Polysulfone hollow fiber membranes, their preparation methods and applications

By optimizing the internal surface characteristic parameters of polysulfone hollow fiber membranes, the problems of membrane pore blockage and shear force damage were solved, achieving efficient protein and cell retention and metabolite discharge, and obtaining high-concentration protein feed solutions.

CN123102182APending Publication Date: 2026-11-17HANGZHOU COBETTER FILTRATION EQUIPMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611280442.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polysulfone hollow fiber membranes are difficult to effectively obtain high concentrations of protein solution in ATF perfusion culture, mainly because the adsorption of proteins and cells on the membrane surface leads to membrane pore blockage and shear force damage, which affects the efficiency of cell culture and protein expression.

Method used

By adjusting the internal surface characteristic parameters of hollow fiber membranes, including initial water contact angle, pore area ratio, SEM average width of strip fibers, and distance between adjacent strip fibers, the hydrophilicity and pressure resistance of the membrane can be optimized to reduce protein and cell adsorption and shear force damage.

Benefits of technology

It achieves efficient retention of IgG molecules and cells, reduces membrane pore blockage, ensures timely discharge of metabolites, reduces shear force damage to cells and proteins, and obtains high-concentration protein feed solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102182A_ABST
    Figure CN123102182A_ABST
Patent Text Reader

Abstract

This application provides a polysulfone hollow fiber membrane, its preparation method, and its application. The polysulfone hollow fiber membrane of this application comprises a main body with an inner cavity. The side of the main body facing the inner cavity is the inner surface, and the side of the main body away from the inner cavity is the outer surface. The hollow fiber membrane has an IgG retention efficiency of ≥98%; the pore area ratio of the inner surface is 2%-15%; the initial water contact angle of the inner surface is 55°-80°; the inner surface contains multiple strip-shaped fibers, the average SEM width of the strip-shaped fibers is 70nm-200nm, and the average SEM distance between two adjacent strip-shaped fibers is 80nm-150nm. Based on the combined effect of the above parameters, the polysulfone hollow fiber membrane of this application can be used for ATF perfusion culture, and can obtain a high concentration of protein solution when used for ATF perfusion culture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of membrane material technology, and in particular relates to a polysulfone hollow fiber membrane, its preparation method and application. Background Technology

[0002] Biologics are a class of therapeutic drugs derived from living organisms or prepared through biotechnology, primarily used to treat immune-related diseases and tumors. Compared to traditional chemical drugs, biologics are widely used due to their stronger targeting and more precise efficacy. The active ingredients of biologics (such as proteins) are mainly obtained through cell amplification and expression, followed by a series of purification steps. Cell amplification and expression are the primary and crucial steps in obtaining proteins.

[0003] Currently, alternating tangential flow (ATF) perfusion culture is an advanced process for achieving efficient cell expansion and expression, with the perfusion membrane being its core component. ATF perfusion membranes are mostly made of polymer membrane materials. Due to the excellent chemical stability and biocompatibility of polysulfone polymers, as well as their superior acid and alkali resistance, temperature resistance, and high mechanical strength, and the high specific surface area of ​​hollow fiber membranes, polysulfone-based hollow fiber membranes are the preferred choice for ATF perfusion membranes.

[0004] Since obtaining high-concentration protein during the cell expansion and expression stage can eliminate the need for subsequent concentration steps, it is beneficial to obtain high-concentration protein solutions more efficiently. Therefore, in order to obtain high-concentration protein solutions during the cell expansion and expression stage, it is urgent to develop a hollow fiber membrane for ATF perfusion that can obtain high-concentration protein solutions to meet the growing market demand for high-concentration biopharmaceuticals. Summary of the Invention

[0005] The purpose of this application is to provide a polysulfone hollow fiber membrane, its preparation method and application. By controlling the IgG retention efficiency of the hollow fiber membrane, the pore area ratio of the inner surface, the initial water contact angle of the inner surface, the SEM average width of the strip fibers contained in the inner surface, and the SEM average distance between adjacent strip fibers, the aim is to solve the technical problem of how to obtain high protein concentration when the polysulfone hollow fiber membrane is used for ATF perfusion culture.

[0006] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows:

[0007] In a first aspect, this application provides a polysulfone hollow fiber membrane, comprising a body having an inner cavity, the side of the body facing the inner cavity being the inner surface, and the side of the body away from the inner cavity being the outer surface. The polysulfone hollow fiber membrane has the following characteristics: (1) the hollow fiber membrane has a IgG retention efficiency ≥98%; (2) the pore area ratio of the inner surface is 2%-15%; (3) the initial water contact angle of the inner surface is 55°-80°; (4) the inner surface contains multiple strip fibers, the average SEM width of the strip fibers is 70nm-200nm, and the average SEM distance between two adjacent strip fibers is 80nm-150nm.

[0008] ATF perfusion devices generally include a bioreactor, a hollow fiber membrane module, and a diaphragm pump. Material in the bioreactor flows into the hollow fiber membrane module under the downward force of the diaphragm pump. The hollow fiber membrane filters the material in a tangential flow manner (the liquid flow direction is perpendicular to the filtration direction). Smaller substances (such as metabolites from cell expansion and protein expression, nutrient solutions, etc.) pass through the pores on the inner surface of the hollow fiber membrane, then through the membrane interior and out through the outer surface. Larger substances (such as cells and other macromolecules) are retained. The retained material is then returned to the bioreactor by the reverse force of the diaphragm pump. By continuously alternating the direction of the diaphragm pump's force, metabolites during the perfusion culture process are continuously discharged. In this invention, the hollow fiber membrane used for perfusion culture retains proteins and cells on its inner surface to obtain a high-concentration protein solution. Specifically:

[0009] First, we control the initial water contact angle of the inner surface of the polysulfone hollow fiber membrane to be 55°-80°. For example, the initial water contact angle of the inner surface can be any single value or a range between any two values, such as 55°, 56°, 58°, 59°, 60°, 62°, 64°, 65°, 68°, 70°, 72°, 74°, 75°, 76°, 78°, or 80°. This means the inner surface of the hollow fiber membrane of this invention has relatively good hydrophilicity, and when protein molecules pass through the inner surface of the hollow fiber membrane, they are not... Proteins are easily adsorbed onto the inner surface of hollow fiber membranes. Even if there is adsorption between protein molecules and the inner surface, the binding force between the protein molecules and the inner surface is very weak. At the same time, when the inner surface of the hollow fiber membrane has relatively good hydrophilicity, even if cells are adsorbed onto the inner surface, the binding force between them and the inner surface is relatively weak. Under a small shear force, cells and proteins can be peeled off from the inner surface. In other words, the inner surface with good hydrophilicity reduces the adsorption between proteins and cells and the inner surface from the source, that is, it reduces the "anchoring" between proteins and cells and the inner surface. However, if the initial water contact angle of the inner surface of the hollow fiber membrane is large, such as greater than 85°, the inner surface of the hollow fiber membrane has poor hydrophilicity and easily adsorbs proteins in the feed solution. Moreover, the binding force between the adsorbed proteins and the inner surface is large, requiring a large shear force to peel the proteins off the inner surface of the hollow fiber membrane. The large shear force can easily damage the proteins and cells, affecting the normal progress of cell culture and protein expression, making it difficult to obtain a high concentration of protein feed solution. Furthermore, the proteins adsorbed on the inner surface can easily clog the membrane pores on the inner surface, thus preventing the continuous discharge of metabolites and making perfusion culture impossible.

[0010] The initial water contact angle of the inner surface of the hollow fiber membrane can be measured using water as the test solution and a contact angle meter. The contact angle is determined by the moment 10100 microliters of water is uniformly dropped onto the inner surface of the hollow fiber membrane (typically within 0.4 seconds), forming a regular contact angle. Multiple tests are conducted, and the average value is taken. The test temperature is 20℃-25℃. Of course, those skilled in the art can obtain the above parameters through other testing methods; the above testing methods are for reference only.

[0011] Secondly, the polysulfone hollow fiber membranes of this application exhibit IgG retention efficiencies as high as 98%, 98.5%, or 99%, or even above 99%. The IgG retention efficiency of the hollow fiber membranes of this invention refers to the test results on the third day after the start of protein expression in ATF perfusion culture (typically, ATF perfusion culture first performs cell expansion, then simultaneously performs cell expansion and protein expression). In other words, as protein expression continues, the protein retention efficiency of the hollow fiber membrane is ≥98%, indicating that protein retention mainly occurs on the inner surface of the hollow fiber membrane, rather than throughout the entire membrane (this is because if protein retention occurs inside the hollow fiber membrane, the protein will block the interior of the membrane, preventing the perfusion culture from continuing). Since the size of IgG molecules is around 10 nm, the effective pore size of the inner surface pores of the hollow fiber membrane (the minimum pore size after superimposing the pores on the cross-section near the inner surface) is very small. Correspondingly, the inner surface with this effective pore size can also effectively retain cells. Even if cells are embedded in the membrane pores of the inner surface, the embedding depth is very small. Combined with the relatively weak binding force between the cells and the inner surface due to its good hydrophilicity, the cells can return to the reaction solution under very small shear forces. If the hollow fiber membrane has a low IgG retention efficiency, for example, below 98%, then more protein permeates, resulting in protein loss.

[0012] The method for testing the IgG retention efficiency is as follows: On the third day after protein expression begins in ATF perfusion culture, the stock solution in the bioreactor and the permeate solution through the hollow fiber membrane module are taken, and the absorbance at UV280nm is measured respectively, denoted as A. 透过 and A 原液 Then the IgG retention efficiency = 1 - A 透过 / A 原液 .

