Disc for disc brakes and method for manufacturing discs for disc brakes
By using a nickel-free or low-nickel steel base layer and intermediate layer on the brake disc, combined with laser metal deposition technology, the problems of nickel particle release and easy peeling of traditional coatings have been solved, resulting in a high-performance brake disc.
Patent Information
- Application Number
- CN202480087268.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-29
- Filing Date
- 2024-12-19
- Publication Date
- 2026-11-10
AI Technical Summary
The presence of nickel in existing brake disc materials leads to the release of nickel particles, which can affect health. At the same time, traditional protective coatings are prone to peeling and thermal cracking, and cannot simultaneously guarantee sufficient thermal and mechanical properties.
A base layer and an intermediate layer made of nickel-free or low-nickel steel are used, combined with laser metal deposition technology to form a base layer covering the braking surface. The base layer contains carbides such as TiC and WC, while the intermediate layer is composed of nickel-free or low-nickel steel. A metallurgical bond is formed through laser deposition technology.
It effectively reduces nickel particle release, improves the thermal and mechanical properties of the brake disc, reduces environmental impact, and enhances wear resistance and corrosion resistance.
Smart Images

Figure CN123076735A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to discs for disc brakes and methods for manufacturing discs for disc brakes. Background Technology
[0002] A vehicle's disc brake system comprises a brake disc with a ring-shaped structure or brake band and a central fixing element called a bell, through which the disc is fixed to a rotating part of the vehicle suspension, such as a wheel hub. The brake band has opposing braking surfaces adapted to cooperate with friction elements (brake pads) housed in at least one caliper body arranged to straddle this brake band and be integral with a non-rotating component of the vehicle suspension. The controlled interaction between the opposing brake pads and the opposing braking surfaces of the brake band determines the braking action through friction, allowing the vehicle to decelerate or stop.
[0003] Brake discs are typically made of gray cast iron or steel. In fact, this material allows for good braking performance (especially in limiting wear) at a relatively low cost. Discs made of carbon or carbon ceramic materials offer even greater performance, but at a much higher cost.
[0004] The limitations of traditional brake discs made of cast iron or steel involve excessive wear. Another very negative aspect for discs made of gray cast iron involves excessive surface oxidation, leading to rust formation. This affects both the performance and appearance of the brake disc, as rust on the brake disc is aesthetically unacceptable to the user.
[0005] These problems have been addressed by providing discs made of gray cast iron or steel with a protective coating. The protective coating serves two purposes: reducing disc wear and protecting the gray cast iron base from surface oxidation, thus preventing the formation of rust.
[0006] However, while currently available protective coatings applied to discs offer abrasion resistance, they are prone to peeling, causing the coating to detach from the disc itself. Furthermore, such coatings are susceptible to thermal cracking during use and are also prone to cracking during the application of the protective coating.
[0007] Peeling can promote the release of nickel particles through friction, and nickel is a metal that greatly contributes to allergies in the population.
[0008] However, in the production of steel used for brake discs, the presence of nickel has been considered essential to date because it increases the strength and toughness of the steel. Furthermore, nickel increases the steel's resistance to oxidation and corrosion, but more importantly, it increases the steel's wear resistance and heat resistance—aspects highly relevant to the stresses that brake discs experience during use.
[0009] Therefore, there is a particular need for discs made of gray cast iron or steel that can reduce the release of nickel particles while ensuring sufficient thermal and mechanical properties, including high resistance to disc wear and long-term reliability. Summary of the Invention
[0010] The aforementioned problems are solved by the disc for disc brakes and the method for manufacturing disc brakes as outlined in the appended claims, the definition of which forms part of this specification.
[0011] The first object of the present invention is to provide a disc for a disc brake, the disc comprising a brake band having two opposite braking surfaces, the brake band being made of gray cast iron or steel. The disk includes: A base layer covering at least one of the two braking surfaces of the brake band, wherein the base layer comprises nickel-free steel, or steel containing nickel in a weight percentage not exceeding 15%, 7.5%, or 5%, and includes at least one carbide selected from titanium carbide (TiC), tungsten carbide (WC), chromium carbide, niobium carbide (NbC), molybdenum carbide (Mo2C), and silicon carbide (SiC), and the steel of the base layer (30) includes at least 10% chromium (Cr) by weight; and An intermediate layer is disposed between the base layer and at least one of the two braking surfaces of the brake band, wherein the intermediate layer comprises nickel-free steel, or steel containing no more than 15%, no more than 7.5%, or no more than 5% by weight of nickel.
