An antioxidant and alkali-resistant nanofiltration membrane and its preparation method
By improving the materials and processes of the support layer, intermediate layer, and desalination layer, an antioxidant and alkali-resistant nanofiltration membrane was formed, solving the problem that existing alkali-resistant nanofiltration membranes are easily oxidized and damaged under high concentrations of alkaline solutions and oxidants, and improving alkali resistance and antioxidant performance.
Patent Information
- Application Number
- CN202611599198.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing alkali-resistant nanofiltration membranes are easily oxidized and damaged in the presence of high-concentration alkaline solutions and oxidants, leading to cracking and detachment of the desalination layer, short service life, high operating costs for enterprises, and performance degradation in complex water quality environments.
By improving materials and processes in the support layer, intermediate layer and desalination layer, a dense structure is formed using polyethersulfone, polyhydroxy polymers and porous inorganic nanomaterials. Combined with pyridine catalysts and stabilizers, the primary and secondary amine structures are converted to form an antioxidant and alkali-resistant nanofiltration membrane.
It improves the alkali resistance and antioxidant properties of nanofiltration membranes, extends their service life, reduces operating costs, and increases desalination rate and flux.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of separation membrane technology, specifically to an antioxidant and alkali-resistant nanofiltration membrane and its preparation method. Background Technology
[0002] The global textile industry generates nearly 100 million tons of dyeing and printing wastewater, accounting for one-fifth of the world's total industrial wastewater, posing a significant challenge to wastewater treatment and reuse. Currently, the mainstream alkali-resistant membrane products on the market have a polyamine structure for their desalination layer, obtained through interfacial polymerization of polyethyleneimine and cyanuric chloride. These membranes are widely used in industries with complex and extreme liquid environments, such as viscose fiber, dyeing and papermaking, food and pharmaceutical production, dairy products, and precision electronics. Their application is relatively concentrated in viscose fiber and pharmaceuticals, with alkali concentrations typically between 200-220 g / L. However, the membrane module's service life is only 12-18 months, after which the retention rate of organic matter and salt removal rate show a sharp decline. This is mainly due to two reasons: firstly, the high branching degree of polyethyleneimine leads to incomplete reaction; secondly, the uneven activity of the functional groups in the cyanuric chloride monomer limits the reaction, both resulting in a low degree of cross-linking in the desalination layer. In high-concentration alkaline solutions, the swelling degree increases irreversibly with prolonged operation, leading to a decline in basic performance. Furthermore, with the increasing complexity of water treatment environments, the feed liquid in the application process has begun to contain oxidant (H2O2) components in the past two years, further shortening the service life of membrane modules to 3-6 months. Analysis of these phenomena revealed the direct cause to be the pulverization and detachment of the support layer and cracking of the desalination layer. The primary internal cause is the hyperbranched nature of the polyethyleneimine molecular chain, where the active functional groups of primary and secondary amines in its structure are incompletely reacted and remain in large quantities. These residual groups easily become attack sites for oxidant (H2O2), leading to polymer chain breakage upon oxidation, rapidly destroying the desalination layer structure. This results in insufficient oxidation resistance of the polyamine structure and a severe decline in performance.
[0003] Therefore, by regulating the structure and surface properties of the support layer, improving the crosslinking degree of the surface desalination layer, and eliminating the negative impact of residual primary and secondary amines on oxidation resistance, a nanofiltration membrane with strong oxidation resistance and high alkali stability can be obtained. This is of practical significance for promoting the strategic development of my country's industry, reducing production costs, and improving production efficiency.
[0004] Currently, most commercially available alkali-resistant membrane desalination layers are polyamine-based, primarily used in the chemical fiber industry. These layers are produced by the reaction of aqueous polyethyleneimine and oil-phase cyanuric chloride, maintaining stable resistance in high-concentration 20% NaOH alkaline solutions. However, in feed processes containing oxidants (H2O2), the desalination layer is quickly damaged, cracking and detaching. Imported membrane elements have a shorter lifespan (generally 6-12 months), while domestically produced membrane elements have a lifespan of no more than 3 months.
[0005] There are already some related studies, for example: Designing Pyridinium-Catalyzed Interfacial Polymerization for High-Performance Acid-Resistant Nanofiltration Membranes[J]. Angewandte Chemie, (2026). This paper presents a method for improving the conversion efficiency of cyanuric chloride monomer catalyzed by pyridinium groups. This method increases the substitution reaction activity of cyanuric chloride by an order of magnitude. After improving the crosslinking degree of the desalination layer, the acid resistance of the membrane is significantly enhanced, and the resistance to Co... 2+ The retention rate increased from 1.7% to 94.5%; Regulating Interfacial Polymerization via a Hybrid PVA / BCNNanocomposite Interlayer for High-performance Reverse Osmosis Membranes[J].Desalination,(2026). This study provides a method for regulating the structure and surface properties of the support layer, desalination layer, and intermediate layer through the structure of the intermediate layer, resulting in a reverse osmosis membrane with strong hydrophilicity and smoother surface, and a water flux that is doubled to 4.5 LMH / bar. The patent "A Method for Preparing an Antioxidant and Acid- and Alkali-Resistant Nanofiltration Membrane" (CN109692586A) describes a nanofiltration membrane prepared by treatment with 4% NaOH for 30 days, with an optimal experimental group membrane flux of 17.9 L / m³. 2 •h (approximately 10gfd), test pressure up to 2MPa (approximately 290psi), desalination rate 98.26%, desalination rate after oxidation 97.78% (oxidation test method, type of oxidant, concentration and time not specified), membrane flux and desalination rate are both low and its application prospects in high concentration alkaline solutions are unclear.
[0006] The main problem lies in the high amount of unreacted primary amines (-NH2) and secondary amines (-NH-) remaining in the hyperbranched macromolecular PEI chains. These are easily oxidized and broken by hydrogen peroxide (H2O2), leading to defects in the desalination layer and rendering the membrane element unusable. Furthermore, the functional layer of the polyamine alkali-resistant membrane is primarily composed of aliphatic amines, inherently lacking in oxidation resistance. This results in frequent membrane element replacements in industrial applications, leading to high operating costs for enterprises. Imported membranes of similar products are 3-5 times more expensive than domestically produced membranes and hold a market share exceeding 80% in the domestic market. Therefore, strengthening the alkali resistance stability of the desalination layer and endowing it with oxidation resistance is of strategic significance for improving the core competitiveness of domestic manufacturers and reducing operating costs for users. Simultaneously, this represents two major technical challenges that need to be addressed in the chemical fiber and pharmaceutical industries. Summary of the Invention
[0007] In order to solve the above-mentioned technical problems in the prior art, the present invention provides a method for preparing an antioxidant and alkali-resistant nanofiltration membrane.