[0013] The pore area ratio of the inner surface of the hollow fiber membrane in this application embodiment is 2%-15%; for example, the pore area ratio of the inner surface can be any one value or a range formed between any two values ​​such as 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%. In other words, the hollow fiber membrane has a certain area of ​​pores on its inner surface. Combined with the hollow fiber membrane's IgG retention efficiency of ≥98%, the number of pores on the inner surface of the hollow fiber membrane is slightly higher, meaning there are more pathways for the excretion of metabolites, which is beneficial for their timely removal. Simultaneously, the presence of pores on the inner surface provides entry points for shear force removal of the filter cake layer formed around the pores. Correspondingly, the slightly higher number of pores on the inner surface provides more entry points, preventing the formed filter cake layer from compacting before returning to the solution. Furthermore, the pore area ratio within this range helps ensure the compressive strength of the inner surface. Moreover, the slightly higher number of pores per unit area of ​​the inner surface results in a relatively low single-pore load and good long-term operational stability. If the pore area ratio of the inner surface is too large, the membrane pores will be too densely distributed, and the compressive strength of the inner surface will be low, which is not conducive to the continuous perfusion culture. If the pore area ratio of the inner surface is too small, there will be very few channels on the inner surface for the discharge of metabolites, and the metabolites cannot be discharged in time, which is not conducive to the continuous cell culture and protein expression.

[0014] The porosity of the inner surface is the ratio of the sum of the areas of all pores on the inner surface to the area of ​​the inner surface. It can be measured using ImageJ. Specifically,

[0015] ① Open the image and adjust the pixels; Open the image (electron microscope image of the inner surface) in the image processing software ImageJ. File>Open, select the electron microscope image and click Open, then select Image>Type>8-bit to convert the image to an 8-bit grayscale image;

[0016] ② Measure the porosity of the inner surface; select Image>Adjust>Threshold, and adjust the fill ratio of the membrane pores in the dialog box that appears so that all the membrane pores are filled with color. The percentage displayed in the dialog box is the porosity.

[0017] Finally, by adjusting the SEM average width of the strip fibers on the inner surface of the hollow fiber membrane and the SEM average distance between adjacent strip fibers, for example, the SEM average width of the strip fibers on the inner surface is 70nm-200nm; exemplarily, the SEM average width of the strip fibers on the inner surface can be any single value or a range formed between any two values, such as 70nm, 75nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm. The SEM average distance between two adjacent strip fibers is 80nm-150nm; exemplarily, the SEM average distance between two adjacent strip fibers on the inner surface can be any single value or a range formed between any two values, such as 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm. Because the hollow fiber membrane of the present invention is composed of polysulfone polymers, it has good strength. Combined with the 2%-15% pore area ratio of the inner surface of the hollow fiber membrane, the small effective membrane pores on the inner surface, the SEM average width of the strip fibers in a specific range, and the SEM average distance between adjacent strip fibers, the inner surface of the hollow fiber membrane has good compressive strength, which enables continuous perfusion culture.Meanwhile, the average SEM width of the strip-like fibers is relatively small. When cells are adsorbed onto the strip-like fibers, the contact area between the cells and the fibers is small. Combined with the weak binding force between the cells and the inner surface, only a small shear force is needed to detach the cells from the strip-like fibers. Similarly, when proteins are adsorbed onto the small strip-like fibers, even if the proteins cover the entire fiber, the total area of ​​protein on the fiber is relatively small. The weak binding force between the bound proteins and the inner surface also requires only a relatively small shear force to detach the proteins from the fibers. In other words, within this range of strip-like fiber width, both proteins and cells adsorbed onto the fibers can be detached from them with relatively small shear force. The average SEM distance between adjacent strip-like fibers is also relatively small. When proteins or cells are adsorbed in the middle of the fibers, only a relatively small shear force is needed. The shear force is sufficient to separate cells and proteins between the strip fibers. If the average SEM width of the strip fibers is too low, the compressive strength of the corresponding inner surface will be low, which is not conducive to the continuous perfusion culture. If the average SEM width of the strip fibers is too high, there is a risk of protein forming a large filter cake layer. If the average SEM distance between adjacent strip fibers is too small, the number of pores on the corresponding inner surface will be too small (the pores on the inner surface are located between adjacent strip fibers), which is not conducive to the timely discharge of metabolites. If the average SEM distance between adjacent strip fibers is too large, the compressive strength of the corresponding inner surface will be low, and there is a risk of forming a large filter cake layer in the area between adjacent strip fibers. In other words, whether the average SEM width of the strip fibers is too low or too high, or the average SEM distance between adjacent strip fibers is too large or too small, a high concentration of protein solution cannot be obtained.

[0018] During the membrane preparation process, in the direction perpendicular to the membrane thickness (the membrane of the present invention is a hollow fiber membrane, which is perpendicular to the radial direction), its various characteristics, such as the width of the strip fibers on the inner surface, the distance between adjacent strip fibers, and the pore size of the pores on the inner surface, are roughly uniform and basically consistent. Therefore, a portion of the corresponding plane can be used as the measurement object.

[0019] Strip-like fibers are a general term for fibers that appear as protrusions on the inner surface of hollow fiber membranes in electron micrographs (see attached image). Figure 1 As shown in the box in the middle, the average width of its strip-like fibers in the SEM is determined by selecting a certain area of ​​the inner surface from the electron micrograph (enough to measure the diameter of the strip-like fibers), for example, 4 μm. 2 (2μm*2μm), 1μm 2The area (1μm*1μm) depends on the actual situation. The width of the strip fiber in the circumferential direction of the hollow fiber membrane is then measured using appropriate computer software (such as Matlab, NIS-Elements, etc.) or manually. Preferably, the width of more than 10 strip fibers is measured, and the average value is calculated as the SEM average width of the strip fiber. If the width of a single strip fiber is inconsistent, the width at different locations of a single strip fiber can be measured and the average value taken as the width of that single strip fiber. The SEM average distance between adjacent strip fibers refers to the distance between adjacent strip fibers in the circumferential direction of the hollow fiber membrane, and its measurement method is similar to that of the SEM average width of the strip fiber.

[0020] It is evident that when cells adsorb onto the strip-shaped fibers on the inner surface or the areas between the strip-shaped fibers, the contact area is small and the binding force is weak. Under relatively small shear forces, the cells can return to the feed solution, and the transmembrane pressure difference is insufficient to compact the cells on the inner surface to form a dense filter cake layer. Similarly, when proteins adsorb onto the strip-shaped fibers on the inner surface or the areas between the strip-shaped fibers, the binding force between the protein and the inner surface is very weak. Under relatively small shear forces, the protein can be detached from the inner surface. Even if a filter cake layer covering the strip-shaped fibers or the areas between the strip-shaped fibers is formed, the area of ​​the formed filter cake layer is small, and the binding force between the protein and the inner surface is very weak. Therefore, under relatively small shear forces, the protein can also return to the feed solution. In the feed solution, the synergistic effect of the hydrophilic inner surface, the specific width of the strip fibers, and the specific distance between adjacent strip fibers ensures that a filter cake layer does not easily form on the inner surface of the hollow fiber membrane, keeping the membrane pores on the inner surface in a constant state of flow. This means that small molecules such as metabolites can be continuously discharged with minimal protein loss. In addition, the appropriate pore area ratio of the inner surface and the good retention efficiency of the hollow fiber membrane for IgG result in more channels for the discharge of metabolites, allowing for timely and continuous discharge of metabolites. This results in less metabolite residue in the culture system, enabling effective perfusion culture. Furthermore, the synergistic effect of the polysulfone material ensures good compressive strength of the inner surface, allowing for continuous perfusion culture and ultimately obtaining a high-concentration protein feed solution.

[0021] In summary, polysulfone hollow fiber membranes, with their IgG retention efficiency ≥98%, inner surface pore area ratio of 2%-15%, initial water contact angle of 55°-80°, multiple strip-shaped fibers on the inner surface, SEM average width of the strip-shaped fibers of 70nm-200nm, and SEM average distance between two adjacent strip-shaped fibers of 80nm-150nm, can be used for perfusion culture to obtain high-concentration protein solutions.

[0022] In some embodiments, the SEM average minor axis of the pores on the inner surface of the polysulfone hollow fiber membrane is 10 nm to 50 nm; exemplaryly, the SEM average minor axis of the pores on the inner surface can be any single value or a range formed between any two values, such as 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 40 nm, 45 nm, 50 nm. The ratio of the SEM average major axis to the SEM average minor axis of the pores on the inner surface is 1.1 to 5.5; exemplaryly, the ratio of the SEM average major axis to the SEM average minor axis of the pores on the inner surface can be any single value or a range formed between any two values, such as 1.1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5.

[0023] As mentioned above, the effective pore size of the inner surface pores of hollow fiber membranes is very small, which can achieve the retention of IgG molecules. The effective pore size mentioned here refers to the minimum pore size after the superposition of the pores on the inner surface and the cross-section near the inner surface. Therefore, under the premise that the effective pore size meets the requirement of high retention efficiency for IgG, the short axis of the pores on the inner surface of polysulfone hollow fiber membranes can be larger than the size of protein molecules. For example, the short axis of the pores on the inner surface is 10nm-50nm. The pores on the inner surface that are larger than the size of protein molecules can provide a wider pathway for metabolites. The resistance when metabolites pass through the inner surface is smaller, which is conducive to the rapid discharge of metabolites and makes perfusion culture more effective.

[0024] Furthermore, by controlling the ratio of the SEM average major axis to the SEM average minor axis of the pores on the inner surface to be 1.1-5.5, we determined that the SEM average major axis of the pores on the inner surface is relatively long, approaching an elliptical shape. Compared to a circle with a diameter equal to the minor axis, these pores provide a larger fluid channel area, resulting in less resistance to the passage of metabolites and facilitating their faster excretion. Combined with the SEM average minor axis of the pores on the inner surface being 10nm-50nm and the pore area ratio being 2%-15%, the inner surface exhibits a certain number of relatively large pores, accelerating the excretion of small molecules such as metabolites. This promotes more effective perfusion culture. Additionally, the ratio of the SEM average major axis to the SEM average minor axis of the pores on the inner surface is not particularly large, resulting in better compressive strength and allowing for longer perfusion culture duration. In addition, the synergistic effect of the SEM average minor axis of the pores on the inner surface being 10nm-50nm and the ratio of the SEM average major axis to the SEM average minor axis of the pores on the inner surface being 1.1-5.5 results in a larger overall perimeter of the individual pores on the inner surface, and more entry points for shear force. This helps to reduce the shear force required to peel cells or proteins adsorbed around the pores on the inner surface from the inner surface. The reduced shear force causes less damage to cells and proteins, which is beneficial for obtaining a higher concentration of protein solution.

