Preparation method of potassium adsorbent with chromium-zirconium-tungsten ternary composite oxide heterojunction structure

The preparation method of potassium adsorbent with chromium-zirconium-tungsten ternary composite oxide heterojunction structure solves the problems of insufficient selectivity and stability of existing potassium adsorbents in complex brine systems, and achieves potassium adsorption effect with high selectivity and high adsorption capacity, which is suitable for large-scale potassium extraction applications in complex water bodies.

CN123102292APending Publication Date: 2026-11-17BEIJING HUATEYUAN TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611512851.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing potassium adsorbents have shortcomings in terms of adsorption capacity, selectivity, and stability, making it difficult to meet the economic and reliability requirements for industrial applications. In particular, they have weak anti-interference ability, limited adsorption capacity, poor selectivity, and unstable structure in complex brine systems, making it difficult to meet the needs of efficient, stable, and large-scale potassium extraction.

Method used

A method for preparing potassium adsorbents with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure was adopted. Through dual-path co-precipitation, in-situ imprinting of solid-phase potassium source and segmented controllable calcination, and precise template removal process with weak acid and weak base, a highly selective potassium extraction adsorbent was constructed, forming a stable multi-metal oxide framework and exclusive imprinted micropores, and optimizing ion diffusion channels.

Benefits of technology

It achieves high selectivity and high adsorption capacity in complex water systems, has strong structural stability, and excellent cycling performance. It can maintain high adsorption performance in multiple adsorption-desorption cycles and is suitable for large-scale potassium extraction applications in complex water bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102292A_ABST
    Figure CN123102292A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing a potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure, belonging to the field of potassium adsorbent technology. The highly selective potassium adsorbent prepared by this invention has a Cr-Zr-W ternary composite oxide heterojunction structure, with chromium, zirconium, and tungsten multimetallic oxides as the main framework. It is constructed through dual-path co-precipitation, in-situ imprinting of a solid-phase potassium source, segmented controllable calcination, and precise template removal using weak acid and weak base processes. It can accurately identify and selectively adsorb potassium ions in complex aqueous environments containing competing ions such as sodium, lithium, calcium, and magnesium. Simultaneously, its excellent cross-linked framework structure can withstand multiple adsorption-desorption regeneration cycles, ensuring the material possesses high adsorption capacity, strong selectivity, and excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of potassium adsorbent technology, and specifically to a method for preparing a potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure. Background Technology

[0002] Adsorption is one of the effective techniques for extracting potassium from complex liquid systems. The adsorbent is the core of the adsorption method, and its performance directly determines the efficiency and cost of potassium extraction. However, existing potassium adsorbents still have shortcomings in terms of adsorption capacity, selectivity, and stability, making it difficult to meet the economic and reliability requirements of industrial applications. Therefore, there is an urgent need to develop new high-performance potassium adsorbents.

[0003] Natural clinoptilolite, due to its three-dimensional porous structure, exhibits good selectivity for potassium ions and is the most widely studied natural potassium adsorbent. Zeolites are typically modified with acid, alkali, or salt solutions to improve their adsorption capacity and selectivity. Chinese invention patent application CN86106921A discloses a technique for preparing modified zeolite using natural zeolite as the main raw material. Through processes such as flotation, granulation, roasting, and modification, the effective component clinoptilolite is extracted from natural zeolite and then modified. However, due to the limited grade of the raw ore, the content of the effective component (clinoptilolite) in natural zeolite is low, with a potassium ion exchange capacity of only 14–20 mg K. + The low potassium content in the eluent, resulting in low production costs, makes it difficult to reduce production costs.

[0004] An existing method for synthesizing potassium ion sieves involves heating manganese carbonate and carbonic acid to obtain a manganese-type potassium ion sieve, which demonstrates specific selectivity for potassium ions through ion exchange selectivity studies. Alternatively, a method using manganese carbonate and potassium methoxide as raw materials is employed to prepare crypto-potassium manganese dioxide via a high-temperature solid-phase method (calcination temperature 620℃, calcination time 12h), followed by acid washing to obtain the potassium ion sieve. This material exhibits a potassium ion exchange capacity of 29.11 mg / g⁻⁵ for seawater. However, the adsorption capacity of this material is relatively low. Furthermore, the active component is easily lost during the acidification process, making powder material forming difficult and hindering industrial application due to powder loss.

[0005] While the aforementioned existing technologies have achieved potassium adsorption to some extent, they still have significant shortcomings: the core problem with zeolite adsorbents is their low adsorption capacity, with a saturated adsorption capacity for potassium ions typically only 25–30 mg / g. Treating low-concentration potassium-containing solutions requires large amounts of adsorbent and bulky equipment, significantly increasing investment and operating costs. Simultaneously, their selectivity is poor; in complex systems containing high concentrations of coexisting sodium, calcium, and magnesium ions, the separation coefficient for potassium ions is low, especially under high sodium and low potassium conditions (Na / K mass ratio > 10), where the potassium adsorption capacity drops sharply, resulting in an actual recovery rate far lower than the theoretical value. Furthermore, the zeolite framework is prone to structural collapse and a reduction in active sites after multiple adsorption-desorption cycles, leading to a gradual decrease in regeneration efficiency, significant degradation of adsorption performance, and limited service life. In layered manganese oxide potassium ion sieves, during acid treatment activation and adsorption-desorption cycles, trivalent manganese ions in the manganese oxide framework are prone to disproportionation reactions, resulting in severe manganese dissolution and continuous loss of active components, causing the adsorption capacity to decrease rapidly with increasing cycle number. Meanwhile, it is quite sensitive to interference from coexisting ions such as lithium ions and magnesium ions, and its selectivity in actual brine systems still needs to be further improved, making it difficult to meet the requirements for long-term stable operation in industrial applications.

[0006] In summary, existing potassium extraction adsorbents generally suffer from weak anti-interference capabilities, poor selectivity for potassium ion adsorption, and low separation precision in complex brine and seawater systems containing multiple competing ions such as sodium, lithium, calcium, and magnesium. Furthermore, traditional adsorbents exhibit poor controllability of pore structure, lack dedicated potassium ion recognition channels, resulting in high ion mass transfer resistance and poor adsorption kinetics. Conventional template removal processes easily corrode and damage the adsorbent's main framework, leading to easy collapse of the imprinted cavity and a limited number of effective adsorption sites. These technical defects include limited adsorption capacity, insufficient cycle regeneration stability, and poor batch performance reproducibility, making it difficult to meet the application requirements for efficient, stable, and large-scale selective potassium extraction in complex aquatic environments. Summary of the Invention

[0007] The purpose of this invention is to provide a method for preparing a potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure, so as to solve at least one of the technical problems existing in the background art.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] This invention provides a method for preparing a potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure, comprising:

[0010] The bottom liquid of the reactor is an appropriate amount of deionized water. A dispersant is added, the temperature is controlled by an ice-water bath, and stirring is started. Solutions A, B, and C are fed simultaneously in a three-way parallel dripping manner. Specifically, chromium chloride and zirconium oxychloride are dissolved in deionized water, and dilute hydrochloric acid is added to inhibit the hydrolysis of trivalent zirconium ions. The mixture is stirred until completely dissolved to prepare a mixed salt solution, solution A. Sodium tungstate is dissolved in deionized water to prepare a tungstate solution, solution B. Solid NaOH is dissolved in deionized water to prepare a sodium hydroxide solution, solution C.

[0011] After the three-way simultaneous addition of solutions A, B, and C is completed and the feed pump is shut off, hydrated tungsten oxide precipitate is obtained and in situ composite precipitate is formed with Cr(OH)3 and Zr(OH)4 flocs. Then, the reactor is heated and crystallized in a sealed environment at a constant temperature. After crystallization, the mixture is filtered, washed until neutral, and dried to obtain a composite Cr(OH)3·0.1-0.3Zr(OH)4·0.1-0.3WO3·nH2O hydroxide precursor. The precursor is washed to remove free water and adsorbed solvent, pulverized, and sieved to obtain ternary composite hydroxide powder.

[0012] Ternary hydroxide powder and anhydrous potassium carbonate powder are mixed at a certain molar ratio to obtain a solid-phase homogeneous composite powder.

[0013] The composite powder was calcined in stages under controlled temperature: In an air atmosphere, the temperature was increased from room temperature to 150-180 ℃ at a certain rate and held at a constant temperature to remove residual physically adsorbed water from the powder; then, a high-purity nitrogen inert atmosphere was switched, and the temperature was increased to 480-550 ℃ at a certain rate and held at a constant temperature to allow the ternary hydroxide to simultaneously dehydrate and transform into an initial composite oxide framework, fixing the spatial position of potassium carbonate microcrystals and preventing their displacement and aggregation; next, a buffer atmosphere of nitrogen and carbon dioxide was used, and the temperature was further increased to 790-850 ℃ at a certain rate to complete the high-temperature shaping of the framework; then, the temperature was decreased to 630-650 ℃ at a certain rate, switched to a normal pressure flowing air atmosphere, and calcined at a constant temperature of 630-650 ℃. After calcination, the powder was naturally cooled to room temperature in the furnace, finally yielding K. 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Crude products of ternary composite oxides;

[0014] The crude product was soaked in citric acid to dissolve most of the potassium template within the imprinted cavity without damaging the main oxide lattice framework. After filtration and washing with water until neutral, it was soaked in sodium bicarbonate at room temperature to fine-tune the hydroxyl structure and surface charge of the cavity wall, widen the ion diffusion mesoporous channels, and remove insoluble residual potassium impurities. This process was repeated with alternating immersion cycles and vacuum drying to completely remove the template, yielding Na. 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder;

[0015] Will Na 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder and organic binder are added to a granulator in a certain ratio and granulated, then cured at room temperature to finally obtain Na. 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 -PVDF ternary composite oxide highly selective potassium extraction adsorbent.

[0016] As a further limitation of the first aspect of the present invention, under normal temperature and light-protected conditions, chromium chloride and zirconium oxychloride are dissolved in deionized water at a molar ratio of Cr:Zr=1:0.1-0.3, a small amount of 0.1-0.5 mol / L dilute hydrochloric acid is added to inhibit the hydrolysis of chromium ions, and the mixture is stirred until completely dissolved to prepare a mixed salt solution A; sodium tungstate is dissolved separately in deionized water at a molar ratio of W:Cr=0.1-0.3 to prepare a 0.5-1.0 mol / L tungstate solution B; and solid NaOH is dissolved in deionized water to prepare a 2-4 mol / L sodium hydroxide solution C.

