A method for preparing a moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material
By employing differential wetting control and staged in-situ reduction techniques, a high-silica β-molecular sieve carrier with a hydrophobic outer surface and hydrophilic inner pores was prepared. This solved the problems of pore blockage and mass transfer resistance in manganese oxide materials under high humidity conditions, and achieved the effect of efficiently removing gaseous pollutants such as formaldehyde.
Patent Information
- Application Number
- CN202611543744.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are difficult to effectively remove gaseous pollutants such as formaldehyde in high humidity environments. Manganese oxide materials are prone to forming agglomerates during drying or heat treatment, leading to pore blockage and increased mass transfer resistance. Furthermore, manganese salts are prone to detachment, and both hydrophilic and hydrophobic carriers have low adsorption efficiency.
By employing a synergistic technique of differential wetting control, pore volume-limited permeation, and staged in-situ reduction, a high-silica β-molecular sieve support with a hydrophobic outer surface and hydrophilic inner pores was prepared. The permanganate ions were reduced in situ in the internal pores by vacuum-pressurized permeation of potassium permanganate aqueous solution. Combined with the fractional addition of hydrogen peroxide and nucleation-growth cycles, the particle size and distribution of MnOx active domains were controlled. Finally, the pore volume-limited washing and low-concentration gas activation were performed using ammonium acetate solution.
This study achieved directional loading and confined growth of potassium permanganate in hierarchical high-silica β-molecular sieve particles, improving the efficiency of pollutant transfer and reaction under high humidity conditions, reducing the adverse effects of moisture on mass transfer, and enhancing mechanical stability and environmental safety.
Smart Images

Figure CN123102298A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of indoor air purification materials technology, specifically a method for preparing a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material. Background Technology
[0002] Formaldehyde, ammonia, trimethylamine, hydrogen sulfide, and other gaseous pollutants can persist for extended periods in indoor spaces, vehicles, warehouses, and solid waste storage environments. Porous adsorbents can enrich pollutants through their pores, but in high-humidity air, water molecules compete with polar pollutants for adsorption sites, forming a continuous water film on the particle's outer surface. Relying solely on physical adsorption also presents limitations in capacity and the risk of desorption. Manganese oxides possess multivalent state transitions and surface-active oxygen species, making them suitable for oxidizing formaldehyde and sulfur- and nitrogen-containing odor molecules. However, conventional impregnation-drying processes easily cause manganese salts to migrate to the particle's outer surface during evaporation, forming large agglomerates during drying or heat treatment, leading to pore blockage, increased mass transfer resistance, and the shedding of manganese-containing dust.
[0003] Existing technologies include deodorizing materials using potassium permanganate-supported porous carriers, as well as schemes that use resin or inorganic carriers to immobilize permanganate to improve wet stability. For example, CN104084034B relates to deodorizing materials immobilized with potassium permanganate; CN117772184B relates to hydrophilic carriers and manganese-containing components; and CN118594402A relates to the gas-phase reduction treatment of manganese materials. These schemes respectively illustrate the effects of permanganate, carrier hydrophilicity, or reduction treatment on pollutant removal, but do not provide the following coordinated preparation control: first, establish a spatial wetting gradient of "external hydrophobicity and internal hydrophilicity" for the same millimeter-sized particles; then, use atomized liquid addition at a volume not exceeding the available pore volume, combined with vacuum-pressurization, to directionally deliver permanganate ions into the internal channels; reduce peroxide fractionally under conditions where there is no continuous liquid phase externally; and limit the active domain to the sub-3nm scale through concentration programs of nucleation and growth cycles; finally, regulate the mixed valence state through pore volume-limited washing, low-hydrogen activation, inert replacement, and low-oxygen passivation.
