diagram is provided illustrating a first example of a novel continuous system for refining metals from a metal-bearing support material. In this particular example, the apparatus is configured for the thermal reduction of magnesium using the Pidgeon process (as described above). However, it should be understood that this apparatus can also be configured for other metal refining / separation / refining processes, such as metal distillation, which will be described below.

[0071] Figure 2 The main parts of this example of a thermal reduction apparatus 100 are shown. The illustrated thermal reduction apparatus 100 is formed within a vacuum chamber 104 (also referred to as an atmosphere-controlled chamber), which includes a cylindrical vacuum body 105 forming a main atmosphere-controlled chamber housing the feed unit and metal refining unit of the apparatus 100. The vacuum chamber 104 includes a sealable access / pressure-bearing door 107, allowing access to the interior outside of operation. The access door 107 is sealed during operation. As described below, the vacuum chamber 104 includes multiple peripheral ports through which various other units of the apparatus communicate with the chamber 104.

[0072] Reference Figure 2 The main components of the device are: (A) Feeding unit 110, in the illustrated embodiment, the feeding unit includes a pellet hopper 112 and a spiral conveyor belt 113 configured to feed pellet raw material 116 into one of a series of movable feed trays 120.

[0073] (B) A metal refining unit 130, which is connected to a feed unit 110. The metal refining unit 130 includes a vacuum distillation vessel arrangement in which a thermal reduction reaction of particulate feedstock 116 occurs, producing metal vapors 135, 136. As will be described in more detail below, the metal refining unit 130 includes a divided internal space 135A, which is heated and, under vacuum (low pressure), the thermal reduction reaction takes place within the internal space. The metal refining unit 130 is enclosed within a furnace 133, which is operated to heat the internal space 135A of the metal refining unit 130 to the desired thermal reduction reaction temperature.

[0074] (C) Two condensers 140 and 142 are disposed within vapor collection conduits 150 and 152, which are connected to the internal space 135A of the metal refining unit 130. The condensers are operated to condense metal vapor from the internal space 135A to form a metal product thereon.

[0075] (D) A drive unit 160 for driving a movable feed tray 120 to move through the feed unit 110 and the metal refining unit 130. In the illustrated embodiment, the movement includes sliding the feed tray 120 on a plane of a table 162, which is shared by the bases in the feed unit 110 and the metal refining unit 130.

[0076] (E) Residue collection unit 169, wherein the residue remaining after magnesium is separated from the particulate feed 116 is collected from the movable feed tray 120.

[0077] (F) Atmosphere control system 170, comprising a vacuum chamber 104 (atmosphere-controlled chamber) housing each of the feed unit 110, the feed tray 120, the metal refining unit 130, the condenser 140 or 142, the vapor collection conduit 150 or 152, and the drive unit 160. As described above, the integral vacuum chamber 104 comprises a cylindrical body 105 that houses a portion of the feed unit 110 and the metal refining unit 130, wherein the drive unit 160 and the condensers 140, 142, and a portion of the feed unit 110 communicate with and extend from the cylindrical body 105. The integral vacuum chamber 104 is sealed within a low-pressure atmosphere generated by a vacuum pump (described in more detail below).

[0078] A more detailed description will follow. Figure 2 The components of the device shown: 1. Drive unit 160 The drive unit 160 shown includes a drive wheel 164 located in a drive chamber 161 of a cylindrical body 105 attached to a vacuum chamber 104 in the device. The drive chamber 161 and the drive wheel are located in a cold zone (typically about 40°C) outside the furnace 133 in the loop.

[0079] The drive wheel 164 shown comprises a rotating wheel including a series of circumferentially spaced blade plates, such as steel blade plates, configured with a spacing that allows the feed trays to fit neatly therebetween. The wheel shown includes seven blades. However, it should be understood that any number of blades can be used depending on the size of the feed tray 120 and the size of the device 100. In operation, the drive wheel 164 rotates, thereby pushing the feed trays 120 onto the table 162, whereby the feed trays slide along the table 162 in a row of adjacent feed trays 120 through the feeding unit 110, in which particulate raw materials are dispensed into the feed trays 120 and then through the metal refining unit 130. The front and rear ends of adjacent feed trays 120 are abutted, thus forming a line with the table 162, which is driven (pushed) by the rotation of the drive wheel 164 and the addition of additional feed trays 120 connected thereto. After the feed tray 120 is ejected from the metal refining unit 130, it falls into the chute 166, where it is flipped to dispose of any residual material remaining after leaving the metal refining unit 130. It is then transported back to the drive wheel 164 via a chain-driven tray return mechanism 168, awaiting placement on the table 162, into the tray row, and pushed into the feed unit 110 to receive the next batch of granular raw materials. The feed tray 120 moves through the metal refining unit 130 at a speed of 0.5 m / h to 2 m / h, preferably 0.8 m / h to 1.5 m / h, more preferably about 1 m / h.

