A high-concentration calcium chloride gradient purification process and device based on thermodynamic distortion control

The high-concentration calcium chloride gradient purification device, regulated by thermodynamic distortion, utilizes the salting-out force and ionic strength characteristics of high-concentration calcium chloride to solve the problem of removing sulfate and organic colloidal impurities in high-concentration calcium chloride solutions, thus achieving stable production of high-quality calcium chloride.

CN123102031APending Publication Date: 2026-11-17新疆湘润新材料科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611177844.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively remove sulfate and organic colloidal impurities when processing high-concentration calcium chloride solutions, leading to problems with product color and turbidity. Furthermore, conventional membrane separation and adsorption technologies fail at high concentrations, and equipment is prone to corrosion and caking.

Method used

A high-concentration calcium chloride gradient purification device based on thermodynamic distortion control is adopted, which includes a rigid skeleton filter layer and a flexible adsorption filter layer in a pressure vessel. Through gradient transition zone and constant temperature viscosity reduction treatment, the salting-out force and ionic strength characteristics of high-concentration calcium chloride are utilized to achieve crystallization desulfurization and deep decolorization.

Benefits of technology

It effectively removes sulfate and organic colloidal impurities, improves the quality of calcium chloride, avoids equipment corrosion and caking, and enables long-term stable production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102031A_ABST
    Figure CN123102031A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of chemical separation and solution purification technology, specifically relating to a high-concentration calcium chloride gradient purification process and device based on thermodynamic distortion control. The purification device of this invention includes a pressure vessel, inside which, from top to bottom, are arranged a primary interception zone, a gradient transition zone, and an adsorption filtration zone. The primary interception zone includes a fluid distributor and a rigid frame filter layer at its bottom. The gradient transition zone is formed by mixing titanium alloy fibers with basalt particles or fibers in a specific ratio. The adsorption filtration zone includes a flexible adsorption filter layer, with several layers of elastic support mesh arranged in the middle of the flexible adsorption filter layer along the height direction of the pressure vessel. The process of this invention uses the purification device of this invention, and its process steps strictly conform to and utilize the thermodynamic characteristics of this high-activity system to achieve the purpose of inducing crystallization for desulfurization, removing organic colloidal impurities of color and turbidity, and improving the quality of calcium chloride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical separation and solution purification technology, specifically relating to a high-concentration calcium chloride gradient purification process and device based on thermodynamic distortion control. It is particularly suitable for the deep and synergistic removal of trace amounts of sulfate, turbidity, and color in high-concentration calcium chloride systems with a mass concentration greater than 40%. Background Technology

[0002] Zero discharge of wastewater has become a routine requirement for industrial wastewater treatment, making the separation of impurities an important issue. The recovery of high-concentration (40%) calcium chloride from the separated wastewater into industrial-grade products has attracted attention from relevant enterprises. However, wastewater often contains a certain concentration of sulfate and organic matter, although the content is around 100-300 ppm, which affects the quality of calcium chloride. It also contains trace amounts of organic colloidal impurities that cause color and turbidity, impacting market sales. Current technologies for treating these impurities often employ membrane separation technologies (such as nanofiltration and reverse osmosis), porous adsorption technologies, or conventional fixed-bed filtration technologies.

[0003] However, existing technologies generally have a fatal theoretical blind spot: their process designs all rely on engineering experience with low concentrations, such as 10%-30% calcium chloride systems, and completely lack a deep understanding of the thermodynamic nature of ultra-high concentration systems with a mass concentration of ≥40%.

