A three-layer density down filling unit, its preparation method, and its application in down garments based on human body heat distribution.

By using a three-layer density down filling unit and electrospun nano anti-down leakage membrane technology, the problems of down leakage and down-proof durability in traditional down jackets have been solved. The down filling density is designed according to the human body's heat distribution, achieving high-efficiency warmth and comfort in down jackets.

CN123100899APending Publication Date: 2026-11-17CHANGSHU INSTITUTE OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611225799.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional down jackets suffer from down leakage and insufficient durability of the down-proof layer. Furthermore, the filling method does not meet the body's heat distribution requirements, resulting in a mismatch between warmth and comfort during exercise.

Method used

It adopts a three-layer density down filling unit, and forms an independent sealed cavity through electrospun nano anti-down leakage membrane and polyester thermoplastic polyurethane elastomer and polycaprolactone composite material. The down filling density is arranged differently according to the human body's heat distribution, and the bonding strength is enhanced by hot melt adhesive layer.

Benefits of technology

It effectively solves the problem of down leakage in traditional down jackets, improves the durability and bonding strength of the down-proof layer, and achieves a match between the down filling amount in each area and the heat dissipation needs of the human body, thereby improving warmth retention and sports comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123100899A_ABST
    Figure CN123100899A_ABST
Patent Text Reader

Abstract

This invention discloses a three-layer density down filling unit, its preparation method, and its application in down jackets based on human body heat distribution. The down filling unit includes at least one filling structure, comprising a full-coverage layer and two partitions located inside the full-coverage layer. The two partitions divide the interior of the full-coverage layer into an outer cavity R1, a middle cavity R2, and an inner cavity R3. Differential down filling is performed on each independent sealed cavity, with the down filling amount of the three cavities being R2 > R1 ≥ R3. This invention uses three completely independent sealed cavities as the down filling unit, solving the technical problems of pinhole down leakage and insufficient down-proof durability caused by traditional sewing and sealing. It achieves the technical effect of limiting down migration across cavities from a structural level. Furthermore, this invention uses an electrospun nano-anti-down-leakage membrane to improve the bonding strength and durability of the down-proof layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of down jackets, specifically to a three-layer density down filling unit, its preparation method, and its application in down jackets based on human body heat distribution. Background Technology

[0002] Traditional down jackets are structurally formed using traditional sewing techniques. The outer fabric and lining are sewn together with sewing thread to divide them into multiple independent filling cavities. Down material is then quantitatively filled into each cavity, and the down's fluffy structure inside the cavity provides warmth and insulation. This process is simple to form and has low production costs, making it the mainstream process that the industry has long used.

[0003] However, in actual production and long-term use, the structural defects of traditional sewn-on down jackets continue to become apparent. The edge sealing and compartmentalization of existing down jacket cavities rely entirely on sewing. As the needle and thread penetrate the fabric, they create numerous tiny pinholes at each seam. These pinholes are permanent structural pores and cannot be completely closed by the fabric's own resilience or conventional finishing processes. Down fibers are fine, resilient, and prone to slippage. Under the influence of human activity, clothing compression and rubbing, washing and shaking, down continues to leak outwards through these pinholes, causing down leakage. Even if some manufacturers optimize the stitch length and use finer thread, they can only slightly reduce the probability of down leakage; they cannot completely eliminate the pinhole channels for down leakage at the structural level. The problem persists after long-term wear, severely affecting the appearance and user experience of the garment.

[0004] To improve down leakage, existing solutions involve attaching a down-proof lining to the inside of the fabric, applying a down-proof coating, or using a composite down-proof film to add a down-proof layer and prevent down from escaping. However, conventional down-proof layers are mostly simple bonded composite structures, with the interface between the down-proof layer and the fabric / lining relying solely on ordinary hot melt adhesive or glue. This interface bonding method is simplistic and has poor adhesion stability. Down jackets are frequently subjected to washing, drying, bending, stretching, and compression during daily use. Repeated bending, washing, and rinsing continuously damage the composite adhesive interface between the down-proof layer and the fabric, gradually leading to problems such as localized delamination, separation, and peeling. Once the interface peels off, the down-proof layer will become hollow, shifted, and damaged, completely failing the down-proof barrier. The down-proof effect will continuously decrease with each wear and wash. While the initial down-proof performance is excellent, repeated down leakage problems occur later, significantly reducing the down-proof durability of the down jacket and greatly shortening its lifespan.

[0005] In addition, the traditional down filling layout of down jackets has obvious human-centered design flaws. Existing products all use a uniform down filling method across the entire garment, without considering the human body's physiological structure, heat dissipation patterns, and limb movement characteristics for differentiated adaptation. The core torso, such as the torso and back, loses heat quickly and requires high warmth, while areas like the armpits, joints, and sides of the waist are more frequently used and have greater movement, tending to accumulate sweat and requiring even greater heat dissipation. The uniform down filling method results in both excessive and insufficient warmth. Areas prone to sweating have excessive down filling and an overly thick loft layer, preventing heat and sweat from dissipating quickly, leading to a stuffy and sticky feeling. In areas with frequent limb movement, the down filling is too full, limiting the fabric's elasticity and significantly restricting limb flexion and movement, resulting in poor flexibility. Summary of the Invention

[0006] The purpose of this invention is to provide a three-layer density down filling unit, a preparation method, and its application in down garments based on human body heat distribution. It solves the technical problems of down leakage in existing down filling structures and the mismatch between warmth retention and sports comfort caused by uniform down filling density in various parts.

[0007] The present invention achieves the above objectives through the following technical solutions: The primary objective of this invention is to provide a method for preparing a three-layer density down filling unit. The down filling unit includes at least one filling structure, which comprises a full-coverage layer and two partitions located inside the full-coverage layer. The two partitions divide the interior of the full-coverage layer into an outer cavity R1, a middle cavity R2, and an inner cavity R3. The preparation method includes the following steps: Polyester-type thermoplastic polyurethane elastomer and polycaprolactone are dissolved in a mixed solvent containing hydrophobic fumed silica to form a spinning solution. The nano anti-fleece membrane is obtained by electrospinning and low-temperature thermal activation. The four layers of nano-anti-down-leakage membrane are cut to the shape of the designated cavity of the down jacket, and the edges are sealed along the contour line and / or rib line. Each filling structure retains the down filling port area to form three independent sealed cavities. Each independent sealed cavity is filled with down in a differentiated manner, with the down filling amount of the three cavities being R2 > R1 ≥ R3, and the filling port is sealed to obtain a three-layer density down filling unit.

