A nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method and application

By preparing nanofiber-like titanium dioxide precursors and combining them with lithiation, calcination, and elution treatments, the problem of uneven particle size in nanoscale lithium-ion sieves was solved, improving adsorption performance and recovery efficiency, reducing preparation costs, and making it suitable for the extraction of liquid lithium resources.

CN123102291APending Publication Date: 2026-11-17BEIJING INST OF FUTURE SCI & TECH ON BIOINSPIRED INTERFACE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611005384.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare nanoscale lithium-ion sieves with uniform particle size distribution, resulting in poor adsorption performance and difficulty in efficient recovery. Traditional methods are prone to agglomeration and are costly.

Method used

By transforming titanium dioxide precursor into nanofiber-like titanium dioxide precursor, and then subjecting it to lithiation, calcination, and elution, a nanoscale lithium-ion sieve with uniform particle size distribution was prepared. Alkali etching and heating reaction were carried out in a polytetrafluoroethylene reaction vessel to form an internal self-condensation process. Combined with calcination and acid washing, a nanoscale titanium-based lithium-ion sieve with a regular hexahedral morphology was formed.

Benefits of technology

The uniform particle size distribution of nanoscale lithium-ion sieves was achieved, which improved the adsorption capacity and adsorption performance, reduced the solubility loss rate, reduced the preparation cost, and exhibited excellent lithium-ion adsorption capacity under different pH environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102291A_ABST
    Figure CN123102291A_ABST
Patent Text Reader

Abstract

This invention provides a uniformly sized nanoscale lithium-ion sieve, its preparation method, and its application. By transforming titanium dioxide precursor particles into nanofiber-like titanium dioxide precursors (length-to-diameter ratio 1:10~100), and then subjecting them to lithiation, calcination, and elution treatments, a uniformly sized nanoscale lithium-ion sieve is obtained. This invention not only produces adsorbent materials with excellent performance but also effectively reduces labor and preparation costs. The titanium-based lithium-ion sieve Li2TiO3 adsorbent has a uniformly sized and regularly morphologically regular nanoscale particle distribution. The titanium-based lithium-ion sieve is regularly hexahedral with a particle size of approximately 20 nm to 80 nm, exhibiting the characteristic of uniform distribution in various solvents (dynamic light scattering tests conform to a normal distribution). The titanium-based lithium-ion sieve particles prepared by this invention have a regular morphology, high adsorption capacity, and low solubility loss. Under different pH conditions, its lithium-ion adsorption capacity is 30~120 mg / g, and the adsorption equilibrium time is 8~12 hours, making it suitable for the extraction of liquid lithium resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of general physical or chemical methods or apparatus, and specifically to a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application. Background Technology

[0002] Lithium, as a key strategic mineral resource, holds an irreplaceable position in modern industrial and social development and is known as "white oil." Lithium is widely used in ceramics, chemicals, pharmaceuticals, nuclear industry, and lithium batteries, playing a particularly crucial role in the new energy industry. According to relevant research, it is predicted that the world may consume about one-third of its current exploitable lithium resources within the next thirty years, leading to a tightening supply-demand relationship. Currently, the world's proven exploitable lithium reserves are approximately 140 million tons, mainly found in ore and brine. Traditional ore-based lithium extraction processes are energy-intensive and generate significant pollution. In contrast, low-grade liquid lithium resources such as salt lake brines and seawater are extremely rich in dissolved lithium, especially seawater, which has a theoretical reserve of approximately 230 billion tons, equivalent to more than 1600 times the current global exploitable lithium reserves. Therefore, liquid-phase lithium extraction technology has attracted widespread attention, and the focus of lithium resource development is gradually shifting from solid ore to liquid resources such as salt lake brines and seawater.

[0003] my country possesses abundant lithium resources in its salt lakes, but extraction efficiency and environmental impact remain significant challenges, necessitating the development of new, efficient, and environmentally friendly lithium extraction materials. Among various liquid-phase lithium extraction materials, lithium-ion sieve adsorbents are considered one of the most promising, possessing advantages such as high selectivity, good cycle stability, and relatively simple processing.

[0004] Currently, the most studied lithium-ion adsorbents are mainly manganese-based and titanium-based. Manganese-based ion sieves have poor structural stability, resulting in severe manganese loss during acid leaching, leading to short cycle life and water pollution. Titanium-based ion sieves, due to their strong titanium-oxygen bonding energy, exhibit less titanium loss during elution, facilitating repeated adsorption-desorption cycles. By preparing titanium-based lithium-ion sieves into nanoscale particles with uniform size distribution, the specific surface area and effective adsorption sites are increased.