[0080] Although not shown, drive wheel 164 can be driven by an external gear drive via a sealed rotary feedthrough arrangement (not shown). The rotational speed of drive wheel 164 can be adjusted using a variable frequency drive (not shown). The rotational speed of drive wheel 164 determines the residence time of the material within metal refining unit 130. The speed can be adjusted to provide the desired product conversion time for the thermal reduction reaction; for example, if the desired conversion is not achieved, the speed can be reduced to increase the residence time within the internal space 135A of the metal refining unit.

[0081] The feed tray 120 may comprise a metal tray having recesses disposed between its four walls. In the illustrated embodiment, the tray is made of a 2 mm thick Ni / Cr alloy and has a width and length of 100 mm × 115 mm and a height of 20 mm. However, it should be understood that these dimensions can be adjusted to suit specific applications, equipment sizes, etc.

[0082] like Figure 2As shown, the feed tray 120 chain can be formed from a series of separate or loosely connected trays. However, it should be understood that the feed tray 120 can also form part of a tray conveyor or other connected tray chain driven by drive wheels 164 as a chain or belt around the system's drive path. Alternatively, a screw conveyor or other helical conveyor belt material conveyor can be used to convey the particulate raw material 116 through the equipment 100, and specifically through the metal refining unit 130.

[0083] 2. Feeding unit 110

[0084] The cylindrical body 105 of the vacuum chamber 104 is roughly divided into a feeding unit area 111 and a metal refining unit 130 by a baffle 138A (described in more detail below).

[0085] Starting with the feeding unit 110 and the feeding unit area 111, the unit 110 includes a pellet hopper 112 and a spiral conveyor belt 113 configured to feed pellet raw material 116 into one of a series of movable feeding trays 120 located in the feeding unit area 111 within the cylindrical body 105.

[0086] The pellet hopper 112 contains any suitable pellet / powder feed hopper that can be maintained at a low pressure under vacuum conditions. This low pressure can be maintained by filling the pellet hopper 112 with argon protective gas / covering gas using a valve interlock system (not shown). An argon inlet 117 (input-type inlet) is used to keep the feed fresh; the added argon passes through the hopper from the vacuum chamber 104 and enters the metal refining unit 130. It should be understood that the atmosphere control system 170 will operate to maintain the low-pressure conditions within the vacuum chamber 104, including balancing any additional pressure that may be introduced into it by the argon inlets 117 and 137.

[0087] The granular raw material 116, at ambient temperature (25°C), can be in any suitable form, such as powder or pellets, and falls from the hopper 116 into the screw feeder 114 with the aid of an intermittent vibrator (not shown). Alternatively, briquettes can be used, fed using a suitable briquetting feeder. The screw of the screw conveyor 114 is driven by an external motor via a sealed rotary feeder arrangement (not shown) and has variable speed and an intermittent timer to prevent raw material bridging. The granular raw material 116 is distributed from the screw feeder 114 through a feed pipe 117, which communicates via a port to the feed unit area 111 and falls into a feed tray 120 positioned below it. The fed granular raw material 116 can optionally be uniformly dispersed using a plate feed comb (not shown) to achieve a uniform thickness before entering the metal refining unit 130.

[0088] Figure 1 The apparatus 100 shown is preferably configured to produce magnesium using the Pidgeon process. However, it should be understood that the apparatus can also be configured for other metal refining processes using thermal reduction processes. In these embodiments, the particulate feedstock 116 comprises a MgO-rich mixture mixed with a reducing agent mixture (e.g., ferrosilicon). As mentioned above, the MgO-rich mixture can be formed from calcined dolomite. Dolomite typically contains 60% calcium carbonate and 40% magnesium carbonate, as well as trace impurities Na, K, and Cl. These trace impurities remain in the MgO-rich mixture and are preferably removed during the process to collect pure Mg metal product. Similarly, MgO-rich mixtures from other sources (mined magnesite (MgCO3) or magnesium chloride hydrolyzed into hydroxide) may also include these and other impurities, which are preferably removed during the Mg production process.

[0089] 3. Metal refining unit 130 (distillation tank section)

[0090] The metal refining unit 130 includes a heated vacuum distillation tank unit. As shown, the metal refining unit 130 includes a cylindrical body 105 located within a furnace 133. The furnace 133 is configured to heat the internal space 135A within the metal refining unit 130 to a high temperature—for example, 1200°C—to produce magnesium.