[0008] A method for preparing an antioxidant and alkali-resistant nanofiltration membrane includes the following steps: (1) Preparation of polymer solution: Polyethersulfone (PES) and polymer-based macromolecular pore-forming agent are dissolved in organic solvent to prepare a polymer solution. After vacuum degassing at 30-35℃ for 4 hours, the solution is kept warm. The polymer solution is scraped onto polypropylene (PP) nonwoven fabric using a scraper. The room temperature is 20-25℃, the ambient humidity is 80-85%, the scraping speed is 6m / min, the temperature of the first coagulation bath is 10-15℃, the exposure time in the coagulation bath is 10-15s, the temperature of the second hot water tank is 60-70℃, and after rinsing with deionized water, a porous base membrane (UF membrane) is obtained.
[0009] (2) Preparation of intermediate layer blending solution: A liquid phase solution composed of highly hydrophilic and highly adhesive polyhydroxy polymer macromolecules and porous inorganic nanomaterials is coated onto the UF membrane. After being heated at 80°C, a homogeneous high-porosity thermal cross-linking layer is formed and anchored to the surface of the UF membrane.
[0010] (3) Preparation of aqueous solution: The aqueous solution consisting of the main monomer polyethyleneimine, the second monomer aromatic amine (Ar-NH2), the stabilizer difunctional aldehyde (OHC-R-CHO) and the auxiliary agent is uniformly applied to the surface of the UF membrane. After 60-90 seconds, the solution is purged with hydraulic air until there is no residue.
[0011] (4) Preparation of oil phase solution: The ethyl solution composed of the main monomer cyanuric chloride, the catalyst pyridine and the co-solvent is uniformly applied to the membrane surface of (3) above. After 60-90s, the residual solution is removed with a rubber guide roller to form a nascent nanofiltration membrane.
[0012] (5) Preparation and treatment of the first post-treatment solution: The solution composed of acid anhydride and organic solvent is used as the first post-treatment solution. The nascent nanofiltration membrane obtained in (4) above is statically immersed in the first post-treatment solution for 20-30s and heat-treated at 60-80℃ for 2min to completely convert the unreacted primary amine (-NH2) in the polymer structure into a polyimide (-CO-NR-CO-) structure.
[0013] (6) Preparation of the second post-treatment solution: The second post-treatment solution is an aqueous solution composed of nitrite or sulfite and protic acid. The nanofiltration membrane (5) above is statically immersed in the second post-treatment solution for 60-90s and heat-treated at 80-100℃ for 3min to completely convert the unreacted secondary amine (-NH-) in the polymer structure into a nitrosamine (-NR-N=O) structure.
[0014] (7) The nanofiltration membrane with the above (6) function is immersed in an aqueous solution of 1wt% N, N-dimethylformamide (DMF) and 8wt% H2SO4 for 24h to remove oligomers in the molecular chain structure. At the same time, the N atoms are protonated to give the desalination layer a higher positive charge density, thereby obtaining an antioxidant and alkali resistant nanofiltration membrane with enhanced performance.
[0015] Furthermore, the polymer solution is any one or a combination of two or more of polysulfone, polyethersulfone, sulfonated polyethersulfone, and polyetheretherketone in any proportion. The polymer has a molecular weight of 60,000-100,000 Da, and the polymer solution has a mass concentration of 17-22 wt%.
[0016] Furthermore, the organic solvent used to prepare the polymer solution is any one or a combination of two or more of N,N'-dimethylformamide (DMF), N,N'-dimethylhexamethylene (DMAc), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO) in any proportion.
[0017] Furthermore, the polymer-based macromolecular pore-forming agent is any one or a combination of two or more of the following: polyethylene glycol (PEG) with a molecular weight of 400-2000 Da, polyethyleneimine (PEI) with a molecular weight of 1000-6000 Da, polyvinyl alcohol (PVA) with a molecular weight of 1000-6000 Da (degree of hydrolysis 89-90%), and amphiphilic block copolymer F-127 with a molecular weight of 2000-6000 Da, in any proportion. The content of the pore-forming agent is 0.1-6 wt%, preferably 1-3 wt%.
[0018] Furthermore, the preparation conditions for the porous UF membrane are as follows: room temperature 20-25℃, ambient humidity 80-85%, membrane scraping speed 5-6m / min, front coagulation bath temperature 10-15℃, coagulation bath exposure time 10-15s, and rear hot water tank temperature 60-70℃.
[0019] Furthermore, the intermediate layer solution is a homogeneous aqueous solution composed of a highly adhesive polyhydroxy polymer and porous inorganic nanomaterials. The polyhydroxy polymer is any one or more of polyvinyl alcohol (PVA), polydopamine (PDA), chitosan (CS), hyaluronic acid (HA), and dextran (DT) in any proportion, with a solution content of 0.2-2 wt%, preferably 0.5-1.5 wt%.
[0020] Furthermore, the porous inorganic nanomaterial is any one or two or more of zero-dimensional, one-dimensional, two-dimensional and three-dimensional configurations in any proportion, and the solution addition content is 0.01-1wt%, preferably 0.05-0.5wt%.
[0021] Furthermore, the zero-dimensional porous inorganic nanomaterial is any one or two or more of silicon dioxide, titanium dioxide, aluminum oxide, zeolite, zinc oxide, manganese oxide, molybdenum oxide, and silicon carbide in any proportion, with a particle size of 20-40 nm, preferably 25-30 nm.
[0022] Furthermore, the one-dimensional porous inorganic nanomaterial is any one or more of carbon nanotubes, carbon nanorods, carbon nanowires, and carbon nanowhiskers in any proportion, with a length of 50-100 nm and an aspect ratio of 50-80, preferably 60.
[0023] Furthermore, the two-dimensional porous inorganic nanomaterial is any one or more of graphene oxide, boron carbon nitride nanosheets (BCN), montmorillonite, MXene (composed of transition metals and carbon / nitrogen atoms), and hydrotalcite (LDHs) in any proportion, with a length of 10-15 nm × width of 6-12 nm. The preferred size is 12-14 nm × 8-10 nm.
[0024] Furthermore, the three-dimensional porous inorganic nanomaterial is any one or two or more of COF, MOF, POSS, ZIF, and nanomolecular sieves in any proportion, with a surface pore size of 0.5-5 nm, preferably 2-3 nm.
[0025] Furthermore, the intermediate layer coating solution has a thermal crosslinking temperature of 80-90℃, an immersion time of 5-10s, and an intermediate setting time of 2-3min.
[0026] Furthermore, the aqueous phase second monomer aromatic amine (Ar-NH2) is any one or two or more of aromatic monoamines, aromatic diamines, aromatic triamines and their derivatives, combined in any proportion. The aqueous phase content is 0.2-2 wt%, preferably 0.5-1.5 wt%.
[0027] Furthermore, the aromatic monoamine is any one or two or more of aniline, o-nitroaniline, 4-ethylaniline, acetaniline, 3-chloroaniline, 2,5-dimethylaniline, p-methylaniline, o-methylaniline, 3-nitroaniline, p-methoxyaniline, and their derivatives, in any proportion.