[0008] As a further improvement of the present invention, the spinning solution, based on a total mass of 100%, comprises: 10wt%-16wt% polyester thermoplastic polyurethane elastomer, 1wt%-3wt% polycaprolactone, 0.3wt%-0.8wt% hydrophobic fumed silica, and the balance being a mixed solvent and dispersant of N,N-dimethylformamide and acetone.

[0009] As a further improvement of the present invention, the electrospinning process parameters are: feed rate 0.7-1.1 mL·h -1 · Single needle -1 The applied voltage is 17-20kV, the spinning distance is 17-20cm, the ambient temperature is 25±2℃, and the relative humidity is 36%-44%; the low-temperature thermal activation and setting temperature is 62-70℃, and the time is 2.5-3.5min.

[0010] As a further improvement of the present invention, each partition consists of two layers of electrospun nano-anti-fleece diaphragms, wherein the central axis of the outer diaphragm is connected to the full-coverage layer by hot melt adhesive, dividing the outer cavity R1 and the inner cavity R3 into two small cavities respectively.

[0011] As a further improvement of the present invention, the six layers of nano-anti-down-leakage membrane are cut to the shape of the designated cavity of the down jacket, wherein the edges are sealed along the contour line and / or the rib line, and the edges in each filling structure are sealed along the central axis of the first and second, fifth and sixth layers.

[0012] As a further improvement of the present invention, the edge sealing is at least one of adhesive coating or stitching, the line width of the adhesive coating on the outline is 2.0-3.0 mm; the coating temperature is 145-160℃, the width of the adhesive strip of the adhesive coating on the center line or rib line is 1.8-2.2 mm, and the coating thickness is 0.08-0.12 mm; the line width of the stitching is 0.5 mm-1.0 mm.

[0013] As a further improvement of the present invention, the mass ratio of the down filling amount of the three cavities is R1:R2:R3 = (0.5-0.6):1:(0.3-0.5).

[0014] The second objective of this invention is to provide a three-layer density down filling unit placed in an independent cavity formed by the outer and inner fabrics of a sewn-on down jacket.

[0015] A third objective of this invention is to provide the application of the aforementioned three-layer density down filling unit in a down jacket based on human body heat distribution, wherein the front chest and back of the down jacket serve as the core area, the elbows and armpits serve as the active area, and the arms, neck, front placket, and hem serve as the edge area. The three-layer density down filling unit is placed in the core area, a single-layer down filling unit is placed in the active area, and a double-layer down filling unit is placed in the edge area. The down filling unit is located between the outer fabric and the inner fabric of the down jacket.

[0016] As a further improvement of the present invention, the filling structure of the single-layer down filling unit is that down is filled in the entire layer, and the down filling amount is equal to the R1 filling amount; the filling structure of the double-layer down filling unit is that two independent cavities, an outer cavity R1 and an inner cavity R3, are formed in the entire layer through a partition layer, and the down filling amount is the same as that of the outer cavity R1 and the inner cavity R3 of the three-layer density down filling unit.

[0017] The beneficial effects of this invention are as follows: (1) The present invention uses four layers of diaphragms to form three completely independent sealed cavities as down filling units, which solves the technical problems of needle hole down penetration and insufficient down-proof durability caused by traditional sewing and sealing, and achieves the technical effect of restricting down migration across cavities from the structural level.

[0018] (2) The present invention uses an electrospun nano anti-fleece membrane composed of polyester thermoplastic polyurethane elastomer and polycaprolactone. During the hot pressing process, the polycaprolactone component forms an interfacial interpenetration bond with the polyamide hot melt adhesive layer, which improves the bonding strength between the membrane and the hot melt adhesive layer. This solves the technical problem that the anti-fleece layer composite interface is easy to peel off and fail after washing and bending, and achieves improved bonding strength and service durability of the anti-fleece layer.

[0019] (3) By setting down filling units separate from the inner and outer layers of the down jacket, the present invention can prevent down from escaping while maintaining the breathability of the inner and outer layers of the fabric.

[0020] (4) The present invention arranges the down filling density according to the heat dissipation needs and movement range of different parts of the human body, which solves the technical problem of insufficient local heat dissipation and limited activity caused by uniform down filling method, and achieves the technical effect that the down filling amount in each area corresponds to the actual heat preservation and heat dissipation needs of the human body. Attached Figure Description

[0021] Figure 1 This is a schematic diagram of the down filling unit structure involved in the present invention. Detailed Implementation

[0022] The present application will now be described in further detail with reference to the accompanying drawings. It should be noted that the following specific embodiments are only used to further illustrate the present application and should not be construed as limiting the scope of protection of the present application. Those skilled in the art can make some non-essential improvements and adjustments to the present application based on the above application content.

[0023] This invention discloses a three-layer density down filling unit, its preparation method, and its application in down garments based on human body heat distribution, specifically including the following steps: Step 1: Preparation of electrospun nano-anti-lint separator Step 1.1: Add hydrophobic fumed silica (specific surface area) Particles with a particle size of 7-40 nm were added to a mixed solvent of N,N-dimethylformamide and acetone, with the mass ratio of N,N-dimethylformamide to acetone being 6:4. After magnetic stirring at room temperature for 60 min, the mixture was ultrasonically dispersed at 300 W for 40 min to obtain a uniform dispersion.