[0091] As shown in the figure, the internal space 135A within the metal refining unit 130 is divided into two heating spaces: a first heating space 136 and a second heating space 137. These spaces are defined by three spaced-apart baffles 138A, 138B, and 138C. The baffles 138A, 138B, and 138C are spaced apart along the direction in which the feed tray 120 moves through the metal refining unit 130, thus removing vapors emitted at different temperatures as the raw material moves through the first heating space 136 and the second heating space 137 of the metal refining unit 130 for heating. The first baffle 138A and the third baffle 138C are positioned at the beginning and end of the internal space 135A defining the metal refining unit 130, respectively. These baffles 138A and 138C are adjacent to the starting and ending hot zones of the furnace 133. The first baffle 138A separates the metal refining unit 130 within the cylindrical body 105 of the vacuum chamber 104 from the feed unit area 111. An optional second baffle 138B is positioned between the first baffle 138A and the third baffle 138C. The baffles comprise sheets or plates configured to guide vapors generated from heating the feed product within adjacent internal spaces to corresponding fluidly connected condensers 140, 142. Each baffle 138A, 138B, 138C includes a guide configured to space the baffles 138A, 138B, 138C from the feed tray 120, which moves across the platform 162. The guide ensures that the baffles 138A, 138B, 138C do not jam the feed tray as it moves through the metal refining unit 130.

[0092] Each of the first heating space 136 and the second heating space 137 has a vapor collection conduit 150, 152 that fluidly directs fluid through a specific condenser 140, 142. Each vapor collection conduit 150, 152 includes a pipe that is sealed to and extends outward from a cylindrical body 105 of a vacuum chamber 104. The vapor collection conduits 150, 152 include pipes that extend from a body 130A of a metal refining unit 130, outward from the furnace, to a condenser section 140A of the device 100. The illustrated vapor collection conduits 150, 152 comprise two 100 mm nominal diameter (NB) pipe conduits that extend outward from the furnace 133 housing and are maintained at a temperature greater than 900°C using an electric / ceramic pipe heater (not shown).

[0093] A first vapor collection conduit 150 connects to a first heating space 136 and is positioned to collect vapor (heated by furnace 133) from a feed tray 120 entering the metal refining unit, the feed tray being heated to approximately 200°C to 1150°C. Within this temperature range, impurities such as Na, K, Cl, H₂O, and CO₂ are primarily emitted from the heated particulate feedstock 116. A second collection conduit 152 connects to a second heating space 137 and is positioned to collect vapor from a feed tray in which the feedstock has reached its maximum temperature (its initial temperature at feed unit 110 is below 100°C). In the illustrated embodiment, this maximum temperature is greater than 1150°C, for example, approximately 1200°C. At this temperature, Mg metal is primarily released as vapor from the particulate feedstock 116.

[0094] In the illustrated embodiment, the different temperatures in the first heating space 136 and the second heating space 137 can be generated by gradually heating the particulate feed 116 from its feed temperature (typically less than 100°C) to a temperature within the heating zone (approximately 1200°C). The particulate feed 116 moves through the internal space 135A of the metal refining unit 130, causing the metal-containing feed to gradually move through the first heating space 136 into the second heating space 137, while the feed 116 is gradually heated within the aforementioned temperature zones. The speed at which the particulate feed 116 moves through the internal space 135A and the heating rate of the particulate feed 116 can be used to selectively extract impurities and metals as described above. Alternatively, each of the first heating space 136 and the second heating space 137 can have different or separate heat sources, which can be controlled to generate different temperatures within the different heating zones.

[0095] A small argon inlet 137 is included upstream of the third baffle 138C to retain magnesium vapor in the hot zone (i.e., the metal refining unit within furnace 133). Any Mg vapor that comes into contact with the opposite side of the corresponding hot zone of baffles 138A and 138C may deposit as metal on the cooler parts of the equipment. The inventors do not consider this a problem because this metal can help create a smaller gap between the feed tray 120 and the corresponding baffles 138A and 138C, thus requiring less argon purging. Any metal deposits are also likely to be knocked off by movement of the feed tray column.

[0096] When included in the device, the second baffle 138B (intermediate baffle) functions to assist in guiding impurities such as Na, K, Cl, H2O, and CO2 precipitated from the heated particulate feedstock in the first heating space 136 toward the first condenser 140. This facilitates the generation of pure Mg vapor in the second heating space 137. Here, almost all the metal vapor generated in the second heating space 137 (not mixed with the vapor from the first heating space 136) can flow into the second condenser 142, allowing the condenser 142 to collect high-purity Mg metal from the metal vapor generated in the second heating space 137. The Mg metal collected in the second condenser 142 typically does not require refining.