[0004] Especially in high humidity environments, if the carrier is highly hydrophilic, a water film easily condenses on the outer surface, inhibiting the transfer of gaseous formaldehyde into the pores; if the carrier is hydrophobic, potassium permanganate aqueous solution and hydrogen peroxide aqueous solution will have difficulty entering the internal channels and completing a uniform reaction. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a method for preparing a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material. Through the synergistic technology of differential wetting control, pore volume limited permeation, and staged in-situ reduction, the method achieves directional loading and restricted growth of potassium permanganate precursor in hierarchical high-silica β-molecular sieve particles.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material, comprising the following steps: S1. Fill the internal channels of the graded high-silica β molecular sieve particles with polyethylene glycol aqueous solution, remove the continuous liquid film on the outer surface of the particles, remove water under 45-65℃ and 8-25kPa absolute pressure, so that polyethylene glycol remains in the internal channels; silanize the outer surface of the particles with C8-C12 alkyltrialkoxysilane in a non-aqueous medium, and then extract polyethylene glycol to obtain a differential wetting carrier with a hydrophobic outer surface and a hydrophilic internal channel. S2. Place the differentially wetting carrier in a sealed rotating container and evacuate it. Add potassium permanganate aqueous solution by atomization at a liquid addition rate not exceeding its usable pore volume. After vacuum-pressurized permeation, remove the free liquid on the outer surface and remove moisture with nitrogen gas at 40-60°C, so that the permanganate ions remain in the internal pores. The usable pore volume is the water absorption volume per unit mass of carrier measured by the vacuum saturated water absorption method at 25°C. The potassium permanganate is the only manganese source in the preparation process. S3. At 5–25°C, add 4%–8% hydrogen peroxide aqueous solution by atomization at a ratio of 1.50–1.65 mol hydrogen peroxide per mole of permanganate. This allows the permanganate to be reduced and nucleated in situ in the internal pores under conditions where there is no continuous liquid phase outside the support. After the oxygen release rate drops to less than 5% of the peak value, dehydrate at 60–90°C. Steps S2 and S3 are repeated 4 to 8 times until the dry-basis manganese loading, calculated as elemental manganese, is 2.5% to 5.5%; S4, pore volume limiting washing is performed with ammonium acetate solution, followed by activation in nitrogen gas containing 0.2% to 1.0% hydrogen at 160 to 220°C, then replacement with pure nitrogen gas until the outlet hydrogen gas fraction is less than 0.05%, and then passivation in nitrogen gas containing 0.5% to 2.0% oxygen at the same temperature, to obtain MnO with an equivalent particle size D50 of 0.8 to 2.5 nm, confined and dispersed in the internal mesopores. x The active domain is cooled and granulated to obtain the material.
[0007] Preferably, the high-silica β-zeolite particles in step S1 are obtained by the following method: β-zeolite raw material with a SiO2 / Al2O3 molar ratio of 80–160 is added to a treatment solution containing 0.08–0.18 mol / L sodium hydroxide and 0.03–0.10 mol / L tetrapropylammonium hydroxide, treated at 55–75°C for 15–40 min, washed with water, and then treated with 0.10–0.40 mol / L citric acid solution at 60–80°C for 20–60 min. After ammonium exchange, drying, and calcination at 450–550°C, a hierarchical β-molecular sieve with an average mesopore diameter of 3–12 nm, a mesopore volume of 0.20–0.55 cm³ / g, and a micropore volume retention rate of not less than 70% of that before treatment is obtained. The hierarchical β-molecular sieve is mixed with silica sol at 5%–12% of its mass based on SiO₂ to form granules, which are then dried at 100–130°C and calcined at 450–550°C to obtain high-silica β-molecular sieve particles with a particle size of 0.5–3.0 mm.
[0008] Preferably, the polyethylene glycol aqueous solution has a mass fraction of 15%–30%, the number average molecular weight of the polyethylene glycol is 400–1000, and the amount of polyethylene glycol aqueous solution used is 85%–105% of the usable pore volume of the high-silica β-molecular sieve particles; The alkyltrialkoxysilane is at least one of n-octyltriethoxysilane and dodecyltrimethoxysilane, with a mass fraction of 0.5% to 3.0% in a non-aqueous medium. The reaction temperature is 65 to 90°C and the reaction time is 1 to 4 hours. After the reaction, polyethylene glycol is extracted sequentially with ethanol and water at 50 to 70°C until the total organic carbon in the final water extract is not higher than 50 mg / L, so that the apparent static water contact angle of the differential wetting carrier on the particle monolayer fixed sample is 105° to 135°.
[0009] Preferably, in step S2, the sealed rotating container is first evacuated to a gauge pressure of -0.060 to -0.095 MPa and maintained for 5 to 20 minutes. Then, potassium permanganate aqueous solution is added as droplets with an average droplet diameter of 20 to 80 μm while the carrier is agitated. After the addition is completed, nitrogen gas is introduced to a gauge pressure of 0.15 to 0.35 MPa and maintained for 2 to 10 minutes. Then, the container is centrifuged at 300 to 900 × g for 1 to 4 minutes to remove the free liquid on the outer surface.
[0010] Preferably, in step S3, the hydrogen peroxide aqueous solution is divided into 3 to 8 equimolar portions and added sequentially via atomization. The carrier is continuously agitated between adjacent portions, and the next portion is added only after the oxygen volume fraction at the container outlet drops below 20% of the previous peak value. The carrier temperature is maintained at 8 to 20°C by a jacket. The volume of any portion of the hydrogen peroxide aqueous solution does not exceed 20% of the available pore volume of the carrier before the current reaction, and the total volume of the hydrogen peroxide aqueous solution does not exceed 50% of the available pore volume.
[0011] Preferably, the cycles in steps S2 and S3 include 2 to 3 nucleation cycles and 2 to 5 growth cycles; the concentration of potassium permanganate aqueous solution used in the nucleation cycle is 0.05 to 0.10 mol / L, and the concentration of potassium permanganate aqueous solution used in the growth cycle increases by 1.2 to 1.8 times the concentration of the previous cycle, reaching 0.30 mol / L and then maintaining it at 0.30 mol / L; after each cycle, the water content of the carrier is reduced to below 3% by nitrogen gas at 60 to 90°C before entering the next cycle.