[0025] The average minor axis of the pores on the inner surface can be obtained by first characterizing the inner surface using a microscope (at a magnification that clearly identifies as many pore shapes as possible, such as 50,000x or 100,000x) to obtain the corresponding SEM image. Since the pore size on the inner surface is roughly uniform, a certain area, such as 4 μm, is selected. 2 (2μm×2μm), 1μm 2 (1μm × 1μm), the specific area size depends on the actual situation. Then, using appropriate computer software (such as Matlab, NIS Elements, etc.) or manually, the longest line segment among the two points on the outer periphery of the connecting hole is measured as the major axis, and the longest line segment among the two points on the outer periphery of the connecting hole that intersects the major axis perpendicularly is measured as the minor axis. Several tests are performed (preferably more than 10 times, the specific number depends on the situation), and the average value is calculated, which is the SEM average major axis and SEM average minor axis of the holes on the inner surface of this application, respectively. Of course, those skilled in the art can also obtain the above parameters through other measurement methods, and the above measurement methods are for reference only.

[0026] Further adjustments are made to ensure that the length direction of the strip fibers is parallel to the length direction of the hollow fiber membrane. In this invention, "parallel to the length direction of the hollow fiber membrane" means that the acute angle between the length directions of the strip fibers and the hollow fiber membrane is less than 20°. Such strip fibers can form a supporting framework along the membrane's length. Combined with the average SEM width of the strip fibers (70nm-200nm), the strip fibers form a support framework with a certain width, which can better disperse shear force and transmembrane pressure, resulting in better pressure resistance of the inner surface and better maintenance of the pore shape on the inner surface, thus better maintaining retention efficiency. Simultaneously, this strip fiber orientation reduces the resistance when the feed solution passes through the hollow fiber membrane cavity, correspondingly reducing shear force. The reduced shear force causes less damage to cells and proteins, which is beneficial for obtaining a higher concentration of protein feed solution.

[0027] In some embodiments, the roughness of the inner surface of the polysulfone hollow fiber membrane is 2.5 μm-14 μm; exemplaryly, the roughness of the inner surface can be any single value or a range formed between any two values, such as 2.5 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm. The roughness of the inner surface of a hollow fiber membrane reflects its smoothness. The smaller the roughness, the smoother the inner surface. The inner surface roughness of the hollow fiber membrane in this invention is 2.5μm-14μm, which is relatively small. This means that the inner surface of the hollow fiber membrane is relatively smooth, and the binding force between proteins and cells and the inner surface is relatively weak. With the synergistic effect of the initial water contact angle of the inner surface, the binding force between proteins and cells and the inner surface is even weaker. Under the action of less shear force, they can return to the reaction system, making it less likely to form a filter cake layer and less likely to cause membrane pore blockage. This keeps the membrane pores in a better flow state and continuously provides a channel for the excretion of metabolites. Moreover, the lower shear force causes less damage to cells and proteins. At the same time, the lower roughness of the inner surface itself causes less mechanical damage to cells and proteins, which is conducive to more effective perfusion culture, obtaining higher concentrations of protein solution, and less protein loss.

[0028] Roughness was measured using a Keyence VHX-7000 ultra-depth-of-field 3D microscope. Specifically, the filter membrane was placed on the sample stage under the microscope (with the inner surface facing the lens). The position and focus were adjusted until the texture on the filter membrane could be clearly observed. Then, the following steps were taken: "Depth Up," "Fast 3D Synthesis," "Execute Synthesis," "Display Synthesis," "3D Display," and "Surface Roughness." The test area was selected in the image, and the obtained Sa value is the roughness value. Multiple measurements were taken, and the average value was calculated. Of course, those skilled in the art can obtain the above parameters through other testing methods; the above testing methods are for reference only.

[0029] Based on the roughness of the inner surface of polysulfone hollow fiber membranes ranging from 2.5 μm to 14 μm, the pore area ratio of the inner surface is further increased to 3% to 13%. This pore area ratio corresponds to a membrane pore distribution that provides a more suitable flow channel area for metabolites. Furthermore, with the synergistic effect of the SEM average minor axis of the pores on the inner surface being 10 nm to 50 nm and the ratio of the SEM average major axis of the pores to the SEM average minor axis of the inner surface being 1.1 to 5.5, the inner surface has a more suitable number of flow channels. This results in good dispersion of small molecules such as metabolites, and the flow rate is relatively stable when the feed solution flows on the relatively smooth inner surface. Therefore, the synergistic effect of the above characteristics helps to reduce concentration polarization, reduce damage to proteins and cells, and facilitate more effective perfusion culture, thereby obtaining a higher concentration of protein feed solution.

[0030] In some embodiments, along the thickness direction from the inner surface to the outer surface of the polysulfone hollow fiber membrane, the SEM pore size of the membrane wall cross-section first increases and then decreases. Small molecules such as metabolites first pass through the expanding channel (the region where the SEM pore size of the membrane wall cross-section first increases), meaning the small molecules flow from a narrow flow path to a wide flow path, resulting in lower mass transfer resistance. Then, the small molecules pass through the constricting channel (the region where the SEM pore size of the membrane wall cross-section decreases again), meaning the small molecules enter from a wide flow path to a narrow flow path. Because the small molecules have a certain flow velocity in the expanding channel, they can generate turbulence in the constricting channel. The turbulence generated can accelerate the flow of small molecules such as metabolites, which offsets the deceleration caused by the narrowing of the channel. This means that the flow rate can be maintained at the same level as the channel. Overall, small molecules such as metabolites pass through the entire cross-section at a faster speed, allowing them to be discharged more quickly. At the same time, a smaller transmembrane pressure difference is needed for small molecules such as metabolites to flow from the inner surface to the outer surface. A smaller transmembrane pressure difference also slows down the formation rate of the filter cake layer on the inner surface. Consequently, cells and proteins adsorbed on the inner surface can return to the feed solution under a smaller shear force. The smaller shear force also causes less damage to cells and proteins, which is beneficial for better perfusion culture and obtaining a higher concentration of protein feed solution.

[0031] In the region where the SEM pore size of the membrane wall cross-section first increases, the area near the inner surface is a support layer with a thickness of 0.8 μm-5 μm. For example, the thickness of the support layer can be any single value or a range between any two values, such as 0.8 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 4.5 μm, or 5 μm. The presence of this thickness of support layer provides support to the inner surface, resulting in better compressive strength. Combined with the average SEM width of the strip fibers (70 nm-200 nm) and the average SEM distance between adjacent strip fibers (80 nm-150 nm), the effective pore size of the membrane is better maintained. Consequently, the continuous retention efficiency of protein is higher, and metabolites can be continuously discharged, facilitating longer perfusion culture and thus obtaining higher protein concentrations.

[0032] The location of the support layer is determined by using a scanning electron microscope (SEM) to characterize the cross-section near the inner surface in this invention. For example, an SEM image of the membrane cross-section near the inner surface with a magnification of 20,000, 50,000, or 100,000 is obtained (if a single image cannot capture the entire support layer, continuous imaging is used). The pore diameter of each plane is measured from the inner surface to the outer surface, and the average value is calculated until the first time the SEM average pore diameter is twice the SEM average minor diameter of the pores on the inner surface appears. The plane P1 with this average pore diameter is one plane of the support layer, and the other plane of the support layer is the inner surface. The thickness of the support layer is the distance between the inner surface and plane P1. The thickness of the support layer is measured by measuring the distance between the inner surface and plane P1 on the cross-sectional SEM image of the membrane using computer software (such as Matlab, NIS-Elements, etc.) or manually.

[0033] In some embodiments, the average SEM pore size of the support layer near the inner surface in the region where the SEM pore size of the membrane wall cross-section first increases is 15nm-60nm; exemplaryly, the average SEM pore size of the support layer can be any single value or a range formed between any two values ​​such as 15nm, 18nm, 20nm, 22nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, etc.

[0034] The SEM average pore size of the support layer is relatively small. In synergy with the support layer thickness of 0.8μm-5μm, it can better support the inner surface, giving the inner surface better compressive strength, which is conducive to a longer perfusion culture time. At the same time, the average pore size of the support layer is slightly larger than the SEM average minor axis (10nm-50nm) of the pores on the inner surface. Metabolites and other small molecules that permeate through the pores on the inner surface enter the support layer at a more uniform rate, thereby reducing concentration polarization on and around the inner surface and slowing down the compaction rate of cells and proteins on the inner surface. The membrane pores on the inner surface can better maintain the flow state during perfusion culture, so that the discharge rate of metabolites and other small molecules can be better maintained. Perfusion culture can be carried out more effectively, thereby obtaining a higher concentration of protein solution. If the average pore size of the support layer is too large, the expansion rate of small molecules such as metabolites entering the support layer from the inner surface will be relatively fast, and the flow rate of these small molecules will change more rapidly. This is not conducive to further reducing concentration polarization, and therefore not conducive to obtaining a higher concentration of protein solution. If the average pore size of the support layer is too small, the small molecules such as metabolites entering the support layer from the inner surface may experience backflow (be squeezed back to the inner surface), which is also not conducive to the rapid discharge of these small molecules, and similarly not conducive to obtaining a higher concentration of protein solution.

[0035] The SEM average pore diameter test of the support layer can refer to the SEM average minor diameter test procedure of the pores on the inner surface. The difference is that the measurement object is the SEM image of the cross section of the support layer.

[0036] Furthermore, the support layer also includes support fibers for forming the pores in the support layer, and the SEM average diameter of the support fibers is 25nm-90nm; for example, the SEM average diameter of the support fibers can be any single value or a range formed between any two values ​​such as 25nm, 28nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, etc.