[0097] Impurities within the particulate feedstock 116 are released at a temperature lower than that of Mg metal vapor. Therefore, the amount of Mg metal solidified on the first condenser 140 will be less because the particulate feedstock 116 in the feed tray 120 has not yet reached, or has just reached, the temperature required to form Mg vapor before passing through the second baffle 138B into the second heating space 137. Consequently, the Mg metal from the first condenser 140 may require refining.

[0098] 4. Condenser

[0099] The two condensers 140 and 142 are described in more detail below. Condensers 140 and 142 are controlled to approximately 400°C and are respectively installed inside each of the vapor collection conduits 150 and 152. At this temperature, any impurities released from the particulate feedstock 116 do not deposit on the heated surfaces of condensers 140 and 142, but instead travel through condensers 140 and 142 into an impurity collection unit, which, in the illustrated embodiment, comprises a water-cooled waste tank 145. During operation, Mg vapor travels from the metal refining unit 130 through vapor collection conduits 150 and 152 (typically approximately 800°C) at a temperature of approximately 1200°C and condenses on condensers 140 and 142, controlled to approximately 400°C (see below). The vapor or gas traveling through condensers 140 and 142 typically exits the waste tank 145 at approximately 200°C (see below). Figure 3 ).

[0100] Figure 3 Provided shows that it can be used Figure 2The diagram illustrates an example of a condenser system 140A, comprising a condenser 140 or 142 and a metal collection system, in the device 100 shown. The condenser 140 / 142 shown includes a polished steel truncated cone with a taper of approximately 2 degrees. The truncated cone is hollow and includes a hollow body 174 forming a sealed chamber therein. The sealed chamber includes an air cooling system 176, which includes a cooling air inlet 176A and an air outlet 176B, the inlet and outlet allowing cooling air to flow through the sealed chamber to maintain the temperature of the truncated cone at approximately 400°C. The condenser system 140A also includes a metal scraper system 178, which includes a sliding conduit 179 that periodically (approximately every 30 minutes) drives downward along the truncated cone (relative to the angle of rotation). Figure 3 (As shown in the orientation), to scrape off deposited metal 180, in this example Mg metal, deposited on the outer surface of condenser 140 / 142. The sliding conduit 179 includes a cutout 187 to accommodate the piping / duct of air cooling system 176. The scraped-off metal deposit 181 falls into metal collection unit 182, typically a metal collection tank 182A with valve interlock 183 for online collection by disassembly and / or replacement of metal collection tank 182A.

[0101] As described above, a scraper device is used to scrape away Mg metal deposits from each condenser 140, 142. This scraper device includes a sliding conduit 179 that connects to a hydraulic cylinder 184 with a flexible metal sealing sleeve (not shown). The scraper operates to scrape off the Mg metal crowns formed on the respective condensers 140, 142 and is then configured to retract into a tightly fitting housing 185 to prevent any long-term metal buildup. A metal scraper system 178 is also in high vacuum and is in fluid communication with a vacuum chamber 104. An argon purge 188 is located on top of the metal scraper system 178.

[0102] It should be understood that the distance between the two condensers 140, 142 can be designed to optimize the selectivity of the vapor components condensed on the respective condensers 140, 142. However, this distance is a function of several system parameters, including the composition of the particulate feedstock 116, the design and speed of the drive unit 160, and the design of the metal refining unit. However, it should be understood that placing an intermediate baffle 138B between the vapor collection conduits 150, 152 will have a greater impact on the vapor distribution.

[0103] 5. Vacuum chamber 104

[0104] The atmosphere control system 170 also includes a vacuum pump (not shown) that generates a low-pressure atmosphere within the vacuum chamber 104. In the illustrated arrangement, the vacuum pump is in fluid communication with the vacuum chamber 104 via a water-cooled waste tank 145. However, it should be understood that the vacuum pump can be positioned in any other suitable location in the illustrated device 100. A conventional paper filter is typically placed between the waste tank and the vacuum pump. The vacuum pump can be any suitable low-pressure pump. In the illustrated example, a Roots / claw pump capable of achieving high flow rates and generating a high vacuum is used. During operation, the pressure in the metal refining unit 130 (and thus the vacuum chamber 104) is less than 50 Pa, typically between 25 Pa and 35 Pa absolute. When feeding is stopped, the pressure can be approximately 8 Pa. To maintain optimal conditions for the metal extraction process, the pressure within the metal refining unit 130 is preferably kept below 40 Pa. The atmosphere control system 170 may also include a control unit (not shown) that operates the vacuum pump and Ar inlets 117, 137 to control the atmosphere conditions (pressure, composition, etc.) within the vacuum chamber 104.