[0004] Through long-term research, the inventors discovered that calcium chloride solutions with a concentration greater than 40% cross the physical boundaries of conventional electrolyte solutions, belonging to an extremely non-ideal ultra-high ionic strength system (I>18 mol / kg). Precise calculations based on the Pitzer activity coefficient model with temperature correction throughout the entire process show that the average ionic activity coefficient γ±143 of the 40% calcium chloride system represents a nearly 20-fold nonlinear abrupt change compared to the 30% system (γ±≈7.03). This extreme activity surge directly leads to three major thermodynamic distortions in the system. Osmotic pressure distortion: the estimated osmotic pressure of the 40% system is as high as >230 atm, theoretically rendering any conventional membrane separation technology physically ineffective under this condition. Crystallization distortion: The extremely high effective activity of calcium ions leads to an extreme enhancement of the salting-out effect, forcing trace amounts of NaCl to precipitate. Simultaneously, the fine calcium sulfate exhibits colloidal nucleation and directional growth tendencies, causing the porous structure of the adsorbent to break down under the stress of the calcium sulfate crystals. This results in adsorbent breakage, shortened adsorbent lifespan, and the entry of small particles into the solution, increasing turbidity. Rheological and corrosion distortion: Fluid viscosity and corrosivity increase exponentially. Industrial-grade titanium (TA2) is unable to withstand the corrosion of the solution, especially at temperatures above 80°C during concentration, significantly reducing the equipment's lifespan. When using conventional flexible filter beds, under the aforementioned extreme activity-driven high pressure differential and microcrystalline expansion stress, the flexible fiber bed will be rapidly compacted and agglomerated, becoming a non-permeable, dense, hard plate. Forced cooling to reduce viscosity will lead to further crystal precipitation, further accelerating agglomeration and forming calcium chloride hexahydrate crystals, causing system failure.

[0005] Therefore, there is an urgent need for a new purification process and device specifically designed for the thermodynamic distortion characteristics of calcium chloride systems with a concentration of 40% or higher and a temperature of 60-80°C or higher.

[0006] In view of this, the present invention is hereby proposed. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art and propose a high-concentration calcium chloride gradient purification process and device based on thermodynamic distortion control. Extreme activity surges can directly lead to three major thermodynamic distortions in high-concentration calcium chloride systems with a concentration of 40% or higher.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: On the one hand, the present invention provides a high-concentration calcium chloride gradient purification device based on thermodynamic distortion control, including a pressure vessel, wherein the interior of the pressure vessel is provided with a primary interception zone, a gradient transition zone, and an adsorption filtration zone arranged sequentially from top to bottom; The primary interception zone includes a fluid distributor and a rigid skeleton filter layer located at its bottom; The gradient transition zone is formed by mixing titanium alloy fibers with basalt particles or fibers in a specific ratio. The adsorption filtration zone includes a flexible adsorption filtration layer, and several layers of elastic support mesh are provided in the middle of the flexible adsorption filtration layer along the height direction of the pressure vessel.

[0009] Furthermore, the rigid skeleton filter layer includes at least one titanium alloy fiber layer, which contains multiple pores with a porosity controlled at 30% to 40%.

[0010] Furthermore, the titanium alloy fiber layer is formed by stacking corrugated plates or disc-shaped plates pressed from titanium alloy fibers.

[0011] Furthermore, the titanium alloy fiber is a titanium alloy fiber with calcium active sites loaded on its surface.

[0012] Furthermore, the gradient transition zone is formed by mixing titanium alloy fiber fragments with basalt particles or fibers in a manner that proceeds from bottom to top, with the volume content of titanium alloy fiber fragments decreasing from 80% to 0% and the volume content of basalt particles or fibers increasing from 20% to 100%.

[0013] Furthermore, the height of the gradient transition zone is 10% to 20% of the sum of the heights of the rigid skeleton filter layer and the adsorption filter zone.

[0014] Furthermore, the flexible adsorption filter layer is made of heat-resistant polyester fiber or basalt fiber.

[0015] Preferably, the heat-resistant polyester fiber can be a comet-shaped polyester fiber filter media, a polyester fiber bundle filter media, or a polyester filament cotton tied fiber ball, etc.

[0016] On the other hand, the present invention provides a high-concentration calcium chloride gradient purification process based on thermodynamic distortion control, comprising the following steps: Step 1, Constant temperature and viscosity reduction feeding: Heat the calcium chloride solution with a mass concentration greater than 40% to 85~90℃, and then introduce it into the high concentration calcium chloride gradient purification device as described above. Step 2, Sodium removal by salt effect and sulfur removal by surface ion induction: Calcium chloride solution is evenly introduced into the rigid skeleton filter layer through the nozzle of the fluid distributor, and enters the gradient transition zone after primary filtration. Step 3, Deep Decolorization and Turbidity Reduction: After filtration, the material enters a flexible adsorption filter layer, where it is deeply intercepted and adsorbed by surface charges to retain organic macromolecules and residual suspended matter that cause color.