[0037] By controlling the average SEM diameter of the supporting fibers, a suitable average diameter is achieved. This better maintains the membrane pores of the supporting layer, allowing small molecules such as metabolites to maintain a better discharge rate during perfusion culture, thus facilitating effective perfusion culture and obtaining a higher concentration of protein solution. Simultaneously, the suitable diameter of the supporting fibers, in synergy with the average SEM pore size of the supporting layer, results in a suitable number of membrane pores. This means that the number of flow paths for small molecules such as metabolites is moderate, allowing for faster discharge and more effective perfusion culture, further increasing the concentration of the obtained protein solution. Furthermore, in synergy with a suitable supporting layer thickness, it better supports the membrane pores on the inner surface, resulting in better compressive strength and better maintenance of the effective membrane pores. This further maintains the discharge rate of small molecules such as metabolites, promoting continuous perfusion culture and further increasing the concentration of the obtained protein solution.

[0038] Specifically, the average diameter of the support fiber is determined by selecting a certain area (e.g., 4 μm) from the SEM image of a cross-section near the inner surface (enough to measure the diameter of the support fiber). 2 (2μm*2μm), 1μm 2 (1μm*1μm), the specific area size depends on the actual situation. Then, use appropriate computer software (such as Matlab, NIS-Elements, etc.) or manually measure the diameter of the support fiber. Preferably, measure the diameter of more than 10 support fibers and calculate the average value, which is the SEM average diameter of the support fiber.

[0039] In some embodiments, the porosity of the support layer cross section is 4%-16%; exemplaryly, the porosity of the support layer cross section can be any one value or a range formed between any two values, such as 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%.

[0040] The pore area ratio of the support layer cross-section is 4%-16%, which is slightly larger than that of the inner surface. This design allows for more flow paths for small molecules such as metabolites to pass through the membrane pores of the inner surface into the support layer. This facilitates the smooth entry of metabolites into the membrane pores of the support layer, promoting faster expulsion of these small molecules. Furthermore, the relatively smaller pore area ratio of the support layer cross-section results in better strength and better support for the inner surface structure, both of which contribute to obtaining higher concentrations of protein solution. The synergistic effect of the pore area ratio of the support layer cross-section and the average SEM pore size of 15nm-60nm also results in a slightly larger number of pores in the support layer, meaning more and wider flow paths. This allows for faster expulsion of small molecules such as metabolites, leading to higher concentrations of protein solution.

[0041] The test method for the pore area ratio of the support layer cross section can refer to the test method for the pore area ratio of the inner surface. The difference is that the cross-sectional electron microscope image of the support layer is used as the test object.

[0042] In some embodiments, the porosity of the polysulfone hollow fiber membrane is 55%-80%; exemplaryly, the porosity of the polysulfone hollow fiber membrane can be any single value or a range formed between any two values, such as 55%, 58%, 60%, 62%, 65%, 70%, 72%, 75%, 78%, 80%.

[0043] The porosity of a hollow fiber membrane refers to the percentage of the total volume of all pores within the membrane material. A higher porosity means a larger proportion of the overall pore volume and a greater flow path for small molecules such as metabolites. The polysulfone hollow fiber membrane of this invention has a porosity of 55%-80%, meaning it has a relatively high porosity. This provides more flow paths for small molecules such as metabolites, resulting in lower flow resistance and facilitating rapid discharge. Furthermore, the high porosity structure provides the hollow fiber membrane with a large contaminant-holding capacity. Even if a small amount of protein is trapped inside the membrane through the pores on the inner surface, the hollow fiber membrane still has ample flow paths, maintaining a high rate of metabolite discharge. This allows for more effective perfusion culture. Simultaneously, the synergistic effect of this porosity range, along with the reasonable range of the average SEM width of the strip fibers and the reasonable range of the average SEM distance between adjacent strip fibers, better maintains the strength of the hollow fiber membrane, enabling longer perfusion culture and ultimately obtaining a higher concentration of protein solution.

[0044] Commonly used methods for testing porosity include mercury intrusion porosimetry, density method, and wet-dry film weighing method. Of course, those skilled in the art can also obtain the above parameters through other testing methods. The above testing methods are for reference only.

[0045] In some embodiments, the pore area ratio of the outer surface of the polysulfone hollow fiber membrane is 8%-25%; exemplaryly, the pore area ratio of the outer surface can be any single value or a range formed between any two values, such as 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, 22%, 24%, 25%. The SEM average pore size of the pores on the outer surface of the polysulfone hollow fiber membrane is 100nm-500nm; exemplaryly, the SEM average pore size of the pores on the outer surface can be any single value or a range formed between any two values, such as 100nm, 120nm, 150nm, 180nm, 200nm, 250nm, 280nm, 300nm, 320nm, 350nm, 380nm, 400nm, 420nm, 450nm, 480nm, 500nm.

[0046] The pores on the outer surface are the final area for the discharge of small molecules such as metabolites. By setting a moderate number and slightly larger pores on the outer surface, the resistance to the passage of metabolites is reduced, which is the final guarantee for the rapid discharge of small molecules such as metabolites. This is conducive to more effective perfusion culture. At the same time, the outer surface has better pressure resistance, and the hollow fiber membrane has better overall strength, which allows perfusion culture to be maintained for a longer time. With the synergistic effect of the SEM average minor diameter of the pores on the inner surface being 10nm-50nm and the pore area ratio of the inner surface being 2%-15%, the mass transfer resistance of small molecules such as metabolites through the membrane is lower, the required transmembrane pressure difference is also lower, and the damage to cells and proteins is also less, which is conducive to obtaining higher concentrations of protein solution.

[0047] The test method for the porosity of the outer surface can refer to the test method for the porosity of the inner surface, the difference being that the test object is the electron microscope image of the outer surface; the SEM average pore diameter of the pores on the outer surface refers to the minor diameter of the pores on the outer surface, and its test method can refer to the test method for the SEM average minor diameter of the pores on the inner surface, the difference being that the test object is the electron microscope image of the outer surface.

[0048] In some embodiments, the water flux of the polysulfone hollow fiber membrane is 1.5 LMH / psi to 20 LMH / psi.

[0049] Permeation flux, also known as permeation rate or simply flux, refers to the amount of substance that permeates through a unit area of ​​a polysulfone hollow fiber membrane per unit time under a certain operating pressure. The magnitude of the flux reflects the rate at which small molecules such as metabolites are expelled; a higher flux indicates a faster rate of expulsion. The polyethersulfone hollow fiber membrane of this invention has a water flux of 1.5 LMH / psi-20 LMH / psi, which is quite good. This indicates that when the hollow fiber membrane is used for perfusion culture, the expulsion rate of small molecules such as metabolites is relatively fast, and the residual amount of metabolites in the culture system is relatively low. This is beneficial for the effective perfusion culture and ultimately yields a high-concentration protein solution, resulting in higher economic benefits.

[0050] For the test method of water flux of hollow fiber membrane, please refer to paragraphs 0150-0153 of the specification of patent CN119607899A.

[0051] In some embodiments, the tensile strength of the polysulfone hollow fiber membrane is 5 MPa-8 MPa.

[0052] Tensile strength reflects the ability of a hollow fiber membrane to resist tensile force without breaking, and reflects the tensile, fracture, and deformation resistance of the membrane fibers. The polysulfone hollow fiber membrane prepared by this invention has a tensile strength of 5 MPa-8 MPa, indicating that it has excellent mechanical properties, high industrial practical value, and is beneficial for the continuous perfusion culture.

[0053] Tensile strength testing can be performed by uniformly stretching each sample at a tensile tester at room temperature (e.g., 25℃-30℃) (stretching speed of 50mm / min, distance between upper and lower clamps of 30mm) until fracture, thereby measuring the tensile strength. Repeat this process 3 times and take the average value. The average value obtained is the final tensile strength value.

[0054] In some embodiments, the thickness of the polysulfone hollow fiber membrane is 130 μm-200 μm; exemplaryly, the thickness of the polysulfone hollow fiber membrane can be any single value or a range between any two values, such as 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm. The polysulfone hollow fiber membrane of the present invention has a relatively thick thickness, which is beneficial for the continuous perfusion culture. The measurement method is to measure the distance between the inner and outer surfaces on the cross-sectional electron microscope image of the membrane using computer software (such as Matlab, NIS-Elements, etc.) or manually.

[0055] In some embodiments, the protein concentration of polysulfone hollow fiber membranes used for ATF perfusion culture is 5 mg / mL to 15 mg / mL.

[0056] Protein concentration refers to the concentration of protein in the feed solution of the bioreactor at the end of perfusion culture. The higher the protein concentration, the more protein is obtained during the perfusion culture. When the hollow fiber membrane of this invention is used for perfusion culture, its protein concentration is 5 mg / mL-15 mg / mL, which is a good protein concentration.

[0057] The protein concentration testing method of this invention is as follows: After the perfusion culture is completed, the feed solution in the bioreactor is centrifuged, and the supernatant is collected. The protein concentration is then obtained by testing the supernatant using an ELISA kit. Of course, those skilled in the art can also obtain the above parameters through other testing methods; the above testing methods are for reference only.

[0058] Secondly, embodiments of this application provide a method for preparing the above-mentioned polysulfone hollow fiber membrane, comprising the following steps:

[0059] Step 1: Preparation of casting solution and core solution. The casting solution consists of a polysulfone polymer, sulfonated polyethersulfone, a first organic solvent, and additives. The combined mass of the polysulfone polymer and sulfonated polyethersulfone accounts for 21%-25% of the casting solution's mass, and the first organic solvent accounts for 40%-70% of the casting solution's mass. The mass ratio of the polysulfone polymer to sulfonated polyethersulfone in the casting solution is (10-15):1. The core solution includes polyethyleneimine, polyethylene glycol, water, and a second organic solvent. The mass of polyethyleneimine accounts for 3%-7% of the core solution's mass, polyethylene glycol accounts for 0.5%-2%, and water accounts for no less than 40% of the core solution's mass.