[0028] Furthermore, the aromatic diamine is any one or more of the following, in any proportion: m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, 4,5-dimethyl-1,2-phenylenediamine, 4-nitro-o-phenylenediamine, 5-chloro-m-phenylenediamine, 2,5-diaminobenzoic acid, 2,5-diaminobenzenesulfonic acid, 2,4-diaminophenol, 3,4-diaminotoluene, 1,5-diamino-2,4-dichlorobenzene, 2,3-diaminobenzyl alcohol, and their derivatives.
[0029] Furthermore, the aromatic triamine is any one or two or more of 1,2,3-triaminobenzene, 1,3,5-triaminobenzene, 2,4,6-triaminobenzene, 1,2,4-triaminobenzene, 2,4,6-triaminotoluene, 2,4,6-triaminochlorobenzene, 2,4,5-triaminobenzoic acid, and their derivatives, in any proportion.
[0030] Furthermore, the stabilizer is an aliphatic dialdehyde or an aromatic dialdehyde, and the amount added is 0.1-1 wt%, preferably 0.3-0.8 wt%.
[0031] Furthermore, the stabilizer, an aliphatic dialdehyde, is any one or more of the following: glyoxal, glutaraldehyde, succinaldehyde, octanaldehyde, adipaldehyde, malonaldehyde, heptaldehyde, nonadialdehyde, cis-2-butenedial, 2-methylglutaraldehyde, trans-2-butenedial, and their derivatives, with a carbon number of C2-C10, or a combination of two or more in any proportion. Preferably, it is an aliphatic dialdehyde with a carbon number of C2-C6.
[0032] Furthermore, the stabilizer aromatic dialdehyde is any one or more of the following monobenzene ring dialdehydes and their derivatives, in any proportion: 2-nitro-terephthalaldehyde, 5-bromoisophthalaldehyde, 1,4-dialdehyde-2,5-divinylbenzene, 2,3-dihydroxyterephthalaldehyde, terephthalaldehyde, isophthalaldehyde, 2,5-diethoxy-1,4-terephthalaldehyde, 2-methylterephthalaldehyde, 2,3,5,6-tetrafluoroterephthalaldehyde, 1H-pyridine-2,5-dicarboxaldehyde.
[0033] Furthermore, the organic phase pyridine catalyst is any one or more of monopyridine, dipyridine, ternary pyridine, and their derivatives, in any proportion. The amount of organic phase added is 0.01-1 wt%, preferably 0.1-0.5 wt%, and preferably the number of pyridine groups n≥2.
[0034] Furthermore, the monopyridine is any one or more of 3-aminopyridine, 4-dimethylaminopyridine, 4-dimethylpyridine, 2,6-di-tert-butylpyridine, 2,6-diaminopyridine, 2,4,6-trimethylpyridine, 4-pyrrolylpyridine, 3-pyridinemethanol, 3-bromopyridine, 2-fluoropyridine, 4-sulfonic acid pyridine, 2-carboxylic acid pyridine, 6-bromopyridine-2,3-diamine, 2,5-dichloropyridine-4-amine, 2,4-dihydroxypyridine, 2-methyl-3,6-diaminopyridine, and their derivatives, in any proportion.
[0035] Furthermore, the binary pyridine is any one or more of 2,4'-dipyridine, 2-methanedipyridine, 2,2'-dipyridineamine, 2,2'-dithiodipyridine, 4,4'-dipyridine sulfide, 3,4'-dipyridine-2'-amine, 6-fluoro-2,2'-dipyridine, 4,4'-difluoro-2,2'-dipyridine, 1,3-dipyridine-2-ylurea, 2-chloro-4-pyrrolidinedipyridine, 6,6'-bis(chloromethyl)-2,2'-dipyridine, 4,4'-bis(hydroxymethyl)-2,2'-dipyridine, and their derivatives, in any proportion.
[0036] Furthermore, the ternary pyridine is any one or more of 2,2′:6′,2′′-tripyridine, 2,4,6-tris(pyridin-4-yl)pyridine, 1,3,5-tris(pyridin-4-yl)benzene, 3,2':4',3''-bitripyridine, 4-(2,4,5-tripyridin-4-ylphenyl)pyridine, 4,4',4'-(1H-imidazol-2,4,5-triyl)pyridine, 4′-(4-methylphenyl)-2,2′:6′,2′′-tripyridine, 4'-(4-methoxyphenyl)-2,2':6',2''-tripyridine, and their derivatives, in any proportion.
[0037] Furthermore, the content of the acid anhydride in the first post-treatment solution in the organic solution is 0.5-5 wt%, preferably 1-3 wt%. The acid anhydride is any one or more of monofunctional acid anhydrides, difunctional acid anhydrides, and their derivatives, in any proportion.
[0038] Furthermore, the monofunctional anhydride is any one or more of acetic anhydride, propionic anhydride, butyric anhydride, benzoic anhydride, maleic anhydride, difluoroacetic anhydride, isovaleric anhydride, isobutyric anhydride, 3,3-dimethylglutaric anhydride, phenylacetic anhydride, trifluoromethylmaleic anhydride, acrylic anhydride, succinic anhydride, phthalic anhydride, tebufenozide, 2,3-pyridinedicarboxylic anhydride, and their derivatives, in any proportion.
[0039] Furthermore, the binary functional anhydride is any one or more of the following, or a combination of two or more, in any proportion: pyromellitic dianhydride, diacetic anhydride, dibromopyromellitic dianhydride, ethylenediaminetetraacetic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, diethylenetriaminepentaacetic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, tetrahydrofuran-2,3,4,5-tetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, and their derivatives.
[0040] Furthermore, the organic solvent for dissolving the acid anhydride is any one or two or more of dichloromethane, chloroform, toluene, ethyl acetate, acetone, m-xylene, and mesitylene, combined in any proportion.
[0041] Furthermore, the initial ecological membrane undergoes a first post-treatment process for 10-60 seconds, preferably 20-40 seconds. After impregnation in the post-treatment solution, the membrane is subjected to heat treatment at a temperature of 60-100°C, preferably 70-80°C. The heat treatment time is 1-5 minutes, preferably 2-3 minutes.
[0042] Furthermore, the nitrite content of the second post-treatment solution is 0.01-1 wt%, preferably 0.1-0.5 wt%. The protic acid content is 0.01-1 wt%, preferably 0.3-0.6 wt%.
[0043] Furthermore, the second post-treatment solution contains nitrite or sulfite, which is any one or two or more of sodium nitrite, potassium nitrite, calcium nitrite, ammonium nitrite, sodium sulfite, and potassium sulfite in any proportion.
[0044] Furthermore, the protic acid in the second post-treatment solution is an inorganic acid and an organic acid. The inorganic acid is any one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, sulfurous acid, and boric acid, combined in any proportion. The organic acid is any one or more of methanesulfonic acid, trifluoroacetic acid, trichloroacetic acid, acetic acid, benzenehexacarboxylic acid, oxalic acid, p-toluenesulfonic acid, citric acid, oxalic acid, and nitrobenzoic acid, combined in any proportion.
[0045] Furthermore, the second post-treatment process takes 30-120 seconds, preferably 60-90 seconds. The heat treatment following immersion in the post-treatment solution is performed at a temperature of 80-100°C, preferably 85-95°C. The heat treatment time is 2-5 minutes, preferably 3-4 minutes.