[0012] A second objective of this invention is to provide a method for manufacturing a brake disc, the method comprising the following steps: a) Provide a brake disc (1) comprising a brake band having two opposite brake surfaces, the brake band being made of gray cast iron or steel; a1) After step a), an intermediate layer is deposited on at least one of the two opposite braking surfaces, the intermediate layer comprising nickel-free steel, or steel containing nickel by weight of no more than 15%, or by weight of no more than 7.5%, or by weight of no more than 5%. b) Following step a1), the particulate composition is deposited onto an intermediate layer of at least one of the braking surfaces using a laser deposition technique selected from LMD (Laser Metal Deposition), HSLMD (High-Speed Laser Metal Deposition), High-Speed Laser Cladding, Ultra-High-Speed Laser Cladding (EHLA), and Extremely High-Speed Cladding, thereby forming a base layer that covers at least one of the two braking surfaces of the brake band. The particulate composition comprises Mx C y -FeCr, and nickel-free steel or steel containing no more than 15%, 7.5%, or 5% nickel by weight, or the particulate composition being made of M x C y -FeCr, and steel that does not contain nickel or steel containing nickel by weight not exceeding 15%, or by weight not exceeding 7.5%, or by weight not exceeding 5%, wherein M is selected from Ti, W, Cr, Nb, Mo, Si, x is an integer selected from 1, 2 and 3, and y is an integer selected from 1 and 2.
[0013] Another object of the present invention is to provide a disc for a disc brake that can be obtained by the above method.
[0014] The target disk of the present invention advantageously allows for a reduction in the release of nickel particles while simultaneously ensuring sufficient or equivalent thermal and mechanical properties.
[0015] To better understand the present invention and appreciate its advantages, some exemplary, rather than limiting, embodiments of the present invention will be described below with reference to the accompanying drawings. Attached Figure Description
[0016] Figure 1 A top plan view of a disc brake according to an embodiment of the present invention is shown.
[0017] Figure 2 The following is shown according to an embodiment of the invention. Figure 1 The section line II-II shown in the figure intercepts the cross-section. Figure 1 A cross-sectional view of the disk.
[0018] Figure 3 A cross-sectional view of half of a brake band according to an embodiment of the present invention is shown.
[0019] Figure 4 A cross-sectional view of half of a brake band according to another embodiment of the present invention is shown.
[0020] Elements or parts of elements common to the embodiments described below will be indicated by the same reference numerals. Detailed Implementation
[0021] In the following description, the phrase "nickel-free steel" means steel that may include up to 0.2% nickel by weight.
[0022] Referring to the above figures, reference numeral 1 generally indicates a disc for a disc brake according to the present invention.
[0023] The disc 1 includes a brake band 2 having two opposing brake surfaces 2a and 2b, each of the two brake surfaces 2a and 2b at least partially defining one of the two main surfaces of the disc.
[0024] Brake band 2 is made of gray cast iron or steel.
[0025] Preferably, the brake band 2 is made of gray cast iron. Preferably, the entire disc 1 is made of gray cast iron. Therefore, in the following description, reference will be made to a disc made of gray cast iron, but the possibility of the disc being made of steel is not excluded.
[0026] The disc 1 is provided with a base layer 30, which covers at least one of the two braking surfaces 2a and 2b of the brake band 2. According to an embodiment, the base layer 30 is in direct contact with the braking surfaces 2a and 2b.
[0027] According to an embodiment of the present invention, the base layer 30 comprises steel having a nickel content of no more than 15%, preferably no more than 7.5%, and more preferably no more than 5%. According to this embodiment, preferably, the steel of the base layer 30 has a nickel content of less than 15%, more preferably less than 7.5%, and even more preferably less than 5%.
[0028] According to another embodiment of the invention, the base layer 30 comprises nickel-free steel.
[0029] This allows for limiting or even preventing the dispersion of nickel particles during the service life of the brake disc 1.
[0030] In both of the above embodiments, the steel of the base layer 30 includes at least 10% chromium (Cr) by weight.
[0031] According to the two embodiments described above, the base layer 30 further includes at least one carbide selected from the following: titanium carbide (TiC), tungsten carbide (WC), chromium carbide (e.g., Cr3C2), niobium carbide (NbC), molybdenum carbide (Mo2C), and silicon carbide (SiC).
[0032] According to an embodiment, the at least one carbide is incorporated into the steel.
[0033] According to an embodiment, the base layer 30 comprises nickel-free steel, or steel containing nickel in a weight percentage not exceeding 15%, 7.5%, or 5%, and the base layer 30 comprises at least one carbide selected from titanium carbide (TiC), tungsten carbide (WC), chromium carbide, niobium carbide (NbC), molybdenum carbide (Mo2C), and silicon carbide (SiC), and the steel of the base layer 30 comprises at least 10% chromium (Cr) by weight.
[0034] It is obvious to those skilled in the art what is meant when referring to the percentage of nickel content or any other component of steel alloy or cast iron. For example, it usually refers to the percentage by mass relative to the total alloy content. Therefore, in the remainder of this disclosure, a particular calculation of a percentage will only be specified if the specific calculation of the percentage deviates from the definition given above; where not specified, the percentages shown should be regarded as understood by those skilled in the art.