[0060] Step 2: Spinning: The casting solution and core solution obtained in Step 1 are extruded together from the spinneret to obtain the molded product.

[0061] Step 3: Phase separation: Separate the molded product obtained in Step 2 to obtain film I.

[0062] Step 4: Cleaning and drying: After cleaning and drying the raw membrane I obtained in Step 3, a polysulfone hollow fiber membrane is obtained.

[0063] In some embodiments, the phase separation in step three includes pre-phase separation and complete phase separation. The pre-phase separation is carried out in an air section, and a stretching treatment is performed simultaneously during the pre-phase separation stage. The stretching treatment has a stretching rate of 3%-10%. The polysulfone polymer includes at least one of bisphenol A polysulfone, polyethersulfone, and polyphenylsulfone, and the additive includes at least one of polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol.

[0064] In some embodiments, the water content in the core solution is 45%-80% of the core solution mass; the core solution temperature is 30℃-50℃; and the casting solution temperature is higher than the core solution temperature, with a difference of no more than 10℃.

[0065] In some embodiments, the relative humidity of the air section is below 20%RH, the temperature is 10℃-25℃, the pre-phase separation time is 1s-3s, and the complete phase separation is carried out in a coagulation bath composed of water and a third organic solvent, wherein the mass percentage of the third organic solvent is 70%-90%; the complete phase separation time is 100s-150s, and the temperature is 30℃-50℃; the first organic solvent, the second organic solvent, and the third organic solvent each independently include at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.

[0066] In preparing the polysulfone-based hollow fiber membrane of the present invention, a casting solution is first prepared. The casting solution includes a film-forming substance, a polysulfone polymer, and sulfonated polyethersulfone, additives, and a first organic solvent for dissolving the polysulfone polymer and sulfonated polyethersulfone. The polysulfone polymer includes at least one of bisphenol A polysulfone, polyethersulfone, and polyphenylene sulfone. The additives include at least one of polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol. The first organic solvent includes at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide. The addition of sulfonated polyethersulfone improves the hydrophilicity of the prepared hollow fiber membrane. By controlling the mass ratio of polysulfone polymer to sulfonated polyethersulfone in the casting solution to (10~15):1, the amount of sulfonated polyethersulfone added is relatively small compared to the mass of the polysulfone polymer, thus improving hydrophilicity and also contributing to obtaining a hollow fiber membrane with good strength. The addition of additives can adjust the viscosity of the casting solution system, affecting the pore formation of the hollow fiber membrane. By adjusting the ratio of polysulfone polymers, sulfonated polyethersulfone, hydrophilic additives, and the first organic solvent, such as the sum of the mass of polysulfone polymers and sulfonated polyethersulfone accounting for 21%-25% of the mass of the casting solution, and the mass of the first organic solvent accounting for 40%-70% of the mass of the casting solution, the casting solution can be made to have a suitable viscosity. The viscosity of the casting solution has a certain influence on the structure and performance of the final hollow fiber membrane, such as the pore size of the hollow fiber membrane. With the synergistic effect of the core liquid, the final hollow fiber membrane has an ideal internal surface structure.

[0067] The presence of the core liquid enables the pressure inside the prepared hollow fiber membrane to remain balanced with the external pressure, thereby stabilizing the cavity of the hollow fiber membrane and making the overall wall thickness of the membrane basically the same. The core liquid used in the extrusion of the hollow fiber membrane of the present invention includes polyethyleneimine, polyethylene glycol, water and a second organic solvent, wherein the second organic solvent includes at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone and dimethyl sulfoxide. Polyethyleneimine contains a large number of amino groups, which are positively charged, while the polysulfone polymers and sulfonated polyethersulfones in the casting solution are negatively charged. The charges between polyethyleneimine and polysulfone polymers and sulfonated polyethersulfones are opposite, and the positive charge of polyethyleneimine is stronger. When the casting solution and the core solution are extruded together, polyethyleneimine anchors at the molecular level with some of the polysulfone polymer chains and sulfonated polyethersulfone chains on and near the inner surface through charge adsorption, and further induces the local aggregation of polysulfone polymer chains and sulfonated polyethersulfone chains. By controlling the mass content of polyethyleneimine in the core solution and through the synergistic effect with the composition of the casting solution, a suitable width of strip fiber and the distance between two adjacent strip fibers can be obtained. In addition, controlling the water content in the core solution to be relatively high, for example, not less than 40%, is beneficial to accelerating the phase separation rate. Combined with the effect of a small amount of polyethylene glycol, it is conducive to the formation of relatively small membrane pores. Furthermore, with the synergistic effect of the percentage of the total mass of polysulfone polymers and sulfonated polyethersulfone in the casting solution, the resulting hollow fiber membrane has smaller pore sizes on its inner surface. This allows for efficient retention of IgG while also providing a certain area of ​​pores for the discharge of small molecules such as metabolites during perfusion culture.

[0068] The second step is to extrude the prepared casting solution and core solution together from the spinneret. The casting solution forms a molded product with an inner surface and an outer surface in the nozzle, namely a hollow fiber membrane. The extruded hollow fiber membrane has an inner surface facing the inner cavity and an outer surface opposite to the cavity.

[0069] Step 3, phase separation, involves separating the molded product obtained in step 2 to obtain film I.

[0070] After phase separation, the resulting biofilm I is washed with pure water and dried to obtain a polysulfone hollow fiber membrane. When used for perfusion culture, this polysulfone hollow fiber membrane can achieve efficient retention of proteins and cells, is less likely to form a filter cake layer, and the pores on the inner surface of the membrane are in a flow state, allowing metabolites to be discharged in time. At the same time, the shear force is small during perfusion culture, resulting in less damage to cells and proteins, thus obtaining a high concentration of protein feed solution.

[0071] Preferably, the phase separation in step three includes pre-phase separation and complete phase separation. Pre-phase separation is completed in an air section. By controlling the relative humidity and temperature of the air section (e.g., the relative humidity below 20% RH and the temperature between 10°C and 25°C), when the casting liquid is extruded, the casting liquid on the outer surface of the molded product comes into direct contact with the air section. Due to the low relative humidity and temperature of the air section, the phase separation of the casting liquid on the outer surface is very slow, which is beneficial for forming relatively large pores on the outer surface. Furthermore, because during pre-phase separation… The time is relatively short; the air section only completes phase separation near the outer surface of the molded part or only a part of the outer surface of the molded part. After pre-phase separation, the molded part then enters the coagulation bath for phase separation. The coagulation bath consists of water and a third organic solvent (including at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide), and the mass percentage of the third organic solvent is relatively high. Generally, the higher the mass percentage of the third organic solvent, the slower the phase separation rate of the casting solution system, which is more conducive to the formation of macropores. Therefore, a higher mass percentage... The coagulation bath, composed of a third organic solvent, works in conjunction with the percentage of the combined mass of polysulfone polymers and sulfonated polyethersulfones in the casting solution, and further with the synergistic effects of pre-phase separation in the air section under specific conditions and the temperature of the coagulation bath. This results in relatively large pore sizes on the outer surface, within a preferred range. Simultaneously, the third organic solvent and water in the coagulation bath enter the interior through these pores on the outer surface, causing phase separation of the casting solution inside the molded part near the outer surface. The further away from the outer surface, the less of the coagulation bath enters. The slower the phase separation rate, the larger the resulting membrane pores. This means that the SEM pore size of the membrane wall cross-section decreases in the thickness direction from the inner surface to the outer surface. Simultaneously, the core liquid enters the interior through the membrane pores formed on the inner surface, separating the casting liquid near the inner surface of the molded product. Similarly, the farther from the inner surface, the less core liquid enters, the slower the phase separation rate, and the larger the resulting membrane pores. This means that the SEM pore size of the membrane wall cross-section initially increases in the thickness direction from the inner surface to the outer surface. Furthermore, the pre-phase separation stage also involves stretching, for example, a stretching rate of 3%-10%. Appropriate stretching facilitates the migration of the formed strip fibers along the stretching direction, ultimately resulting in strip fibers parallel to the length direction of the membrane. Simultaneously, during the pre-phase separation stage, the casting liquid on the inner surface is subjected to stretching forces during phase separation to form pores on the inner surface. The pores on the inner surface are elongated along the length direction of the membrane, resulting in a preferred ratio of the SEM average major axis to the SEM average minor axis of the pores on the inner surface.

[0072] Preferably, the water content in the core solution is controlled within a more preferred range as a percentage of the core solution's mass. This, combined with the core solution temperature being 30℃-50℃ and the casting solution temperature being higher than the core solution temperature by a difference of no more than 10℃, results in a relatively low core solution temperature and a relatively low casting solution temperature. This is more conducive to forming a more favorable pore area ratio on the inner surface. Simultaneously, the presence of polyethylene glycol in the core solution delays its movement speed. Combined with the specific composition of the casting solution, the core solution temperature, and the temperature difference between the casting solution and the core solution, this facilitates the formation of a more suitable support layer thickness, pore size, fiber diameter, and pore area ratio.

[0073] Thirdly, embodiments of this application provide an application in which the polysulfone hollow fiber membrane provided in the first aspect of this application is used for: (a) expression of monoclonal antibodies; (b) expression of fusion proteins; and (c) expression of biclonal antibodies.

[0074] Compared with the prior art, the embodiments of this application have the following beneficial technical effects:

[0075] 1. In this embodiment, by scientifically controlling the retention efficiency of polysulfone hollow fiber membrane for IgG, the pore area ratio of the inner surface, the initial water contact angle of the inner surface, the width of the strip fibers contained on the inner surface, and the distance between two adjacent strip fibers within a reasonable range, the polysulfone hollow fiber membrane prepared can be used for perfusion culture and can obtain a high concentration of protein solution.

[0076] 2. In the preparation process of the polysulfone hollow fiber membrane of this application, through the specific composition of casting solution and core solution, and after phase separation, cleaning and drying, the prepared polysulfone hollow fiber membrane has a specific internal surface structure.