[0105] Each unit of the apparatus 100 is completely enclosed within a vacuum chamber 104 operating under a high vacuum (i.e., pressure less than 100 Pa, preferably less than 50 Pa). Any dust present will settle rapidly because there is virtually no atmosphere, or none at all, that would suspend fine particles. It should be noted that dust is an impurity that may mix into the condenser metal crown. Throughout the operation of the apparatus 100, the temperature and environment within the vacuum chamber 104 remain constant. The vacuum chamber 104 is neither opened nor closed during operation. Under these conditions, the metal refining unit 130 is expected to operate for a much longer period, which is an important consideration when using the Pidgeon process.

[0106] Vacuum chamber 104 can have any suitable configuration. In the illustrated embodiment, atmosphere-controlled chamber 104 comprises a vacuum chamber body (cylindrical body 105) divided by baffle 138A into at least a feed unit area 111 and a metal refining unit 130. However, it should be understood that it can also be configured as two or more interconnected vacuum chambers, rather than a single chamber with peripheral communication.

[0107] 5. Residue Collection

[0108] The granular material 116 that does not fall into the feed tray and is scattered on the table 162 should not adversely affect the process. In fact, the scattered granular material can help the feed tray 120 slide along the table 162, and the required driving wheel force is smaller.

[0109] After passing through the metal refining unit 130, some solid residue may remain in the feed tray 120, which will be cooled. The feed tray 120 will be pushed away from the end 163 of the table 162 and into a chute 166, which includes a conduit connecting to the end of the cylindrical body 105 of the vacuum chamber 104. The feed tray 120 will then slide down the chute 166, where it will rapidly change direction and be overturned. The remaining material in the feed tray 120 is poured into the residue collection unit, namely the residue collection tank 169. A valve interlock (not shown) with argon injection is provided to allow for tank 169 to be changed while the equipment 100 is still running. The amount of residual Mg in the residue is preferably less than 4%. If this content is found to be high, the rotational speed of the drive wheel 164 can be reduced to achieve a longer residence time within the metal refining unit 130.

[0110] When producing magnesium from dolomite using the Pidgeon process, the residue formed after separating metallic magnesium from particulate feedstock 116 can primarily contain Portland cement. In this respect, the chemical composition of the MgO-rich mixture, particularly when derived from dolomite, can be supplemented with calcium-containing materials (such as lime), thereby generating a residue composed of Portland cement. Therefore, the residue (typically comprising about 80% of the mass of the metallic feedstock) can provide secondary commercial products derived from said feedstock.

[0111] 6. Feed pallet return

[0112] After the feed tray 120 is emptied, the empty feed tray 120 remains behind the residue collection tank 169 and awaits triggering to initiate the return journey to the drive wheel 164. The orientation of the drive wheel 164 will trigger a mechatronic switch at a precise moment, which in turn activates a gear drive to initiate the chain-driven tray conveyor 168 or other arrangement. A counterweight roller assembly at the end of the drive wheel 164 ensures that the returning feed tray 120 is securely positioned between the blades 165 of the drive wheel 164. This initiation can be controlled by a gear-driven VFD (not shown). However, it should be understood that alternative return arrangements can also be used.

[0113] Therefore, there are no moving parts or valves in the high-temperature zone within the metal refining unit 130 of the equipment 100; only a tray of raw material slides along the plane of the table 162. Furthermore, the loading and unloading of the feed tray 120 is automated and carried out within a controlled atmosphere within the equipment 100. The operator only needs to fill the feed hopper and replace the residue container 169 and the metal collection container (not shown). The raw material moving through the hot zone of the distillation tank is not disturbed. It is only transferred when it is in a cooler zone of the equipment 100.

[0114] 7. Structural Materials

[0115] The illustrated device 100 is configured as a vacuum chamber 104 formed by a cylindrical tube constructed of Ni / Cr 150NB tubing with a wall thickness of 40 or 80 and reinforcing rings to help resist collapse under extreme high vacuum and high temperature conditions. The illustrated tube is 2.5 meters long. However, it should be understood that any suitable length can be used depending on the size and configuration of the device. In some embodiments, the metal refining unit 130 can be up to 5 meters long, thereby achieving higher yields in the same amount of time. However, since the length of the metal refining unit 130 exceeds 2.5 meters, it may need to be tilted downwards at a 14° angle to assist the feed tray 120 in sliding along the table surface 162.