[0017] During the constant temperature operation at 85~90℃, the rigid frame filter layer always maintains its initial porosity, preventing the overall bed from becoming dense and compacted, and ultimately obtaining a high-quality purified calcium chloride solution.

[0018] Compared with the prior art, the present invention has the following beneficial effects: Based on the understanding of thermodynamic distortion in the Pitzer model, this invention accurately identifies the separation mechanism of extremely difficult-to-handle impurities. It abandons empirical extrapolation for low concentrations and, for the first time, quantifies the extreme characteristic of an activity coefficient as high as 143 in a 40% system based on Pitzer model calculations.

[0019] The process of this invention employs the purification device of this invention, and its process steps strictly conform to and utilize the thermodynamic characteristics of the high-activity system. The aim is to induce crystallization for desulfurization, remove organic colloidal impurities that contribute to color and turbidity, and improve the quality of calcium chloride. Specifically, the salting-out force of the system (high-concentration calcium chloride with a concentration greater than 40%) is used to remove trace impurities. The local high-activity micro-regions at the fiber interface induce the growth of fine CaSO4 particles into large particles, upgrading the traditional "physical interception" to "thermodynamically guided phase change separation." This overcomes the taboo of ">230 atm osmotic pressure," establishing the inevitable path of non-membrane separation. Based on ionic strength theory, the feasibility of using membrane separation in high-concentration systems is eliminated from the source. An innovative fluid-permeable rigid + flexible coupled bed is adopted, which is the only feasible engineering path conforming to the physical laws of high-concentration systems, completely avoiding unnecessary waste of equipment investment. This invention uniquely employs a synergistic correction mechanism of "85~90℃ low viscosity window" and "rigid + flexible coupling anti-densification."

[0020] Meanwhile, to address the challenges of microcrystallization caused by high activity and "densification and compaction" resulting from high viscosity, this invention proposes a dual correction mechanism: First, calculations using Pitzer temperature correction show that strictly controlling the operating temperature between 85 and 90°C can effectively reduce the system's activity coefficient and viscosity by about 20%, giving the fluid the initial kinetic energy to penetrate the bed, and avoiding excessive corrosion and a sharp increase in energy consumption at higher temperatures. Secondly, for hard crystals that still exhibit high-activity-driven explosive growth at 85-90℃, a unique "rigid titanium alloy skeleton + flexible basalt layer" structure was developed. The rigid titanium layer provides absolutely incompressible physical support, forcefully resisting the crystallization expansion stress driven by extreme activity; the resistant and flexible fiber layer provides high specific surface area induction sites and a deep decolorization network. The two are perfectly joined through a gradient transition zone, completely eliminating channeling short-circuiting that is prone to occur in high-viscosity fluids, and enabling long-cycle, non-disassembly-washing continuous production of high-quality calcium chloride solutions. Attached Figure Description

[0021] The accompanying drawings are incorporated in and form part of this specification, and together with the description serve to explain the principles of the invention.

[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0023] Figure 1 This is a schematic diagram of the high-concentration calcium chloride gradient purification device of the present invention; Figure 2 This is a flowchart of the high-concentration calcium chloride gradient purification process of the present invention; Figure 3 The image shows the experimental results after removing the titanium alloy fibers from the gradient filtration zone following filtration using the device of the present invention.

[0024] Wherein: 1 is the pressure vessel; 11 is the primary interception zone; 12 is the gradient transition zone; 13 is the adsorption filtration zone; 111 is the fluid distributor; 112 is the rigid skeleton filter layer; 131 is the elastic support net; 132 is the flexible adsorption filtration layer; 2 is the feed inlet; 3 is the discharge outlet. Detailed Implementation

[0025] Exemplary embodiments will now be described in detail. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples consistent with some aspects of the invention as detailed in the appended claims.