[0035] Advantageously, the base layer 30 is formed by a metallurgical bond formed between at least one of the braking surfaces 2a, 2b and a particulate composition deposited on the braking surfaces 2a, 2b by at least one laser beam. The particulate composition includes M... x C y -FeCr, and nickel-free steel or steel containing no more than 15%, 7.5%, or 5% nickel by weight, or the particulate composition is made of M x C y -FeCr, and steel that does not contain nickel or steel containing nickel by weight not exceeding 15%, or by weight not exceeding 7.5%, or by weight not exceeding 5%, wherein M is selected from Ti, W, Cr, Nb, Mo, Si, x is an integer selected from 1, 2 and 3, and y is an integer selected from 1 and 2.
[0036] Further advantageously, the base layer 30 is formed by depositing the above-mentioned particulate composition on at least one of the two braking surfaces 2a and 2b using a laser deposition technology selected from LMD (laser metal deposition), HSLMD (high-speed laser metal deposition), high-speed laser cladding, ultra-high-speed laser cladding (EHLA) and ultra-fast cladding.
[0037] The term "laser cladding" advantageously refers to the formation of a metallurgical bond between a substrate and a layer deposited or welded onto the substrate by means of one or more laser beams.
[0038] Preferably, M x C y -FeCr is a sintered and agglomerated particulate material. Preferably, M x C y -FeCr is in powder form.
[0039] Preferably, M x C y - The weight ratio of FeCr carbides to FeCr is between 20:80 and 80:20, for example, M x C y- The weight ratio of FeCr carbides to FeCr is between 30:70 and 70:30 or between 40:60 and 60:40.
[0040] According to a preferred embodiment, the steel of the base layer 30 comprises at least titanium carbide (TiC). Preferably, the base layer 30 is formed by a metallurgical bond between at least one of the braking surfaces 2a, 2b and a particulate composition deposited on the braking surfaces 2a, 2b by at least one laser beam, wherein the particulate composition comprises TiC-FeCr and nickel-free steel or steel containing nickel in a weight percentage not exceeding 15%, 7.5%, or 5%, or more; or the particulate composition consists of TiC-FeCr and nickel-free steel or steel containing nickel in a weight percentage not exceeding 15%, 7.5%, or 5%, or more.
[0041] The presence of one or more carbides in the base layer 30 can impart sufficient mechanical strength and wear resistance.
[0042] According to an embodiment, the steel of the base layer 30 may include one or more metal oxides and / or ceramic materials. For example, the steel of the base layer 30 may include a mixture of alumina (Al2O3).
[0043] Preferably, the base layer 30 has a thickness between 30 μm and 1500 μm, for example, the base layer 30 has a thickness between 50 μm and 300 μm or between 800 μm and 1200 μm.
[0044] The steel of the base layer 30 includes at least 10% chromium (Cr) by weight, for example, the steel of the base layer 30 includes between 10% and 25% chromium by weight.
[0045] According to an embodiment of the present invention, the steel of the base layer 30 includes at least 15% chromium by weight, for example, the steel of the base layer 30 includes between 15% and 25% by weight, or between 20% and 25% by weight, or between 16% and 18% by weight of chromium.
[0046] Preferably, the steel of the base layer 30 further includes manganese (Mn) in an amount not exceeding 5% by weight. For example, the steel of the base layer 30 includes manganese (Mn) in an amount between 0.5% and 5% by weight, including the extreme values, or includes manganese (Mn) in an amount between 0.5% and 2% by weight, including the extreme values, in order to at least partially compensate for the lack of steel alloy properties usually conferred by the presence of nickel, thereby increasing mechanical strength.
[0047] According to an embodiment, the steel of the base layer 30 comprises at least 55% iron (Fe) by weight. For example, the steel of the base layer 30 comprises at least 65% iron or at least 75% iron by weight. For example, the steel of the base layer 30 comprises iron in an amount between 65% and 85% by weight or in an amount between 75% and 80% by weight.
[0048] According to the embodiment, in order to compensate for low or no nickel content and obtain sufficient performance of the brake disc, the steel of the base layer 30 is composed of 10% to 20% by weight chromium (Cr), up to 1.5% by weight silicon (Si), up to 2% by weight manganese (Mn), up to 0.03% by weight carbon (C), and the remaining percentage of iron (Fe), i.e., the remaining percentage of iron by weight. Preferably, the steel of the base layer 30 is composed of 16% to 18% by weight chromium (Cr), up to 1.5% by weight silicon (Si), up to 2% by weight manganese (Mn), up to 0.03% by weight carbon (C), and the remaining percentage of iron (Fe), i.e., the remaining percentage of iron by weight.