[0116] The feed tray can be constructed from any suitable high-temperature metal, refractory material, or ceramic. However, it should be understood that the strength of a metal tray may decrease significantly at 1200°C, and buckling may occur if the force exerted by the drive wheel 164 along the table 162 on the feed tray 120 is excessive. A ceramic feed tray 120 may be used. However, the thermal coefficient of the metal substrate differs greatly from that of the residue, and this will facilitate the release of particles from the feed tray 120 after a certain degree of cooling.

[0117] Importantly, no air infiltrates the vacuum chamber 104, or more specifically, the metal refining unit 130. Three rotary feeders (not shown) and multiple valve seals (not shown) are provided, positioned away from the heating zone of the furnace 133. These lower temperatures allow for the use of general-purpose silicone and elastomeric seals throughout the device 100, providing excellent sealing over extended periods. Finally, although not shown, cooling of the device 100 outside the furnace is achieved by winding water-cooled copper tubing around pipes on both sides of the furnace 133.

[0118] Figure 1 Another example application of the process illustrated is metal distillation to assist in the purification or refining of metals, such as magnesium. Metal distillation is a thermodynamic process that uses the differences in boiling points of metal alloys to separate different metallic components from each other and from any impurities. In a distillation system, condensing elements can be matched to the different boiling points of the components, allowing these selected metals to be selectively condensed and purified.

[0119] Reference Figure 2 A second example of a novel continuous system for refining metals from a metal-bearing carrier material can also be described. In this particular example, apparatus 100 is configured as a metal distillation apparatus for magnesium refining. It should be understood that the various units of the apparatus are substantially the same as those described above with reference to the first embodiment.

[0120] In this embodiment, the metal refining unit 130 is configured to purify magnesium from impurities in the magnesium-containing feedstock 116 by using the difference in boiling points between the metal therein and any impurities therein.

[0121] In this regard, the internal space 135A within the metal refining unit 130 is further divided into two heating spaces, a first heating space 136 and a second heating space 137, defined therein by three spaced-apart baffles 138A, 138B, and 138C, as described above with respect to the first example. Each of the first heating space 136 and the second heating space 137 has a vapor collection conduit 150, 152 that fluidly directs fluid through specific condensers 140, 142. In this distillation system, the condensers 140, 142 are matched to the different boiling points of the components, thereby enabling the selective condensation and purification of these selected metals. Here, the first heating space 136 is configured to vaporize impurities from the feedstock 116, while the second heating space 137 is configured to vaporize / boil magnesium. Impurities discharged from the heating feedstock 116 within the first heating space 136 are directed to the first condenser 240, causing the second condenser 142 to collect higher purity Mg metal from the metal vapor generated in the second heating space 137, thereby producing higher purity Mg, for example, greater than 99% purity, more specifically greater than 99.5% purity, and more specifically greater than 99.7% purity. Impurities within the feedstock 116 are released at a lower temperature than the Mg metal vapor.

[0122] Finally, it should be understood that, in combination Figures 1 to 3 The processes and equipment shown and described can also be configured to produce magnesium using a distillation process without substantial changes to the equipment and processes.

[0123] Those skilled in the art will understand that the invention described herein is capable of various modifications and variations beyond those specifically described. It should be understood that the invention includes all such modifications and variations falling within its spirit and scope.

[0124] When the terms “comprise”, “comprises”, “comprised” or “comprising” are used in this specification (including the claims), they should be interpreted as indicating the presence of the said feature, integration, step or component, but not excluding the presence of one or more other features, integrations, steps, components or combinations thereof.

Claims

1. A metal refining apparatus for extracting selected metals from metallic raw materials, the apparatus comprising: A feeding unit configured to feed the metal-containing raw material into at least one movable hopper; A metal refining unit connected to the feeding unit, the metal refining unit including an internal space, the internal space being heated, and in the internal space, the selected metal being separated from the metal-containing raw material in the form of metal vapor; At least one condenser is in fluid communication with the internal space of the metal refining unit to condense the metal vapor from the internal space to form a metal product. as well as A drive unit is configured to drive the at least one movable hopper to move through the feeding unit and the metal refining unit. The feeding unit, the metal refining unit, the at least one condenser, and the movable feed box therein are enclosed in an atmosphere-controlled chamber or in multiple atmosphere-controlled chambers in fluid communication.