[0024] It should be noted that the amount of hydrophobic fumed silica used is based on the total mass of the spinning solution, with a mass fraction of 0.3wt%-0.8wt%, preferably 0.5wt%; the amount of polyether silicone dispersant used is based on the total mass of the spinning solution, with a mass fraction of 0.1wt%-0.2wt%, preferably 0.15wt%. The hydrophobic fumed silica nanoparticles embed between fibers to form physical barrier nodes, controlling the average pore size of the membrane within the range of 0.35-1.2μm. This pore size range is smaller than the minimum diameter of down fibers but larger than the free path of water vapor molecules, thus balancing down-proofing and breathability. The polyether silicone dispersant is used to improve the dispersion stability of the hydrophobic fumed silica nanoparticles in the organic solvent system, preventing particle agglomeration that could lead to spinning blockage or membrane defects.

[0025] Furthermore, in step 1.1, N,N-dimethylformamide is an organic solvent with reproductive toxicity, and acetone is a flammable solvent with a low flash point. The above operations must be carried out in a fume hood, and operators must wear organic solvent-resistant gloves and protective goggles, and keep away from open flames and heat sources.

[0026] Step 1.2: Add polyester-type thermoplastic polyurethane elastomer particles (Shore hardness 85A, number average molecular weight 80,000-120,000 g / mol, elongation at break not less than 700%) to the uniform dispersion obtained in Step 1.1 in batches, and stir at a constant temperature of 48℃ and 220 r / min for 6 hours until completely dissolved; then add polycaprolactone particles (number average molecular weight 60,000-100,000 g / mol, preferably 80,000 g / mol; melting point 58-62℃), and continue stirring for 4 hours until the system becomes transparent and homogeneous, thus obtaining the spinning solution.

[0027] It should be noted that, based on 100% of the total mass of the spinning solution, the mass fraction of polyester thermoplastic polyurethane elastomer is 10wt%-16wt%, preferably 13wt%; the mass fraction of polycaprolactone is 1wt%-3wt%, preferably 2wt%; the balance is a mixed solvent of N,N-dimethylformamide and acetone, and the powder components added in step 1.1. As the elastic matrix of the fiber membrane, the polyester thermoplastic polyurethane elastomer, with its elongation at break of not less than 700%, ensures that the resulting diaphragm does not crack or delaminate during the bending process of clothing wear. The melting point of polycaprolactone (58-62℃) is lower than the hot-pressing temperature range of polyamide hot melt adhesive (112-118℃). During hot pressing, the polycaprolactone component locally softens and melts, forming an interfacial interpenetration bond with the hot melt adhesive layer, thereby increasing the hot-pressing peel strength between the diaphragm and the hot melt adhesive by more than -1.6 N / cm.

[0028] Furthermore, the polymer dissolution process in step 1.2 is carried out in an air atmosphere. The polyester thermoplastic polyurethane elastomer particles are added in batches with an interval of no less than 30 minutes between each batch to avoid excessively high local concentrations that could cause particle clumping and affect the uniformity of dissolution.

[0029] Step 1.3: The spinning solution obtained in Step 1.2 is heated at 48°C under negative pressure. Vacuum degassing was performed for 120 minutes under the specified conditions to eliminate dissolved bubbles; then, negative pressure filtration was performed using a 10μm PTFE filter membrane to remove undissolved impurities and large particle agglomerates, resulting in a clean spinning solution.

[0030] Step 1.4, at temperature In a constant temperature and humidity environment of ℃ and 36%-44% relative humidity, the clean spinning solution obtained in step 1.3 is fed at a rate of 0.7-1.1 mL·h. -1 · Single needle -1 Electrospinning is performed by applying a voltage of 17-20kV and a spinning distance of 17-20cm to obtain a nascent fiber membrane by depositing a nanofiber layer on the surface of the base fabric collecting roller.

[0031] It should be noted that the relative humidity is controlled within the range of 36%-44%, which is the balance window between fiber formation and solvent evaporation rate. When the humidity is below 36%, the solvent evaporates too quickly, causing a beaded structure on the fiber surface. When the humidity is above 44%, ambient moisture penetrates the jet, causing uneven fiber diameter distribution. A spinning distance of 17-20cm and a voltage of 17-20kV allow sufficient stretching time and solvent evaporation time for the jet, resulting in a uniform fiber membrane with an average fiber diameter of 200-380nm.

[0032] Furthermore, the electrospinning process in step 1.4 is carried out under normal pressure air atmosphere. The concentration of N,N-dimethylformamide and acetone vapor in the spinning environment must be maintained below the safe concentration through the ventilation and exhaust system to ensure operational safety and the stability of the spinning environment.

[0033] Furthermore, during the spinning process, both the polyester thermoplastic polyurethane elastomer and polycaprolactone are in solution, and there is no significant risk of oxidation or thermal degradation side reactions in the system. Solvent evaporation is the main pathway for substance loss. The concentration drift of the spinning solution caused by uneven solvent evaporation can be effectively suppressed by constant temperature and humidity control and ventilation and exhaust systems, thereby ensuring the consistency of fiber diameter distribution.

[0034] Furthermore, the exhaust gas containing N,N-dimethylformamide and acetone vapors discharged during the spinning process in step 1.4 must be treated by an activated carbon adsorption device or a condensation recovery device before it can be discharged. The condensate containing N,N-dimethylformamide must be collected and handed over to a professional waste liquid treatment agency for treatment, and must not be directly discharged into the sewer.

[0035] Step 1.5: The nascent fiber membrane obtained in step 1.4 is sent into a hot air box and hot-air shaped at 62-70℃ for 2.5-3.5 minutes. This allows the polycaprolactone component to soften locally at the fiber cross nodes to form bonding points, thereby improving the overall mechanical strength and dimensional stability of the fiber membrane and obtaining the finished electrospun nano anti-fleece membrane.

[0036] It should be noted that the thermal activation temperature of 62-70℃ is above the initial melting temperature (58-62℃) and below the complete melting temperature of polycaprolactone. This temperature window allows the polycaprolactone component to adhere only locally at the fiber overlap points without completely melting and collapsing, thus preserving the porous and breathable structure of the fiber membrane while providing the necessary structural integrity to the membrane layer. The finished electrospun nano anti-lint separator has a surface weight of 5-10 g / m³. 2 Elongation at break greater than 650%, air permeability 70-145mm / s, hot-pressing window 100-118℃.