[0077] 3. The polysulfone hollow fiber membrane of this application is integrally formed by casting liquid, which has the advantages of simple preparation method, better cost, green and environmentally friendly, and suitable for industrial production. Attached Figure Description

[0078] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0079] Figure 1 This is a scanning electron microscope (SEM) schematic diagram of the inner surface of the polysulfone hollow fiber membrane prepared in Example 2, with a magnification of 50000×.

[0080] Figure 2This is a scanning electron microscope (SEM) schematic diagram of the cross-section of the polysulfone hollow fiber membrane prepared in Example 2, with a magnification of 500×.

[0081] Figure 3 This is a scanning electron microscope (SEM) schematic diagram of a cross-section near the inner surface of the polysulfone hollow fiber membrane prepared in Example 2, with a magnification of 10000×. Detailed Implementation

[0082] The present application will be further described in detail below with reference to the accompanying drawings and embodiments.

[0083] Example 1

[0084] The preparation of a polysulfone hollow fiber membrane includes the following steps:

[0085] Step 1: Prepare casting solution and core solution.

[0086] The casting solution comprises the following components by mass percentage: 24.3% total content of polyethersulfone and sulfonated polyethersulfone (with a mass ratio of approximately 10:1), 50% content of N-methylpyrrolidone, and 25.7% content of polyethylene glycol. The temperature of the casting solution is 35°C.

[0087] The core fluid is composed of the following components by mass percentage: 4% polyethyleneimine, 1.3% polyethylene glycol, 75% water, and 19.7% N-methylpyrrolidone. The core fluid temperature is 30°C.

[0088] Step 2: Extrude the casting solution and core solution obtained in Step 1 together from the spinneret to obtain the molded product.

[0089] Step 3: Phase separation: Separate the molded product obtained in Step 2 to obtain film I.

[0090] The phase separation process includes pre-phase separation and complete phase separation. Pre-phase separation is carried out in an air section, simultaneously with a stretching treatment with a 10% stretching rate. The relative humidity in the air section is 10%RH, the temperature is 15℃, and the pre-phase separation time is 3 seconds. Complete phase separation is carried out in a coagulation bath composed of water and N-methylpyrrolidone, where N-methylpyrrolidone accounts for 70% by mass. The temperature of the coagulation bath is 50℃, and the complete phase separation time is 100 seconds.

[0091] Step 4: Wash the biofilm I obtained in Step 3 with pure water and then dry it to obtain a polysulfone hollow fiber membrane.

[0092] Example 2

[0093] The preparation of a polysulfone hollow fiber membrane includes the following steps:

[0094] Step 1: Prepare casting solution and core solution.

[0095] The casting solution comprises the following components by mass percentage: a total content of 23.6% for polyethersulfone and sulfonated polyethersulfone (with a mass ratio of approximately 12:1), a content of 55% for dimethylacetamide, and a content of 21.4% for polyvinyl alcohol. The temperature of the casting solution is 50°C.

[0096] The core fluid is composed of the following components by mass percentage: 5% polyethyleneimine, 1% polyethylene glycol, 65% water, and 29% dimethylacetamide. The core fluid temperature is 40℃.

[0097] Step 2: Extrude the casting solution and core solution obtained in Step 1 together from the spinneret to obtain the molded product.

[0098] Step 3: Phase separation: Separate the molded product obtained in Step 2 to obtain film I.

[0099] The phase separation process includes pre-phase separation and complete phase separation. Pre-phase separation is carried out in an air section, simultaneously with a stretching treatment of 8% (relative humidity 18% RH) at a temperature of 10°C, for a duration of 2.5 seconds. Complete phase separation is carried out in a coagulation bath composed of water and dimethylacetamide, with dimethylacetamide comprising 75% by mass, at a temperature of 45°C, for a duration of 110 seconds.

[0100] Step 4: Wash the biofilm I obtained in Step 3 with pure water and then dry it to obtain a polysulfone hollow fiber membrane.

[0101] Example 3

[0102] The preparation of a polysulfone hollow fiber membrane includes the following steps:

[0103] Step 1: Prepare casting solution and core solution.

[0104] The casting solution is composed of the following components by mass percentage: 22.5% total content of bisphenol A polysulfone and sulfonated polyethersulfone (wherein the mass ratio of bisphenol A polysulfone and sulfonated polyethersulfone is approximately 15:1), 60% content of dimethylformamide, and 17.5% content of polyvinylpyrrolidone. The temperature of the casting solution is 50℃.

[0105] The core fluid is composed of the following components by mass percentage: 7% polyethyleneimine, 0.8% polyethylene glycol, 55% water, and 37.2% dimethylformamide. The core fluid temperature is 45℃.

[0106] Step 2: Extrude the casting solution and core solution obtained in Step 1 together from the spinneret to obtain the molded product.

[0107] Step 3: Phase separation: Separate the molded product obtained in Step 2 to obtain film I.

[0108] The phase separation process includes pre-phase separation and complete phase separation. Pre-phase separation is carried out in an air section, simultaneously with a stretching treatment at a stretching rate of 3%. The relative humidity in the air section is 5% RH, the temperature is 25°C, and the pre-phase separation time is 1 second. Complete phase separation is carried out in a coagulation bath composed of water and dimethylformamide, where the dimethylformamide accounts for 85% of the mass. The temperature of the coagulation bath is 35°C, and the complete phase separation time is 140 seconds.

[0109] Step 4: Wash the biofilm I obtained in Step 3 with pure water and then dry it to obtain a polysulfone hollow fiber membrane.

[0110] Example 4

[0111] The preparation of a polysulfone hollow fiber membrane includes the following steps:

[0112] Step 1: Prepare casting solution and core solution.

[0113] The casting solution is composed of the following components by mass percentage: a total content of 21.8% of polyphenylene sulfone and sulfonated polyether sulfone (where the mass ratio of polyphenylene sulfone and sulfonated polyether sulfone is approximately 13:1), a content of 70% of dimethyl sulfoxide, and a content of 8.2% of polyvinyl alcohol. The temperature of the casting solution is 60°C.

[0114] The core fluid is composed of the following components by mass percentage: 6% polyethyleneimine, 1.6% polyethylene glycol, 45% water, and 47.4% dimethyl sulfoxide. The core fluid temperature is 50°C.

[0115] Step 2: Extrude the casting solution and core solution obtained in Step 1 together from the spinneret to obtain the molded product.

[0116] Step 3: Phase separation: Separate the molded product obtained in Step 2 to obtain film I.

[0117] The phase separation process includes pre-phase separation and complete phase separation. Pre-phase separation is carried out in an air section, simultaneously with a stretching treatment with a stretching rate of 6%. The relative humidity in the air section is 15%RH, the temperature is 20℃, and the pre-phase separation time is 2 seconds. Complete phase separation is carried out in a coagulation bath composed of water and dimethyl sulfoxide (DMSO), where DMSO accounts for 90% by mass. The temperature of the coagulation bath is 30℃, and the complete phase separation time is 150 seconds.

[0118] Step 4: Wash the biofilm I obtained in Step 3 with pure water and then dry it to obtain a polysulfone hollow fiber membrane.

[0119] In Examples 1-4, the length direction of the strip-shaped fibers on the inner surface of the polysulfone hollow fiber membranes was parallel to the length direction of the hollow fiber membrane. The SEM pore size of the membrane wall cross section of the hollow fiber membrane along the thickness direction from the inner surface to the outer surface first increased and then decreased. The structure, overall porosity, IgG retention efficiency, inner surface roughness, thickness, water flux, tensile strength, and protein concentration during ATF perfusion culture of the hollow fiber membranes were characterized. The specific results are shown in Table 1.

[0120] Table 1 - Characterization results of hollow fiber membranes in Examples 1-4

[0121] Test parameters Example 1 Example 2 Example 3 Example 4 IgG retention efficiency / % 99.8 99.6 99.3 99.2 Pore ​​area ratio of inner surface / % 3.2 3.9 9.2 12.8 Initial water contact angle of inner surface / ° 58.7 67.0 76.8 69.6 SEM average width of strip fibers / nm 86.4 117.6 158.9 128.4 SEM average distance between two adjacent strip fibers / nm 93.1 101.2 132.7 109.9 SEM mean minor axis of pores on the inner surface (nm) 11.7 18.2 32.3 45.1 The ratio of the SEM mean major axis to the SEM mean minor axis of the pores on the inner surface. 4.8 3.2 1.1 2.7 Roughness of inner surface / μm 2.8 4.3 13.4 6.7 Support layer thickness / μm 1.4 2.1 4.5 0.9 SEM average pore size of the support layer (nm) 16.7 22.8 41.4 57.2 SEM average diameter of supporting fibers (nm) 26.7 33.4 68.5 86.4 Pore ​​area ratio of the support layer cross section / % 4.7 6.0 9.3 15.5 Pore ​​area ratio of outer surface / % 8.4 12.7 18.7 24.4 SEM average pore size of pores on the outer surface (nm) 104.8 125.7 318.2 474.4 Porosity / % 56.7 64.1 69.2 75.7 Water flux / LMH / psi 3.6 8.5 12.6 18.7 Tensile strength / MPa 7.4 7.9 7.2 6.9 Hollow fiber membrane thickness / μm 132.7 151.8 168.4 182.5 Protein concentration used in ATF perfusion culture / mg / mL 10.9 11.8 14.7 12.6

[0122] The results above show that the polysulfone hollow fiber membranes prepared in Examples 1-4 have excellent tensile strength, not less than 6.5 MPa, and can be used for long-term perfusion culture. They also have excellent water flux, which is above 3.5 LMH / psi. When used for perfusion culture (the application of protein and cell retention on the inner surface), the protein concentration can reach more than 10 mg / mL at the end of the perfusion culture.