[0046] Furthermore, the content of the polar protonic organic solvent in the activation solution is 0.3-3 wt%, preferably 0.8-2 wt%. The content of the strong protic acid is 5-15 wt%, preferably 8-10 wt%.
[0047] Furthermore, the activated solution's polar protonic organic solvent is any one or a combination of two or more of N,N'-dimethylformamide (DMF), N,N'-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), acetonitrile (ACN), ethyl acetate (ETA), dimethyl sulfoxide (DMSO), hexamethylphosphoramide (HMPA), dichloromethane (DCM), and tetrahydrofuran (THF) in any proportion.
[0048] Furthermore, the strong protic acid in the activation solution is any one or two or more of hydrochloric acid, sulfuric acid, phosphoric acid, benzenesulfonic acid, formic acid, dichloroacetic acid, squaric acid, and citric acid in any proportion.
[0049] Furthermore, the membrane is activated in the activation solution for 24-48 hours to remove oligomers in the molecular chain structure, and after protonation, a performance-enhanced antioxidant and alkali-resistant nanofiltration membrane is obtained.
[0050] The antioxidant and alkali-resistant nanofiltration membrane was prepared by the above method.
[0051] The above-mentioned antioxidant and alkali-resistant nanofiltration membranes have applications in the chemical fiber industry and the biopharmaceutical field.
[0052] Compared with the prior art, the technical effects of this invention are reflected in: This invention enhances the alkali resistance and oxidation resistance of alkali-resistant membranes from three aspects: the support layer, the intermediate layer, and the desalination layer. First, a functional nonwoven fabric (low density, high air permeability) is used as the support structure to enhance the anti-peeling properties of polymeric PES inside and on the surface of the membrane pores, solving the problem of easy oxidation and shedding of the PES layer in UF membranes. Second, a thermally cross-linked, highly adhesive polyhydroxy polymer macromolecule and porous inorganic nanomaterials are used as the intermediate layer. This further enhances the stability of the PES layer and regulates the structure of the desalination layer, providing more water molecule transport channels and ensuring the membrane's water production. Then, under the regulation of catalysts and stabilizers, the conversion efficiency of monomers in the reaction phase solution is improved, increasing the cross-linking degree of the desalination layer and enhancing the alkali resistance of the functional layer. Finally, the first treatment solution, the second post-treatment solution, and the activation solution are used as modifiers to enhance the oxidation resistance of the desalination layer and improve the desalination rate, obtaining an alkali-resistant nanofiltration membrane with high alkali resistance and oxidation resistance. This invention describes the technical solution from two aspects: material preparation and production process. The specific material preparation and production process are as follows: (1) Enhanced peel resistance of the support layer This invention uses low-density, high-permeability polypropylene nonwoven fabric as the support. During the phase transformation process in the coagulation bath, the polymer solution penetrates more deeply and with greater permeability within the nonwoven fabric, thereby increasing the anchoring strength of PES within the nonwoven fabric, enhancing peel resistance, and preventing physical detachment. Secondly, the low-density, high-permeability nonwoven fabric exhibits low water resistance, resulting in higher water flux for the functional layer. Furthermore, by selecting polymer-based macromolecules (non-traditional PVP series, as PVP molecular structures are not resistant to oxidation) as the pore-forming agent, the phase separation process is delayed, resulting in a support layer with high surface pore density and uniformly sized bubble-like pores in the lower layer. This solves the technical problem of PES layers being oxidized and destroyed and detached in a feed solution containing oxidants within a short period.
[0053] (2) Improving flux in the intermediate layer and regulating the structure of the desalination layer This invention uses highly hydrophilic and adhesive polyhydroxy polymer macromolecules and porous inorganic nanomaterials as an interlayer. Polymer macromolecules exhibit high self-polymerization upon heating and have a dense structure, but this leads to low flux in the functional layer. Inorganic nanomaterials possess a porous structure, ensuring flux, but their dispersibility and anchoring stability in the matrix are poor. Combining these two materials to form an interlayer solves the problems of easy aggregation and loss of porous inorganic nanomaterials, and also improves the problem of low desalination flux caused by excessive polymer crosslinking. The interlayer has three effects: First, it further regulates the pore structure, porosity, and pore size distribution of the UF membrane, resulting in higher porosity and more uniform pore size distribution. The interlayer contains polyhydroxy functional groups, which have strong hydrogen bonding with amine groups, thus slowing down the diffusion of aqueous amine monomers and improving the uniformity of the desalination layer, resulting in a thin and smooth surface desalination layer. Second, the crosslinked interlayer, sandwiched between the support layer and the desalination layer, can directly resist the erosion, damage, and isomerization of the PES layer under harsh environments. Thirdly, the intermediate layer has a dense porous structure, which provides additional water channels for water molecule transport, ensuring that the UF membrane maintains high flux performance even with the cross-linked intermediate layer applied.
[0054] (3) Enhanced alkali resistance stability of the desalination layer This invention uses hyperbranched polyethyleneimine as the aqueous phase master monomer, aromatic amine as the aqueous phase second monomer, and small molecule aldehyde as the polymer chain structure stabilizer, with pyridine as the oil phase reaction catalyst. First, the aromatic amine groups in this invention have high steric hindrance, reacting with the oil phase monomer cyanuric chloride to form CN single bonds, transforming the desalination layer from an aliphatic amine structure to an aliphatic amine-aromatic amine copolymer structure. A strong π-π bond stacking effect exists between the benzene ring and the cyanuric chloride heterocycle, enhancing the alkali and oxidation resistance of the desalination layer. Second, this invention uses a small molecule aldehyde solution as an aqueous phase stabilizer, which cross-links with the master monomer polyethyleneimine, pre-consuming some of the highly reactive primary amine groups in the molecular chain structure and forming C=N double bonds to further stabilize the alkali and oxidation resistance of the desalination layer. Third, this invention uses pyridine as an oil-phase reaction catalyst. The pyridine group has a strong electron-withdrawing ability and can chemically combine with cyanuric chloride to form pyridinium salt, effectively reducing the electron cloud density of the cyanuric chloride heterocycle, increasing the reactivity of the second and third groups in its structure, increasing monomer conversion efficiency, improving the crosslinking degree of the desalting layer, and enhancing alkali resistance and oxidation resistance.
[0055] (4) Enhanced antioxidant properties of the desalination layer First, this invention uses an organic solution composed of acid anhydride and organic solvent in a certain proportion as the first post-treatment solution. Unreacted primary amines (-NH2) in the polymer molecular structure undergo an imidization reaction with the acid anhydride, followed by cyclization at 80°C to produce a polyimide (-CO-NR-CO-) structure, thereby reducing the residual amount of -NH2 in the polymer structure. Second, this invention uses an aqueous solution composed of nitrite or sulfite and protic acid in a certain proportion as the second post-treatment solution. Unreacted secondary amines (-NH-) in the polymer molecular structure undergo a nitroso reaction in an oxidation system to generate a nitrosamine (-NR-N=O) structure, thereby completely consuming and converting the easily oxidized active sites (primary and secondary amines) in the structure. This results in a special nanofiltration membrane with strong oxidation resistance and high alkali stability.