[0037] To improve the water-wash resistance and durability of the finished electrospun nano anti-lint membrane, a fluorocarbon hydrophobic finishing process can be performed on the finished electrospun nano anti-lint membrane after step 1.5: The finished electrospun nano anti-lint membrane is immersed in a short-chain C6 fluorocarbon waterproofing agent aqueous dispersion with a mass concentration of 0.8%-1.2% for 15-20 seconds, and the roll-off rate is controlled at 65%-75%. Then, it is baked at 130℃ for 60-90 seconds to complete cross-linking and curing, so that the surface contact angle of the finished electrospun nano anti-lint membrane is increased to more than 140°. After 50 standard water washes, the anti-lint performance does not significantly decrease.

[0038] Step 2: Pre-shrinking and shaping of electrospun nano anti-fleece separator The finished electrospun nano anti-lint separator obtained in step 1 is flattened and fed into a continuous heat setter. It is then relaxed and set at 120℃ and a pressure not exceeding 0.05MPa, ensuring the separator's pre-shrinkage rate is controlled within 1.2%. The 120℃ setting temperature is lower than the softening temperature range (approximately above 150℃) of the polyester thermoplastic polyurethane elastomer matrix in the finished electrospun nano anti-lint separator, thus avoiding damage to the fiber structure and pore size distribution of the finished electrospun nano anti-lint separator.

[0039] Furthermore, the relaxation setting time in step 2 is 30-60 seconds, and the fabric feeding rate is 8-15 m / min, to ensure that the fabric receives a sufficiently uniform heat treatment time in the heat setting machine.

[0040] Step 3: Edge sealing Step 3.1: Cut the electrospun nano anti-down-leakage membrane to fit the shape of the inner and outer cavities of the down jacket. On the outer surface of the electrospun nano anti-down-leakage membrane, at the rib line or central axis position, use a precision hot melt adhesive coating equipment to continuously coat polyamide hot melt adhesive strips with a width of 1.8-2.2mm and a coating thickness of 0.08-0.12mm.

[0041] It should be noted that the polyamide hot melt adhesive has a melting point of 105-115℃, an open time of 8-15s, and a Shore hardness of 55-65D after curing. The polyamide hot melt adhesive strips on the rib line form horizontal down jacket grids (multiple) after hot pressing. The central axis polyamide hot melt adhesive strip bonds and fixes the central axis of the diaphragm during subsequent hot pressing, causing the double-layer structure to expand outwards, making the outer cavity R2 and the inner cavity R3 stand upright, forming a sandwich-like gradient three-dimensional filling structure (single grid). A strip width of 1.8-2.2mm is the preferred range to balance adhesive strength and softness: a width less than 1.8mm results in insufficient bonding area, making it prone to detachment after bending and wearing under the force of the cavity opening; a width greater than 2.2mm leads to excessive adhesive area and a locally hardened feel.

[0042] Furthermore, in step 3.1, the polyamide hot melt adhesive coating temperature is 145-160℃ and the coating rate is 10-20m / min, to ensure that the polyamide hot melt adhesive is in a fully melted and flowing state at the outlet of the coating equipment and to achieve uniform and continuous coating.

[0043] Step 3.2: Apply polyamide hot melt adhesive along the preset edge sealing contour line at the corresponding positions of the outer edges of the three-layer cavity (R1, R2, R3) of the fabric assembly after adhesive application in Step 3.1. The adhesive line width is 2.0-3.0mm to form a continuous closed border pattern, which completely covers the outer edges of the three-layer cavity, and obtains the adhesive-coated fabric.

[0044] Furthermore, the coating temperature of the polyamide hot melt adhesive used in step 3.2 is the same as that in step 3.1, which is 145-160℃. After coating, the polyamide hot melt adhesive strip must complete the subsequent overlapping operation within the open time (8-15s) to ensure effective wetting and bonding between the adhesive layer and the fabric fibers.

[0045] Step 3.3: Optionally, after applying adhesive in steps 3.1 and 3.2, sew along the outline and rib lines using a 7 / 9 gauge ultra-fine round-tipped needle; 60S / 2 polyester high-elastic down-proof thread, double-stitched for high strength and small needle hole gaps; synchronous feed presser foot / roller presser foot; rib main thread 2.2-2.8mm; down filling seal tightened to 1.5-2mm. For everyday down jackets, the stitching can be done together with the finished down jacket, i.e., the down filling unit and outer fabric are sewn together with the rib line, and then the lining is sewn to the other side of the down filling unit; for windproof down jackets, the rib line of the down filling unit is sewn separately.

[0046] Step 4: Hot pressing of partitioned heat insulation pads The fabric assembly obtained in step 3 after adhesive application was hot-pressed using a contoured partitioned heat insulation pad. The structure of the contoured partitioned heat insulation pad is as follows: a silicone rubber heat insulation layer is attached to the surface of a metal heating plate. Hollow channels corresponding to the adhesive application areas (central axis, rib lines, and outline lines) are cut into the silicone rubber heat insulation layer according to the cavity layout. At the hollow channels, the metal heating plate directly contacts the adhesive application area of ​​the fabric, applying heat and pressure. The remaining main cavity area is covered by the silicone rubber heat insulation layer, leaving the fabric suspended without pressure or heat. The hot-pressing parameters are: hot-pressing temperature 112-118℃, pressure 0.25-0.32MPa, and holding time 6-9s.

[0047] After hot pressing, the polyamide hot melt adhesive strip melts and penetrates the gaps between the fabric fibers, and solidifies after cooling to form a dense adhesive layer; the central axis polyamide hot melt adhesive strip bonds the double-layer discontinuous composite fabric R1 and opens the three cavities in three dimensions, and the edge sealing polyamide hot melt adhesive strip completely seals the edges of each cavity, forming a three-layer independent sealed cavity frame that is not interconnected, thus obtaining the hot-pressed semi-finished product.