[0005] Currently, lithium-ion sieves obtained through high-temperature solid-phase reactions suffer from limitations such as poor particle size control, easy agglomeration, and difficulty in particle size control. Suspension polymerization granulation involves first modifying the surface of hydrophilic lithium titanate powder with a silane coupling agent to achieve stable dispersion in an organic phase, followed by suspension polymerization to prepare lithium-ion sieves. However, this method is affected by the reaction of the coupling agent, making it unsuitable for preparing nanoscale lithium-ion sieves with uniform particle size distribution. Methods such as thermal synthesis and calcination are used to precisely control the micro / nano structure, preparing titanium-based lithium-ion sieves into nanoscale particles with uniform size distribution, increasing specific surface area and effective adsorption sites, and improving the adsorption performance of titanium-based lithium-ion sieves. The limitation of difficult recovery of nanoscale adsorbents can be addressed through granulation, bonding, and composite methods to improve recovery efficiency; however, the adsorption performance is still determined by the adsorption performance of the titanium-based lithium-ion sieve.

[0006] Therefore, there is a need for a nanoscale lithium-ion sieve capable of producing uniform particle size distribution. Summary of the Invention

[0007] This invention addresses the issues of particle size and adsorption capacity in nanoscale lithium-ion sieves by providing a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its applications. The method involves transforming titanium dioxide precursor particles into nanofiber-like titanium dioxide precursors (length-to-diameter ratio 1:10~100), followed by lithiation, calcination, and elution treatments to create a nanoscale lithium-ion sieve with uniform particle size distribution. This invention not only yields adsorbent products with excellent performance but also effectively reduces labor and preparation costs. The titanium-based lithium-ion sieve Li2TiO3 adsorbent exhibits uniform particle size distribution and regular morphology, with the titanium-based lithium-ion sieve being a regular hexahedron with a particle size of approximately 20 nm to 80 nm. It also demonstrates uniform distribution in various solvents (dynamic light scattering tests show a normal distribution). The titanium-based lithium-ion sieve prepared by this invention has regular particle morphology, high adsorption capacity, and low solubility loss. Under different pH conditions, its lithium-ion adsorption capacity is 30~120 mg / g, and the adsorption equilibrium time is 8~12 hours, making it suitable for the extraction of liquid lithium resources.

[0008] This invention provides a nanoscale lithium ion sieve with uniform particle size distribution. The nanoscale lithium ion sieve is obtained by eluting a nanoscale titanium-based lithium ion sieve. The capacity to adsorb lithium ions in the pH range of 5 to 12 is 30 to 130 mg / g. The nanoscale titanium-based lithium ion sieve is a regular hexahedral Li2TiO3 with a particle size of 20 nm to 80 nm. The nanoscale titanium-based lithium-ion sieve is obtained by calcining a nanofiber titanium source precursor with a lithium source. The nanofiber titanium source precursor is titanium dioxide with an aspect ratio of 1:(10~100).

[0009] This invention provides a method for preparing nanoscale lithium-ion sieves with uniform particle size distribution, comprising the following steps: S1. Add titanium-based lithium-ion sieve precursor powder to a polytetrafluoroethylene reaction vessel, then add alkaline solution, then seal the polytetrafluoroethylene reaction vessel and place it in an oil bath to carry out alkaline etching reaction under normal pressure, and then separate, wash, dry and calcine in sequence to obtain nanofiber titanium source precursor. The molar ratio of the titanium-based lithium-ion sieve precursor powder to the solute in the alkaline solution is 1:(10~25). The precursor powder for titanium-based lithium-ion sieves is metatitanic acid or rutile or anatase titanium dioxide with a particle size of 10~3000nm. S2. The nanofiber titanium source precursor and the lithium source are placed in a polytetrafluoroethylene reaction vessel, mixed evenly, and then the polytetrafluoroethylene reaction vessel is sealed and placed in an oil bath for heating, reaction, separation, washing, drying and calcination under normal pressure to obtain a nano-scale titanium-based lithium ion sieve. S3. The nano-sized titanium-based lithium ion sieve is eluted with dilute acid as an eluent, then washed and dried to obtain a nano-sized lithium ion sieve with a uniform particle size distribution.

[0010] The present invention discloses a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. In a preferred embodiment, in step S1, the polytetrafluoroethylene reaction vessel includes a bottle body and a bottle frame, both made of polytetrafluoroethylene and sealed by threaded connection. Titanium-based lithium ion sieve precursor powder and alkali are placed in a polytetrafluoroethylene reaction vessel and sealed. After ultrasonication for 20-40 minutes, the mixture is then placed in an oil bath. When titanium-based lithium-ion sieve precursor powder and alkali are etched in a polytetrafluoroethylene (PTFE) reaction vessel, 1 / 5 to 1 / 3 of the PTFE reaction vessel is heated in an oil bath, and 2 / 3 to 4 / 5 of the vessel is above the oil bath. During the etching reaction, the PTFE reaction vessel forms an internal self-condensation process. As the solvent boils, the vapor is condensed and refluxed. A near-solid-state process is formed at the bottom of the PTFE reaction vessel, transforming irregular titanium dioxide into fibrous titanium dioxide precursor. In step S2, when both the nanofiber titanium source precursor and the lithium source are placed in a polytetrafluoroethylene (PTFE) reaction vessel for reaction, 1 / 5 to 1 / 3 of the PTFE reaction vessel is heated in an oil bath, and 2 / 3 to 4 / 5 of the PTFE reaction vessel is above the oil bath. During the reaction, the PTFE reaction vessel forms an internal self-condensation process. As the solvent boils, the vapor is condensed and refluxed, and a near-solid-state process is formed at the bottom of the PTFE reaction vessel, resulting in a nanoscale titanium-based lithium ion sieve.