[0026] Example 1 Please see Figure 1 This invention provides a high-concentration calcium chloride gradient purification device based on thermodynamic distortion control, including a pressure vessel 1. The pressure vessel 1 has a primary interception zone 11, a gradient transition zone 12, and an adsorption filtration zone 13 arranged sequentially from top to bottom inside the pressure vessel 1. The pressure vessel 1 has an inlet 2 at the top and an outlet 3 at the bottom. The primary interception zone 11 includes a fluid distributor 111 and a rigid skeleton filter layer 112 located at its bottom; The gradient transition zone 12 is formed by mixing titanium alloy fibers with basalt particles or fibers in a specific ratio. The adsorption filtration zone 13 includes a flexible adsorption filtration layer 132, and several layers of elastic support nets 131 are provided at intervals along the height direction of the pressure vessel 1 in the middle of the flexible adsorption filtration layer 132.

[0027] Furthermore, the flexible adsorption filter layer 132 is made of heat-resistant polyester fiber or basalt fiber.

[0028] The elastic support net 131 can be a single layer disposed in the middle of the flexible adsorption filter layer 132, or it can be two or more layers disposed at intervals in the middle of the flexible adsorption filter layer 132.

[0029] In this invention, the elastic support mesh 131 is a porous plate made of titanium alloy with a pore size of 3~10mm, and the total throughput of its pores is matched with the pressure and flow rate of the entire device.

[0030] like Figure 1 As shown, the total height of the adsorption filtration zone 13 is 800~1200mm (1200mm is selected in this embodiment). A titanium alloy corrugated mesh is used as the elastic support mesh 131 in the middle, with a height of 150mm. Heat-resistant polyester fiber (comet-type polyester fiber filter media, polyester fiber bundle filter media, or polyester filament cotton tied fiber balls, etc.) or basalt fiber is laid on the elastic support mesh 131. The elastic support mesh 131 absorbs the volume expansion stress caused by crystal accumulation in the flexible adsorption layer through elastic deformation, maintaining a constant porosity within the layer.

[0031] In this invention, the rigid skeleton filter layer 112 includes at least one titanium alloy fiber layer, which contains a plurality of compressible rigid pores with a porosity controlled at 30% to 40%.

[0032] The rigid skeleton filter layer 112, whether it is a single titanium alloy fiber layer or two or more layers, has a porosity controlled between 30% and 40%. The titanium alloy fiber layer is made of corrugated plates or disc-shaped plates pressed from titanium alloy fibers and has compressible rigid pores to provide absolute support and serve as a primary crystallization interception zone.

[0033] Preferably, the rigid skeleton filter layer 112 has a height of 500 mm. It should be noted that the rigid skeleton filter layer 112 can be made by sintering Ti-O-Ca rivet-modified titanium alloy fibers into corrugated plate modules and stacking them, with a porosity controlled at 35%. The thickness deformation rate of this rigid skeleton filter layer 112 is <3% under a pressure difference of 0.6 MPa. Alternatively, it can be made by sintering unmodified titanium alloy fibers into corrugated plate modules and stacking them. Here, titanium alloy fibers are titanium wires processed from titanium material.

[0034] Specifically, the pressure vessel 1 of the present invention is made of a titanium alloy containing molybdenum and nickel to form its shell.

[0035] In this invention, the fluid distributor 111 is a standard inverted umbrella-shaped distributor, used for uniformly spraying liquid material; Furthermore, the gradient transition zone 12 is formed by mixing titanium alloy fiber fragments with basalt particles or fibers in a manner that proceeds from bottom to top, with the volume content of titanium alloy fiber fragments decreasing from 80% to 0% and the volume content of basalt particles or fibers increasing from 20% to 100%.

[0036] Furthermore, the gradient transition zone 12 has a height of 200 mm, with the lower layer being a mixture of 80% titanium fiber fragments and 20% basalt short fibers, and the upper layer being 100% pure basalt short fibers, forming a smooth transition in pore size from approximately 50 μm to 10 μm; or the lower layer being a mixture of 80% titanium fiber fragments and 20% basalt particles, and the upper layer being 100% pure basalt particles, forming a smooth transition in pore size from approximately 50 μm to 10 μm; or the lower layer being a mixture of 80% titanium fiber fragments and 20% basalt short fibers, and the upper layer being 100% pure basalt particles, forming a smooth transition in pore size from approximately 50 μm to 10 μm.