[0048] It should be noted that the hot-pressing process of the contoured partitioned heat insulation pad only applies high temperature and pressure to the glued edge sealing area, while the main insulation area of ​​the cavity is suspended without pressure or heat, thus avoiding the closure of fabric micropores and the hardening and hardening of the fabric to the touch. The hot-pressing temperature of 112-118℃ is above the melting point of polyamide hot melt adhesive (105-115℃), ensuring that the adhesive layer is fully melted and penetrated; at the same time, this temperature is lower than the softening temperature of the polyester thermoplastic polyurethane elastomer matrix, so as not to damage the fiber structure of the finished electrospun nano anti-fleece membrane. The holding time is 6-9 seconds, and the pressure is 0.25-0.32MPa, which allows the molten polyamide hot melt adhesive to fully penetrate into the gaps between the fabric yarns to form a mechanical anchor, forming a high peel strength adhesive interface after cooling.

[0049] Step 5: Low-temperature post-curing The hot-pressed semi-finished product obtained in step 4 is laid flat and passed through a constant temperature channel at 75-85℃ at a uniform speed for 2.5-4 minutes to obtain a post-cured semi-finished product. Low-temperature post-curing allows the polyamide hot melt adhesive to complete secondary crystallization and molecular chain relaxation and rearrangement, improving the peel strength and water wash stability of the polyamide hot melt adhesive layer.

[0050] It should be noted that the post-curing temperature of 75-85℃ is lower than the melting point of polyamide hot melt adhesive, and will not cause the polyamide hot melt adhesive layer to remelt and flow; it only promotes the orderly arrangement of molecular chain segments within the polyamide hot melt adhesive layer. Samples without post-curing treatment have a risk of softening and debonding of the polyamide hot melt adhesive layer after repeated water washing. Post-curing treatment can improve the water resistance of hot-pressed joints.

[0051] Step 6: Reserve independent down filling port and fill separate cavities with down. Step 6.1, Independent Filling Port Reservation: For the three cavities R1, R2 and R3 in the post-cured semi-finished product obtained in Step 5, independent filling ports that are not connected to each other are opened at the non-sealed edge of the fabric. The filling port of each cavity is only connected to the cavity itself, and there is no through channel between the cavities, thus completing the cavity prefabrication.

[0052] Step 6.2, Independent quantitative filling of each cavity: Fill the R1, R2 and R3 cavities with quantitative filling through the independent filling port of each cavity. The mass ratio of filling amount of the three cavities is R1:R2:R3 = (0.5-0.6):1:(0.3-0.5).

[0053] Filling density is determined based on ergonomically differentiated layout: Core areas of the torso, chest, and back: densely arranged complete three-layer cavity units of R1, R2, and R3, with R2 down filling density of 62-75 g / m². 2 R1 down filling density 31-45g / m 2 R3 down filling density 18-38g / m 2 .

[0054] Elbow and armpit areas: Single-layer down filling unit, down density 31-45g / m² 2 .

[0055] Arms, neck, front placket, and hem edge areas: Double-layered down-filled units, with an outer cavity R1 and an inner cavity R3 formed by a partition layer. The down filling density of R1 is 31-45 g / m². 2 R3 down filling density 18-38g / m 2 .

[0056] Step 6.3, Low-frequency vibration homogenization: After the down filling is completed, each cavity is subjected to low-frequency vibration treatment for 3-5 minutes, with a vibration frequency of 8-15Hz, so that the down is evenly spread in the cavity and the local accumulation near the down filling port is eliminated.

[0057] Step 6.4: Use a local hot-pressing process to seal all down filling ports. The hot-pressing parameters are the same as in Step 4 (temperature 112-118℃, pressure 0.25-0.32MPa, holding time 6-9s) to form a tight seal between the fabric and the polyamide hot melt adhesive layer at the down filling port, thus obtaining the down filling sealing module.

[0058] Step 7: Garment sewing and finishing The down-filled sealing modules obtained in step 6 are spliced ​​and sewn together according to the ergonomic pattern, and after finishing the process, the finished down jacket is obtained.

[0059] Experiment 1 Electrospun nano-anti-fleece separators were prepared according to the parameters shown in Table 1: Table 1. Preparation parameters of electrospun nano-anti-fleece separator

[0060] Note: ① The balance is "N,N-dimethylformamide and acetone are mixed in a mass ratio of 6:4"; ② "-" indicates that it is not added.

[0061] (1) The fiber morphology was characterized and the average fiber diameter was measured by scanning electron microscopy. The average pore size of the membrane was determined by capillary flowmeter. The elongation at break was determined by electronic universal testing machine according to GB / T 24218.3-2010 standard. The air permeability was determined by fabric air permeability meter according to GB / T 5453-2025 standard. The surface contact angle was determined by optical contact angle meter according to GB / T 30693 standard. The results are shown in Table 2.

[0062] (2) Take three parallel samples from each of samples 1-9 and prepare a 50cm×50cm down lining. Use 90% white duck down from the same batch (fill weight 700+, down content 90%) as filling material. Test the down-proofness according to the garment turning box method in GB / T 14272-2021 and record the number of down threads. The results are shown in Table 2.

[0063] Table 2 Performance of electrospun nanofiber anti-fleece separator

[0064] From the table above, we can see that: In the three groups of samples from this invention, the SiO2 content increased linearly with increasing SiO2 addition. Increased powder content increased the viscosity of the spinning solution, leading to increased jet tensile resistance and coarser fibers. The increased proportion of inorganic fillers also resulted in a simultaneous increase in mass per unit area. SiO2 nanoparticles filled the fiber network, forming physical barrier nodes. Higher addition levels resulted in more complete filling of fiber gaps and a continuously decreasing pore size, with the 0.38–1.15 μm range perfectly meeting the requirements for blocking down and allowing moisture permeation. An appropriate amount of nano-silica acted as a reinforcing point in the fiber network, inhibiting tensile breakage. Elongation increased continuously with increasing SiO2 content, with all three groups exceeding 650%, demonstrating excellent bending resistance. Air permeability was positively correlated with pore size; more SiO2 resulted in finer pores and a gradually decreasing air permeability rate, with a permeability range of 76–138 mm / s, balancing heat dissipation and down prevention. Hydrophobic fumed silica is a low surface energy filler; higher addition levels resulted in stronger hydrophobicity of the membrane surface and a continuously increasing contact angle. All three groups in this invention maintained extremely low down leakage levels, with sample 2 exhibiting the least down leakage. By comprehensively balancing pore size, elasticity, and interfacial adhesion, sample 2 demonstrated the best down leakage prevention durability.