[0123] The specific process flow for applying this polysulfone hollow fiber membrane to perfusion culture is shown below (taking CHO cell expression of IgG protein and γ-ray irradiation sterilization process as an example):

[0124] The prepared polysulfone hollow fiber membranes were assembled into hollow fiber membrane modules using standard processes and sterilized by gamma irradiation. After sterilization, the membrane modules were thoroughly rinsed, and integrity and pressure holding tests were performed sequentially. Only after passing the tests could the modules be connected to the aseptic culture system. Basic culture medium was added to the sterilized bioreactor and preheated to the target culture temperature. The qualified hollow fiber membrane modules were connected to the bioreactor piping, and the ATF (Alternating Tangential Flow) system and peristaltic pump were started to ensure thorough wetting of the membrane modules. Before formal culture, the bioreactor's operating parameters were calibrated, and then CHO cell suspension was inoculated at the set initial inoculation density. The feeding program and ATF system were simultaneously started and adjusted to the target perfusion flow rate to formally commence CHO cell perfusion culture. When the cell density and cell viability reached the cooling trigger threshold, the cooling program was executed to allow the CHO cells to enter the stage of efficient expression of the target protein. The timing of harvesting the feed solution was determined according to the established process procedures and real-time monitoring of cell status. After the culture cycle is completed, the target protein concentration in the harvested liquid is the protein concentration when the polysulfone hollow fiber membrane is applied to ATF perfusion culture.

[0125] Example 5

[0126] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: a total content of 21.1% of polyethersulfone and sulfonated polyethersulfone (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), a content of 70% dimethylformamide, and a content of 8.9% polyvinyl alcohol. The temperature of the casting solution was 45°C. The core solution consisted of the following components by mass percentage: a content of 6% polyethyleneimine, a content of 2% polyethylene glycol, a content of 40% water, and a content of 52% dimethylformamide. The temperature of the core solution was 20°C.

[0127] The SEM average minor diameter of the pores on the inner surface of the final polysulfone hollow fiber membrane was 56.7 nm, and the IgG retention efficiency was 98.1%. Compared with Example 2, the tensile strength of the hollow fiber membrane obtained in Example 5 was reduced to 5.3 MPa, and the protein concentration was 5.8 mg / mL when used for ATF perfusion culture.

[0128] Example 6

[0129] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: a total content of 25% of polyethersulfone and sulfonated polyethersulfone (wherein the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), a content of 40% of N-methylpyrrolidone, and a content of 35% of polyvinyl alcohol. The temperature of the casting solution was 60°C. The core solution consisted of the following components by mass percentage: a content of 4% of polyethyleneimine, a content of 1.5% of polyethylene glycol, a content of 80% of water, and a content of 14.5% of N-methylpyrrolidone. The temperature of the core solution was 60°C.

[0130] The SEM average minor diameter of the pores on the inner surface of the final polysulfone hollow fiber membrane was 9.3 nm. Compared with Example 2, the water flux of the hollow fiber membrane obtained in Example 6 was 1.7 LMH / psi, and the protein concentration was 5.9 mg / mL when used for ATF perfusion culture.

[0131] Example 7

[0132] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that the stretching rate of the stretching treatment in the pre-phase separation process of step three was 12%.

[0133] The final polysulfone hollow fiber membrane had a SEM average major axis to SEM average minor axis ratio of pores on the inner surface of 6.4; the average SEM width of the strip fibers was 72.3 nm, and the average SEM distance between two adjacent strip fibers was 81.4 nm; the roughness of the inner surface was 2.1 μm; compared with Example 2, the hollow fiber membrane obtained in Example 7 had a tensile strength of 5.5 MPa and a protein concentration of 6.3 mg / mL when used for ATF perfusion culture.

[0134] Example 8

[0135] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that the stretching treatment in the pre-phase separation process of step three was omitted.

[0136] The final polysulfone hollow fiber membrane has a SEM average major axis to SEM average minor axis ratio of the pores on the inner surface of less than 1.1; the SEM average width of the strip fibers is 198.5 nm, and the SEM average distance between two adjacent strip fibers is 149.2 nm; the roughness of the inner surface is 15.4 μm; compared with Example 2, the hollow fiber membrane obtained in Example 8 has a water flux of 4.3 LMH / psi and a protein concentration of 6.1 mg / mL when used for ATF perfusion culture.

[0137] Example 9

[0138] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: a total content of 24.9% of polyethersulfone and sulfonated polyethersulfone (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), a content of 65% of dimethylacetamide, and a content of 10.1% of polyvinyl alcohol. The temperature of the casting solution was 65°C. The core solution consisted of the following components by mass percentage: a content of 3% of polyethyleneimine, a content of 2% of polyethylene glycol, a content of 90% of water, and a content of 5% of dimethylacetamide. The temperature of the core solution was 50°C.

[0139] The final polysulfone hollow fiber membrane had an inner surface porosity of 2.4%; compared to Example 2, the hollow fiber membrane obtained in Example 9 had a water flux of 1.9 LMH / psi and a protein concentration of 6.2 mg / mL when used for ATF perfusion culture.

[0140] Example 10

[0141] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: a total content of 21.2% of polyethersulfone and sulfonated polyethersulfone (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), a content of 50% of dimethylacetamide, and a content of 28.8% of polyvinyl alcohol. The temperature of the casting solution was 40°C. The core solution consisted of the following components by mass percentage: a content of 6% of polyethyleneimine, a content of 1.5% of polyethylene glycol, a content of 45% of water, and a content of 47.5% of dimethylacetamide. The temperature of the core solution was 35°C.

[0142] The final polysulfone hollow fiber membrane had an inner surface porosity of 14.5% and an IgG retention efficiency of 98.3%. Compared to Example 2, the hollow fiber membrane obtained in Example 10 had a tensile strength of 5.6 MPa and a protein concentration of 6.3 mg / mL when used for ATF perfusion culture.

[0143] Example 11

[0144] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one, the core liquid consisted of the following components by mass percentage: 6% polyethyleneimine, 2% polyethylene glycol, 60% water, and 32% dimethylacetamide. In step three, the coagulation bath consisted of water and dimethylacetamide, with dimethylacetamide comprising 60% by mass, and the temperature of the coagulation bath was 55°C.

[0145] The final polysulfone hollow fiber membrane had a support layer thickness of 0.6 μm; an IgG retention efficiency of 98.5%; a pore area ratio of 6.8% on the outer surface; and a SEM average pore size of 88.7 nm. Compared to Example 2, the hollow fiber membrane obtained in Example 11 had a tensile strength of 6.1 MPa and a protein concentration of 7.2 mg / mL when used for ATF perfusion culture.

[0146] Example 12

[0147] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one, the core liquid consisted of the following components by mass percentage: polyethyleneimine 6%, polyethylene glycol 0.5%, water 70%, and dimethylacetamide 23.5%. In step three, the coagulation bath consisted of water and dimethylacetamide, with dimethylacetamide accounting for 98% by mass. The temperature of the coagulation bath was 35°C, and the die extrusion width of the casting solution was also varied.

[0148] The final polysulfone hollow fiber membrane had a support layer thickness of 5.8 μm; an outer surface pore area ratio of 28.4%; an average SEM pore size of 553.2 nm; and a hollow fiber membrane thickness of 197.5 μm. Compared to Example 2, the hollow fiber membrane obtained in Example 12 had a water flux of 2.1 LMH / psi and a protein concentration of 7.5 mg / mL for ATF perfusion culture.

[0149] Example 13

[0150] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: a total content of 24.5% of polyethersulfone and sulfonated polyethersulfone (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), a content of 60% dimethylacetamide, and a content of 15.5% polyvinyl alcohol. The temperature of the casting solution was 35°C. The core solution consisted of the following components by mass percentage: a content of 5% polyethyleneimine, a content of 0.6% polyethylene glycol, a content of 80% water, and a content of 14.4% dimethylacetamide. The temperature of the core solution was 30°C. The coagulation bath in step three consisted of water and dimethylacetamide, wherein the mass percentage of dimethylacetamide was 95%.

[0151] The final polysulfone hollow fiber membrane had an average SEM pore size of 13.9 nm, an average SEM diameter of 23.3 nm for the supporting fiber, a pore area ratio of 3.4%, and a porosity of 51.4%. Compared to Example 2, the hollow fiber membrane obtained in Example 13 had a water flux of 3.4 LMH / psi and a protein concentration of 7.8 mg / mL when used for ATF perfusion culture.

[0152] Example 14

[0153] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: a total content of 21.4% of polyethersulfone and sulfonated polyethersulfone (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), a content of 50% dimethylacetamide, and a content of 28.6% polyvinyl alcohol. The temperature of the casting solution was 55°C. The core solution consisted of the following components by mass percentage: a content of 5% polyethyleneimine, a content of 1.9% polyethylene glycol, a content of 40% water, and a content of 53.1% dimethylacetamide. The temperature of the core solution was 50°C. The coagulation bath in step three consisted of water and dimethylacetamide, wherein the mass percentage of dimethylacetamide was 35%.

[0154] The final polysulfone hollow fiber membrane had an average SEM pore size of 63.7 nm for the support layer, an average SEM diameter of 94.8 nm for the support fibers, a pore area ratio of 17.3% for the support layer cross-section, and a porosity of 84.2%. The IgG retention efficiency was 98.7%. Compared to Example 2, the hollow fiber membrane obtained in Example 14 had a tensile strength of 6.1 MPa and a protein concentration of 9.3 mg / mL when used for ATF perfusion culture.

[0155] As can be seen from the results of Examples 1-14, when the SEM average short diameter of the pores on the inner surface of the polysulfone hollow fiber membrane in Examples 5-14, or the ratio of the SEM average long diameter to the SEM average short diameter of the pores on the inner surface, or the pore area ratio of the inner surface, or the roughness of the inner surface, or the thickness of the support layer, or the SEM average pore size of the support layer, or the SEM average diameter of the support fiber, or the pore area ratio of the support layer cross section, or the porosity, or the pore area ratio of the outer surface, or the SEM average pore size of the pores on the outer surface are not within the preferred range, the hollow fiber membrane obtained has acceptable tensile strength, can be used in perfusion culture, and has acceptable water flux, with a protein concentration of 5.5 mg / mL or higher when used for ATF perfusion culture.