[0017] As a further limitation of the first aspect of the present invention, when polyethylene glycol-400 with a mass fraction of 1-3% is used as a dispersant and is fed synchronously in a three-way parallel flow dripping manner, the pH of the system is monitored and adjusted in real time to 9.0-10.0, the temperature is controlled at 10±2℃ throughout the process, and the dripping rate is controlled at 1-5 mL / min.

[0018] As a further limitation of the first aspect of the present invention, after the three-way simultaneous addition of solutions A, B and C is completed and the feed pump is turned off, in order to promote the recovery of tungsten precipitate remaining in the supernatant in the form of residual tungstate ions, while keeping the stirring and temperature control of the reactor constant, a 0.5-1.0 mol / L dilute hydrochloric acid or citric acid solution is slowly added to the reactor through a peristaltic pump to slowly lower the pH of the system from 9.0-10.0 to 7.0±0.2, with the addition rate controlled at 0.5-2 mL / min; after adjusting back to the target pH, the system is kept at a constant temperature for 30-60 min to allow the residual tungstate ions to be fully converted into hydrated tungsten oxide precipitate and to recombine in situ with Cr(OH)3 and Zr(OH)4 flocs.

[0019] As a further limitation of the first aspect of the present invention, the reaction vessel is heated to 45-60℃ and sealed for crystallization for 6-24 hours. After crystallization, it is filtered, washed until neutral, and dried at 60-80℃ for 12 hours to obtain the composite Cr(OH)3·0.1-0.3Zr(OH)4·0.1-0.3WO3·nH2O hydroxide precursor.

[0020] As a further limitation of the first aspect of the present invention, the precipitated slurry after crystallization is subjected to plate and frame low-pressure filtration to initially remove the supernatant; an alternating washing mode of "deionized water hot washing + low-temperature alcohol washing" is adopted: repeated washing with 40°C warm water 4 times to remove residual sodium ions and chloride ions impurities in the system, followed by soaking and washing with anhydrous ethanol 2 times to replace the interparticle moisture and prevent drying agglomeration; low-temperature pre-drying at 35°C for 18 h → constant temperature drying at 65°C for 12 h → deep drying at 105°C for 10 h to completely remove free water and adsorbed solvent; after ultrafine airflow pulverization, it is passed through a 200-mesh standard sieve to obtain a ternary composite hydroxide pure phase powder with uniform particle size and uniform composition.

[0021] As a further limitation of the first aspect of the present invention, ternary hydroxide powder and anhydrous potassium carbonate ultrafine powder are fed into a closed double cone mixer at a molar ratio of 1:0.5-1 and mixed at a low speed of 160-300 r / min at room temperature for 4 hours. Every 30-50 minutes, the mixer is turned on at a high speed of 200-500 r / min for 2-5 minutes to ensure that potassium carbonate microcrystals are uniformly embedded in the gaps between hydroxide particles, without local enrichment or stratification, so as to obtain a solid-phase uniform composite powder.

[0022] As a further limitation of the first aspect of the present invention, a tube furnace is used for programmed temperature control and segmented calcination: first, an air atmosphere with a flow rate of 20-60 mL / min is introduced, and the temperature is increased from room temperature to 150-180 °C at a heating rate of 1.5-5.0 °C / min and held at this temperature for 4-8 h to remove residual physically adsorbed water from the powder; then, a high-purity nitrogen inert atmosphere is introduced, and the temperature is increased to 480-550 °C at a heating rate of 1.2-3.0 °C / min and held at this temperature for 5-10 h to allow the ternary hydroxide to undergo simultaneous dehydration and transformation to form the initial composite oxide framework; then, a buffer atmosphere of nitrogen and carbon dioxide is introduced, and the temperature is increased to 790-850 °C at a rate of 0.7-2.5 °C / min to complete the high-temperature shaping of the framework, and then the temperature is slowly decreased to 630-650 °C at a rate of 0.8-2.0 °C / min, after which the flow rate is switched to 40-80 mL / min. It is subjected to a normal pressure flowing air atmosphere and calcined at a constant temperature of 630-650 ℃ for 5–10 h.

[0023] As a further limitation of the first aspect of the present invention, the crude product was soaked in a 0.12-0.5 mol / L citric acid weak acid solution and shaken at a constant temperature for 2-5 h to gently dissolve most of the potassium template in the imprinted cavity; after filtration and washing with water until neutral, it was soaked in a 0.07-0.1 mol / L sodium bicarbonate weak alkali solution at room temperature for 2-5 h to fine-tune the hydroxyl structure and surface charge of the cavity wall, widen the ion diffusion mesoporous channels, and remove insoluble residual potassium impurities; the alternating weak acid-weak alkali immersion cycle was repeated twice, with thorough water washing each time, followed by vacuum drying at 40-60℃ to completely remove the template and obtain Na.0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder.

[0024] As a further limitation of the first aspect of the present invention, a PVDF organic binder with a solid content of 20-30 wt% is prepared, and Na... 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder and organic binder are added to a high-speed rotary granulator at a mass ratio of 1:0.3-0.5.

[0025] The beneficial effects of this invention are as follows: The prepared highly selective potassium extraction adsorbent is a Cr-Zr-W ternary composite oxide heterojunction structure, with chromium, zirconium, and tungsten multimetal oxides as the main framework. It is constructed through dual-path co-precipitation, in-situ imprinting of solid-phase potassium source and segmented controllable calcination, and precise template removal process using weak acid and weak base. It can accurately identify and selectively adsorb potassium ions in complex aqueous environments containing competing ions such as sodium, lithium, calcium, and magnesium. At the same time, the excellent cross-linked framework structure can withstand multiple adsorption-desorption regeneration, ensuring that the material has high adsorption capacity, strong selectivity, and excellent cycle stability.

[0026] The advantages of additional aspects of the invention will be set forth more clearly in the following description or will be learned by practice of the invention. Attached Figure Description

[0027] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 This is a flowchart illustrating the preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to an embodiment of the present invention.

[0029] Figure 2 This is a schematic diagram of the XRD pattern of the potassium adsorbent powder described in Example 1 of the present invention.

[0030] Figure 3 This is a SEM image of the potassium adsorbent powder described in Example 1 of the present invention.

[0031] Figure 4 This is a schematic diagram of the XRD pattern of the potassium adsorbent powder described in Example 2 of the present invention.

[0032] Figure 5This is a SEM image of the potassium adsorbent powder described in Example 2 of the present invention.

[0033] Figure 6 This is a schematic diagram of the XRD pattern of the potassium adsorbent powder described in Example 3 of the present invention.

[0034] Figure 7 This is a SEM image of the potassium adsorbent powder described in Example 3 of the present invention. Detailed Implementation

[0035] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0036] It will be understood by those skilled in the art that, unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0037] It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with their meanings in the context of the prior art, and should not be interpreted in an idealized or overly formal sense unless defined as here.

[0038] Those skilled in the art will understand that, unless specifically stated otherwise, the singular forms “a,” “an,” “the,” and “the” used herein may also include the plural forms. It should be further understood that the term “comprising” as used in this specification means the presence of the stated features, integers, steps, operations, elements, and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, and / or groups thereof.

[0039] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of those different embodiments or examples.

[0040] To facilitate understanding of the present invention, the present invention will be further explained and described below with reference to the accompanying drawings and specific embodiments. However, the specific embodiments do not constitute a limitation on the embodiments of the present invention.

[0041] Those skilled in the art should understand that the accompanying drawings are merely schematic diagrams of embodiments, and the components in the drawings are not necessarily essential for implementing the present invention.

[0042] This invention provides a method for preparing a high-performance potassium adsorbent, which is constructed using chromium, zirconium, and tungsten multimetal oxides as the main framework through dual-path co-precipitation, in-situ imprinting of solid-phase potassium source and segmented controllable calcination, and precise template removal process using weak acid and weak base. It has several core technological advantages: (1) By using Cr-Zr-W multi-metal atomic-level doping and cross-linking, it avoids the shortcomings of single oxide structure, greatly improves the strength and chemical stability of material skeleton, and strengthens the potassium ion specific recognition ability by relying on the multi-metal synergistic effect, effectively shielding the interference of competing ions in complex water systems; (2) By using solid-phase potassium source in-situ imprinting combined with segmented controllable calcination process, it can accurately construct potassium ion exclusive imprint micropores with matching size and stable structure. The pores are regular and not easy to collapse, ensuring ultra-high adsorption selectivity from the structure; (3) By using weak acid and weak base alternating mild template removal technology, while completely preserving the main skeleton and imprint sites, it constructs multi-level through-mesoporous channels, reduces ion mass transfer resistance, and takes into account both high selectivity and rapid adsorption kinetic performance; (4) With the matching optimized co-precipitation, precise mixing and gradient drying crystallization process, it ensures that the material composition is uniform, without segregation and agglomeration, and the batch performance reproducibility is excellent. Moreover, the adsorbent can be easily regenerated in situ, with good cycle stability and high adsorption capacity, which can be efficiently adapted to the industrial application scenario of large-scale potassium extraction in complex water bodies.

[0043] The highly selective potassium extraction adsorbent prepared in this invention is a Cr-Zr-W ternary composite oxide heterojunction structure, prepared through co-precipitation, in-situ potassium source imprinting, segmented calcination, and precise template removal using weak acid and weak base processes. This adsorbent is formed by the uniform cross-linking of chromium, zirconium, and tungsten components at the atomic scale, creating a stable ternary oxide crystal phase. This overcomes the structural defects of single metal oxides and enhances structural stability and ion recognition capability through the synergistic effect of the heterojunction. Using anhydrous potassium carbonate as an in-situ template, segmented calcination etches custom-imprinted micropores matching the size of hydrated potassium ions within the framework. The template is then removed by alternating weak acid and weak base immersion, and the surface properties of the pores are controlled to construct multi-level interconnected mesoporous channels, effectively improving potassium ion transport efficiency. The material is bonded and molded into regular spherical particles, possessing a stable framework, custom-imprinted potassium ion channels, and a highly efficient ion diffusion system. It can precisely and selectively adsorb potassium ions in complex aqueous systems containing competing ions such as sodium, lithium, calcium, and magnesium. Simultaneously, the framework structure exhibits strong stability, high adsorption capacity, good selectivity, and excellent cycle performance.