[0065] Sample 4 contains no nano-barrier particles, and its average pore size is 1.64 μm, exceeding the minimum diameter of down fibers, indicating a lack of physical barriers. The absence of a dispersant contributes to system defects, resulting in a significant decrease in the mechanical properties of the fiber membrane (elongation of only 546%). After washing, the membrane layer and hot melt adhesive interface lack powder support and are prone to delamination, exhibiting the highest down leakage rate among all samples, rendering its down-proof performance completely ineffective. Its air permeability of 152 mm / s is the highest in the group, but this only provides simple air permeability without down-proof value. Its contact angle of 126° is the lowest in the group, indicating the worst hydrophobicity.

[0066] Sample 5 lacked low-melting-point PCL, resulting in no melt bonding at fiber overlaps during the heat setting stage. This led to a decrease in the overall structural strength of the diaphragm, with an elongation at break of 613%, lower than the gradient group. During hot pressing, it failed to interpenetrate and bond with the polyamide hot melt adhesive, and after multiple washes, the interface delaminated, exhibiting significantly higher fiber penetration than samples 1-3. While its pore size of 0.75 μm was similar to sample 2, its durability was significantly deteriorated.

[0067] Sample 6, with its polyacrylic acid dispersant, exhibited poor compatibility with DMF / acetone organic solvents, resulting in severe agglomeration of silica powder. This led to uneven fiber thickness during spinning, with an average fiber diameter of 346 nm, significantly higher than that of Sample 2 with the same SiO2 content. Agglomerated particles caused numerous pore defects on the film surface, increasing the pore size to 1.42 μm. After washing, these defects preferentially resulted in fiber leakage. Powder agglomeration formed stress concentration points, causing a simultaneous decrease in elongation and air permeability.

[0068] In Sample 7, excessive powder caused a sharp increase in the viscosity of the spinning solution, resulting in a fiber diameter that reached the highest value of 412 nm across the entire group. Numerous nanoparticles clogged the fiber pores, with an average pore size of only 0.26 μm, causing a precipitous drop in air permeability to 48 mm / s, leading to stuffiness and discomfort when worn. Excessive inorganic fillers reduced membrane elasticity, resulting in an elongation at break of only 524%, making it prone to microcracks when bent. Although it had extremely small pore size and the highest contact angle of 158° across the group, with only 8 fibers / m² of down leakage after washing, its air permeability and mechanical properties were severely substandard, rendering it unusable.

[0069] Sample 8 had insufficient barrier nodes, with an average membrane pore size of 1.33 μm. The pores continued to expand after repeated washing and extrusion. The amount of powder added was extremely low, with a surface weight of only 4.5 g / m³. 2 The membrane is thin but has a loose structure and poor durability; its air permeability of 144mm / s is too high, resulting in a poor balance between heat preservation and heat dissipation.

[0070] In sample 9, PCL was relatively excessive, resulting in a large amount of melting during hot air setting. This caused extensive adhesion and collapse at the fiber overlaps, shrinking the pore size to 0.41μm and reducing the air permeability to only 42mm / s, the lowest in the group. Excessive PCL also reduced fiber elasticity, with a breaking elongation of 605%, lower than the gradient group. Although the pore size was small and the hydrophobic properties were excellent, resulting in good down-draining effect after washing, the air permeability was extremely poor, leading to sweat accumulation and stuffiness after long-term wear, highlighting significant comfort deficiencies.

[0071] Experiment 2 Experimental Example 1 The diaphragm in sample 2 was fed into a continuous heat setter at a rate of 8 m / min and relaxed and set for 30 s at 120 ℃ and a pressure not exceeding 0.05 MPa to obtain a pre-shrinked and set diaphragm.

[0072] The four layers of the nano-anti-down filling membrane are cut to the designated shape (chest area), and the edges are sealed along the contour line and rib line. The filling structure between adjacent rib lines retains the down filling opening area, forming three independent sealed cavities. Figure 1 As shown in the top left corner; Polyamide hot melt adhesive strips are continuously coated along the rib line at a coating temperature of 145℃ and a coating rate of 10m / min. The strip width is 1.8mm and the coating thickness is 0.08mm. Polyamide hot melt adhesive is also coated along the outline with a coating line width of 2.0mm to form a continuous closed frame, resulting in the coated fabric assembly.

[0073] A contoured partitioned heat insulation pad with a silicone rubber heat insulation layer thickness of 3mm was used. The coated fabric assembly was hot-pressed at a hot pressing temperature of 112℃, a pressure of 0.25MPa, and a holding time of 6s to obtain a hot-pressed semi-finished product.

[0074] The hot-pressed semi-finished product was cured in a constant temperature channel at 75℃ for 2.5 minutes to obtain the post-cured semi-finished product.

[0075] Independent filling ports are opened at the unsealed edges of the three cavities R1, R2, and R3. Each cavity is filled with a fixed amount of down: R2 filling density 72 g / m³. 2 R1 down filling density 43.2g / m² 2 R3 down filling density 36g / m 2 The filling tubes were subjected to low-frequency vibratory texturing at a frequency of 8 Hz for 3 minutes. All filling tubes were then sealed by hot pressing at a temperature of 112℃, a pressure of 0.25 MPa, and a holding time of 6 seconds to obtain product 1.

[0076] Experimental Example 2 The diaphragm in sample 2 was fed into a continuous heat setter at a rate of 8 m / min and relaxed and set for 30 s at 120 ℃ and a pressure not exceeding 0.05 MPa to obtain a pre-shrinked and set diaphragm.