[0011] The present invention discloses a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. In a preferred embodiment, the mouth size of the polytetrafluoroethylene reaction vessel is smaller than the diameter of the vessel body, the vessel body is cylindrical, and the height of the vessel body is 1.5 to 4 times the diameter of the vessel body.

[0012] The present invention discloses a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. In a preferred embodiment, in step S1, the alkaline solution is any one of ammonia, piperidine, pyridine, triethylamine, lithium hydroxide, sodium hydroxide, potassium hydroxide, tert-butyllithium, sodium phenolate, and potassium tert-butoxide.

[0013] The present invention discloses a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. In a preferred embodiment, in step S1, the oil bath temperature is 50~180℃ and the etching reaction time is 12~36h. After the etching reaction, turn off the heating device and cool to room temperature. Add 30-100 mL of deionized water to the polytetrafluoroethylene reaction vessel and stir thoroughly. After standing for 1-5 hours, separate the product by filtration, dialysis, or centrifugation. Wash the white product repeatedly with water and ethanol alternately. Stop washing when the pH of the washing solution is 7-10. Dry the sample at 40-80℃ for 0.5-24 hours. After drying, the product is placed in a muffle furnace for calcination in an air or oxygen atmosphere. The temperature is increased by 1~10℃ / min during calcination and maintained at 200~850℃. After calcination for 2~24 hours, the temperature is reduced to room temperature by 1~10℃ / min to obtain nanofiber titanium source precursor.

[0014] The present invention discloses a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. In a preferred embodiment, in step S1, the diameter of the nanofiber titanium source precursor is 10~50nm and the aspect ratio is 1:(10~100).

[0015] The present invention discloses a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. In a preferred embodiment, in step S2, the lithium source is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium hydroxide, lithium carbonate, lithium oxalate, and lithium acetate. The molar ratio of nanofiber titanium source precursor to lithium source is 1:(1~5). After being mixed evenly in a mortar, it is placed in a muffle furnace for calcination. The heating rate during calcination is 1~10℃ / min. After heating to 200~850℃, the temperature is held for 2~12h. The cooling rate is 1~10℃ / min. When the temperature drops to room temperature, a nano-scale titanium-based lithium ion sieve is obtained. The nano-scale titanium-based lithium ion sieve is Li2TiO3. In step S3, during elution, the dilute acid is hydrochloric acid, nitric acid, or sulfuric acid solution with an ion concentration of 0.1~1 mol / L; the amount of eluent used is 20~100 mL / g of adsorbent precursor; the elution temperature is 15~80℃, the time is 0.5~48 h, and after elution, the solution is washed with water until neutral. The PDI of nanoscale lithium-ion sieves is less than or equal to 0.5.

[0016] The present invention discloses a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. In a preferred embodiment, a portion of the alkaline solution in step S1 is collected during separation, and the supernatant is collected during washing for dilution and recovery of the other portion. In step S2, the lithium source is recycled and reused.

[0017] This invention provides a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method. The nanoscale lithium-ion sieve is used as an adsorbent for lithium adsorption in dissolved lithium solutions, including salt lakes.

[0018] This invention provides nanoscale titanium-based lithium-ion sieve particles with uniform particle size distribution and their preparation method. The titanium-based lithium-ion sieve particles have a regular hexahedral appearance and a uniform particle size distribution; the nanoparticles have a diameter of 20-80 nm and can be uniformly distributed in various solvents (dynamic light scattering tests show a normal distribution). Titanium dioxide precursor particles are transformed into titanium dioxide nanowire precursors (aspect ratio 1:10-100), which are then subjected to lithiation and calcination to obtain nanoscale titanium-based lithium-ion sieve particles with uniform particle size distribution. The titanium-based lithium-ion sieve particles prepared by this invention have regular morphology, high adsorption capacity, and low solubility loss. Their lithium-ion adsorption capacity is 30-120 mg / g under different pH conditions, making them suitable for the extraction of liquid lithium resources.

[0019] This invention provides a method for preparing uniformly distributed nanoscale titanium-based lithium-ion sieve particles, the method comprising the following steps: (1) After the titanium-based lithium ion sieve precursor powder (titanium dioxide) is evenly dispersed in a solvent containing alkali, it is reacted, separated, washed, dried and calcined to obtain a modified nanofiber state source precursor. The titanium dioxide particle size is 10~10000nm, preferably 30~500nm; the titanium source is selected from one or more of rutile type, anatase type titanium dioxide, and metatitanic acid; the titanium source particle size is 10~3000nm, preferably 30~500nm; the alkali is selected from one or more of ammonia, piperidine, pyridine, triethylamine, lithium hydroxide, sodium hydroxide, potassium hydroxide, tert-butyllithium, sodium phenolate, and potassium tert-butoxide; the reaction temperature is 50~180℃; the calcination temperature and temperature control are as follows: the temperature is increased by 1~10℃ / min, and the calcination temperature is maintained in the range of 200~800℃, with the temperature varied or maintained at a certain level, and the calcination time is 2~12 hours (to stabilize the crystal lattice); the molar ratio of titanium to alkali is 1:(10~25).