[0056] (5) Evaluation of overall performance improvement and alkali resistance and oxidation resistance This invention uses an aqueous solution composed of a polar protic organic solvent and a strong protic acid as the activation solution to remove oligomers from the molecular chain structure. Simultaneously, the protonation of nitrogen atoms imparts a higher positive charge density to the desalination layer, resulting in a nanofiltration membrane with enhanced performance and improved oxidation and alkali resistance. At an operating pressure of 110 psi, with an initial flux of 44.2 L / m²·h (26 gfd), the MgSO₄ rejection rate was 99.8%. After static treatment with 20 wt% NaOH for 7 days, the desalination rate reached 99.5%. After continuous dynamic oxidation operation in a 1000 ppm H₂O₂ aqueous solution at 45°C for 72 hours, the membrane retained 98.8% of the MgSO₄, with the desalination rate decreasing by only 0.7 percentage points, maintaining the alkali and oxidation resistance of the desalination layer. Detailed Implementation
[0057] The present invention will be described in detail below with reference to embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the present invention in any way. It should be noted that those skilled in the art can make several adjustments and improvements without departing from the concept of the present invention. These all fall within the protection scope of the present invention.
[0058] Unless otherwise specified, all materials and instruments used in the following embodiments are commercially available.
[0059] Example 1 Enhanced peel resistance of the support layer: A PES polymer solution with a mass concentration of 18% using DMF as solvent and a PEG400 pore-forming agent content of 0.3 wt% was prepared. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric, followed by coagulation bath and heat setting processes to obtain the support layer (UF film-1). Using the same process, a polymer solution with PVP as a pore-forming agent was coated onto a conventional nonwoven fabric to obtain a traditional UF film-2. The peel resistance and oxidation resistance of the support layer (PES) were tested. UF membrane-1, the polymer solution penetrates deeply into the nonwoven fabric, preventing the support layer from being completely peeled off, resulting only in tiny fragments. After 72 hours of oxidation with 1000ppm H2O2 and subsequent dehydration and drying, the support layer remains intact, without cracks or peeling. The peel strength and oxidation resistance of the support layer (PES) are maintained.
[0060] In UF membrane-2, the polymer solution penetrates only shallowly into the nonwoven fabric, allowing the support layer to be easily and completely peeled off completely, with a low peel force of 0.6-0.8 N / cm. After 72 hours of oxidation with 1000 ppm H2O2 followed by dehydration and drying, localized cracking and detachment of the support layer were observed. The support layer (PES) exhibits poor peel resistance and oxidation resistance.
[0061] Example 2 Intermediate layer regulation of support layer (PES) structure and flux: A PES polymer solution with a mass concentration of 18% using DMF as solvent and a polymer-based pore-forming agent PEI1800 content of 0.8 wt% was prepared. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric, and after coagulation bath and heat setting processes, a support layer (UF membrane-3) was obtained. Then, intermediate layer aqueous solutions containing 0.5 wt% polyhydroxy polymer and 0.5 wt% polyhydroxy polymer + 0.05 wt% porous inorganic nanomaterials were prepared, respectively. UF membrane-3 was immersed in the intermediate layer aqueous solution for 5 s without effect and then set at 85℃ for 2 min to obtain UF membrane-4 and UF membrane-5, respectively. The flux and physical properties of the UF membranes were tested. The UF membrane-3 has a relatively large surface pore size of 6-10 nm, a high flux of 446.8 gfd, and a hydrophilic contact angle of 78.3°. The diffusion rate of the aqueous phase amine monomer is extremely fast and uncontrolled, resulting in a thick desalination layer and high roughness of the membrane.
[0062] UF membrane-4 has a small surface pore size of 0.3-1.0 nm, a low flux of 120-150 gfd, and a hydrophilic contact angle of 62-66°. The diffusion rate of aqueous amine monomers is slowed down, resulting in a thinner desalination layer and lower roughness of the membrane.
[0063] The UF membrane-5 has a moderate surface pore size of 2.0-3.0 nm, a moderate flux of 250-300 gfd, and a hydrophilic contact angle of 42-45°, which further slows down the diffusion rate of aqueous amine monomers and further reduces the thickness and roughness of the membrane desalination layer.
[0064] Example 3 Enhanced alkali resistance of the desalination layer: A PES polymer solution with a mass concentration of 18% using DMF as solvent and a polymer-based pore-forming agent PEI1800 content of 0.8 wt% was prepared. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric and subjected to a coagulation bath and heat setting process to obtain a support layer (UF membrane). Then, the UF membrane was immersed in an aqueous solution containing 0.5 wt% polyhydroxy polymer and 0.05 wt% porous inorganic nanomaterials for 5 seconds and set at 85°C for 2 minutes to obtain a modified support layer (m-UF). Next, the m-UF was subjected to an aqueous solution containing a second monomer, aromatic amine, and a stabilizer, dialdehyde, for 60 seconds, followed by hydraulic air purging until no solution residue remained on the surface. Then, it was subjected to an oil solution containing a catalyst, pyridine, for 60 seconds, followed by drying at 85°C to obtain an alkali-resistant and oxidation-resistant NF membrane.
[0065] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested.
[0066] Example 4 Enhanced Oxidation Stability of Desalination Layer: A 18% (w / w) PES polymer solution was prepared using DMF as solvent, with 0.8 wt% PEI1800 as the polymer-based pore-forming agent. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric, and then coated and heat-set using a coagulation bath to obtain a support layer (UF membrane). The UF membrane was then immersed in an aqueous solution containing 0.5 wt% polyhydroxy polymer and 0.05 wt% porous inorganic nanomaterials for 5 seconds, followed by setting at 85°C for 2 minutes to obtain a modified support layer (m-UF). Next, the m-UF was passed through an aqueous solution containing a second monomer, aromatic amine, and a stabilizer, dialdehyde, for 60 seconds, followed by hydraulic air purging until no solution residue remained on the surface. Finally, it was passed through an oil solution containing a catalyst, pyridine, for 60 seconds, and then dried at 85°C to obtain an alkali-resistant and oxidation-resistant NF membrane. Next, the NF membrane was immersed in a first post-treatment solution containing 0.8 wt% organic solvent for 20 s and then heat-treated at 60°C for 2 min to remove primary amines (-NH2) from the desalination layer structure, thus obtaining an oxidation-resistant NF-m-1 nanofiltration membrane. Then, the NF-m-1 nanofiltration membrane was subjected to a second treatment solution consisting of nitrite or sulfite (0.05 wt%), protic acid (0.1 wt%), and pure water for 30 s and then heat-treated at 80°C for 2 min to remove secondary amines (-NH-) from the desalination layer structure, thus obtaining an oxidation-resistant NF-m-2 nanofiltration membrane. Finally, the oxidation resistance of the membrane was tested.
[0067] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested.