[0077] The six layers of the nano-anti-down filling membrane are cut to the designated shape (chest area), and the edges are sealed along the contour line and rib line. Additionally, the edges of each filling structure (between adjacent rib lines) are sealed along the central axis of the first and second, fifth, and sixth layers. The filling structures between adjacent rib lines each retain the down filling opening area. Figure 1 As shown in the upper right, the outer cavity R1 and the inner cavity R3 are divided into two smaller cavities, forming seven independent sealed cavities; Polyamide hot melt adhesive strips are continuously coated along the rib line and the center axis at a coating temperature of 145℃ and a coating rate of 10m / min. The strip width is 1.8mm and the coating thickness is 0.08mm. Polyamide hot melt adhesive is also coated along the contour line with a coating line width of 2.0mm to form a continuous closed frame, resulting in the coated fabric assembly.

[0078] A contoured partitioned heat insulation pad with a silicone rubber heat insulation layer thickness of 3mm was used. The coated fabric assembly was hot-pressed at a hot pressing temperature of 112℃, a pressure of 0.25MPa, and a holding time of 6s to obtain a hot-pressed semi-finished product.

[0079] The hot-pressed semi-finished product was cured in a constant temperature channel at 75℃ for 2.5 minutes to obtain the post-cured semi-finished product.

[0080] Independent filling ports are opened at the unsealed edges of R1, R2, R3, and the multi-layered cavities of R1 and R3. Each cavity is filled with a fixed amount of down: R2 filling density 72 g / m³. 2 R1 down filling density 43.2g / m² 2 (Equal amount in three areas), R3 fill density 36g / m² 2 (Equal quantities in three regions). Each cavity was vibrated at a low frequency of 8Hz for 3 minutes, and all filling tubes were sealed by hot pressing at a temperature of 112℃, a pressure of 0.25MPa, and a holding time of 6s to obtain product 2.

[0081] Experimental Example 3 Based on Experiment 2, the fill density of R2 is 72 g / m². 2 R1 down filling density 36g / m 2 (Equal amount in three areas), R3 fill density 21.6g / m² 2 (The three regions were of equal quantity), and the remaining parameters were the same as in Experiment 2, resulting in Product 3.

[0082] Test Example 4 Based on Experiment 2, the fill density of R2 is 72 g / m². 2 R1 down filling density 43.2g / m² 2 (Equal amount in three areas), R3 fill density 21.6g / m² 2 (The three regions were of equal quantity), and the remaining parameters were the same as in Experiment 2, resulting in product 4.

[0083] Experimental Example 5 Based on Experiment 2, the fill density of R2 is 72 g / m². 2 R1 down filling density 43.2g / m² 2 (Equal amount in three areas), R3 filler density 43.2g / m² 2 (The three regions were of equal quantity), and the remaining parameters were the same as in Experiment 2, resulting in product 5.

[0084] Experimental Example 6 Based on Experiment 2, the fill density of R2 is 72 g / m². 2 R1 down filling density 21.6g / m 2 (Equal amount in three areas), R3 fill density 21.6g / m² 2 (The three regions were of equal quantity), and the remaining parameters were the same as in Experiment 2, resulting in product 6.

[0085] Experimental Example 7 Cut the two layers of the aforementioned nano-anti-down filling membrane to the predetermined shape (chest area), seal the edges along the contour line and rib line, and retain the filling opening area between adjacent rib lines, such as... Figure 1 The lower left shows a single-layer down filling unit; the other parameters are the same as in Experiment 2, resulting in product 7.

[0086] Experimental Example 8 Cut the three layers of the nano-anti-down filling membrane to the designated shape (chest area), seal the edges along the contour line and rib line, and retain the filling opening area between adjacent rib lines, such as... Figure 1 The bottom right shows a double-layer down filling unit; the other parameters are the same as in Experiment 2, and product 8 is obtained.

[0087] Three parallel samples were prepared for each product number (1-8) for repeated testing. All samples used the same batch of 90% white duck down (700+ fill power, 90% down content) as filling material, with consistent filling patterns in the chest area (approximately 0.18m²). 2 This is to eliminate the influence of fabric differences on the results.

[0088] The down-proof property was tested according to the garment turning box method in GB / T 14272-2021, and the number of down threads was recorded. The results are shown in Table 3.

[0089] The thermal insulation performance was tested according to GB / T 11048-2018 "Determination of thermal and moisture resistance of textiles under steady-state conditions for physiological comfort (evaporative hot plate method)". The clo value before washing and the clo value after 50 washings, as well as the thermal resistance decay rate, were recorded. The results are shown in Table 3.

[0090] Table 3 Performance of Down Filling Units

[0091] From the table above, we can see that: Products 2, 4, and 5, employing a seven-layer subdivided independent sealed cavity structure, exhibit the best overall down-proof performance. The completely independent cavity design effectively limits the large-scale displacement of down during washing, rubbing, and squeezing, preventing concentrated down compression that could puncture the membrane layer. Product 6, due to its lower inner and outer layer down filling ratio, suffers from weakened down support within the cavity, resulting in a slight increase in down leakage after repeated deformation and squeezing. Product 1, with its larger single-cavity volume and wider down movement space, exhibits a higher probability of localized down leakage under long-term external force. In contrast, Products 7 and 8, with only single-layer and double-layer filling structures, lack a multi-level independent sealing and isolation system, failing to structurally constrain down migration. Relying solely on the nano-membrane for protection, their down-proof stability is significantly inferior to that of this invention. Overall test results indicate that the synergistic protective effect of the subdivided independent heat-sealed cavity structure and the nano-anti-down leakage membrane is the core key to achieving long-lasting low down leakage performance.

[0092] The three-layer gradient cavity structure designed in this invention relies on the composite thermal insulation effect of multiple static air interlayers, resulting in significantly better thermal insulation performance than single-layer and double-layer structures. Products 2 and 4 have a reasonable down filling ratio and good overall filling uniformity, providing excellent all-weather warmth retention. Products 3 and 6, by reducing the down filling density of the inner and outer buffer layers, have a reduced air insulation layer thickness, leading to a regular decrease in overall thermal insulation performance and a drop in clo value. Under the same total down filling level, the thermal insulation effect of the multi-cavity subdivided structure is significantly better than that of a conventional integral three-cavity structure, proving that cavity subdivision can refine the internal air insulation layers and effectively improve overall thermal resistance without significantly increasing the fabric surface weight.