[0020] The liquid phase heating reaction temperature is 50~180℃, preferably 80~150℃; the high-temperature solid phase sintering atmosphere is air or oxygen; the heating rate is 1~10℃ / min, preferably 3~6℃ / min; the sintering temperature is 200~850℃, preferably 200~400℃; and the sintering time is 2~24h, preferably 3~10h.

[0021] (2) The pretreated titanium source and lithium source are mixed evenly, and then a uniformly distributed nanoscale titanium-based lithium ion sieve is obtained by heating and reacting in a solid phase, separating, washing, drying and calcining. The modified titanium source has a diameter of 10-50 nm; the lithium source is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium hydroxide, lithium carbonate, lithium oxalate, and lithium acetate. The reaction temperature is 50-180℃, preferably 90-150℃; the calcination temperature and temperature control are as follows: the temperature is increased at a rate of 1-10℃ / min, and the calcination temperature is maintained within the range of 200-850℃, with the calcination temperature varying or maintained at a certain level, and the calcination time is 2-12 hours.

[0022] In steps (1) and (2), the separation is performed by filtration, dialysis and centrifugation; the washing is done with deionized water; in step (1), the solution is washed until the pH is 7 to 10; in step (2), the solution is washed until the pH is 7 to 10; the drying temperature is 25 to 120°C, preferably 40 to 80°C; the drying time is 0.5 to 24 hours.

[0023] The length is in the micrometer range, and the diameter is 10~25 nm. The uniformly sized titanium-based lithium-ion sieve (Li2TiO3) has a regular hexahedral shape and a particle size of about 20 nm to 80 nm.

[0024] The dilute acid is selected from one or more of hydrochloric acid, nitric acid, and sulfuric acid solutions, preferably a dilute acid solution with a hydrogen ion concentration of 0.1~1 mol / L; the amount of eluent used in the elution process is 20~100 mL / g of adsorbent precursor; the elution process temperature is 15~80℃, preferably 15~50℃; the time is 0.5~48 h, preferably 2~24 h; after acid washing, the elution process requires water washing until neutral.

[0025] The titanium-based lithium-ion sieve particles prepared in this invention are used as adsorbents in lithium extraction from salt lakes or other dissolved lithium solutions. Temperature control during the reaction process is achieved using an oil bath (with a tolerance of ±5°C). A self-made Teflon (polytetrafluoroethylene) reaction apparatus with a volume of 200 mL is used. An alumina crucible is used in the sintering process. The uniform distribution is characterized by a single peak during dynamic light scattering (DLS) testing, conforming to a normal distribution, with a PDI below 0.5.

[0026] The present invention has the following advantages: (1) The uniformly distributed nanoscale titanium-based lithium-ion sieve particles and their preparation method provided by the present invention not only produce lithium adsorbent products with excellent performance, but also effectively reduce labor and equipment costs. The uniformly distributed nanoscale titanium-based lithium-ion sieve particle adsorbent prepared by this preparation method uses fibrous titanium dioxide precursor as a precursor, controls the amount of titanium source, lithium source and substance, and then further lithiation, calcination and acid washing to obtain a uniformly distributed nanoscale titanium-based lithium-ion sieve particle adsorbent (H2TiO3).

[0027] (2) During the heating process in the alkaline etching process, due to the special characteristics of the polytetrafluoroethylene (PTFE) reactor (volume 200 mL; one-quarter of the reactor is heated in an oil bath, and three-quarters of the reactor is above the oil bath), the upper and lower temperatures of the PTFE reactor differ during heating, which can form an internal self-condensation process. As the solvent boils, the vapor rises and then condenses and refluxes, forming a near-solid-state process at the bottom of the reactor, transforming the irregular titanium dioxide into fibrous titanium dioxide precursor. The alkali used in this process can be recovered and reused through dilution and precipitation. After calcination, the dried titanium dioxide precursor forms fibrous titanium dioxide precursor. Then, through lithiation and calcination processes, nanoscale titanium-based lithium-ion sieve particles with uniform particle size distribution are obtained. This modification method allows the raw material to be fully etched, forming a fibrous titanium dioxide precursor. During heating, the titanium dioxide precursor can fully react with lithium ions, which is beneficial for forming more lithium ion interaction sites. Finally, through high-temperature sintering, nanoscale titanium-based lithium ion sieve particles with uniform particle size distribution can be obtained. After acid washing to remove the lithium ions, nanoscale titanium-based lithium ion sieve particle adsorbent (H2TiO3) with uniform particle size distribution can be obtained.

[0028] (3) Compared with traditional methods, this invention has two major improvements. First, it uses a solid-state etching method to prepare fibrous titanium dioxide precursors, which can fully combine with lithium ions due to their nanostructure, resulting in a more complete lithiation process. Second, it controls the synthesis process to prepare nanoscale titanium-based lithium ion sieve particles with uniform particle size distribution, while their special micro-nano structure ensures the adsorbent has greater adsorption characteristics.