[0068] Example 5 Enhancement of the overall performance (flux + desalination rate) of the desalination layer: A PES polymer solution with a mass concentration of 18% using DMF as solvent and a polymer-based pore-forming agent PEI1800 content of 0.8 wt% was prepared. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric, and after coagulation bath and heat setting processes, a support layer (UF membrane) was obtained. Then, the UF membrane was immersed in an aqueous solution of 0.5 wt% polyhydroxy polymer + 0.05 wt% porous inorganic nanomaterials for 5 s, and then set at 85°C for 2 min to obtain a modified support layer (m-UF). Next, the m-UF was subjected to an aqueous solution containing a second monomer aromatic amine and a stabilizer dialdehyde for 60 s, and then purged with hydraulic air until no solution residue remained on the surface. Then, it was subjected to an oil solution containing a catalyst pyridine for 60 s, and then dried at 85°C to obtain an alkali-resistant and oxidation-resistant NF membrane. Next, the NF membrane was immersed in a first post-treatment solution containing 0.8 wt% anhydride in an organic solvent for 20 s, followed by heat treatment at 60°C for 2 min to remove primary amines (-NH2) from the desalination layer structure, yielding an oxidation-resistant NF-m-1 nanofiltration membrane. Then, the NF-m-1 nanofiltration membrane was subjected to a second treatment solution consisting of 0.05 wt% nitrite or sulfite, 0.1 wt% protic acid, and pure water for 30 s, followed by heat treatment at 80°C for 2 min to remove secondary amines (-NH-) from the desalination layer structure, yielding an oxidation-resistant NF-m-2 nanofiltration membrane. Finally, the oxidation-resistant NF-m-2 nanofiltration membrane was activated in an aqueous solution containing a strong protic acid and a polar protic solvent (8 wt% strong protic acid, 0.8% polar protic solvent, for 24 h). This resulted in an alkali-resistant and oxidation-resistant nanofiltration membrane, NF-HOR, with improved overall performance, and its basic properties were tested.
[0069] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested; ④ Calculation of the percentage decrease in desalination rate: Percentage decrease in desalination rate = Desalination rate after alkali treatment - Desalination rate after oxidation.
[0070] Example 6 Preferred process formula one: Comprehensive Performance Enhancement: A PES polymer solution with a mass concentration of 18% using DMF as solvent and a polymer-based pore-forming agent PEI3000 content of 1.0 wt% was prepared. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric and subjected to a coagulation bath and heat setting process to obtain a support layer (UF film). Then, the UF film was immersed in an aqueous solution containing 0.5 wt% polyhydroxy polymer PVA and 0.05 wt% porous zero-dimensional inorganic nanomaterial silica for 5 seconds, followed by setting at 85°C for 2 minutes to obtain a modified support layer (m-UF). Next, the m-UF was subjected to an aqueous solution containing 0.5 wt% p-methylaniline (a second monomer) and 0.3 wt% 2-nitro-terephthalaldehyde (a stabilizer) for 60 seconds, followed by hydraulic air purging until no solution residue remained on the surface. Finally, it was subjected to an oil-phase solution containing the catalyst 2,6-diaminopyridine for 60 seconds, followed by drying at 85°C to obtain an alkali-resistant and oxidation-resistant NF film. Next, the NF membrane was immersed in a first post-treatment solution containing 1.0 wt% acetic anhydride organic solvent for 20 s, followed by heat treatment at 70°C for 2 min to remove primary amines (-NH2) from the desalination layer structure, yielding an oxidation-resistant NF-m-1 nanofiltration membrane. Then, the NF-m-1 nanofiltration membrane was subjected to a second treatment solution consisting of sodium nitrite (0.1 wt%), hydrochloric acid (0.3 wt%), and pure water for 60 s, followed by heat treatment at 85°C for 3 min to remove secondary amines (-NH-) from the desalination layer structure, yielding an oxidation-resistant NF-m-2 nanofiltration membrane. Finally, the oxidation-resistant NF-m-2 nanofiltration membrane was activated in an aqueous solution containing a strong protic acid and a polar protic solvent (8 wt% strong protic sulfuric acid and 0.8% DMAc), with an activation time of 24 h. This resulted in an alkali-resistant and oxidation-resistant nanofiltration membrane, NF-HOR, with improved overall performance, and its basic properties were tested.
[0071] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested; ④ Calculation of the percentage decrease in desalination rate: Percentage decrease in desalination rate = Desalination rate after alkali treatment - Desalination rate after oxidation.
[0072] Example 7 Preferred process formula two: Comprehensive Performance Enhancement: A 19% PES polymer solution with DMAc as solvent and 1.5 wt% PEG400 polymer-based pore-forming agent were prepared. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric and subjected to a coagulation bath and heat setting process to obtain a support layer (UF membrane). The UF membrane was then immersed in an aqueous solution containing 0.7 wt% PDA (polyhydroxy polymer) and 0.1 wt% carbon nanowires (porous one-dimensional inorganic nanomaterial) for 5 seconds, followed by setting at 85°C for 2 minutes to obtain a modified support layer (m-UF). Next, the m-UF was subjected to an aqueous solution containing 0.7 wt% 3,4-diaminotoluene (second monomer) and 0.4 wt% 2,3-dihydroxyterephthalaldehyde (stabilizer) for 60 seconds, followed by hydraulic air purging until no solution residue remained on the surface. Finally, it was subjected to an oil solution containing 2,4'-dipyridine (catalyst) for 60 seconds, followed by drying at 85°C to obtain an alkali-resistant and oxidation-resistant NF membrane. Next, the NF membrane was immersed in a first post-treatment solution containing 1.5 wt% benzoic anhydride organic solvent for 20 s, followed by heat treatment at 70°C for 2 min to remove primary amines (-NH2) from the desalination layer structure, yielding an oxidation-resistant NF-m-1 nanofiltration membrane. Then, the NF-m-1 nanofiltration membrane was subjected to a second treatment solution consisting of potassium nitrite (0.2 wt%), sulfuric acid (0.3 wt%), and pure water for 60 s, followed by heat treatment at 85°C for 3 min to remove secondary amines (-NH-) from the desalination layer structure, yielding an oxidation-resistant NF-m-2 nanofiltration membrane. Finally, the oxidation-resistant NF-m-2 nanofiltration membrane was activated in an aqueous solution containing a strong protic acid and a polar protic solvent (8 wt% strong protic hydrochloric acid, 0.8% DMF, and 24 h). This resulted in an alkali-resistant and oxidation-resistant nanofiltration membrane, NF-HOR, with improved overall performance, and its basic properties were tested.
[0073] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested; ④ Calculation of the percentage decrease in desalination rate: Percentage decrease in desalination rate = Desalination rate after alkali treatment - Desalination rate after oxidation.