[0044] like Figure 1 As shown, the preparation method of the high-performance potassium adsorbent of the present invention includes the following steps:

[0045] 1. Solution preparation: Under normal temperature and light-protected conditions, dissolve chromium chloride (CrCl3·6H4O) and zirconium oxychloride (ZrOCl2·8H2O) in deionized water at a molar ratio of Cr:Zr = 1:0.1-0.3. Add a small amount of 0.1-0.5 mol / L dilute hydrochloric acid to inhibit the hydrolysis of chromium ions, and stir until completely dissolved to prepare a clear mixed salt solution (solution A). Dissolve sodium tungstate (Na2WO4·2H2O) separately in deionized water at a molar ratio of W:Cr = 0.1-0.3 to prepare a 0.5-1.0 mol / L clear tungstate solution (solution B). Separately, dissolve solid NaOH in deionized water at low temperature to prepare a 2-4 mol / L sodium hydroxide solution (solution C), and allow it to stand and cool to room temperature for later use.

[0046] 2. Coprecipitation Reaction: The bottom liquid of the reactor is an appropriate amount of deionized water, with 1-3% (w / w) of polyethylene glycol-400 (PEG-400) added as a dispersant. The temperature is controlled at 10±2℃ in an ice-water bath. After starting the stirrer and calibrating the online pH probe, the system is fed simultaneously using a three-pronged parallel flow method: solution A (Cr+Zr mixed salt), solution B (sodium tungstate solution), and solution C (NaOH alkaline solution). The pH of the system is monitored and adjusted in real time to 9.0-10.0, and the temperature is controlled at 10±2℃ throughout the process. The dropping rate is strictly controlled at 1-5 mL / min to prevent excessive local alkalinity from causing particle agglomeration. After the three-pronged parallel flow of solutions A, B, and C is completed and the feed pump is turned off, Cr and Zr have completely precipitated, but some W remains in the supernatant as tungstate ions. To promote the recovery of residual W precipitate, and to maintain constant stirring and temperature control in the reactor, a 0.5-1.0 mol / L dilute hydrochloric acid or citric acid solution was slowly added dropwise to the reactor using a peristaltic pump. The pH of the system was gradually lowered from 9.0-10.0 to 7.0±0.2, with the addition rate controlled at 0.5-2 mL / min to prevent sudden local pH drops that could cause acid dissolution of Zr(OH)4. After adjusting back to the target pH, the reactor was kept at a constant temperature for 30-60 min to allow the residual tungstate to fully convert into hydrated tungsten oxide precipitate and recombine with Cr(OH)3 and Zr(OH)4 flocs in situ. The reactor was then heated to 45-60℃ and sealed for crystallization for 6-24 h. After crystallization, the mixture was filtered, washed until neutral, and dried at 60-80℃ for 12 h to obtain the composite Cr(OH)3·0.1-0.3Zr(OH)4·0.1-0.3WO3·nH2O hydroxide precursor. After crystallization, the precipitated slurry was subjected to plate and frame low-pressure filtration to initially remove the supernatant. An alternating washing mode of "deionized water hot washing + low-temperature alcohol washing" was adopted: repeated washing with 40℃ warm water for 4 times to remove residual sodium and chloride ion impurities in the system, followed by soaking and washing with anhydrous ethanol twice to replace the interparticle moisture and prevent drying agglomeration; low-temperature pre-drying at 35℃ for 18 h → constant temperature drying at 65℃ for 12 h → deep drying at 105℃ for 10 h to completely remove free water and adsorbed solvent; after ultrafine airflow pulverization, it was passed through a 200-mesh standard sieve to obtain a ternary composite hydroxide pure phase powder with uniform particle size and composition.

[0047] 3. Potassium Source Introduction: Anhydrous potassium carbonate is dried in a vacuum oven at 120℃ for 8 hours to completely remove adsorbed water and trace amounts of crystal water. After cooling, it is quickly passed through a 300-mesh sieve and stored in a moisture-proof, sealed container to prevent deliquescence and failure. The ternary hydroxide powder and anhydrous potassium carbonate ultrafine powder are fed into a closed double cone mixer at a molar ratio of 1:0.5-1. A trace amount of nitrogen is introduced into the equipment for moisture protection. The "low-speed long-time mixing + intermittent high-speed tumbling" mode is adopted: low-speed mixing at 160-300 r / min at room temperature for 4 hours, followed by high-speed tumbling at 200-500 r / min for 2-5 minutes every 30-50 minutes to ensure that potassium carbonate microcrystals are uniformly embedded in the gaps between hydroxide particles, without local enrichment or stratification, resulting in a solid-phase homogeneous composite powder.

[0048] 4. Staged Calcination and Crystallization: The composite powder is spread evenly in a corundum crucible, with the layer thickness controlled at 4–5 mm. Staged calcination is performed using a tube furnace with programmed temperature control: First, an air atmosphere with a flow rate of 20–60 mL / min is introduced, and the temperature is increased from room temperature to 150–180 °C at a rate of 1.5–5.0 °C / min and held at this temperature for 4–8 h to remove residual physically adsorbed water from the powder. Then, a high-purity nitrogen inert atmosphere is introduced, and the temperature is increased to 480–550 °C at a rate of 1.2–3.0 °C / min and held at this temperature for 5–10 h. This allows the ternary hydroxide to simultaneously dehydrate and transform, forming the initial composite oxide framework, fixing the spatial position of potassium carbonate microcrystals and preventing their displacement and agglomeration. Next, a nitrogen + 3 vol% carbon dioxide buffer atmosphere is introduced, and the temperature is increased at a low rate of 0.7–2.5 °C / min to 790–850 °C to complete the high-temperature shaping of the framework. Finally, the temperature is increased at a rate of 0.8–2.0 °C / min. The temperature was slowly lowered to 630-650 °C at a rate of 40-80 mL / min, then switched to a normal pressure air atmosphere and calcined at 630-650 °C for 5-10 hours. Anhydrous potassium carbonate embedded in the interstitial crystal structure slowly decomposed at this temperature, releasing carbon dioxide. The gas escaped directionally from the solidified ternary oxide framework, and in-situ etching was used to generate bulk-specific imprinted micropores that perfectly matched the size of hydrated potassium ions. The potassium oxide remained inside the cavities, acting as a reversible template. After all calcination processes were completed, the furnace was allowed to cool naturally to room temperature, finally yielding K... 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Ternary composite oxides.

[0049] 5. Removal of potassium template: The crude product is soaked in a 0.12-0.5 mol / L citric acid solution with a weak organic acid and shaken at a constant temperature for 2-5 hours to gently dissolve most of the potassium template in the imprinted cavity without damaging the main oxide lattice framework. After filtration and washing with water until neutral, the product is soaked in a 0.07-0.1 mol / L sodium bicarbonate solution with a weak alkaline solution at room temperature for 2-5 hours to fine-tune the hydroxyl structure and surface charge of the cavity wall, widen the ion diffusion mesoporous channels, and remove insoluble residual potassium impurities. The alternating weak acid-weak alkaline immersion cycle is repeated twice, with thorough water washing each time. The product is then vacuum dried at 40-60℃ to completely remove the template and obtain Na. 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder.

[0050] 6. Granulation and molding: Prepare a PVDF organic binder (PVDF+DMAC) with a solid content of 20-30wt%, and add Na... 0.5- 1CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder and organic binder were added to a high-speed rotary granulator at a mass ratio of 1:0.3-0.5. The mixture was rotated at 1000 rpm for 30-60 minutes. After sieving, spherical particles of 0.5-1.2 mm were obtained. The particles were then cured at room temperature for 3 hours to finally obtain Na. 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 -PVDF ternary composite oxide highly selective potassium extraction adsorbent.

[0051] In this invention, the potassium extraction performance of the ternary composite oxide highly selective potassium extraction adsorbent prepared above is evaluated. The specific process is as follows:

[0052] The spherical potassium adsorbent Na prepared above is packed into an plexiglass column. 0.5-1 CrZr 0.1-0.3 W 0.1- 0.3 O 4.25-5.5-PVDF, adsorption column length-to-diameter ratio 8-15:1, with sieve plates and distributors at both ends of the column to ensure uniform flow of the feed solution within the bed, avoiding channeling and wall flow phenomena, thus ensuring the stability and reproducibility of the adsorption process. Self-prepared brine (simulated seawater) is used as the feed solution, employing a bottom-in, top-out feeding method, controlling the feed flow rate at 5-15 BV / h (empty bed volumetric flow rate), maintaining the operating temperature at 20-30℃, and adjusting and stabilizing the system pH within the natural seawater range (7.5-8.5). Under these conditions, continuous operation is performed, utilizing the selective adsorption performance of the adsorbent for potassium ions to achieve dynamic enrichment and concentration of potassium ions in the brine. During adsorption, the potassium ion concentration in the outlet liquid is periodically monitored until the adsorption column reaches breakthrough or saturation. When the adsorption column is saturated, feeding is stopped and the residual liquid in the column is drained. Then, a 2-4 mol / L sodium chloride (NaCl) solution is switched as the eluent, and the adsorption bed is washed in the same direction at a flow rate of 3-8 BV / h. Under the competitive exchange of high-concentration sodium ions, adsorbed potassium ions are released from the active sites of the adsorbent and enter the eluent, thus achieving efficient desorption and enrichment of potassium ions. Simultaneously, the active sites of the adsorbent are occupied by sodium ions, completing in-situ regeneration. After the regeneration operation, no additional activation steps such as water washing, acid-base activation, or heat treatment are required. The regenerated adsorbent can be directly switched back to the feed mode and recycled for the next round of adsorption.

[0053] This invention employs a Cr-W-Zr ternary composite oxide to construct the heterojunction framework. The three metal components are uniformly doped and cross-linked at the atomic scale. Compared with single-component metal oxides, this significantly reduces lattice defects and improves the overall mechanical strength and chemical stability of the framework. The synergistic effect of multiple metals simultaneously optimizes the surface charge distribution and potassium ion specific recognition sites of the material. In brine and saline bodies where sodium, lithium, calcium, and magnesium coexist in large quantities, this invention can significantly weaken the interference of competing ions, achieve ultra-high selectivity capture of hydrated potassium ions, and effectively improve the adsorption and separation accuracy.