[0049] According to an embodiment of the invention, in order to compensate for low or no nickel content and to obtain sufficient performance of the brake disc, the steel of the base layer 30 contains molybdenum in a weight percentage between 0.5% and 3%, including the extreme values, and manganese in a weight percentage between 0.1% and 5%, including the extreme values. The presence of molybdenum and manganese in the aforementioned percentages enables sufficient corrosion resistance while simultaneously obtaining sufficient mechanical strength.
[0050] According to the embodiment, a nickel-free steel intermediate layer 300 is disposed between the base layer 30 and at least one of the two braking surfaces 2a, 2b of the brake band 2.
[0051] According to an alternative embodiment, an intermediate layer 300 of steel containing no more than 15%, or no more than 7.5%, or no more than 5% nickel is disposed between the base layer 30 and at least one of the two braking surfaces 2a, 2b of the brake band 2. Preferably, if the base layer 30 is nickel-free, the intermediate layer 300 has a nickel content of at least 5% and no more than 15% or less.
[0052] The presence of the intermediate layer 300 allows for a disk with sufficient mechanical properties, while at the same time reducing the environmental impact due to the presence of the base layer 30.
[0053] Preferably, the intermediate layer 300 has a thickness between 30 μm and 1000 μm, for example, the intermediate layer 300 has a thickness between 60 μm and 200 μm.
[0054] According to the embodiment, the auxiliary ferrite nitrocarburizing layer or the auxiliary iron-aluminum layer is disposed between one of the two braking surfaces 2a and 2b of the brake band 2 and the base layer 30, or between one of the two braking surfaces 2a and 2b of the brake band 2 and the intermediate layer 300, or between the intermediate layer 300 and the base layer 30.
[0055] Advantageously, the brake disc is provided with a portion suitable for securing the disc to the vehicle, the portion including an annular portion 4, which is centrally arranged to the disc 1 and concentric with the brake band 2. The securing portion 4 supports the connecting element 5 (i.e., the bell-shaped element) to the wheel hub. The bell-shaped element can be integrally formed with the annular securing portion (as shown in the figures) or can be formed separately and then secured to the securing portion by suitable connecting elements.
[0056] The annular fixing part 4 can be made of the same material as the brake band, i.e., gray cast iron, or of another suitable material. The bell-shaped part 5 can also be made of gray cast iron or other suitable materials. In particular, the entire disc (i.e., the brake band, the fixing part, and the bell-shaped part) can be made of gray cast iron.
[0057] Preferably, the brake band 2 is formed by casting. Similarly, when the fixing part and / or the bell-shaped part is made of gray cast iron, the fixing part and / or the bell-shaped part can be formed by casting.
[0058] The annular fixed portion can be formed as a single body with the brake band (as shown in the attached figure) or it can be formed as a separate body mechanically connected to the brake band.
[0059] As mentioned above, the base layer 30 and the intermediate layer 300 (if present) cover at least one of the two braking surfaces 2a and 2b of the braking band.
[0060] In the following text, the term "coating" will refer to the base layer 30 or the assembly formed by the base layer 30 and the intermediate layer 300.
[0061] Preferably, such as Figure 2 As shown, disc 1 is provided with a coating covering the two braking surfaces 2a and 2b of the brake band 2.
[0062] Specifically, the coating can cover the brake band on a single brake surface or on two brake surfaces.
[0063] According to a technical solution not shown in the accompanying drawings, the coating may also extend to other parts of the disc 1, such as the annular fixing portion 4 and the bell-shaped element 5, until it covers the entire surface of the disc 1. In particular, in addition to covering the brake band, the coating may also cover only the fixing portion or only the bell-shaped element. This choice is essentially determined by aesthetic reasons in order to achieve a uniform color and / or finish across the entire disc or between certain portions of the disc.
[0064] Advantageously, the deposition of particulate material for forming the coating can be carried out on the surface of the disk in a differentiated manner, at least in terms of coating thickness.
[0065] At the brake band, the coating can be formed with the same thickness on two opposite brake surfaces. Alternative solutions are available where the coating is formed with a different thickness between the two brake surfaces of the brake band.
[0066] The brake disc 1 is preferably, but not necessarily, manufactured by the method described below according to the invention.