[0029] (4) The preparation method of the present invention not only ensures high adsorption activity, but also avoids cumbersome synthesis process and the resulting performance loss, thus balancing performance and practicality. At the same time, the alkali in the etching process can be recycled and reused; the lithium solution in the solution lithiation process can also be recycled and reused; the entire synthesis process does not use a high-temperature reactor, and the synthesis process is simple and unrestricted. Attached Figure Description

[0030] Figure 1 A flowchart illustrating the preparation process of H2TiO3, a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application. Figure 2 A schematic SEM image of the fibrous titanium dioxide precursor prepared in Example 1, showing a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application. Figure 3 Comparative Example 1: SEM image of the fractional titanium dioxide precursor prepared by a nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method and application. Figure 4 Example 1 shows a schematic SEM image of the nanoscale lithium-ion sieve prepared with uniform particle size distribution, its preparation method, and its application. Figure 5 Example 1 shows a transmission electron microscope (TEM) schematic diagram of the prepared nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application. Figure 6 Example 1 shows the XRD pattern of a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application. Figure 7 Optical photographs of the nanoscale titanium-based lithium adsorbent prepared in Example 1 of a nanoscale lithium ion sieve with uniform particle size distribution, its preparation method and application, after dispersion in various solvents (water (a), ethanol (b), dimethyl sulfoxide (c)). Figure 8 Example 1 shows the dynamic light scattering particle size distribution of the prepared nanoscale titanium-based lithium adsorbent after dispersion in ethanol, which is a nanoscale lithium ion sieve with uniform particle size distribution, its preparation method and application. Figure 9 This is a schematic SEM image of the lithium-ion sieve prepared in Comparative Example 1. Figure 10 SEM schematic diagram of the nanofiber-like titanium dioxide precursor and the nanoscale titanium-based lithium ion sieve obtained in Example 2, which is a nanoscale lithium ion sieve with uniform particle size distribution and its preparation method and application. Figure 11 A schematic diagram of a polytetrafluoroethylene reaction device for a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application. Detailed Implementation

[0031] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Example 1

[0032] like Figures 1-9 As shown, a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application are illustrated. Figure 1As shown, the preparation method of nanoscale titanium-based lithium-ion sieve particles with uniform particle size distribution includes the following steps: S1. Add 2.25 g of anatase titanium dioxide with a particle size of 30~500 nm to a polytetrafluoroethylene reaction vessel (e.g., Figure 11 Add 40 mL of 10M sodium hydroxide solution (i.e., the mass molar ratio of titanium-based lithium ion sieve precursor powder to alkali is 1:14) to the mixture. After sonication for 30 minutes, place the sealed reaction vessel in an oil bath at 110°C and continue the reaction for 24 hours. One-quarter of the polytetrafluoroethylene reaction vessel is in the oil bath, and three-quarters is in the air. Turn off the heating device and let it cool to room temperature. Add 50 mL of deionized water, stir thoroughly, and let stand for 2 hours. Then wash the product repeatedly with water and ethanol alternately. The product is white. Stop washing when the pH of the washing solution reaches 9. Dry the sample at a temperature of 40-80℃ for 0.5-24 hours.

[0033] The dried sample was calcined in a muffle furnace at a heating rate of 5℃ / min, reaching 300℃ and holding at that temperature for 6 hours. The temperature was then lowered to 25℃ at a cooling rate of 5℃ / min to obtain fibrous nano-titanium dioxide precursors.

[0034] The separation methods are vacuum filtration, dialysis, and centrifugation; Wash with deionized water until the solution pH = 7 ~ 10; Calcination temperature and temperature control: Increase the temperature by 1~10℃ / min, maintain the calcination temperature in the range of 200~850℃, vary or maintain a certain temperature for calcination, and the calcination time is 2~12 hours; The fibrous nano-titanium dioxide precursor prepared in this embodiment is as follows: Figure 2 As shown, the diameter is 10~25 nm and the aspect ratio is 1:20; S2. Weigh 0.5 g of the fibrous nano-titanium dioxide precursor prepared in step S1 and 0.8 g of lithium hydroxide, place them in a polytetrafluoroethylene container, add 50 mL of deionized water, sonicate the solution for 30 min, and place the reaction vessel in an oil bath at 110℃ for 24 h. Turn off the heating device, allow it to cool to room temperature, and let it stand for 2 h. Collect the supernatant, precipitate and filter to obtain a white-brown product. Stop washing when the pH of the washing solution reaches 10, and dry the sample. Calcinate the dried sample in a muffle furnace. Calcination process: Preferably, the heating rate is 5℃ / min, raising it to 500℃ and holding it at that temperature for 4 h. Cooling process: Preferably, the temperature is raised to 25℃ at a rate of 5℃ / min to obtain nano-sized titanium-based lithium ion sieves (Li2TiO3) with uniform particle size distribution. The nano-sized titanium-based lithium ion sieves are regular hexahedral with a particle size of approximately 20 nm to 80 nm.