[0054] This invention employs anhydrous potassium carbonate solid-phase in-situ imprinting technology, combined with a segmented gradient calcination process: first, high-temperature shaping at 790℃, then cooling to 630℃ for controlled-rate decomposition of potassium salts. The high-temperature stage fully solidifies the ternary oxide framework, preventing the potassium salt microcrystals from migrating and agglomerating due to heat. The low-temperature air constant-temperature stage allows potassium carbonate to slowly decompose and release carbon dioxide, directionally etching out exclusive imprinted micropores with sizes highly matched to hydrated potassium ions. The pores are regular, and the recognition sites are directionally distributed, endowing the material with specific potassium ion adsorption capacity from the structural root. The imprinted cavities are not easy to collapse, and the pore structure is highly controllable.

[0055] This invention employs a gentle template removal process using alternating weak acid citric acid and weak base sodium bicarbonate, which differs from the single elution method using strong acid and strong base. This process can fully dissolve the potassium template inside the cavity and remove residual potassium impurities without corroding or damaging the main ternary oxide lattice. At the same time, it precisely controls the number of hydroxyl functional groups and surface charge on the inner wall of the pores, and simultaneously constructs a through-type multi-level mesoporous diffusion channel, which significantly reduces the mass transfer resistance of potassium ions, improves the adsorption kinetic rate, and balances high selectivity and fast adsorption rate.

[0056] The precursor preparation of this invention adopts a dual-mother liquor simultaneous double-droplet addition and constant temperature and pH control co-precipitation process, in which Cr, Zr and W metal hydroxides are simultaneously and uniformly precipitated, completely avoiding the problems of component segregation and local metal enrichment caused by stepwise precipitation. Combined with low-temperature crystallization, water washing-alcohol washing multi-stage impurity removal, gradient drying and ultrafine grinding processes, the resulting precursor powder has uniform composition and no impurity agglomeration, ensuring the uniformity and stability of the ternary heterojunction phase after subsequent calcination, and excellent batch-to-batch reproducibility of material adsorption performance.

[0057] The present invention uses a double-cone mixer with nitrogen protection and intermittent high and low speed mixing process to uniformly disperse potassium template and ternary hydroxide powder. Potassium carbonate microcrystals are uniformly dispersed and embedded in the interstices of precursor particles, without local enrichment and stratification. This ensures that the entire material bulk phase uniformly generates imprinted micropores, avoiding defects such as local lack of recognition sites and uneven adsorption capacity. The overall material has a higher density of effective adsorption sites and a significantly improved adsorption capacity per unit mass.

[0058] Table 1

[0059]

[0060] Example 1

[0061] In this embodiment 1, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0062] 1. Solution preparation: Under normal temperature and light-protected conditions, dissolve chromium chloride (CrCl3·6H2O) and zirconium oxychloride (ZrOCl2·8H2O) in deionized water at a molar ratio of Cr:Zr=1:0.2. Add a small amount of 0.3 mol / L dilute hydrochloric acid to inhibit the hydrolysis of chromium ions, and stir until completely dissolved to prepare a clear mixed salt solution (solution A). Dissolve sodium tungstate (Na2WO4·2H2O) separately in deionized water at a molar ratio of W:Cr=0.20 to prepare a clear tungstate solution (solution B). Separately, dissolve solid NaOH in deionized water at low temperature to prepare a 2 mol / L sodium hydroxide solution (solution C), and allow it to stand and cool to room temperature for later use.

[0063] 2. Co-precipitation preparation of hydroxide powder: The bottom liquid of the reactor was an appropriate amount of deionized water, with 2% (w / w) of polyethylene glycol-400 (PEG-400) added as a dispersant. The temperature was controlled at 10±2℃ in an ice-water bath. After starting the stirrer and calibrating the online pH probe, the feed was simultaneously introduced using a three-way parallel flow method: solution A (Cr+Zr mixed salt), solution B (sodium tungstate solution), and solution C (NaOH alkaline solution). The pH of the system was monitored and adjusted in real time to maintain 9.5, and the temperature was controlled at 10±2℃ throughout the process. The dropping rate was strictly controlled at 1.5 mL / min to prevent excessive local alkalinity from causing particle agglomeration. After the three-way parallel flow of solutions A, B, and C was completed and the feed pump was turned off, Cr and Zr had completely precipitated, but some W remained in the supernatant in the form of tungstate ions. To promote the recovery of residual W precipitate, and to maintain constant stirring and temperature control in the reactor, a 0.5 mol / L dilute hydrochloric acid solution was slowly added dropwise to the reactor using a peristaltic pump to gradually lower the pH of the system from 9.5 to 7.0±0.2. The dropping rate was controlled at 0.6 mL / min to prevent localized sudden pH drops that could cause acid dissolution of Zr(OH)4. After adjusting back to the target pH, the reactor was kept at a constant temperature for 30-60 min to allow the residual tungstate to be fully converted into hydrated tungsten oxide precipitate and to recombine with Cr(OH)3 and Zr(OH)4 flocs in situ. Then, the reactor was heated to 50℃ and sealed for crystallization for 12 h. After crystallization, the mixture was filtered, washed until neutral, and dried at 70℃ for 12 h to obtain the composite Cr(OH)3·0.2Zr(OH)4·0.2WO3·nH2O hydroxide precursor. After crystallization, the precipitated slurry was subjected to plate and frame low-pressure filtration to initially remove the supernatant. An alternating washing mode of "deionized water hot washing + low-temperature alcohol washing" was adopted: repeated washing with 40℃ warm water for 4 times to remove residual sodium and chloride ion impurities in the system, followed by soaking and washing with anhydrous ethanol twice to replace the interparticle moisture and prevent drying agglomeration; low-temperature pre-drying at 35℃ for 18 h → constant temperature drying at 65℃ for 12 h → deep drying at 105℃ for 10 h to completely remove free water and adsorbed solvent; after ultrafine airflow pulverization, it was passed through a 200-mesh standard sieve to obtain a ternary composite hydroxide pure phase powder with uniform particle size and composition.

[0064] 3. Potassium Source Introduction: Anhydrous potassium carbonate is dried in a vacuum oven at 120℃ for 8 hours to completely remove adsorbed water and trace amounts of crystal water. After cooling, it is quickly passed through a 300-mesh sieve and stored in a moisture-proof, sealed container to prevent deliquescence and failure. The ternary hydroxide powder and anhydrous potassium carbonate ultrafine powder are fed into a closed double cone mixer at a molar ratio of 1:0.75. A trace amount of nitrogen is introduced into the equipment for moisture protection. The "low-speed long-time mixing + intermittent high-speed tumbling" mode is adopted: low-speed mixing at 160 r / min at room temperature for 4 hours, followed by high-speed tumbling at 500 r / min for 3 minutes every 30 minutes, to ensure that potassium carbonate microcrystals are uniformly embedded in the gaps between hydroxide particles, without local enrichment or stratification, resulting in a solid-phase homogeneous composite powder.

[0065] 4. Staged Calcination and Crystallization: The composite powder is spread evenly in a corundum crucible, with the material layer thickness controlled at 4–5 mm. A tube furnace is used for staged calcination with programmed temperature control: First, an air atmosphere with a flow rate of 60 mL / min is introduced, and the temperature is increased from room temperature to 180 °C at a rate of 3.0 °C / min and held at this temperature for 6 h to remove residual physically adsorbed water from the powder. Then, a high-purity nitrogen inert atmosphere is introduced, and the temperature is increased from 180 °C to 480 °C at a rate of 2.0 °C / min and held at this temperature for 8 h. This allows the ternary hydroxide to simultaneously dehydrate and transform, forming the initial composite oxide framework, fixing the spatial position of potassium carbonate microcrystals and preventing their displacement and aggregation. Next, a nitrogen + 3 vol% carbon dioxide buffer atmosphere is introduced, and the temperature is increased at a low rate of 1.0 °C / min to 790 °C to complete the high-temperature shaping of the framework. Then, the temperature is slowly decreased to 630 °C at a rate of 2.0 °C / min, after which the flow rate is switched to 80 mL / min. Anhydrous potassium carbonate embedded in the interstitial crystal lattice was slowly decomposed at 630 °C for 6 hours under a constant-temperature flowing air atmosphere. The carbon dioxide was released and directionally escaped from the solidified ternary oxide framework. In-situ etching was used to generate bulk-specific imprinted micropores that perfectly matched the size of hydrated potassium ions. The potassium oxide remained inside the cavities, acting as a reversible template. After all calcination processes were completed, the furnace was allowed to cool naturally to room temperature, ultimately yielding K... 0.75 CrZr 0.2 W 0.2 O 4.88 Ternary composite oxides.

[0066] 5. Removal of potassium template: The crude product was soaked in a 0.2 mol / L citric acid weak acid solution and shaken at a constant temperature for 3 h to gently dissolve most of the potassium template in the imprinted cavity without damaging the main oxide lattice framework. After filtration and washing with water until neutral, the product was soaked in a 0.08 mol / L sodium bicarbonate weak alkali solution at room temperature for 3 h to fine-tune the hydroxyl structure and surface charge of the cavity wall, widen the ion diffusion mesoporous channels, and remove insoluble residual potassium impurities. The weak acid-weak alkali alternating immersion cycle was repeated twice, with thorough water washing each time. The product was then vacuum dried at 40-60℃ to completely remove the template and obtain Na. 0.75 CrZr 0.2 W 0.2 O 4.88 Potassium adsorbent powder.

[0067] 6. Granulation and molding: Prepare a PVDF organic binder (PVDF+DMAC) with a solid content of 25wt%, and add Na... 0.75 CrZr 0.2 W 0.2 O 4.88Potassium adsorbent powder and organic binder were added to a high-speed rotary granulator at a mass ratio of 1:0.4 and rotated at 1000 rpm for 40 minutes. The resulting spherical particles (0.5–1.2 mm) were obtained by sieving and then cured at room temperature for 3 hours to finally produce Na. 0.75 CrZr 0.2 W 0.2 O 4.88 -PVDF ternary composite oxide highly selective potassium extraction adsorbent.