[0067] According to the first embodiment, the method according to the present invention includes the following steps: a) Provide a brake disc 1, which includes a brake band 2 having two opposite brake surfaces 2a, 2b, which is made of gray cast iron or steel; b) A base layer (30) is formed by depositing a particulate composition on at least one of the braking surfaces 2a and 2b using a laser deposition technique selected from LMD (laser metal deposition), HSLMD (high-speed laser metal deposition), high-speed laser cladding, ultra-high-speed laser cladding (EHLA), and ultra-fast cladding, thereby forming a base layer (30) that covers at least one of the two braking surfaces (2a and 2b) of the brake band (2). The particulate composition comprises M x C y -FeCr, and nickel-free steel or steel containing no more than 15%, 7.5%, or 5% nickel by weight, or the particulate composition being made of M x C y -FeCr, and steel that does not contain nickel or steel containing nickel by weight not exceeding 15%, or by weight not exceeding 7.5%, or by weight not exceeding 5%, wherein M is selected from Ti, W, Cr, Nb, Mo, Si, x is an integer selected from 1, 2 and 3, and y is an integer selected from 1 and 2.
[0068] Depending on the implementation method, M x C y- The carbides in FeCr are selected from titanium carbide (TiC), tungsten carbide (WC), chromium carbide (preferably Cr3C2), niobium carbide (NbC), molybdenum carbide (Mo2C), and silicon carbide (SiC).
[0069] According to a preferred embodiment, the particulate composition comprises TiC-FeCr and nickel-free steel or steel containing nickel in a weight percentage not exceeding 15%, 7.5%, or 5%, or the weight percentage not exceeding 7.5%, or the weight percentage not exceeding 5%, or the particulate composition consists of TiC-FeCr and nickel-free steel or steel containing nickel in a weight percentage not exceeding 15%, 7.5%, or 5%, or the weight percentage not exceeding 5%, or the weight percentage not exceeding 7.5%, or the weight percentage not exceeding 5%.
[0070] Advantageously, step b) of the above method enables the carbide—preferably TiC—to be incorporated into the steel and enables the steel itself to be enriched with Fe and Cr, thereby forming the base layer 30.
[0071] According to the implementation method, M x C y -FeCr particles are dispersed in the matrix of steel particles, preferably, M x C y -FeCr is an agglomerated and / or sintered material.
[0072] According to an embodiment, the particulate composition includes M in a weight percentage between 10% and 40% relative to the weight of the particulate composition. x C y -FeCr, preferably, the particulate composition comprises M at a weight ratio between 15% and 35% relative to the weight of the particulate composition. x C y -FeCr.
[0073] According to the implementation method, M x C y - The weight ratio of FeCr carbides to FeCr is between 20:80 and 80:20, for example, M x C y The weight ratio of FeCr carbides to FeCr is between 30:70 and 70:30 or between 40:60 and 60:40.
[0074] According to an embodiment, step b) is performed using at least one first laser beam having a power between 6 kW and 30 kW, preferably, step b) is performed using at least one first laser beam having a power between 10 kW and 30 kW, preferably, the laser beam is Gaussian type, flat-top type, or flat-top ring type. Advantageously, the first laser beam performs deposition or welding of the particulate composition on at least one of the two braking surfaces 2a, 2b.
[0075] According to an embodiment, the deposition rate of the particulate composition is between 1 m 2 / h and 14 m 2 The deposition rate of the particulate composition is between 1 m / h, for example, between 1 m / h. 2 / h and 8 m 2 Between / h.
[0076] According to the embodiments, the flow rate (powder flow rate) used for depositing the particulate composition is between 20 g / min and 400 g / min.
[0077] According to an embodiment, during step b), prior to using the first laser beam, an additional laser beam is used to pre-treat at least one of the braking surfaces 2a and 2b. This additional laser beam has a power between 1 kW and 15 kW, preferably between 1 kW and 15 kW. Preferably, the additional laser beam is Gaussian, flat-top, or flat-top annular. The pre-treatment may include preheating—for example, to reduce thermal gradients and deformation (thus increasing the window available for changing process parameters and ensuring greater process stability)—and / or cleaning and / or homogenizing of the surface.
[0078] According to an embodiment, during step b), after using the first laser beam, an additional laser beam with a power between 1 kW and 20 kW is used to perform post-processing on at least one braking surface of the braking surfaces 2a and 2b previously deposited with a particulate composition. Preferably, the additional laser beam is Gaussian, flat-top, or flat-top annular. The post-processing may include heating, for example, to reduce thermal gradients and deformation, or to modify microstructural features or reduce fluctuations and roughness.
[0079] According to an embodiment, the first laser beam and the other laser beam have spot sizes on at least one braking surface 2a, 2b, the spot sizes being between 1 mm and 10 mm.
[0080] According to an embodiment, the steel of the particulate composition may include at least one carbide selected from titanium carbide (TiC), tungsten carbide (WC), chromium carbide (e.g., Cr3C2), niobium carbide (NbC), molybdenum carbide (Mo2C), and silicon carbide (SiC). This means that, according to this embodiment, one or more carbides selected from the above-mentioned carbides are included within the steel of the particulate composition. The inclusion of one or more carbides within the steel of the particulate composition is achieved using techniques known to those skilled in the art for including carbides in steel, such as dissolving the carbides in an alloy.