[0035] In this embodiment, the titanium dioxide particle size is 10~10000nm, preferably 30~500nm; the titanium source is selected from one or more of rutile, anatase, and metatitanic acid; the titanium source particle size is 10~3000nm, preferably 30~500nm; one or more of lithium bromide, lithium hydroxide, lithium chloride, lithium nitrate, lithium acetate, and lithium oxalate are used; lithium acetate is preferred. The molar ratio of the above titanium source to lithium acetate is (1:1~5), preferably 1:2, and they are mixed evenly in a mortar. The sample is then calcined in a muffle furnace. The calcination process is preferably: the heating rate is 5℃ / min, raising the temperature to 700℃, and holding it at that temperature for 4h. The cooling process is preferably: the temperature is raised to 25℃ at a rate of 5℃ / min to obtain a lithium ion sieve.

[0036] S3. Weigh 0.5 g of the uniformly sized lithium-ion sieve (Li2TiO3) prepared in step S2. Use hydrochloric acid as the eluent and wash the nano-sized lithium-ion sieve (Li2TiO3) with a concentration of 0.5 M HCl solution. Soak for 6 h, and repeat the washing process three times. Collect the white powder and dry it. Obtain a uniformly sized titanium-based lithium adsorbent (H2TiO3). The particle size and uniformity of the synthesized nano-sized lithium-ion sieve are characterized by dynamic light scattering testing.

[0037] The application of uniformly sized nanoscale lithium-ion sieves as adsorbents in lithium extraction from salt lakes or other dissolved lithium solutions; temperature control using an oil bath (with a tolerance of ±5℃) during the temperature-controlled reaction process; a self-made Teflon (polytetrafluoroethylene) reaction apparatus with a volume of 200 mL; and an alumina crucible used in the sintering process. The uniform distribution is characterized by a single peak in dynamic light scattering (DLS) testing, conforming to a normal distribution, with a PDI below 0.5.

[0038] The performance of the titanium-based lithium adsorbent obtained in step S3 was tested experimentally. Specifically, four identical samples of 0.025 g of the nanoscale lithium-ion sieve (H2TiO3) obtained in step S3 were added to 50 mL of LiOH / LiCl solution ([Li + [1 g / L, i.e. 1000 ppm; T = 293 K], under different pH values ​​shown in Table 1, after adsorption at room temperature for 12 hours, 5 mL of solution was taken and centrifuged at 9500 rpm to remove the adsorbent, and the supernatant was obtained. After filtration with a filter head, it was diluted with deionized water and tested by ICP-OES or ICP-MS. The final experimental results are shown in Table 1.

[0039] Table 1. Nanoscale titanium-based lithium adsorbent (H2TiO3) obtained in step S2 at different pH solutions Table of experimental results for testing the adsorption capacity of lithium

[0040] As can be seen from the data in the table above, the uniformly sized nano-sized titanium-based lithium adsorbent (H2TiO3) of this application can effectively improve the lithium ion adsorption rate at different pH levels. The uniformly sized nano-sized titanium-based lithium adsorbent (H2TiO3) can effectively improve the internal and external diffusion rate and adsorption sites of the adsorbent, thereby improving the adsorption performance of the adsorbent.

[0041] As shown in Table 1, the optimal adsorption capacity was achieved at pH 11. Therefore, the dissolution rate of the nano-sized titanium-based lithium adsorbent (H2TiO3) in Example 1 was tested under pH 11. The adsorption performance of the uniformly sized nano-sized titanium-based lithium adsorbent (H2TiO3) obtained in step S3 of Example 1 was tested. Specifically, 0.05 g of the uniformly sized nano-sized lithium ion sieve (H2TiO3) prepared in step S3 of Example 1 was added to 50 mL of LiOH / LiCl solution ([Li + [1 g / L, i.e., 1000 ppm; pH=11] After adsorption at room temperature for 12 hours, the adsorbent was removed by centrifugation at 9500 rpm. 5 mL of the supernatant was collected, filtered through a filter, diluted with deionized water, and then tested using ICP-OES or ICP-MS. The adsorbent was freeze-dried to obtain a dried sample. The dissolution rate of the lithium-ion sieve was calculated by weighing. The experiment was repeated three times, and the final results are shown in Table 2.

[0042] Table 2. Cycle count for Li + Summary table of dissolution rates of lithium ion sieves

[0043] As can be seen from the data in the table above, the nano-scale titanium-based lithium adsorbent (H2TiO3) in Example 1 of this application can effectively maintain a high lithium-ion adsorption capacity and a low solubility under cyclic experiments. This indicates that the nano-scale lithium-ion sieve with uniform particle size distribution has a high adsorption capacity and a low solubility under alkaline conditions (pH=11). The nano-membrane lithium-ion sieve has a fast adsorption rate, high adsorption capacity and low solubility, and has the potential for industrial application.