[0068] The spherical potassium adsorbent prepared above was packed into an plexiglass column with an aspect ratio of 10:1. Sieve plates and distributors were installed at both ends of the column to ensure uniform flow of the feed solution within the bed, avoiding channeling and wall flow phenomena, thus ensuring the stability and reproducibility of the adsorption process. Self-prepared brine (simulating nanofiltration seawater) was used as the feed solution, employing a bottom-in, top-out feed method. The feed flow rate was controlled at 6 BV / h (empty bed volumetric flow rate), the operating temperature was maintained at 25℃, and the system pH was adjusted and stabilized within the natural seawater range (7.5~8.5). Under these conditions, continuous operation was performed, utilizing the selective adsorption performance of the adsorbent for potassium ions to achieve dynamic enrichment and concentration of potassium ions in the brine. During the adsorption process, the potassium ion concentration in the effluent was periodically monitored until the adsorption column reached breakthrough or saturation. Once the adsorption column is saturated, the feed is stopped and the residual liquid in the column is drained. Then, a 2 mol / L sodium chloride (NaCl) solution is used as the eluent, and the adsorption bed is washed in the same direction at a flow rate of 5 BV / h. Under the competitive exchange of high-concentration sodium ions, the adsorbed potassium ions are released from the active sites of the adsorbent and enter the eluent, thus achieving efficient desorption and enrichment of potassium ions. Simultaneously, the active sites of the adsorbent are occupied by sodium ions, completing in-situ regeneration. After the regeneration operation, no additional activation steps such as water washing, acid-base activation, or heat treatment are required. The regenerated adsorbent can be directly switched back to the feed mode and recycled for the next round of adsorption.

[0069] The potassium adsorption capacity of the adsorbent prepared in this embodiment after 3 hours of adsorption is shown in Table 1. The adsorption capacity is as high as 107.4 g / L, which is an order of magnitude improvement compared to commercial zeolite-based potassium adsorbents (15.6 g / L) under the same conditions. The material has a significant technical advantage in potassium enrichment and carrying capacity. The total ion concentration of coexisting calcium and magnesium impurities in the eluent is only 15.6 mg / L, far lower than the 34.7 mg / L of commercial zeolite adsorbents, confirming that the adsorbent has excellent sieving, recognition and selective adsorption characteristics for potassium ions. Moreover, after 500 cycles, the adsorption capacity decreases by only 2.5%, while the capacity decay of commercial zeolite adsorbents under the same conditions is as high as 28.6%. This fully demonstrates that the composite oxide framework structure of this system is highly stable and can withstand long-term repetitive ion exchange conditions. Its long-term service performance is significantly superior to existing commercial materials.

[0070] Figure 2 The XRD diffraction pattern of the potassium adsorbent material powder shows that the characteristic diffraction peaks of the sample are sharp and narrow at half maximum, indicating that the prepared adsorbent material has high crystal integrity and regular crystal form. Figure 3 The image shows the SEM microstructure of the powder. It can be seen that the material is composed of orderly stacked thin-film grains. The unique layered structure provides abundant ion exchange channels, which is conducive to potassium ion adsorption and mass transfer.

[0071] Example 2

[0072] In this embodiment 2, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0073] 1. Solution preparation: Under normal temperature and light-protected conditions, dissolve chromium chloride (CrCl3·6H2O) and zirconium oxychloride (ZrOCl2·8H2O) in deionized water at a molar ratio of Cr:Zr=1:0.1. Add a small amount of 0.1 mol / L dilute hydrochloric acid to inhibit the hydrolysis of chromium ions, and stir until completely dissolved to prepare a clear mixed salt solution (solution A). Dissolve sodium tungstate (Na2WO4·2H2O) separately in deionized water at a molar ratio of W:Cr=0.10 to prepare a clear tungstate solution (solution B). Separately, dissolve solid NaOH in deionized water at low temperature to prepare a 2 mol / L sodium hydroxide solution (solution C), and allow it to stand and cool to room temperature for later use.

[0074] 2. Co-precipitation: The bottom liquid of the reactor is an appropriate amount of deionized water, with 1-3% (w / w) of polyethylene glycol-400 (PEG-400) added as a dispersant. The temperature is controlled at 10±2℃ in an ice-water bath. After starting the stirrer and calibrating the online pH probe, the system is fed simultaneously using a three-pronged parallel flow method: solution A (Cr+Zr mixed salt), solution B (sodium tungstate solution), and solution C (NaOH alkaline solution). The pH of the system is monitored and adjusted in real time to 9.0-10.0, and the temperature is controlled at 10±2℃ throughout the process. The dropping rate is strictly controlled at 1 mL / min to prevent excessive alkalinity in some areas from causing particle agglomeration. After the three-pronged parallel flow of solutions A, B, and C is completed and the feed pump is turned off, Cr and Zr have completely precipitated, but some W remains in the supernatant as tungstate ions. To promote the recovery of residual W precipitate, and to maintain constant stirring and temperature control in the reactor, a 0.5 mol / L citric acid solution was slowly added dropwise to the reactor using a peristaltic pump to gradually lower the pH of the system from 9.0-10.0 to 7.0±0.2. The dropping rate was controlled at 0.5 mL / min to prevent sudden local pH drops that could cause acid dissolution of Zr(OH)4. After adjusting back to the target pH, the reactor was kept at a constant temperature for 30 min to allow the residual tungstate to be fully converted into hydrated tungsten oxide precipitate and to recombine with Cr(OH)3 and Zr(OH)4 flocs in situ. Then, the reactor was heated to 45-60℃ and sealed for crystallization for 6 h. After crystallization, the reactor was filtered, washed until neutral, and dried at 60-80℃ for 12 h to obtain the composite Cr(OH)3·0.1Zr(OH)4·0.1WO3·nH2O hydroxide precursor. After crystallization, the precipitated slurry was subjected to plate and frame low-pressure filtration to initially remove the supernatant. An alternating washing mode of "deionized water hot washing + low-temperature alcohol washing" was adopted: repeated washing with 40℃ warm water for 4 times to remove residual sodium and chloride ion impurities in the system, followed by soaking and washing with anhydrous ethanol twice to replace the interparticle moisture and prevent drying agglomeration; low-temperature pre-drying at 35℃ for 18 h → constant temperature drying at 65℃ for 12 h → deep drying at 105℃ for 10 h to completely remove free water and adsorbed solvent; after ultrafine airflow pulverization, it was passed through a 200-mesh standard sieve to obtain a ternary composite hydroxide pure phase powder with uniform particle size and composition.

[0075] 3. Potassium Source Introduction: Anhydrous potassium carbonate is dried in a vacuum oven at 120℃ for 8 hours to completely remove adsorbed water and trace amounts of crystal water. After cooling, it is quickly passed through a 300-mesh sieve and stored in a moisture-proof, sealed container to prevent deliquescence and failure. The ternary hydroxide powder and anhydrous potassium carbonate ultrafine powder are fed into a closed double cone mixer at a molar ratio of 1:0.5. A trace amount of nitrogen is introduced into the equipment for moisture protection. The "low-speed long-time mixing + intermittent high-speed tumbling" mode is adopted: low-speed mixing at 160 r / min at room temperature for 4 hours, followed by high-speed tumbling at 200 r / min for 2 minutes every 30 minutes to ensure that potassium carbonate microcrystals are uniformly embedded in the gaps between hydroxide particles, without local enrichment or stratification, resulting in a solid-phase homogeneous composite powder.

[0076] 4. Staged Calcination and Crystallization: The composite powder is spread evenly in a corundum crucible, with the material layer thickness controlled at 4–5 mm. A tube furnace is used for staged calcination with programmed temperature control: First, an air atmosphere with a flow rate of 20 mL / min is introduced, and the temperature is increased from room temperature to 150 °C at a rate of 1.5 °C / min and held at this temperature for 4 hours to remove residual physically adsorbed water from the powder. Then, a high-purity nitrogen inert atmosphere is introduced, and the temperature is increased to 480 °C at a rate of 1.2 °C / min and held at this temperature for 5 hours to allow the ternary hydroxide to simultaneously dehydrate and transform into an initial composite oxide framework, fixing the spatial position of potassium carbonate microcrystals and preventing their displacement and agglomeration. Next, a nitrogen + 3 vol% carbon dioxide buffer atmosphere is introduced, and the temperature is increased at a low rate of 0.7 °C / min to 790 °C to complete the high-temperature shaping of the framework. Then, the temperature is slowly decreased to 630 °C at a rate of 0.8 °C / min. Afterward, the temperature is switched to a normal pressure flowing air atmosphere with a flow rate of 40 mL / min and held at 630 °C. Anhydrous potassium carbonate embedded in the interstitial crystal lattice was slowly decomposed at a constant temperature of ℃ for 5 h, releasing carbon dioxide. The gas escaped directionally from the solidified ternary oxide framework, and in-situ etching was used to generate bulk-specific imprinted micropores that perfectly matched the size of hydrated potassium ions. The potassium oxide remained inside the cavities, acting as a reversible template. After all the calcination processes were completed, the furnace was allowed to cool naturally to room temperature, finally yielding K 0.5 CrZr 0.1 W 0.1 O 4.25 Ternary composite oxides.

[0077] 5. Removal of potassium template: The crude product was soaked in a 0.12 mol / L citric acid solution for 2 h at a constant temperature with shaking to gently dissolve most of the potassium template in the imprinted cavity without damaging the main oxide lattice framework. After filtration and washing with water until neutral, the product was soaked in a 0.07 mol / L sodium bicarbonate solution at room temperature for 2 h to fine-tune the hydroxyl structure and surface charge of the cavity wall, widen the ion diffusion mesoporous channels, and remove insoluble residual potassium impurities. The alternating weak acid-weak alkali immersion cycle was repeated twice, with thorough water washing each time. The product was then vacuum dried at 40℃ to completely remove the template and obtain Na. 0.5 CrZr 0.1 W 0.1 O 4.25 Potassium adsorbent powder.

[0078] 6. Granulation and Molding: Prepare a PVDF organic binder (PVDF+DMAC) with a solid content of 20wt%. Add potassium adsorbent powder and organic binder at a mass ratio of 1:0.3 to a high-speed rotary granulator. Rotate at 1000 rpm for 30 minutes. Sieve to obtain spherical particles of 0.5–1.2 mm. Cure at room temperature for 3 hours to finally obtain Na. 0.5 CrZr 0.1W 0.1 O 4.25 -PVDF ternary composite oxide highly selective potassium extraction adsorbent.