[0081] According to embodiments, the steel in the particulate composition may include one or more metal oxides and / or ceramic materials; for example, the steel in the particulate composition may include a mixture of alumina (Al2O3).
[0082] The use of laser deposition techniques selected from the above-listed laser deposition techniques includes M x C y The use of a particulate composition of FeCr (preferably TiC-FeCr, preferably in the form of agglomerates and sintered) and steel is advantageous in reducing dust emissions during braking, increasing corrosion resistance, reducing the presence of cracks in the base layer 30, reducing the porosity generated during the deposition of the base layer 30, and reducing the generation of cracks during braking.
[0083] According to an embodiment, the method according to the invention further includes step a1), which is performed after step a) and before step b).
[0084] Step a1) includes depositing an intermediate layer 300 on at least one of two opposing braking surfaces 2a, 2b. The intermediate layer 300 comprises nickel-free steel or steel containing nickel at a content not exceeding 15% by weight, or at a content not exceeding 7.5% by weight, or at a content not exceeding 5% by weight. Therefore, according to this embodiment, the base layer 30 is formed on the intermediate layer 300 during step b).
[0085] According to the embodiment, step a1) of depositing the intermediate layer 300 includes: depositing a particulate composition using a laser deposition technology selected from LMD (laser metal deposition), HSLMD (high-speed laser metal deposition), high-speed laser cladding, ultra-high-speed laser cladding (EHLA), and ultra-fast cladding, wherein the particulate composition includes nickel-free steel, or steel containing nickel in a weight of not more than 15%, not more than 7.5%, or not more than 5% by weight.
[0086] According to an embodiment, step a1 is performed using at least one first laser beam having a power between 6 kW and 30 kW, preferably, step a1 is performed using at least one first laser beam having a power between 10 kW and 30 kW, preferably, the laser beam is Gaussian, flat-top, or flat-top ring-shaped. Advantageously, the first laser beam performs deposition of a particulate composition on at least one of the braking surfaces 2a, 2b.
[0087] According to an embodiment, the deposition rate of the particulate composition is between 1 m 2 / h and 14 m 2 The deposition rate of the particulate composition is between 1 m / h, for example, between 1 m / h. 2 / h and 8 m 2 Between / h.
[0088] According to the embodiments, the flow rate (powder flow rate) used for depositing the composition in particulate form is between 20 g / min and 400 g / min.
[0089] According to an embodiment, during step a1), prior to using the first laser beam, an additional laser beam is used to pre-treat at least one of the braking surfaces 2a and 2b. This additional laser beam has a power between 1 kW and 15 kW, preferably between 1 kW and 15 kW. Preferably, the additional laser beam is Gaussian, flat-top, or flat-top annular. The pre-treatment may include preheating—for example, to reduce thermal gradients and deformation (increasing the window for changing process parameters and ensuring greater process stability)—and / or cleaning and / or homogenizing of the surfaces.
[0090] According to an embodiment, during step a1), after using the first laser beam, an additional laser beam with a power between 1 kW and 20 kW is used to perform post-processing on at least one of the braking surfaces 2a and 2b, on which a composition in particulate form has been previously deposited. Preferably, the additional laser beam is Gaussian, flat-top, or flat-top annular. The post-processing may include heating, for example, to reduce the thermal gradient and homogenize the surface before forming the base layer 30 during step b) above.
[0091] According to an embodiment of the method, step e1) is provided for depositing an auxiliary ferrite nitrocarburization layer between one of the two braking surfaces 2a, 2b of the brake band and the base layer 30, and / or between one of the two braking surfaces 2a, 2b of the brake band and the intermediate layer 300, and / or between the intermediate layer 300 and the base layer 30.
[0092] According to an embodiment of the method, step e2) is provided for depositing an auxiliary iron-aluminum layer between one of the two braking surfaces 2a, 2b of the brake band and the base layer 30, and / or between one of the two braking surfaces 2a, 2b of the brake band and the intermediate layer 300, and / or between the intermediate layer 300 and the base layer 30.
[0093] According to an embodiment, the method includes depositing an auxiliary ferrite nitrocarbon co-diffusion layer and an auxiliary iron-aluminum layer between one of the two braking surfaces 2a, 2b of the braking band and the base layer 30, and / or between one of the two braking surfaces 2a, 2b of the braking band and the intermediate layer 300, and / or between the intermediate layer 300 and the base layer 30.
[0094] Obviously, the described embodiments are merely specific embodiments of the present invention. Without departing from the scope of protection defined in the appended claims, those skilled in the art will be able to make all necessary modifications to the disks and methods described in the present invention to adapt them to specific conditions.