[0044] Example 2 like Figure 1 As shown, a nanoscale lithium-ion sieve with uniform particle size distribution, its preparation method, and its application are described. The steps are the same as in Example 1, with only the following differences: The sodium hydroxide solution was prepared from flake sodium hydroxide with a concentration of 15 M (i.e., the mass molar ratio of titanium-based lithium ion sieve precursor powder to alkali was 1:21.4). The titanium dioxide precursor prepared in this embodiment is shown in the SEM image. Figure 10 As shown in the left side (a) of the image, the SEM diagram of the lithium-ion sieve is as follows. Figure 10As shown in the right-hand (b) section; The performance of the obtained titanium-based lithium adsorbent was tested experimentally. Specifically, 0.025 g of nano-sized lithium-ion sieve (H₂TiO₃) was added to 50 mL of LiOH / LiCl solution ([Li + [1 g / L, i.e. 1000 ppm; T = 293 K], after adsorption at room temperature for 12 hours at different pH values, 5 mL of the solution was taken and centrifuged at 9500 rpm to remove the adsorbent. The supernatant was obtained, filtered with a filter head, and then diluted with deionized water before being tested by ICP-OES or ICP-MS. The final experimental results are shown in Table 3.

[0045] Table 3. Lithium-ion sieve obtained in Example 2 for Li + Adsorption performance summary table

[0046] As can be seen from the data in the table above, the nanoscale lithium-ion sieve (H2TiO3) of this application can effectively adsorb lithium ions at different pH levels. The uniform particle size distribution of the nanoscale lithium-ion sieve (H2TiO3) can effectively improve the internal and external diffusion rates and adsorption sites of the adsorbent, thereby improving the adsorption performance of the adsorbent. In the comparative experiment, the performance of lithium ion adsorption was worse than that of the uniform particle size distribution nanoscale lithium-ion sieve.

[0047] Comparative Example 1 With the reaction conditions in Example 1 unchanged, the polytetrafluoroethylene reaction apparatus in step S1 was replaced with a high-pressure resistant glass reaction flask, and the above experiment was repeated to obtain the fractal structure titanium dioxide precursor; Figure 3 As shown, a solid-state process cannot be formed in a high-pressure glass reaction flask, therefore the obtained titanium dioxide precursor is blocky, and a fibrous nano-titanium dioxide precursor with a large aspect ratio cannot be obtained; the fractal structure titanium dioxide precursor of this comparative example is used to prepare a lithium ion sieve using the methods in steps S2 and S3 of Example 1, as shown. Figure 9 As shown.

[0048] The lithium adsorption performance of the lithium-ion sieve obtained in Comparative Example 1 was tested experimentally. The adsorption performance of the lithium-ion sieve was studied in a solution environment with pH=11. Specifically, 0.05 g (0.0491 g; 0.0494 g) of three identical samples of the lithium-ion sieve prepared in Comparative Example 1—Sample 1, Sample 2, and Sample 3—were added to 50 mL of LiOH / LiCl solution ([Li... +[1 g / L, i.e., 1000 ppm; pH=11], after adsorption at room temperature for 12 hours, the adsorbent was removed by centrifugation at 9500 rpm. 5 mL of the supernatant was taken, filtered through a filter, diluted with deionized water, and then tested by ICP-OES or ICP-MS. The final experimental results are shown in Table 4.

[0049] Table 4 shows the lithium-ion sieve obtained in Comparative Example 1 for Li + Adsorption performance summary table

[0050] As can be seen from the data in the table above, the lithium-ion sieve in Comparative Example 1 of this application performs worse than the uniformly sized nanoscale lithium-ion sieve in Example 1 in the comparative experiment.

[0051] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A nanoscale lithium-ion sieve with uniform particle size distribution, characterized in that: The nanoscale lithium-ion sieve is obtained by eluting a nanoscale titanium-based lithium-ion sieve. The capacity to adsorb lithium ions in the pH range of 5 to 12 is 30 to 130 mg / g. The nanoscale titanium-based lithium-ion sieve is a regular hexahedral Li2TiO3 with a particle size of 20 nm to 80 nm. The nanoscale titanium-based lithium-ion sieve is obtained by calcining a nanofiber titanium source precursor with a lithium source, wherein the nanofiber titanium source precursor is titanium dioxide with an aspect ratio of 1:(10~100).

2. A method for preparing a nanoscale lithium-ion sieve with uniform particle size distribution, characterized in that: Includes the following steps: S1. Add titanium-based lithium ion sieve precursor powder to a polytetrafluoroethylene reaction vessel, then add alkaline solution, then seal the polytetrafluoroethylene reaction vessel and place it in an oil bath to carry out alkaline etching reaction under normal pressure, and then perform separation, washing, drying and calcination in sequence to obtain nanofiber titanium source precursor. The molar ratio of the titanium-based lithium-ion sieve precursor powder to the solute in the alkaline solution is 1:(10~25). The titanium-based lithium-ion sieve precursor powder is metatitanic acid or rutile or anatase titanium dioxide with a particle size of 10~3000nm. S2. The nanofiber titanium source precursor and the lithium source are placed in the polytetrafluoroethylene reaction vessel, mixed evenly, and then the polytetrafluoroethylene reaction vessel is sealed and placed in an oil bath for heating, reaction, separation, washing, drying and calcination under normal pressure to obtain a nano-scale titanium-based lithium ion sieve. S3. The nanoscale titanium-based lithium ion sieve is eluted with dilute acid as an eluent, then washed and dried to obtain a nanoscale lithium ion sieve with uniform particle size distribution.