[0079] The testing method is the same as in Example 1.

[0080] The potassium adsorption capacity of the adsorbent prepared in this embodiment after 3 hours of adsorption is shown in Table 1. The adsorption capacity is as high as 108.2 g / L, which is an order of magnitude improvement compared to commercial zeolite-based potassium-extracting adsorbents (15.6 g / L) under the same conditions. The material has a significant technical advantage in potassium enrichment and carrying capacity. The total ion concentration of coexisting calcium and magnesium impurities in the eluent is only 15.4 mg / L, far lower than the 34.7 mg / L of commercial zeolite adsorbents, confirming that the adsorbent has excellent sieving, recognition, and selective adsorption characteristics for potassium ions. Moreover, after 500 cycles, the adsorption capacity decreases by only 2.7%, while the capacity decay of commercial zeolite adsorbents under the same conditions is as high as 28.6%. This fully demonstrates that the composite oxide framework structure of this system is highly stable and can withstand long-term repetitive ion exchange conditions, and its long-term service performance is significantly superior to existing commercial materials.

[0081] Figure 4 The XRD diffraction pattern of the potassium adsorbent material powder shows that the characteristic diffraction peaks of the sample are sharp and narrow at half maximum, indicating that the prepared adsorbent material has high crystal integrity and regular crystal form. Figure 5 The image shows the SEM microstructure of the powder. It can be seen that the material is composed of orderly stacked thin-film grains. The unique layered structure provides abundant ion exchange channels, which is conducive to potassium ion adsorption and mass transfer.

[0082] Example 3

[0083] In this embodiment 3, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0084] 1. Solution preparation: Under normal temperature and light-protected conditions, dissolve chromium chloride (CrCl3·6H2O) and zirconium oxychloride (ZrOCl2·8H2O) in deionized water at a molar ratio of Cr:Zr = 1:0.3. Add a small amount of 0.5 mol / L dilute hydrochloric acid to inhibit Cr. 3+ Hydrolyze the solution and stir until completely dissolved to prepare a clear mixed salt solution (solution A); dissolve sodium tungstate separately in deionized water at a molar ratio of W:Cr=0.3 to prepare a clear tungstate solution (solution B); separately dissolve solid NaOH in deionized water at low temperature to prepare a 4 mol / L sodium hydroxide solution (solution C), and let it stand and cool to room temperature for later use.

[0085] 2. Co-precipitation preparation of hydroxide powder: The bottom liquid of the reactor is an appropriate amount of deionized water, with 1-3% (w / w) of polyethylene glycol-400 (PEG-400) added as a dispersant. The temperature is controlled at 10±2℃ in an ice-water bath. After starting the stirrer and calibrating the online pH probe, the feed is simultaneously introduced using a three-way parallel flow method: solution A (Cr+Zr mixed salt), solution B (sodium tungstate solution), and solution C (NaOH alkaline solution). The pH of the system is monitored and adjusted in real time to 9.0-10.0, and the temperature is controlled at 10±2℃ throughout the process. The dropping rate is strictly controlled at 1-5 mL / min to prevent excessive local alkalinity from causing particle agglomeration. When the three-way parallel flow of solutions A, B, and C is completed and the feed pump is turned off, Cr and Zr have completely precipitated, but some W remains in the supernatant in the form of tungstate ions. To promote the recovery of residual W precipitate, and to maintain constant stirring and temperature control in the reactor, a 1.0 mol / L dilute hydrochloric acid solution was slowly added dropwise to the reactor using a peristaltic pump to gradually lower the pH of the system from 9.0-10.0 to 7.0±0.2. The dropping rate was controlled at 2 mL / min to prevent local pH drops from causing acid dissolution of Zr(OH)4. After adjusting back to the target pH, the reactor was kept at a constant temperature for 60 min to allow the residual tungstate to be fully converted into hydrated tungsten oxide precipitate and to recombine with Cr(OH)3 and Zr(OH)4 flocs in situ. Then, the reactor was heated to 60℃ and sealed for crystallization for 24 h. After crystallization, the reactor was filtered, washed until neutral, and dried at 60-80℃ for 12 h to obtain the composite Cr(OH)3·0.3Zr(OH)4·0.3WO3·nH2O hydroxide precursor. After crystallization, the precipitated slurry was subjected to plate and frame low-pressure filtration to initially remove the supernatant. An alternating washing mode of "deionized water hot washing + low-temperature alcohol washing" was adopted: repeated washing with 40℃ warm water for 4 times to remove residual sodium and chloride ion impurities in the system, followed by soaking and washing with anhydrous ethanol twice to replace the interparticle moisture and prevent drying agglomeration; low-temperature pre-drying at 35℃ for 18 h → constant temperature drying at 65℃ for 12 h → deep drying at 105℃ for 10 h to completely remove free water and adsorbed solvent; after ultrafine airflow pulverization, it was passed through a 200-mesh standard sieve to obtain a ternary composite hydroxide pure phase powder with uniform particle size and composition.

[0086] 3. Potassium Source Introduction: Anhydrous potassium carbonate is dried in a vacuum oven at 120℃ for 8 hours to completely remove adsorbed water and trace amounts of crystal water. After cooling, it is quickly passed through a 300-mesh sieve and stored in a moisture-proof, sealed container to prevent deliquescence and failure. The ternary hydroxide powder and anhydrous potassium carbonate ultrafine powder are added to a closed double cone mixer at a molar ratio of 1:1. A trace amount of nitrogen is introduced into the equipment for moisture protection. The "low-speed long-time mixing + intermittent high-speed tumbling" mode is adopted: low-speed mixing at 300 r / min at room temperature for 4 hours, followed by high-speed tumbling at 500 r / min for 5 minutes every 50 minutes, to ensure that potassium carbonate microcrystals are uniformly embedded in the gaps between hydroxide particles, without local enrichment or stratification, resulting in a solid-phase homogeneous composite powder.

[0087] 4. Staged Calcination and Crystallization: The composite powder is spread evenly in a corundum crucible, with the material layer thickness controlled at 4–5 mm. A tube furnace is used for staged calcination with programmed temperature control: First, an air atmosphere with a flow rate of 60 mL / min is introduced, and the temperature is increased from room temperature to 180 °C at a rate of 5.0 °C / min and held at this temperature for 8 hours to remove residual physically adsorbed water from the powder. Then, a high-purity nitrogen inert atmosphere is introduced, and the temperature is increased to 550 °C at a rate of 3.0 °C / min and held at this temperature for 10 hours to allow the ternary hydroxide to simultaneously dehydrate and transform into an initial composite oxide framework, fixing the spatial position of potassium carbonate microcrystals and preventing their displacement and agglomeration. Next, the atmosphere is changed to N2 + 3 vol% CO2 buffer atmosphere, and the temperature is increased at a low rate of 2.5 °C / min to 850 °C to complete the high-temperature shaping of the framework. Then, the temperature is slowly decreased to 650 °C at a rate of 2.0 °C / min. Afterward, the temperature is switched to a normal pressure flowing air atmosphere with a flow rate of 80 mL / min and held at 650 °C. Anhydrous potassium carbonate embedded in the interstitial crystal lattice was slowly decomposed and released carbon dioxide during a 10-hour constant-temperature calcination at ℃. The gas escaped directionally from the solidified ternary oxide framework, and in-situ etching was used to generate bulk-specific imprinted micropores that perfectly matched the size of hydrated potassium ions. The potassium oxide remained inside the cavities, acting as a reversible template. After the calcination process was completed, the furnace was allowed to cool naturally to room temperature, ultimately yielding KCrZr. 0.3 W 0.3 O 5.5 Ternary composite oxides.

[0088] 5. Removal of potassium template: The crude product was soaked in a 0.5 mol / L citric acid weak acid solution and shaken at a constant temperature for 5 h to gently dissolve most of the potassium template in the imprinted cavity without damaging the main oxide lattice framework. After filtration and washing with water until neutral, the product was soaked in a 0.1 mol / L sodium bicarbonate weak alkali solution at room temperature for 5 h to fine-tune the hydroxyl structure and surface charge of the cavity wall, widen the ion diffusion mesoporous channels, and remove insoluble residual potassium impurities. The weak acid-weak alkali alternating immersion cycle was repeated twice, with thorough water washing each time. The product was then vacuum dried at 60℃ to completely remove the template, yielding NaCrZr. 0.3 W 0.3 O 5.5 Potassium adsorbent powder.

[0089] 6. Granulation and Molding: Prepare a PVDF organic binder (PVDF+DMAC) with a solid content of 30wt%. Add potassium adsorbent powder and organic binder at a mass ratio of 1:0.5 to a high-speed rotary granulator. Rotate at 1000 rpm for 0 min, and sieve to obtain spherical particles of 0.5–1.2 mm. Cure at room temperature for 3 h to finally obtain NaCrZr. 0.3 W 0.3 O 5.5-PVDF ternary composite oxide highly selective potassium extraction adsorbent.

[0090] The testing method is the same as in Example 1.

[0091] The potassium ion adsorbent prepared in this embodiment showed a potassium adsorption capacity of 106.6 g / L after 3 hours of adsorption, as shown in Table 1. This represents an order-of-magnesium improvement over commercial zeolite-based potassium adsorbents (15.6 g / L) under the same conditions, demonstrating a significant technical advantage in potassium enrichment and carrying capacity. The total concentration of coexisting calcium and magnesium impurities in the eluent was only 15.8 mg / L, far lower than the 34.7 mg / L of commercial zeolite adsorbents, confirming that this adsorbent possesses excellent sieving, recognition, and selective adsorption characteristics for potassium ions. Furthermore, after 500 cycles, the adsorption capacity decreased by only 2.7%, while the capacity decay of commercial zeolite adsorbents under the same conditions reached 28.6%. This fully demonstrates that the composite oxide framework structure of this system is highly stable and can withstand long-term repetitive ion exchange conditions, exhibiting significantly superior long-term service performance compared to existing commercial materials.

[0092] Figure 6 The XRD diffraction pattern of the potassium adsorbent material powder shows that the characteristic diffraction peaks of the sample are sharp and narrow at half maximum, indicating that the prepared adsorbent material has high crystal integrity and regular crystal form. Figure 7 The image shows the SEM microstructure of the powder. It can be seen that the material is composed of orderly stacked thin-film grains. The unique layered structure provides abundant ion exchange channels, which is conducive to potassium ion adsorption and mass transfer.