Claims
1. A disc (1) for a disc brake, the disc (1) comprising a brake band (2) having two opposite brake surfaces (2a, 2b), the brake band (2) being made of gray cast iron or steel, The disk includes: A base layer (30) covering at least one of the two braking surfaces (2a, 2b) of the brake band (2), wherein the base layer (30) comprises nickel-free steel, or steel containing nickel in a weight percentage not exceeding 15%, 7.5%, or 5%, and includes at least one carbide selected from titanium carbide (TiC), tungsten carbide (WC), chromium carbide, niobium carbide (NbC), molybdenum carbide (Mo2C), and silicon carbide (SiC), and the steel of the base layer (30) includes at least 10% chromium (Cr) by weight; and An intermediate layer (300) is disposed between the base layer (30) and at least one of the two braking surfaces (2b, 2b) of the brake band (2), wherein the intermediate layer (300) comprises nickel-free steel, or contains steel with a content of not more than 15%, not more than 7.5%, or not more than 5% by weight.
2. The disk (1) according to claim 1, wherein, The base layer (30) is formed by a metallurgical bond between at least one of the braking surfaces (2a, 2b) and a particulate composition deposited on the braking surfaces (2a, 2b) by at least one laser beam. The particulate composition includes M x C y -FeCr, and nickel-free steel or steel containing no more than 15%, 7.5%, or 5% nickel by weight, or the particulate composition is made of M x C y -FeCr, and steel that does not contain nickel or steel containing nickel by weight not exceeding 15%, or by weight not exceeding 7.5%, or by weight not exceeding 5%, wherein M is selected from Ti, W, Cr, Nb, Mo, Si, x is an integer selected from 1, 2 and 3, and y is an integer selected from 1 and 2.
3. The disk (1) according to claim 1 or 2, wherein, The steel of the base layer (30) comprises at least titanium carbide (TiC). Preferably, the base layer (30) is formed by a metallurgical bond between at least one of the braking surfaces (2a, 2b) and a particulate composition deposited on the braking surfaces (2a, 2b) by at least one laser beam. The particulate composition comprises TiC-FeCr and nickel-free steel or steel containing nickel in a weight of not more than 15%, not more than 7.5%, or not more than 5%, or the particulate composition consists of TiC-FeCr and nickel-free steel or steel containing nickel in a weight of not more than 15%, not more than 7.5%, or not more than 5%, or the particulate composition consists of TiC-FeCr and nickel-free steel or steel containing nickel in a weight of not more than 15%, not more than 7.5%, or not more than 5%, or the particulate composition consists of TiC-FeCr and nickel-free steel or steel containing nickel in a weight of not more than 15%, not more than 7.5%, or not more than 5%, or the particulate composition consists of TiC-FeCr and nickel-free steel or steel containing nickel in a weight of not more than 15%, not more than 7.5%, or not more than 5%, or the particulate composition consists of TiC-FeCr.
4. The disk (1) according to any one of the preceding claims, wherein, The steel of the base layer (30) consists of chromium (Cr) in an amount between 10% and 20% by weight, silicon (Si) in an amount not exceeding 1.5% by weight, manganese (Mn) in an amount not exceeding 2% by weight, carbon (C) in an amount not exceeding 0.03% by weight, and iron in an amount equal to the remaining percentage by weight.
5. The disk (1) according to any one of the preceding claims, wherein, The base layer (30) has a thickness between 30 μm and 1500 μm, for example, the base layer (30) has a thickness between 50 μm and 300 μm or between 800 μm and 1200 μm.
6. The disk (1) according to any one of the preceding claims, wherein, The intermediate layer (300) has a thickness between 30 μm and 1000 μm, for example, the intermediate layer (300) has a thickness between 60 μm and 200 μm.
7. A method for manufacturing a brake disc (1), the method comprising the following steps: a) Provide a brake disc (1) The brake disc (1) includes a brake band (2) provided with two opposite brake surfaces (2a, 2b) and the brake band is made of gray cast iron or steel; a1) After step a), an intermediate layer (300) is deposited on at least one of the two opposite braking surfaces (2a, 2b), the intermediate layer (300) comprising nickel-free steel, or steel containing nickel in a content not exceeding 15% by weight, or a content not exceeding 7.5% by weight, or a content not exceeding 5% by weight. b) Following step a1), the particulate composition is deposited on the intermediate layer (300) of at least one of the braking surfaces (2a, 2b) using a laser deposition technique selected from LMD (laser metal deposition), HSLMD (high-speed laser metal deposition), high-speed laser cladding, ultra-high-speed laser cladding (EHLA), and ultra-fast cladding, thereby forming a base layer (30). The base layer (30) covers at least one of the two braking surfaces (2a, 2b) of the brake band (2). The particulate composition includes M x C y -FeCr, and nickel-free steel or steel containing no more than 15%, 7.5%, or 5% nickel by weight, or the particulate composition is made of M x C y -FeCr, and steel that does not contain nickel or contains nickel by weight not exceeding 15%, or by weight not exceeding 7.5%, or by weight not exceeding 5%, wherein, M is selected from Ti, W, Cr, Nb, Mo, Si, x is an integer selected from 1, 2, and 3, and y is an integer selected from 1 and 2.