[0074] Example 8 Optimal process formula three: Comprehensive Performance Enhancement: A 20% (w / w) polysulfone (PS) polymer solution was prepared using NMP as solvent, with 2.0 wt% PEG1000 as the polymer-based pore-forming agent. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric and subjected to a coagulation bath and heat setting process to obtain a support layer (UF membrane). The UF membrane was then immersed in an aqueous solution containing 1.0 wt% chitosan (CS), a polyhydroxy polymer, and 0.2 wt% boron, carbon, and nitrogen nanosheets (a porous two-dimensional inorganic nanomaterial) for 8 seconds, followed by setting at 85°C for 2 minutes to obtain a modified support layer (m-UF). Next, the m-UF was subjected to an aqueous solution containing 1.0 wt% 2,4-diaminophenol as a second monomer and 0.5 wt% glutaraldehyde as a stabilizer for 70 seconds, followed by hydraulic air purging until no solution residue remained on the surface. Finally, it was subjected to an oil solution containing 3,4'-dipyridin-2'-amine as a catalyst for 70 seconds, followed by drying at 85°C to obtain an alkali-resistant and oxidation-resistant NF membrane. Next, the NF membrane was immersed in a first post-treatment solution containing 2.0 wt% pyromellitic anhydride in an organic solvent for 30 s, followed by heat treatment at 70°C for 2 min to remove primary amines (-NH2) from the desalination layer structure, yielding an oxidation-resistant NF-m-1 nanofiltration membrane. Then, the NF-m-1 nanofiltration membrane was subjected to a second treatment solution consisting of sodium sulfite (0.3 wt%), phosphoric acid (0.4 wt%), and pure water for 70 s, followed by heat treatment at 85°C for 3 min to remove secondary amines (-NH-) from the desalination layer structure, yielding an oxidation-resistant NF-m-2 nanofiltration membrane. Finally, the oxidation-resistant NF-m-2 nanofiltration membrane was activated in an aqueous solution containing a strong protic acid and a polar protic solvent (8 wt% strong protic benzoic acid, 1.0% DMAc, and 24 h). This resulted in an alkali-resistant and oxidation-resistant nanofiltration membrane, NF-HOR, with improved overall performance, and its basic properties were tested.
[0075] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested; ④ Calculation of the percentage decrease in desalination rate: Percentage decrease in desalination rate = Desalination rate after alkali treatment - Desalination rate after oxidation.
[0076] Example 9 Optimal process formula four: Overall performance improvement: A sulfonated polyethersulfone polymer solution with a mass concentration of 21% using DMSO as solvent and a polymer-based pore-forming agent PVA1000 content of 2.0 wt% was prepared. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric, and after coagulation bath and heat setting processes, a support layer (UF film) was obtained. Then, the UF film was immersed in an aqueous solution of 1.2 wt% polyhydroxy polymer hyaluronic acid (HA) and 0.3 wt% porous three-dimensional inorganic nano MOF material as an intermediate layer for 8 s, and set at 90°C for 3 min to obtain a modified support layer (m-UF). Next, the m-UF was subjected to an aqueous solution containing 1.2 wt% of the second monomer 2,4,6-triaminochlorobenzene and 0.6 wt% of the stabilizer hexamethylenetetramine for 80 s, and then purged with hydraulic air until no solution residue remained on the surface. Then, after applying the film to an oil phase solution containing the catalyst 2,4,6-tris(pyridin-4-yl)pyridine for 80 seconds, it is dried at 90°C to obtain an alkali-resistant and oxidation-resistant NF film. Next, the NF membrane was immersed in a first post-treatment solution containing 2.5 wt% ethylenediaminetetraacetic anhydride in an organic solvent for 40 s, followed by heat treatment at 80°C for 3 min to remove primary amines (-NH2) from the desalination layer structure, yielding an oxidation-resistant NF-m-1 nanofiltration membrane. Then, the NF-m-1 nanofiltration membrane was subjected to a second treatment solution consisting of ammonium nitrite (0.4 wt%), trifluoroacetic acid (0.5 wt%), and pure water for 80 s, followed by heat treatment at 85°C for 3 min to remove secondary amines (-NH-) from the desalination layer structure, yielding an oxidation-resistant NF-m-2 nanofiltration membrane. Finally, the oxidation-resistant NF-m-2 nanofiltration membrane was activated in an aqueous solution containing a strong protic acid and a polar protic solvent (9 wt% strong protic dichloroacetic acid and 1.5% NMP) for 48 h. This resulted in an alkali-resistant and oxidation-resistant nanofiltration membrane, NF-HOR, with improved overall performance, and its basic properties were tested.
[0077] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested; ④ Calculation of the percentage decrease in desalination rate: Percentage decrease in desalination rate = Desalination rate after alkali treatment - Desalination rate after oxidation.
[0078] Example 10 Optimal process formula five: Overall performance improvement: A sulfonated polyethersulfone polymer solution with a mass concentration of 22% using DMSO as solvent was prepared, with a polymer-based pore-forming agent F-127 3000 content of 2.5 wt%. After vacuum degassing, the polymer solution was coated onto a functional nonwoven fabric, and after coagulation bath and heat setting processes, a support layer (UF film) was obtained. Then, the UF film was immersed in an aqueous solution containing 1.5 wt% of the polyhydroxy polymer dextran (DT) and 0.4 wt% of the porous two-dimensional inorganic nanomaterial graphene oxide as an intermediate layer for 10 s, and then set at 90°C for 3 min to obtain a modified support layer (m-UF). Next, the m-UF was subjected to an aqueous solution containing 1.2 wt% of the second monomer 4,5-dimethyl-1,2-phenylenediamine and 0.8 wt% of the stabilizer 2-methylglutaraldehyde for 90 s, and then purged with hydraulic air until no solution residue remained on the surface. Then, after applying the film to an oil phase solution containing the catalyst 4-(2,4,5-tripyridin-4-ylphenyl)pyridine for 90 seconds, it is dried at 90°C to obtain an alkali-resistant and oxidation-resistant NF film. Next, the NF membrane was immersed in a first post-treatment solution containing 3.0 wt% 1,2,3,4-cyclopentanetetracarboxylic dianhydride in an organic solvent for 40 s, followed by heat treatment at 80°C for 3 min to remove primary amines (-NH2) from the desalination layer structure, yielding an oxidation-resistant NF-m-1 nanofiltration membrane. Then, the NF-m-1 nanofiltration membrane was subjected to a second treatment solution consisting of 0.5 wt% calcium nitrite, 0.6 wt% benzohexacarboxylic acid, and pure water for 90 s, followed by heat treatment at 95°C for 4 min to remove secondary amines (-NH-) from the desalination layer structure, yielding an oxidation-resistant NF-m-2 nanofiltration membrane. Finally, the oxidation-resistant NF-m-2 nanofiltration membrane was activated in an aqueous solution containing a strong protic acid and a polar protic solvent. The strong protic acid concentration was 10 wt%, and the polar protic solvent hexamethylphosphoramide concentration was 2.0%, with an activation time of 48 h. An alkali-resistant and oxidation-resistant nanofiltration membrane, NF-HOR, with improved overall performance, was obtained, and its basic properties were tested.