[0093] Comparative Example 1

[0094] In Comparative Example 1, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0095] 1. Solution preparation: Under normal temperature and light-protected conditions, dissolve a certain amount of chromium chloride in deionized water, add a small amount of 0.1 mol / L dilute hydrochloric acid to inhibit the hydrolysis of chromium ions, stir until completely dissolved, and prepare a clear mixed salt solution (solution A). Separately, dissolve solid NaOH in deionized water at low temperature to prepare a 2 mol / L sodium hydroxide solution (solution B), and allow it to stand and cool to room temperature for later use.

[0096] 2. Coprecipitation: Same as in Example 1.

[0097] 3. Potassium source introduction: Same as in Example 1.

[0098] 4. Staged roasting and crystallization: Same as in Example 1.

[0099] 5. Potassium removal template: Same as in Example 1.

[0100] 6. Granulation and molding: Same as in Example 1.

[0101] The testing method is the same as in Example 1.

[0102] The difference between the synthesis method of the potassium adsorbent in this comparative example and that in Example 1 is that no oxides of Zr and W are added in this comparative example, only a single metal oxide, chromium oxide.

[0103] The core difference between the potassium adsorbent prepared in this comparative example and that in Example 1 is that the sample uses only chromium oxide as the active metal oxide system and does not introduce zirconium or tungsten metal oxides for doping modification.

[0104] The potassium adsorption capacity after 3 hours of adsorption was measured and is shown in Table 1, which was 28.4 g / L, a significant decrease compared to Example 1. Furthermore, the total concentration of calcium and magnesium ions in the eluent was 60.6 mg / L, indicating a substantial increase in impurity ions and poor selectivity. Additionally, the structure exhibited poor stability (67% decrease in adsorption capacity after 500 cycles), resulting in poor cyclicity.

[0105] The potassium adsorbent prepared in this comparative example uses chromium atoms as the core framework, supplemented by zirconium and tungsten atom doping modification, to synergistically optimize the material structure and adsorption performance. Chromium atoms can construct a stable crystal framework, effectively improving the adsorbent's cycle stability; the introduction of zirconium and tungsten atoms can effectively inhibit the disordered growth of metal chemical bonds, avoiding the formation of large-sized grains and achieving grain refinement. The fine and regular grain structure not only increases the adsorbent's potassium adsorption capacity but also promotes more complete crystal growth and significantly reduces crystal defects, thereby effectively improving the material's adsorption selectivity for potassium ions and overall cycle stability.

[0106] Comparative Example 2

[0107] In Comparative Example 2, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0108] 1. Solution preparation: Under normal temperature and light-protected conditions, dissolve chromium chloride and zirconium oxychloride in deionized water at a molar ratio of Cr:Zr=1:0.2. Add a small amount of 0.3 mol / L dilute hydrochloric acid to inhibit the hydrolysis of chromium ions, and stir until completely dissolved to prepare a clear mixed salt solution (solution A). Separately, dissolve solid NaOH in deionized water at low temperature to prepare a 2 mol / L sodium hydroxide solution (solution C), and allow it to stand and cool to room temperature for later use.

[0109] 2. Coprecipitation: Same as in Example 1.

[0110] 3. Potassium source introduction: Same as in Example 1.

[0111] 4. Staged roasting and crystallization: Same as in Example 1.

[0112] 5. Potassium removal template: Same as in Example 1.

[0113] 6. Granulation and molding: Same as in Example 1.

[0114] The testing method is the same as in Example 1.

[0115] The core difference between this comparative example and Example 1 in preparing potassium adsorbent is that this comparative example uses only chromium as the main metal and is supplemented with zirconium active metal doping, without introducing tungsten metal oxide for modification.

[0116] The potassium adsorption capacity after 3 hours of adsorption, as shown in Table 1, was 37.4 g / L, a significant decrease compared to Example 1. Furthermore, the total concentration of calcium and magnesium ions in the eluent was 64.5 mg / L, indicating a substantial increase in impurity ions and poor selectivity. Additionally, the structure exhibited poor stability; after 500 cycles, the adsorption capacity decreased by 56%, demonstrating poor cycle performance. This is because the system utilizes chromium atoms to construct a stable crystal framework, ensuring the basic cycle stability of the adsorbent; zirconium doping effectively regulates the growth behavior of metal chemical bonds, inhibiting the formation of large-sized grains, refining the grain structure, and reducing crystal defects. However, the lack of tungsten's synergistic modification effect prevented further regularization of the crystal morphology and optimization of the pore structure, ultimately leading to a significant decrease in the material's adsorption capacity, ion selectivity, and cycle stability.

[0117] Comparative Example 3

[0118] In Comparative Example 3, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0119] 1. Solution preparation: Under normal temperature and light-protected conditions, dissolve a certain amount of chromium chloride in deionized water, add a small amount of 0.1 mol / L dilute hydrochloric acid to inhibit the hydrolysis of chromium ions, stir until completely dissolved, and prepare a clear mixed salt solution (solution A); dissolve sodium tungstate separately in deionized water at a molar ratio of W:Cr=0.2 to prepare a clear tungstate solution (solution B); separately dissolve solid NaOH in low-temperature deionized water to prepare a 2 mol / L sodium hydroxide solution (solution C), and let it stand and cool to room temperature for later use.

[0120] 2. Coprecipitation: Same as in Example 1.

[0121] 3. Potassium source introduction: Same as in Example 1.

[0122] 4. Staged roasting and crystallization: Same as in Example 1.

[0123] 5. Potassium removal template: Same as in Example 1.

[0124] 6. Granulation and molding: Same as in Example 1.

[0125] The testing method is the same as in Example 1.

[0126] The core difference between this comparative example and Example 1 in preparing potassium adsorbent is that this comparative example uses only chromium as the main metal and tungsten active metal doping, without introducing zirconium metal oxide for modification.

[0127] The potassium adsorption capacity after 3 hours of adsorption, as shown in Table 1, was 35.6 g / L, a significant decrease compared to Example 1. Furthermore, the total concentration of calcium and magnesium ions in the eluent was 65.7 mg / L, indicating a substantial increase in impurity ions and poor selectivity. Additionally, the structure exhibited poor stability; after 500 cycles, the adsorption capacity decreased by 60%, demonstrating poor cycle performance. This is because the system utilizes chromium atoms to construct a stable crystal framework, ensuring the basic cycle stability of the adsorbent; zirconium doping effectively regulates the growth behavior of metal chemical bonds, inhibiting the formation of large-sized grains, refining the grain structure, and reducing crystal defects. However, the lack of tungsten's synergistic modification effect prevented further regularization of the crystal morphology and optimization of the pore structure, ultimately leading to a significant decrease in the material's adsorption capacity, ion selectivity, and cycle stability.

[0128] Comparative Example 4

[0129] In Comparative Example 4, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0130] 1. Solution preparation: Same as in Example 1.

[0131] 2. Coprecipitation: Same as in Example 1.

[0132] 3. Potassium source introduction: Same as in Example 1.

[0133] 4. Staged Calcination and Crystallization: The composite powder is spread evenly in a corundum crucible, with the material layer thickness controlled at 4–5 mm. A tube furnace is used for staged calcination with programmed temperature control: First, an air atmosphere with a flow rate of 20 mL / min is introduced, and the temperature is increased from room temperature to 150 °C at a rate of 1.5 °C / min and held at this temperature for 4 hours to remove residual physically adsorbed water from the powder. Then, a high-purity nitrogen inert atmosphere is introduced, and the temperature is increased to 480 °C at a rate of 1.2 °C / min and held at this temperature for 5 hours. This allows the ternary hydroxide to simultaneously dehydrate and transform, forming the initial composite oxide framework, fixing the spatial position of potassium carbonate microcrystals and preventing their displacement and aggregation. Next, a nitrogen + 3 vol% carbon dioxide buffer atmosphere is introduced, and the temperature is further increased to 630 °C at a programmable rate of 0.8 °C / min. Afterward, the temperature is switched to a normal-pressure flowing air atmosphere with a flow rate of 40 mL / min and calcined at 630 °C for a long period. h, anhydrous potassium carbonate embedded in the interstices of the crystal lattice decomposes at this temperature to release carbon dioxide. The gas escapes directionally from the solidified ternary oxide framework. In-situ etching generates micropores with bulk-specific imprints that perfectly match the size of hydrated potassium ions. The potassium oxide remains inside the cavity as a reversible template. After all the calcination processes are completed, the furnace is naturally cooled to room temperature, and finally the ternary composite oxide is obtained.

[0134] 5. Potassium removal template: Same as in Example 1.

[0135] 6. Granulation and molding: Same as in Example 1.

[0136] The testing method is the same as in Example 1.

[0137] The key difference between this comparative example and Example 1 in preparing the potassium adsorbent is that in this comparative example, the temperature was not initially raised to 790 degrees Celsius before being reduced to 630 degrees Celsius during the staged calcination and crystallization process.

[0138] The potassium adsorption capacity after 3 hours of adsorption, as shown in Table 1, was 35.6 g / L, a significant decrease compared to Example 1. Furthermore, the total concentration of calcium and magnesium ions in the eluent was 65.7 mg / L, indicating a substantial increase in impurity ions and poor selectivity. Additionally, the structure exhibited poor stability; after 500 cycles, the adsorption capacity decreased by 60%, demonstrating poor cycle performance. This is because the core process of high-temperature setting at 790 °C followed by slow cooling to 630 °C was missing. This resulted in low crystallinity, coarse grains, a lack of potassium-specific imprinted micropores, numerous lattice defects, and poor framework stability in the ternary composite oxide. Consequently, the sample exhibited reduced potassium adsorption capacity, weak resistance to calcium and magnesium impurity interference, and severe capacity decay after multiple adsorption and regeneration cycles.

[0139] Comparative Example 5.

[0140] In Comparative Example 5, a method for preparing a potassium adsorbent is provided, which includes the following steps:

[0141] 1. Solution preparation: Same as in Example 1.

[0142] 2. Coprecipitation: Same as in Example 1.

[0143] 3. Potassium source introduction: Same as in Example 1.

[0144] 4. Staged roasting and crystallization: Same as in Example 1.