3. The nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to claim 2, characterized in that: In step S1, the polytetrafluoroethylene reaction vessel includes a bottle body and a bottle frame, both made of polytetrafluoroethylene and sealed by threaded connection. The titanium-based lithium ion sieve precursor powder and the alkali are placed in the polytetrafluoroethylene reaction vessel and sealed. They are then ultrasonically mixed for 20-40 minutes and placed in an oil bath. When the titanium-based lithium-ion sieve precursor powder and alkali are etched in the polytetrafluoroethylene reaction vessel, 1 / 5 to 1 / 3 of the body of the polytetrafluoroethylene reaction vessel is heated in an oil bath, and 2 / 3 to 4 / 5 of the body is above the oil bath. During the etching reaction, the polytetrafluoroethylene reaction vessel forms an internal self-condensation process. As the solvent boils, the vapor is condensed and refluxed. A near-solid-state process is formed at the bottom of the polytetrafluoroethylene reaction vessel, transforming irregular titanium dioxide into fibrous titanium dioxide precursor. In step S2, when the nanofiber titanium source precursor and the lithium source are both placed in the polytetrafluoroethylene reaction vessel for reaction, 1 / 5 to 1 / 3 of the body of the polytetrafluoroethylene reaction vessel is heated in an oil bath, and 2 / 3 to 4 / 5 of the body is above the oil bath. During the reaction, the polytetrafluoroethylene reaction vessel forms an internal self-condensation process. As the solvent boils, the vapor is condensed and refluxed, and a quasi-solid-state process is formed at the bottom of the polytetrafluoroethylene reaction vessel, thus obtaining the nanoscale titanium-based lithium ion sieve.

4. The nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to claim 2, characterized in that: The opening size of the polytetrafluoroethylene reaction vessel is smaller than the diameter of the vessel body, the vessel body is cylindrical, and the height of the vessel body is 1.5 to 4 times the diameter of the vessel body.

5. The nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to claim 2, characterized in that: In step S1, the alkaline solution is any one of ammonia, piperidine, pyridine, triethylamine, lithium hydroxide, sodium hydroxide, potassium hydroxide, tert-butyllithium, sodium phenoxide, and potassium tert-butoxide.

6. The nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to claim 2, characterized in that: In step S1, the oil bath temperature is 50~180℃, and the etching reaction time is 12~36h; After the etching reaction, turn off the heating device and cool to room temperature. Add 30-100 mL of deionized water to the polytetrafluoroethylene reaction vessel and stir thoroughly. After standing for 1-5 hours, separate the solid and liquid components by filtration, dialysis, or centrifugation. Wash the white product repeatedly with water and ethanol alternately. Stop washing when the pH of the washing solution is 7-10. Dry the sample at 40-80°C for 0.5-24 hours. After drying, the product is placed in a muffle furnace for calcination in an air or oxygen atmosphere. The temperature is increased by 1~10℃ / min during calcination and maintained at 200~850℃. After calcination for 2~24 hours, the temperature is reduced to room temperature by 1~10℃ / min to obtain the nanofiber titanium source precursor.

7. The nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to claim 2, characterized in that: In step S1, the diameter of the nanofiber titanium source precursor is 10~50nm and the aspect ratio is 1:(10~100).

8. The nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to claim 2, characterized in that: In step S2, the lithium source is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium hydroxide, lithium carbonate, lithium oxalate, and lithium acetate. The molar ratio of the nanofiber titanium source precursor to the lithium source is 1:(1~5). After being mixed evenly in a mortar, the mixture is placed in a muffle furnace for calcination. The heating rate during calcination is 1~10℃ / min. After reaching 200~850℃, the temperature is maintained for 2~12h. The cooling rate is 1~10℃ / min. When the temperature drops to room temperature, the nanoscale titanium-based lithium ion sieve is obtained. The nanoscale titanium-based lithium ion sieve is Li2TiO3. In step S3, during elution, the dilute acid is hydrochloric acid, nitric acid, or sulfuric acid solution with an ion concentration of 0.1~1 mol / L; the amount of eluent used is 20~100 mL / g of adsorbent precursor. The elution temperature is 15~80℃, the time is 0.5~48h, and the solution is washed with water until neutral after elution. The PDI of the nanoscale lithium-ion sieve is less than or equal to 0.

5.

9. The nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to claim 2, characterized in that: In step S1, a portion of the alkaline solution is collected during separation, and the supernatant is collected during washing for dilution and recovery of the other portion. The lithium source is recycled and reused as described in step S2.

10. The application of the nanoscale lithium-ion sieve with uniform particle size distribution and its preparation method according to any one of claims 1 to 9, characterized in that: The nanoscale lithium-ion sieve is used as an adsorbent for lithium adsorption in a dissolved lithium solution, which includes a salt lake.