[0093] The thermal resistance attenuation rate of the samples in this invention is generally controlled within the range of 5.8% to 6.2%, with products 2, 4, and 5 showing attenuation rates of only 5.8% and 5.9%, respectively. After washing, the cavity structure maintains high integrity, with no obvious clumping, aggregation, or migration of down, excellent loft retention, and extremely low attenuation of insulation performance. Product 1, with its basic three-cavity structure, has a larger cavity size, resulting in slight down aggregation during washing and a thermal resistance attenuation rate of 6.8%, slightly lower than the subdivided cavity structure. The durability of single-layer and double-layer filling structures decreases significantly; product 8 shows a thermal resistance attenuation rate of 10.3%, and product 7, with its single-layer structure lacking any cavity constraints, is prone to down migration and caking, resulting in a thermal resistance attenuation rate as high as 14.3%. Therefore, the multi-layer independent sealed cavity structure can effectively lock the down distribution, significantly improving insulation stability after multiple washes and completely overcoming the defect of a sharp decline in warmth retention after long-term use of traditional down products.

[0094] In summary, the down filling units (down filling and sealing modules) are stitched together according to an ergonomic pattern. Based on the human body's heat distribution patterns, the down jacket is divided into a core area, an active area, and an edge area: Core areas of the torso, chest, and back: densely arranged complete three-layer cavity units of R1, R2, and R3, with R2 down filling density of 62-75 g / m². 2 R1 down filling density 31-45g / m 2 R3 down filling density 18-38g / m 2 .

[0095] Elbow and armpit areas: Single-layer down filling unit, down density 31-45g / m² 2 .

[0096] Arms, neck, front placket, and hem edge areas: Double-layered down-filled units, with an outer cavity R1 and an inner cavity R3 formed by a partition layer. The down filling density of R1 is 31-45 g / m². 2 R3 down filling density 18-38g / m 2 .

[0097] The pinholes were covered with a 12 mm wide sealing strip under heat sealing conditions of 145℃, 8 s, and 0.20 MPa to obtain the finished down jacket.

[0098] The embodiments described above are merely examples of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a three-layer density down filling unit, characterized in that, The down filling unit includes at least one filling structure, which includes a full-coverage layer and two partitions located inside the full-coverage layer. The two partitions divide the interior of the full-coverage layer into an outer cavity R1, a middle cavity R2, and an inner cavity R3. The preparation method includes the following steps: Polyester-type thermoplastic polyurethane elastomer and polycaprolactone are dissolved in a mixed solvent containing hydrophobic fumed silica to form a spinning solution. The nano anti-fleece membrane is obtained by electrospinning and low-temperature thermal activation. The four layers of nano anti-down leakage membrane are cut to the shape of the designated cavity of the down jacket, and the edges are sealed along the outline and / or rib line, while retaining the down filling area to form three independent sealed cavities; Each independent sealed cavity is filled with down in a differentiated manner, with the down filling amount of the three cavities being R2 > R1 ≥ R3, and the filling port is sealed to obtain a three-layer density down filling unit.

2. The method for preparing the three-layer density down filling unit according to claim 1, characterized in that, Based on a total mass of 100%, the spinning solution comprises: 10wt%-16wt% polyester thermoplastic polyurethane elastomer, 1wt%-3wt% polycaprolactone, 0.3wt%-0.8wt% hydrophobic fumed silica, and the balance being a mixed solvent and dispersant of N,N-dimethylformamide and acetone.

3. The method for preparing the three-layer density down filling unit according to claim 1, characterized in that, The electrospinning process parameters are: feed rate 0.7-1.1 mL·h -1 · Single needle -1 The applied voltage is 17-20kV, the spinning distance is 17-20cm, the ambient temperature is 25±2℃, and the relative humidity is 36%-44%; the low-temperature thermal activation and setting temperature is 62-70℃, and the time is 2.5-3.5min.

4. The method for preparing the three-layer density down filling unit according to claim 1, characterized in that, Each partition consists of two layers of electrospun nano-anti-fleece diaphragms, with the central axis of the outer diaphragm connected to the full-coverage layer by hot melt adhesive, dividing the outer cavity R1 and the inner cavity R3 into two small cavities respectively.

5. The method for preparing the three-layer density down filling unit according to claim 4, characterized in that, The six layers of the nano-anti-down-leakage membrane are cut to the shape of the designated cavity of the down jacket, wherein the edges are sealed along the contour lines and / or rib lines, and the edges are sealed along the central axis of the first and second, fifth and sixth layers in each filling structure.

6. The method for preparing the three-layer density down filling unit according to claim 1, characterized in that, The edge sealing is at least one of adhesive coating or stitching. The width of the adhesive coating on the outline is 2.0-3.0 mm; the coating temperature is 145-160℃; the width of the adhesive strip on the center line or rib line is 1.8-2.2 mm; the coating thickness is 0.08-0.12 mm; and the width of the stitching is 0.5 mm-1.0 mm.

7. The method for preparing the three-layer density down filling unit according to claim 1, characterized in that, The mass ratio of the down filling amount of the three cavities is R1:R2:R3 = (0.5-0.6):1:(0.3-0.5).

8. A three-layer density down filling unit prepared by a method according to any one of claims 1-7.

9. The application of the three-layer density down filling unit as described in claim 8 in a down garment based on human body heat distribution, characterized in that, The down jacket has a core area at the chest and back, an active area at the elbows and armpits, and an edge area at the arms, neck, front, and hem. The core area holds the three-layer density down filling unit, the active area holds a single-layer down filling unit, and the edge area holds a double-layer down filling unit. The down filling unit is located between the outer and inner fabrics of the down jacket.

10. The application according to claim 9, characterized in that, The single-layer down filling unit has a filling structure in which down is filled in the entire layer, and the down filling amount is equal to the R1 filling amount; the double-layer down filling unit has a filling structure in which two independent cavities, an outer cavity R1 and an inner cavity R3, are formed in the entire layer through a partition layer, and the down filling amount is the same as that of the outer cavity R1 and the inner cavity R3 of the three-layer density down filling unit.