[0145] 5. Removal of potassium template: The crude product was soaked in 0.2 mol / L citric acid, a weak organic acid, and shaken at a constant temperature for 3 h to gently dissolve most of the potassium template in the imprint cavity without damaging the main oxide lattice framework. The weak acid immersion cycle was repeated twice, with thorough water washing each time. The product was then vacuum dried at 40-60℃ to completely remove the template and obtain potassium adsorbent powder.

[0146] 6. Granulation and molding: Same as in Example 1.

[0147] The testing method is the same as in Example 1.

[0148] The key difference between this comparative example and Example 1 in preparing the potassium adsorbent is that this comparative example did not involve soaking the potassium template in a weak alkaline solution of sodium bicarbonate at room temperature during the potassium removal process.

[0149] The potassium adsorption capacity after 3 hours of adsorption, as shown in Table 1, was 46.7 g / L, a significant decrease compared to Example 1. Furthermore, the total concentration of calcium and magnesium ions in the eluent was 50.6 mg / L, indicating a substantial increase in impurity ions and poor selectivity. Additionally, the structural stability was poor; after 500 cycles, the adsorption capacity decreased by 43%, demonstrating poor cycle performance. This is because omitting the room-temperature soaking step with a weak sodium bicarbonate base and relying solely on a weak citric acid for template removal results in residual acidic groups in the pores, incomplete potassium template elution, damage to the hydroxyl structure of the pore walls, and an increase in lattice defects. Ultimately, this manifests as a decrease in potassium adsorption capacity, poorer selectivity against calcium and magnesium impurities, and a significant decrease in structural stability after multiple cycles.

[0150] While the specific embodiments of the present invention have been described above in conjunction with the accompanying drawings, this is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that, based on the technical solutions disclosed in the present invention, various modifications or variations that can be made by those skilled in the art without creative effort should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure, characterized in that, include: The bottom liquid of the reactor is an appropriate amount of deionized water. A dispersant is added, the temperature is controlled by an ice-water bath, and stirring is started. Solutions A, B, and C are fed simultaneously in a three-way parallel dripping manner. Specifically, chromium chloride and zirconium oxychloride are dissolved in deionized water, and dilute hydrochloric acid is added to inhibit the hydrolysis of trivalent zirconium ions. The mixture is stirred until completely dissolved to prepare a mixed salt solution, solution A. Sodium tungstate is dissolved in deionized water to prepare a tungstate solution, solution B. Solid NaOH is dissolved in deionized water to prepare a sodium hydroxide solution, solution C. After the three-way simultaneous addition of solutions A, B, and C is completed and the feed pump is shut off, hydrated tungsten oxide precipitate is obtained and in situ composite precipitate is formed with Cr(OH)3 and Zr(OH)4 flocs. Then, the reactor is heated and crystallized in a sealed environment at a constant temperature. After crystallization, the mixture is filtered, washed until neutral, and dried to obtain a composite Cr(OH)3·0.1-0.3Zr(OH)4·0.1-0.3WO3·nH2O hydroxide precursor. The precursor is washed to remove free water and adsorbed solvent, pulverized, and sieved to obtain ternary composite hydroxide powder. Ternary hydroxide powder and anhydrous potassium carbonate powder are mixed at a certain molar ratio to obtain a solid-phase homogeneous composite powder. The composite powder is controlled temperature and segmented calcined: under air atmosphere, from room temperature to 150-180℃ with a certain heating rate and constant temperature, the residual physical adsorption water of the powder is removed; switch to high-purity nitrogen inert atmosphere, heat to 480-550℃ with a certain heating rate, constant temperature, make the ternary hydroxide synchronous dehydration conversion to form the initial composite oxide skeleton, fix the potassium carbonate crystal space position, prevent its displacement and agglomeration; replace the nitrogen and carbon dioxide mixed buffer atmosphere, continue to heat to 790-850℃ with a certain heating rate to complete the skeleton high temperature setting, then cool to 630-650℃ with a certain rate, switch to normal pressure flowing air atmosphere and constant temperature calcination at 630-650℃, after calcination, natural cooling to room temperature in the furnace, finally obtain K 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 The coarse product of the ternary composite oxide; The crude product is soaked in citric acid to dissolve most of the potassium template in the imprint cavity without destroying the crystal lattice framework of the main body oxide; after filtration and washing with water until neutral, the product is soaked in sodium bicarbonate at room temperature to slightly adjust the hydroxyl structure on the inner wall of the cavity and the surface electrical properties, broaden the ion diffusion mesoporous channel, and remove the insoluble residual potassium impurities; after repeating the alternating soaking and washing cycle and vacuum drying, the template is completely removed to obtain Na 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder Will Na 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder and organic binder are added to a granulator in a certain ratio and granulated, then cured at room temperature to finally obtain Na. 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 -PVDF ternary composite oxide highly selective potassium extraction adsorbent.

2. The preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, Under normal temperature and light-protected conditions, chromium chloride and zirconium oxychloride were dissolved in deionized water at a molar ratio of Cr:Zr = 1:0.1–0.

3. A small amount of 0.1–0.5 mol / L dilute hydrochloric acid was added to inhibit the hydrolysis of chromium ions, and the mixture was stirred until completely dissolved to prepare a mixed salt solution A. Sodium tungstate was dissolved separately in deionized water at a molar ratio of W:Cr = 0.1–0.3 to prepare a 0.5–1.0 mol / L tungstate solution B. NaOH solid was dissolved in deionized water to prepare a 2–4 ​​mol / L sodium hydroxide solution C.

3. The preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, When using polyethylene glycol-400 (1-3% by mass) as a dispersant, and feeding simultaneously via a three-channel parallel dripping method, the pH of the system is monitored and adjusted in real time to 9.0-10.0, the temperature is controlled at 10±2℃ throughout the process, and the dripping rate is controlled at 1-5 mL / min.

4. The preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, After the three-way simultaneous addition of solutions A, B, and C is completed and the feed pump is turned off, in order to promote the recovery of tungsten precipitate remaining in the supernatant in the form of tungstate ions, while keeping the reactor stirred and the temperature controlled, 0.5-1.0 mol / L dilute hydrochloric acid or citric acid solution is slowly added to the reactor through a peristaltic pump to slowly lower the pH of the system from 9.0-10.0 to 7.0±0.2, with the addition rate controlled at 0.5-2 mL / min. After adjusting back to the target pH, the system is kept at a constant temperature for 30-60 min to allow the residual tungstate ions to be fully converted into hydrated tungsten oxide precipitate and recombine with Cr(OH)3 and Zr(OH)4 flocs in situ.

5. The preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, Then, the reactor is heated to 45-60℃ and sealed for crystallization for 6-24 h. After crystallization, it is filtered, washed until neutral, and dried at 60-80℃ for 12 h to obtain the composite Cr(OH)3·0.1-0.3Zr(OH)4·0.1-0.3WO3·nH2O hydroxide precursor.

6. The preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 5, characterized in that, After crystallization, the precipitated slurry was subjected to plate and frame low-pressure filtration to initially remove the supernatant. An alternating washing mode of "deionized water hot washing + low-temperature alcohol washing" was adopted: repeated washing with 40℃ warm water 4 times to remove residual impurities in the system, followed by soaking and washing with anhydrous ethanol 2 times to replace the water between particles and prevent drying agglomeration; low-temperature pre-drying at 35℃ for 18 h → constant temperature drying at 65℃ for 12 h → deep drying at 105℃ for 10 h to completely remove free water and adsorbed solvent; after ultrafine airflow pulverization, it was passed through a 200-mesh standard sieve to obtain a ternary composite hydroxide pure phase powder with uniform particle size and composition.

7. The preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, Ternary hydroxide powder and anhydrous potassium carbonate ultrafine powder were fed into a closed double cone mixer at a molar ratio of 1:0.5-1. The mixture was mixed at a low speed of 160-300 r / min at room temperature for 4 hours. Every 30-50 minutes, the mixture was turned on at a high speed of 200-500 r / min for 2-5 minutes to ensure that potassium carbonate microcrystals were uniformly embedded in the gaps between hydroxide particles, without local enrichment or stratification, thus obtaining a solid-phase homogeneous composite powder.

8. The preparation method of the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, A segmented, temperature-controlled calcination process using a tube furnace was employed: First, an air atmosphere with a flow rate of 20-60 mL / min was introduced, and the temperature was increased from room temperature to 150-180 °C at a rate of 1.5-5.0 °C / min, and held at this temperature for 4-8 hours to remove residual physically adsorbed water from the powder. Then, a high-purity nitrogen inert atmosphere was introduced, and the temperature was increased to 480-550 °C at a rate of 1.2-3.0 °C / min, and held at this temperature for 5-10 hours to allow simultaneous dehydration and transformation of the ternary hydroxides into an initial composite oxide framework. Next, a buffer atmosphere of nitrogen and carbon dioxide was introduced, and the temperature was further increased to 790-850 °C at a rate of 0.7-2.5 °C / min to complete the high-temperature sizing of the framework. The temperature was then slowly decreased to 630-650 °C at a rate of 0.8-2.0 °C / min, followed by a switch to a normal-pressure air atmosphere with a flow rate of 40-80 mL / min, and then held at 630-650 °C. Calcination at a constant temperature of ℃ for 5–10 h.

9. The method for preparing the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, The crude product was soaked in a 0.12-0.5 mol / L citric acid solution with constant temperature shaking for 2-5 h to gently dissolve most of the potassium template in the imprinted cavity. After filtration and washing with water until neutral, it was soaked in a 0.07-0.1 mol / L sodium bicarbonate solution at room temperature for 2-5 h to fine-tune the hydroxyl structure and surface charge of the cavity wall, widen the ion diffusion mesoporous channels, and remove insoluble residual potassium impurities. The alternating weak acid-weak base immersion cycle was repeated twice, with thorough water washing each time. After vacuum drying at 40-60℃, Na was obtained after complete template removal. 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder.

10. The method for preparing the potassium adsorbent with a chromium-zirconium-tungsten ternary composite oxide heterojunction structure according to claim 1, characterized in that, To prepare a PVDF organic binder with a solid content of 20-30 wt%, Na... 0.5-1 CrZr 0.1-0.3 W 0.1-0.3 O 4.25-5.5 Potassium adsorbent powder and organic binder are added to a high-speed rotary granulator at a mass ratio of 1:0.3-0.5.