[0037] Operating Results: After 72 hours of continuous operation, the outlet calcium chloride solution was clear and transparent. Test Indicators: NaCl removal rate >95%, sulfate content reduced to 38 ppm, turbidity <0.5 NTU, color <5 times. The system pressure drop stabilized at 0.18 MPa. Upon shutdown and inspection of the bed, no internal compaction or densification was observed, and the titanium alloy skeleton layer showed no deformation.

[0038] Example 2 This invention also provides a high-concentration calcium chloride gradient purification process based on thermodynamic distortion control, targeting the raw material to be treated: a calcium chloride solution, a byproduct of a manufacturer's production, with a mass concentration of 42% and a viscous state at 25°C. It contains 0.5% NaCl, 289 ppm sulfate, a turbidity of 6.5 NTU, and a color of 20 times.

[0039] Includes the following steps: Step 1, Constant Temperature Viscosity Reduction Feeding: The calcium chloride solution with a mass concentration of 42% is heated to the critical low viscosity window of 88℃. At this time, the viscosity of the solution decreases significantly and it has good fluidity. Then, it is pumped into the high-concentration calcium chloride gradient purification device as described above, with an initial pressure drop of 0.15MPa. Step 2, Sodium removal by salt effect and sulfur removal by surface ion: Calcium chloride solution is uniformly introduced into the rigid skeleton filter layer 112 from top to bottom through the fluid distributor 111 at an empty tower flow rate of 0.2 m / h. The local ion effect generated by the calcium active sites on the fiber surface is used to induce the in-situ growth of fine colloidal calcium sulfate into coarse crystals and anchor them. After primary filtration, it enters the gradient transition zone 12. It should be noted that "coarse" refers to crystal growth, and "anchoring" refers to the crystals growing large and being trapped in the pores. The purpose of the purification device in this application is to remove sulfate ions, allowing the sulfate ions to transform into calcium sulfate and form large crystals, which are then trapped in the filter media, thereby achieving the removal of sulfate ions.

[0040] Step 3, Deep Decolorization and Turbidity Reduction: After filtration, the material enters the flexible adsorption filter layer 132, where it is deeply intercepted and adsorbed by surface charge to retain organic macromolecules and residual suspended matter that cause color.

[0041] Example 3 This invention also provides a high-concentration calcium chloride gradient purification process based on thermodynamic distortion control. The feed solution is a calcium chloride solution with a mass concentration of 40% that has been concentrated at high temperature by a certain factory. The raw material is collected in solution form at about 90°C. The sample is taken, cooled and allowed to stand to produce a large amount of crystals.

[0042] Includes the following steps: Step 1, Constant temperature viscosity reduction feeding: The calcium chloride solution with a mass concentration of 40% is heated to the critical low viscosity window of 87°C, and then pumped into the high concentration calcium chloride gradient purification device as described above. Step 2, Sodium removal by salt effect and sulfur removal by surface ion-induced reaction: The calcium chloride solution is uniformly introduced into the rigid skeleton filter layer 112 (using ordinary titanium alloy fiber (i.e., unmodified)) through the spray nozzle of the fluid distributor 111, and enters the gradient transition zone 12 after primary filtration. Step 3, Deep Decolorization and Turbidity Reduction: After filtration, the material enters the flexible adsorption filter layer 132, where it is deeply intercepted and adsorbed by surface charge to retain organic macromolecules and residual suspended matter that cause color.

[0043] Example 4 This invention also provides a high-concentration calcium chloride gradient purification process based on thermodynamic distortion control. The feed solution is a calcium chloride solution with a mass concentration of 41% that has been concentrated at high temperature by a certain factory. The raw material is collected in solution form at about 90°C. The sample is taken, cooled and allowed to stand to produce a large amount of crystals.