2. The metal refining apparatus according to claim 1, wherein the at least one movable feed box is configured to return to the feeding unit to receive the next batch of metal-containing raw materials after the at least one movable feed box leaves the metal refining unit.

3. The metal refining apparatus according to claim 2, wherein the drive unit drives the at least one movable hopper to move back to the feeding unit.

4. The metal refining apparatus according to any one of the preceding claims, wherein the drive unit is enclosed within the atmosphere-controlled chamber.

5. The metal refining apparatus according to any one of claims 1 to 4, comprising a thermal reduction apparatus, wherein a thermal reduction reaction of the metal-containing raw material occurs in the metal refining unit, the thermal reduction reaction producing metal vapor.

6. The metal refining apparatus according to any one of claims 1 to 4, comprising a distillation apparatus, wherein in the metal refining unit, the metal is separated from the metal-containing raw material based on the boiling point of the selected metal to generate the metal vapor.

7. The metal refining apparatus according to any one of the preceding claims, wherein the internal space of the metal refining unit is sequentially divided into at least two heating spaces in the direction of movement of the raw material through the metal refining unit, and each heating space is connected to a separate condenser.

8. The metal refining apparatus according to claim 7, wherein the at least two heating spaces comprise at least a first heating space and a second heating space. Furthermore, the first condenser is in fluid communication with the first heating space of the metal refining unit to condense the first metal vapor from the first heating space; Furthermore, the second condenser is in fluid communication with the second heating space of the metal refining unit to condense the second metal vapor from the second heating space.

9. The metal refining apparatus according to claim 7 or 8, wherein the first heating space is configured to heat the raw material to a temperature at which impurities from the raw material are sufficiently vaporized, and the second heating space is configured to heat the raw material to a temperature at which metals in the raw material are sufficiently vaporized.

10. The metal refining apparatus according to any one of claims 7 to 9, wherein both the first heating space and the second heating space are provided with a steam collection pipe, the steam collection pipe being in fluid communication with a corresponding condenser.

11. The metal refining equipment according to any one of claims 7 to 10, The first heating space is configured to enclose the metal-containing raw material therein and heat the metal-containing raw material to 200°C to 1150°C, preferably 700°C to 1150°C, more preferably 800°C to 1100°C. Furthermore, the second heating space is configured to enclose the metal-containing raw material therein and heat the metal-containing raw material to 1100°C to 1300°C, preferably greater than 1150°C, and more preferably at least 1200°C.

12. The metal refining apparatus according to any one of claims 7 to 11, wherein the internal space of the metal refining unit is divided into at least two heating spaces in the direction of movement of the raw material through the metal refining unit by at least one baffle.

13. The metal refining apparatus of claim 12, wherein the at least one baffle comprises a first baffle, a second baffle, and a third baffle, the first baffle and the third baffle being positioned at or near the end of the internal space, and the second baffle being positioned between the first baffle and the third baffle to divide the internal space into a first heating space and a second heating space.

14. The metal refining apparatus according to claim 12 or 13, wherein each baffle comprises a sheet, plate, or membrane.

15. The metal refining apparatus according to claim 12, 13 or 14, wherein each baffle includes a guide portion configured to space the baffle from the at least one movable hopper.

16. The metal refining apparatus according to any one of the preceding claims, wherein the metal refining unit comprises a heating shell or is located within the heating shell.

17. The metal refining apparatus according to any one of the preceding claims, wherein the metal-containing raw material comprises particulate material or briquettes.

18. The metal refining apparatus according to claim 17, wherein the particulate raw material comprises powdered raw material or pellet raw material at 25°C, and preferably a mixed powder at 25°C.

19. The metal refining apparatus according to any one of the preceding claims, wherein the selected metal comprises at least one of the following: lithium, calcium, magnesium, titanium, silicon, or rare earth metals.

20. The metal refining apparatus according to any one of the preceding claims, comprising a thermal reduction apparatus for producing magnesium, wherein the raw material comprises a magnesium oxide-rich mixture mixed with a reducing agent, and the metal product comprises primarily magnesium.

21. The metal refining apparatus according to claim 20, wherein the reducing agent comprises aluminum, carbon, or at least one silicate, preferably ferrosilicon.

22. The metal refining apparatus according to any one of the preceding claims, wherein the feeding unit comprises a feeding hopper configured to feed the metal-containing raw material onto the at least one movable feed box.

23. The metal refining apparatus according to any one of the preceding claims, wherein the at least one movable hopper comprises at least one concave body, preferably at least one tray.