8. The method according to claim 7, wherein, M x C y - The carbides in FeCr are selected from titanium carbide (TiC), tungsten carbide (WC), chromium carbide, niobium carbide (NbC), molybdenum carbide (Mo2C), and silicon carbide (SiC).
9. The method according to claim 7 or 8, wherein, The particulate composition comprises TiC-FeCr, and nickel-free steel or steel containing nickel by weight not exceeding 15%, or by weight not exceeding 7.5%, or by weight not exceeding 5%, or the particulate composition consists of TiC-FeCr, and nickel-free steel or steel containing nickel by weight not exceeding 15%, or by weight not exceeding 7.5%, or by weight not exceeding 5%.
10. The method according to any one of claims 7 to 9, wherein, M x C y -FeCr particles are dispersed in the matrix of steel particles, preferably, M x C y -FeCr is an agglomerated and / or sintered material.
11. The method according to any one of claims 7 to 10, wherein, The particulate composition comprises M in an amount between 10% and 40% by weight. x C y -FeCr, preferably, the particulate composition comprises M in an amount between 15% and 35% by weight. x C y -FeCr.
12. The method according to any one of claims 7 to 11, wherein, M x C y - The weight ratio of FeCr carbides to FeCr is between 20:80 and 80:20, for example, M x C y The weight ratio of FeCr carbides to FeCr is between 30:70 and 70:30 or between 40:60 and 60:
40.
13. The method according to any one of claims 7 to 12, wherein, Step b) is performed using at least one first laser beam, the first laser beam having a power between 6 kW and 30 kW, preferably the laser beam being Gaussian, flat-top, or flat-top ring-shaped.
14. The method according to any one of claims 7 to 13, wherein: The deposition rate of the particulate composition is between 1 m 2 / h and 14 m 2 The deposition rate of the particulate composition is between 1 m / h, for example, between 1 m / h. 2 / h and 8 m 2 Between / h, and / or The flow rate used for depositing the particulate composition is between 20 g / min and 400 g / min.
15. The method according to claim 13 or 14, wherein, During step b), before using the first laser beam, an additional laser beam with a power between 1 kW and 15 kW is used, preferably a Gaussian, flat-top, or flat-top ring laser beam, which pre-treats at least one of the braking surfaces (2a, 2b).
16. The method according to any one of claims 13 to 15, wherein, During step b), after using the first laser beam, an additional laser beam with a power between 1 kW and 20 kW is used, preferably a Gaussian, flat-top, or flat-top ring laser beam, which performs post-treatment on at least one braking surface (2a, 2b) previously deposited with the particulate composition.
17. The method according to any one of claims 7 to 16, wherein, Step a1) of depositing the intermediate layer (300) includes: depositing a composition in particulate form by a laser deposition technique selected from LMD (laser metal deposition), HSLMD (high-speed laser metal deposition), high-speed laser cladding, ultra-high-speed laser cladding (EHLA) and ultra-fast cladding, wherein the particulate composition comprises nickel-free steel, or steel containing nickel in a weight of not more than 15%, not more than 7.5%, or not more than 5% by weight.
18. The method according to claim 17, wherein, Step a1) is performed using at least one first laser beam having a power between 6 kW and 30 kW. Preferably, the laser beam is Gaussian, flat-top, or flat-top ring-shaped. The first laser beam performs deposition of the particulate composition on at least one braking surface of the braking surfaces (2a, 2b).
19. The method according to claim 17 or 18, wherein: The deposition rate of the particulate composition is between 1 m 2 / h and 14 m 2 The deposition rate of the particulate composition is between 1 m / h, for example, between 1 m / h. 2 / h and 8 m 2 Between / h, and / or The flow rate used for depositing the particulate composition is between 20 g / min and 400 g / min.
20. The method according to claim 18 or 19, wherein, During step a1), before using the first laser beam, an additional laser beam with a power between 1 kW and 15 kW is used, preferably a Gaussian, flat-top, or flat-top ring laser beam, which pre-treats at least one of the braking surfaces (2a, 2b).
21. The method according to any one of claims 18 to 20, wherein, During step a1), after using the first laser beam, an additional laser beam with a power between 1 kW and 20 kW is used, preferably a Gaussian, flat-top, or flat-top ring laser beam, to perform post-treatment on at least one braking surface (2a, 2b) previously deposited with the granular composition.
22. A disc (1) for a disc brake, said disc (1) being obtainable by means of any one of claims 7 to 21.