[0079] ① Desalination rate test conditions: MgSO4 concentration 2000ppm, operating pressure 110psi, water temperature 25℃, recovery rate 15%; ② Alkali resistance stability test: The membrane was statically immersed in 20% NaOH aqueous solution at room temperature for 7 days to test the desalination rate; ③ Oxidation stability test: After the membrane was dynamically operated in a 1000ppm H2O2 aqueous solution for 72 hours, the desalination rate was tested; ④ Calculation of the percentage decrease in desalination rate: Percentage decrease in desalination rate = Desalination rate after alkali treatment - Desalination rate after oxidation.
[0080] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, or alterations made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing an antioxidant and alkali-resistant nanofiltration membrane, characterized in that, Includes the following steps: (1) Preparation of polymer solution: Polyethersulfone (PES) and polymer-based macromolecular pore-forming agent are dissolved in organic solvent to prepare a polymer solution. After vacuum degassing at 30-35℃ for 4 hours, the solution is kept warm. The polymer solution is scraped onto polypropylene (PP) nonwoven fabric with a scraper at room temperature of 20-25℃, ambient humidity of 80-85%, scraping speed of 6m / min, coagulation bath temperature of 10-15℃, coagulation bath exposure time of 10-15s, and hot water bath temperature of 60-70℃. After rinsing with deionized water, a porous base membrane (UF membrane) is obtained. (2) Preparation of intermediate layer blending solution: A liquid phase solution composed of highly hydrophilic and highly adhesive polyhydroxy polymer macromolecules and porous inorganic nanomaterials is coated onto the UF membrane. After being heated at 80°C, a homogeneous high-porosity thermal crosslinking layer is formed and anchored to the surface of the UF membrane. (3) Preparation of aqueous solution: The aqueous solution composed of the main monomer polyethyleneimine, the second monomer aromatic amine (Ar-NH2), the stabilizer difunctional aldehyde (OHC-R-CHO) and the auxiliary agent is uniformly applied to the surface of the UF membrane. After 60-90 seconds, the solution is blown away with hydraulic air until there is no residue. (4) Preparation of oil phase solution: The ethyl solution composed of the main monomer cyanuric chloride, the catalyst pyridine and the co-solvent is uniformly applied to the membrane surface of (3) above. After 60-90s, the residual solution is removed with a rubber guide roller to form a nascent nanofiltration membrane. (5) Preparation and treatment of the first post-treatment solution: The solution composed of acid anhydride and organic solvent is used as the first post-treatment solution; the nascent nanofiltration membrane obtained in (4) above is statically immersed in the first post-treatment solution for 20-30s and heat-treated at 60-80℃ for 2min to completely convert the unreacted primary amine (-NH2) in the polymer structure into a polyimide (-CO-NR-CO-) structure; (6) Preparation of the second post-treatment solution: The second post-treatment solution is an aqueous solution composed of nitrite or sulfite and protic acid; the nanofiltration membrane (5) above is statically immersed in the second post-treatment solution for 60-90s and heat-treated at 80-100℃ for 3min to completely convert the unreacted secondary amine (-NH-) in the polymer structure into nitrosamine (-NR-N=O) structure; (7) The nanofiltration membrane with the above (6) function is immersed in an aqueous solution of 1wt% N, N-dimethylformamide (DMF) and 8wt% H2SO4 for 24h to remove oligomers in the molecular chain structure. At the same time, the N atoms are protonated to give the desalination layer a higher positive charge density, thereby obtaining an antioxidant and alkali resistant nanofiltration membrane with enhanced performance.
2. The preparation method according to claim 1, characterized in that, The polymer solution is any one or two or more of polysulfone, polyethersulfone, sulfonated polyethersulfone, and polyetheretherketone in any proportion; the polymer has a molecular weight of 60,000-100,000 Da and the polymer solution has a mass concentration of 17-22 wt%.
3. The preparation method according to claim 1, characterized in that, The organic solvent used to prepare the polymer solution is any one or two or more of N,N'-dimethylformamide (DMF), N,N'-dimethylhexamethylene (DMAc), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO) in any proportion.
4. The preparation method according to claim 1, characterized in that, The polymer-based macromolecular pore-forming agent is any one or a combination of two or more of the following: polyethylene glycol (PEG) with a molecular weight of 400-2000 Da, polyethyleneimine (PEI) with a molecular weight of 1000-6000 Da, polyvinyl alcohol (PVA) with a molecular weight of 1000-6000 Da (degree of hydrolysis 89-90%), and amphiphilic block copolymer F-127 with a molecular weight of 2000-6000 Da; the content of the pore-forming agent is 0.1-6 wt%.
5. The preparation method according to claim 1, characterized in that: The preparation conditions for the porous UF membrane are as follows: room temperature 20-25℃, ambient humidity 80-85%, membrane scraping speed 5-6m / min, front coagulation bath temperature 10-15℃, coagulation bath exposure time 10-15s, and rear hot water tank temperature 60-70℃.
6. The preparation method according to claim 1, characterized in that: The intermediate layer solution is a homogeneous aqueous solution composed of a highly adhesive polyhydroxy polymer and porous inorganic nanomaterials. The polyhydroxy polymer is any one or two or more of polyvinyl alcohol (PVA), polydopamine (PDA), chitosan (CS), hyaluronic acid (HA), and dextran (DT) in any proportion, with a solution content of 0.2-2 wt%.
7. The preparation method according to claim 1, characterized in that: The aqueous phase second monomer aromatic amine (Ar-NH2) is any one or two or more of aromatic monoamines, aromatic diamines, aromatic triamines and their derivatives in any proportion; the aqueous phase content is 0.2-2wt%, preferably 0.5-1.5wt%.
8. The preparation method according to claim 1, characterized in that: The stabilizer is an aliphatic or aromatic dialdehyde, and the amount added is 0.1-1 wt%.
9. The preparation method according to claim 1, characterized in that: The organic phase pyridine catalyst is any one or more of monopyridine, dipyridine, ternary pyridine and their derivatives in any proportion; the amount of organic phase added is 0.01-1wt%, preferably with n≥2 pyridine groups.
10. The preparation method according to claim 1, characterized in that: The content of the acid anhydride in the first post-treatment solution is 0.5-5 wt% in the organic solution; the acid anhydride is any one or two or more of monofunctional acid anhydrides, difunctional acid anhydrides, and their derivatives in any proportion.
11. The preparation method according to claim 1, characterized in that: The initial ecological membrane is subjected to a first post-treatment solution process for 10-60 seconds; after being impregnated with the post-treatment solution, it undergoes a heat treatment at a temperature of 60-100℃ for 1-5 minutes.
12. The preparation method according to claim 1, characterized in that: The second post-treatment solution has a nitrite content of 0.01-1 wt% and a protic acid content of 0.01-1 wt%, preferably 0.3-0.6 wt%.
13. An antioxidant and alkali-resistant nanofiltration membrane prepared by the preparation method according to any one of claims 1-12.
14. The use of the antioxidant and alkali-resistant nanofiltration membrane according to claim 13 in the chemical fiber industry and the biopharmaceutical field.
Citation Information
Patent Citations
Preparation method of antioxidant acid-base resistant nanofiltration membrane
CN109692586A