24. The metal refining apparatus according to any one of the preceding claims, wherein the at least one movable hopper comprises at least one of the following driven by the drive unit: a series of individual trays, a connected tray chain, a continuous chain or belt including recesses, or a screw conveyor or screw feeder.

25. The metal refining apparatus according to any one of the preceding claims, wherein the drive unit comprises at least one drive wheel configured to drive the at least one movable hopper to move through the feeding unit and the metal refining unit.

26. The metal refining apparatus of claim 25, wherein the drive wheel comprises at least one rib, plate, or blade, the at least one rib, plate, or blade being configured to contact the at least one movable container and drive the movement of the at least one movable container.

27. The metal refining apparatus according to any one of the preceding claims, wherein the feeding unit and the metal refining unit include at least one air inlet to generate an airflow through the respective unit, and wherein at least one air inlet in the metal refining unit is located upstream of the internal space.

28. The metal refining apparatus according to any one of the preceding claims, wherein the condenser is controlled at a temperature of at least 300°C, preferably 300°C to 600°C, and more preferably about 400°C.

29. A method for refining selected metals from metal-containing raw materials, the method comprising: Feed the metal-containing raw material into at least one movable material box; The metal-containing raw material is moved into and through the metal refining unit using the at least one movable container. The selected metal is separated from the metal-containing raw material in the form of metal vapor under low-pressure conditions in the metal refining unit; and The metal vapor is cooled and condensed into a solid product. The feeding, moving, and separating steps are performed in an atmosphere-controlled chamber or a fluid-connected atmosphere-controlled chamber.

30. The method of claim 29, further comprising removing the at least one movable container from the metal refining unit and returning it to its original position to receive the next batch of metal-containing raw materials.

31. The method of claim 29 or 30, wherein the separation step comprises thermally reducing the metal-containing raw material in the metal refining unit under low pressure to generate metal vapor containing the selected metal.

32. The method of claim 29 or 30, wherein the separation step comprises separating the selected metal from the metal-containing raw material based on the boiling point of the selected metal to generate the metal vapor.

33. The method according to any one of claims 29 to 32, wherein the low-pressure condition comprises an absolute pressure of less than 50 Pa, preferably 5 Pa to 50 Pa, more preferably 20 Pa to 40 Pa, and still more preferably 25 Pa to 35 Pa.

34. The method according to any one of claims 29 to 33, wherein the selected metal is separated from the metal-containing raw material in at least two stages, the at least two stages comprising at least two different temperatures.

35. The method of claim 34, wherein the at least two stages comprise: The metal-containing raw material is heated to 200°C to 1150°C, preferably 700°C to 1150°C, more preferably 800°C to 1100°C, to generate a first vapor, the first vapor mainly containing any impurities in the raw material, and the first vapor is cooled and condensed into a first solid product; and The metal-containing raw material is heated to 1100°C to 1300°C, preferably greater than 1150°C, more preferably at least 1200°C, to generate a second vapor, the second vapor mainly containing metal vapor, and the first vapor is cooled and condensed into a second solid product.

36. The method according to any one of claims 29 to 35, wherein the metal-containing raw material comprises particulate material or briquettes.

37. The method according to claim 36, wherein the metal-containing raw material comprises a powder or pellet raw material at 25°C, and preferably a mixed powder at 25°C.

38. The method according to any one of claims 29 to 37, wherein the raw material comprises a magnesium oxide-rich mixture mixed with a reducing agent, and the solid product comprises primarily magnesium.

39. The method according to claim 38, wherein the reducing agent comprises aluminum, carbon, or at least one silicate, preferably ferrosilicon.

40. The method according to any one of claims 29 to 39, wherein the at least one movable container comprises at least one of: a series of individual trays, a connected tray chain, a continuous chain or belt including recesses, or a screw conveyor or screw feeder.

41. The method according to any one of claims 29 to 40, wherein moving the at least one movable container comprises operating at least one drive wheel operatively connected to the at least one movable container to push, pull, or otherwise translate the at least one movable container through the metal refining unit.

42. The method according to any one of claims 29 to 41, wherein the at least one movable container moves through the metal refining unit at a speed of 0.5 m / h to 2 m / h, preferably 0.8 m / h to 1.5 m / h, more preferably about 1 m / h.

43. The method according to any one of claims 29 to 42, wherein the cooling and condensation steps are performed at a temperature of at least 300°C, preferably 300°C to 600°C, more preferably about 400°C.

44. A metal produced using the method according to any one of claims 29 to 43, wherein the metal comprises primarily magnesium.

45. The method according to any one of claims 29 to 44, wherein it is carried out using the metal refining equipment according to any one of claims 1 to 28.