[0156] Comparative Example 1

[0157] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: the total content of polyethersulfone and sulfonated polyethersulfone was 20.3% (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), the content of dimethylacetamide was 38%, and the content of polyvinyl alcohol was 41.7%. The core solution consisted of the following components by mass percentage: the content of polyethyleneimine was 4%, the content of polyethylene glycol was 3%, the content of water was 35%, and the content of dimethylacetamide was 58%.

[0158] The final polysulfone hollow fiber membrane had an IgG retention efficiency of 92.3%; compared with Example 2, the hollow fiber membrane obtained in Comparative Example 1 had a tensile strength of 4.5 MPa and a protein concentration of 1.5 mg / mL when used for ATF perfusion culture.

[0159] Comparative Example 2

[0160] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: a total content of 25.9% for polyethersulfone and sulfonated polyethersulfone (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), a dimethylacetamide content of 38%, and a polyvinyl alcohol content of 36.1%. The core solution consisted of the following components by mass percentage: a polyethyleneimine content of 4%, a polyethylene glycol content of 1%, and a water content of 95%.

[0161] The final polysulfone hollow fiber membrane has a pore area ratio of less than 1.5% on its inner surface. Compared with Example 2, the hollow fiber membrane obtained in Comparative Example 2 has a water flux of 0.6 LMH / psi and a protein concentration of 2.1 mg / mL when used for ATF perfusion culture.

[0162] Comparative Example 3

[0163] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one: the casting solution consisted of the following components by mass percentage: the total content of polyethersulfone and sulfonated polyethersulfone was 20% (where the mass ratio of polyethersulfone to sulfonated polyethersulfone was approximately 12:1), and the content of dimethylacetamide was 80%. The core solution consisted of the following components by mass percentage: the content of polyethyleneimine was 4%, the content of polyethylene glycol was 1%, the content of water was 30%, and the content of dimethylacetamide was 65%.

[0164] The final polysulfone hollow fiber membrane had a pore area ratio of 16.3% on its inner surface. Compared with Example 2, the hollow fiber membrane obtained in Comparative Example 3 had a tensile strength of 4.5 MPa and a protein concentration of 3.2 mg / mL when used for ATF perfusion culture.

[0165] Comparative Example 4

[0166] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that the casting solution in step one did not contain sulfonated polyethersulfone.

[0167] The initial water contact angle of the inner surface of the resulting polysulfone hollow fiber membrane was 89.4°. Compared with Example 2, the protein concentration of the hollow fiber membrane obtained in Comparative Example 4 was 0.8 mg / mL when used for ATF perfusion culture.

[0168] Comparative Example 5

[0169] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one, the core fluid consisted of the following components by mass percentage: 2% polyethyleneimine, 65% water, and 33% dimethylacetamide.

[0170] The final polysulfone hollow fiber membrane had an average SEM width of 61.4 nm and an average SEM distance of 70.5 nm between two adjacent strip fibers. Compared with Example 2, the hollow fiber membrane obtained in Comparative Example 5 had a tensile strength of 3.4 MPa and a protein concentration of 2.7 mg / mL when used for ATF perfusion culture.

[0171] Comparative Example 6

[0172] Polysulfone hollow fiber membranes were prepared according to the preparation method of Example 2, except that in step one, the core fluid was composed of the following components by mass percentage: polyethyleneimine content was 9%, polyethylene glycol content was 2.5%, water content was 65%, and dimethylacetamide content was 23.5%.

[0173] The final polysulfone hollow fiber membrane had an average SEM width of 227.2 nm and an average SEM distance of 168.3 nm between two adjacent strip fibers. Compared with Example 2, the hollow fiber membrane obtained in Comparative Example 6 had a tensile strength of 3.2 MPa and a protein concentration of 2.9 mg / mL when used for ATF perfusion culture.

[0174] The results of Comparative Examples 1-6 show that when the polysulfone hollow fiber membrane prepared has an IgG retention efficiency of less than 98%, or an excessively large or small pore area ratio on the inner surface, or an excessively large initial water contact angle on the inner surface, or an excessively large or small average SEM width of the strip fibers, or an excessively large or small average SEM distance between two adjacent strip fibers, or an excessively small average SEM distance between two adjacent strip fibers, the protein concentration will be below 5 mg / mL when used for ATF perfusion culture. It cannot obtain a high-concentration protein solution and is not suitable for applications that require a high-concentration protein solution.

[0175] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A polysulfone hollow fiber membrane, comprising a body having an inner cavity, wherein the side of the body facing the inner cavity is an inner surface, and the side of the body away from the inner cavity is an outer surface, characterized in that: The hollow fiber membrane has an IgG retention efficiency of ≥98%; The porosity of the inner surface is 2%-15%; The initial water contact angle of the inner surface is 55°-80°; The inner surface contains multiple strip-shaped fibers, the average SEM width of the strip-shaped fibers is 70nm-200nm, and the average SEM distance between two adjacent strip-shaped fibers is 80nm-150nm.

2. The polysulfone hollow fiber membrane as described in claim 1, characterized in that: The average minor axis of the pores on the inner surface, as measured by SEM, is 10 nm to 50 nm. The ratio of the SEM average major axis of the holes on the inner surface to the SEM average minor axis of the holes on the inner surface is 1.1-5.

5. The length direction of the strip-shaped fiber is parallel to the length direction of the hollow fiber membrane.

3. The polysulfone hollow fiber membrane as described in claim 1, characterized in that: The porosity of the inner surface is 3% to 13%; The roughness of the inner surface is 2.5μm-14μm.

4. The polysulfone hollow fiber membrane as described in claim 1, characterized in that: Along the thickness direction from the inner surface to the outer surface, the SEM pore size of the membrane wall cross-section of the polysulfone hollow fiber membrane first increases and then decreases. The region where the SEM pore size of the membrane wall cross-section first increases is a support layer near the inner surface, and the thickness of the support layer is 0.8μm-5μm.

5. The polysulfone hollow fiber membrane as described in claim 4, characterized in that: The average SEM pore size of the support layer is 15nm-60nm; The support layer also includes support fibers for forming pores in the support layer, and the SEM average diameter of the support fibers is 25nm-90nm.

6. The polysulfone hollow fiber membrane as described in claim 4, characterized in that: The porosity of the cross-section of the support layer is 4%-16%; The porosity of the hollow fiber membrane is 55%-80%.

7. The polysulfone hollow fiber membrane as described in claim 1, characterized in that: The porosity of the outer surface is 8%-25%; The average SEM pore size of the holes on the outer surface is 100nm-500nm.

8. The polysulfone hollow fiber membrane as described in claim 1, characterized in that: The water flux of the polysulfone hollow fiber membrane is 1.5 LMH / psi-20 LMH / psi; The tensile strength of the polysulfone hollow fiber membrane is 5MPa-8MPa; The thickness of the polysulfone hollow fiber membrane is 130μm-200μm; The protein concentration of the polysulfone hollow fiber membrane used for ATF perfusion culture is 5 mg / mL-15 mg / mL.

9. A method for preparing a polysulfone hollow fiber membrane as described in any one of claims 18, characterized in that: Includes the following steps: Step 1: Preparation of casting solution and core solution: The casting solution is composed of polysulfone polymers, sulfonated polyethersulfone, a first organic solvent, and additives, wherein the sum of the mass of the polysulfone polymers and sulfonated polyethersulfone accounts for 21%-25% of the mass of the casting solution, and the mass of the first organic solvent accounts for 40%-70% of the mass of the casting solution. The mass ratio of polysulfone polymer to sulfonated polyethersulfone in the casting solution is (10~15):1; The core fluid comprises polyethyleneimine, polyethylene glycol, water, and a second organic solvent, wherein the mass percentage of polyethyleneimine in the core fluid is 3%-7%, the mass percentage of polyethylene glycol in the core fluid is 0.5%-2%, and the mass percentage of water in the core fluid is not less than 40%. Step 2: Spinning: The casting solution and core solution obtained in Step 1 are extruded together from the spinneret to obtain the molded product; Step 3: Phase separation: The molded product obtained in Step 2 is subjected to phase separation to obtain film I; Step 4: Cleaning and drying: After cleaning and drying the raw membrane I obtained in Step 3, a polysulfone hollow fiber membrane is obtained.

10. The method for preparing a polysulfone hollow fiber membrane as described in claim 9, characterized in that: The phase separation in step three includes pre-phase separation and complete phase separation. The pre-phase separation is carried out in an air section, and a stretching treatment is performed simultaneously during the pre-phase separation stage. The stretching treatment has a stretching rate of 3%-10%. The polysulfone polymers include at least one of bisphenol A polysulfone, polyether sulfone, and polyphenyl sulfone; The additives include at least one of polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol.

11. The method for preparing polysulfone hollow fiber membrane as described in claim 9, characterized in that: The water content in the core fluid is 45%-80% of the total core fluid mass. The temperature of the core fluid is 30℃-50℃; The temperature of the casting solution is higher than that of the core solution, and the difference is no more than 10°C.

12. The method for preparing polysulfone hollow fiber membrane as described in claim 10, characterized in that: The relative humidity of the air section is below 20%RH, the temperature is 10℃-25℃, and the pre-phase separation time is 1s-3s; The complete phase separation is carried out in a coagulation bath, which consists of water and a third organic solvent, wherein the mass percentage of the third organic solvent is 70%-90%. The time for complete phase separation is 100s-150s, and the temperature is 30℃-50℃. The first organic solvent, the second organic solvent, and the third organic solvent each independently include at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.

13. An application of a polysulfone hollow fiber membrane as described in any one of claims 1-8, characterized in that: The polysulfone hollow fiber membrane is used for: (a) Expression of monoclonal antibodies; (b) Expression of the fusion protein; (c) Expression of biclonal antibodies.

Citation Information

Patent Citations

  • Sulfone polymer hollow fiber ultrafiltration membrane, preparation method and application thereof, and assembly with ultrafiltration membrane

    CN119607899A