[0044] Includes the following steps: Step 1, Constant temperature viscosity reduction feeding: The calcium chloride solution with a mass concentration of 41% is heated to the critical low viscosity window of 90°C, and then pumped into the high concentration calcium chloride gradient purification device as described above. Step 2, Sodium removal by salt effect and sulfur removal by surface ion induction: Calcium chloride solution is uniformly introduced into the rigid skeleton filter layer 112 through the spray nozzle of the fluid distributor 111. The local ion effect generated by the calcium active sites on the fiber surface is used to induce the in-situ growth of fine colloidal calcium sulfate into coarse crystals and anchor them. After primary filtration, it enters the gradient transition zone 12. Step 3, Deep Decolorization and Turbidity Reduction: After filtration, the material enters the flexible adsorption filter layer 132, where it is deeply intercepted and adsorbed by surface charge to retain organic macromolecules and residual suspended matter that cause color.

[0045] To demonstrate the purification effect of the device of this invention on calcium sulfate, this invention utilizes water backwashing to sample unmodified titanium alloy fibers for testing. The XRD results of the cleaned fiber material are as follows: Figure 3 As shown, calcium sulfate crystal peaks appear (e.g.) Figure 3 The purple lines demonstrate the effectiveness of titanium alloy fibers in purifying sulfate ions.

[0046] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.

[0047] It should be understood that the present invention is not limited to the content already described above, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A high-concentration calcium chloride gradient purification device based on thermodynamic distortion control, characterized in that, It includes a pressure vessel (1), and the interior of the pressure vessel (1) is provided with a primary interception zone (11), a gradient transition zone (12), and an adsorption filtration zone (13) from top to bottom. The primary interception zone (11) includes a fluid distributor (111) and a rigid skeleton filter layer (112) located at its bottom. The gradient transition zone (12) is formed by mixing titanium alloy fiber fragments with basalt particles or fibers in a specific ratio; The adsorption filtration zone (13) includes a flexible adsorption filtration layer (132), and several layers of elastic support net (131) are provided in the middle of the flexible adsorption filtration layer (132) along the height direction of the pressure vessel (1).

2. The high-concentration calcium chloride gradient purification device according to claim 1, characterized in that, The rigid skeleton filter layer (112) includes at least one titanium alloy fiber layer, which contains multiple pores and has a porosity controlled at 30% to 40%.

3. The high-concentration calcium chloride gradient purification device according to claim 2, characterized in that, The titanium alloy fiber layer is formed by stacking corrugated plates or disc-shaped plates made of titanium alloy fibers.

4. The high-concentration calcium chloride gradient purification device according to claim 3, characterized in that, The titanium alloy fiber is a titanium alloy fiber with calcium active sites loaded on its surface.

5. The high-concentration calcium chloride gradient purification device according to claim 1, characterized in that, The gradient transition zone (12) is formed by mixing titanium alloy fiber fragments with basalt particles or fibers in a bottom-up manner, with the volume content of titanium alloy fiber fragments decreasing from 80% to 0% and the volume content of basalt particles or fibers increasing from 20% to 100%.

6. The high-concentration calcium chloride gradient purification device according to claim 1, characterized in that, The height of the gradient transition zone (12) is 10% to 20% of the sum of the heights of the rigid skeleton filter layer (112), the adsorption filter zone (13), and the gradient transition zone (12).

7. The high-concentration calcium chloride gradient purification device according to claim 1, characterized in that, The flexible adsorption filter layer (132) is made of heat-resistant polyester fiber or basalt fiber.

8. A high-concentration calcium chloride gradient purification process based on thermodynamic distortion control, characterized in that, Includes the following steps: Step 1, constant temperature and viscosity reduction feeding: heat the calcium chloride solution with a mass concentration greater than 40% to 85~90℃, and then introduce it into the high concentration calcium chloride gradient purification device according to any one of claims 1 to 7. Step 2, Sodium removal by salt effect and sulfur removal by surface ion induction: Calcium chloride solution is uniformly introduced into the rigid skeleton filter layer (112) through the nozzle of the fluid distributor (111), and enters the gradient transition zone (12) after primary filtration. Step 3, Deep decolorization and turbidity reduction: After filtration, the filter enters the flexible adsorption filter layer (132), where it intercepts organic macromolecules and residual suspended matter that cause color through deep interception and surface charge adsorption.