[0012] Preferably, in step S4, a 0.01–0.08 mol / L ammonium acetate solution is used for two atomized washes. Each addition is 35%–50% of the usable pore volume of the carrier after circulation. After each addition, the carrier is agitated for 5–15 minutes and centrifuged at 300–900 × g. The temperature is then increased to 160–220°C at a rate of 0.5–2°C / min. The mixture is first kept in the hydrogen-containing nitrogen atmosphere for 20–60 minutes, then purged with pure nitrogen for 10–30 minutes until the outlet hydrogen fraction is confirmed to be below 0.05%. Finally, the mixture is switched to the oxygen-containing nitrogen atmosphere and kept for 30–90 minutes to allow the MnO₂ to form a precipitate. x Mn in the active domain as measured by X-ray photoelectron spectroscopy 3+ With Mn 4+ The peak area ratio is 0.20–0.55, and the K / Mn atomic ratio is 0.03–0.15.
[0013] Preferably, by controlling the number of cycles in steps S2 and S3 and the amount of potassium permanganate added in a single step, the MnO... x The equivalent particle size D90 of the active domain, in terms of number, is not greater than 4.0 nm; the equivalent particle size is determined by transmission electron microscopy, and at least 80% of the manganese signal is located in the hierarchical pore region at a depth of 50 μm from the outer surface of the particle, as determined by scanning electron microscopy-energy dispersive X-ray spectroscopy of the particle cross section; the BET specific surface area retention rate of the activated material is not less than 65% of that of the differential wetting carrier.
[0014] Preferably, cooling is carried out in nitrogen gas with a dew point not higher than -20°C. After cooling to below 50°C, free fine powder is removed by sieving through a sieve with a pore size of 0.25–0.45 mm. The material is then equilibrated in air at 25–35°C and a relative humidity of 45%–60% for 4–12 hours to achieve a moisture content of 2%–6%, thereby hydrating MnO without forming an external continuous water film. x The active domain is used to obtain the material to be tested.
[0015] Preferably, the materials to be tested are screened for moisture resistance: the same batch of materials are divided into a high-humidity group and a parallel reference group. 2.0g of the high-humidity group is exposed to air at 25±2℃ and 85%±3% relative humidity for 72h, and 2.0g of the parallel reference group is placed in air at 25±2℃ and 50%±3% relative humidity for 72h. The two groups of materials are placed in a 1m³ sealed chamber and tested for 2h under the conditions of 25±2℃, 85%±3% relative humidity, initial formaldehyde concentration of 1.00±0.05mg / m³, and chamber air circulation of 1.0±0.1m³ / h. Based on the apparent first-order removal rate constant of formaldehyde in the parallel reference group, the materials with a rate constant retention rate of not less than 80% in the high-humidity group are screened. Before and after high-humidity exposure, the materials are sieved with a 0.25mm sieve and the manganese mass in the fine powder under the sieve is measured. The materials with an increase in free manganese fine powder not exceeding 0.5% of the dry basis mass of the material are screened as finished products and sealed and packaged.
[0016] Compared with existing technologies, this invention provides a method for preparing a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material, which has the following beneficial effects: This invention achieves directional loading and restricted growth of potassium permanganate precursors in hierarchical high-silica β-molecular sieve particles through a synergistic technology of differential wetting control, pore volume-limited infiltration, and staged in-situ reduction. Polyethylene glycol pore protection combined with external surface alkylsilanization creates a spatial wetting gradient where the carrier has a hydrophobic outer surface and hydrophilic internal pores. During preparation, the internal hydrophilic pores facilitate the penetration of potassium permanganate aqueous solution into the deep layers of the particles, while the external hydrophobic surface reduces precursor liquid retention and drying migration. During use, the hydrophobic outer surface inhibits the formation of a continuous water film under high humidity conditions, reducing the adverse effects of moisture on the mass transfer of gaseous pollutants. Vacuum-pressurized infiltration, pore volume-limited liquid addition, and removal of free liquid from the external surface further avoid surface shell deposition, pore blockage, and manganese-containing fine powder shedding caused by traditional excessive impregnation, ensuring that manganese is preferentially distributed in the hierarchical pore region inside the particles.
[0017] This invention employs a controlled approach combining the partial addition of hydrogen peroxide with a nucleation-growth cycle, which can reduce the local instantaneous reduction rate, reaction exotherm, and concentrated oxygen release, thus preventing MnO. x The explosive nucleation and excessive aggregation of active domains are beneficial for obtaining ultra-small MnO with uniform particle size and confined dispersion. x The active domain is expanded, increasing the effective active surface area per unit manganese loading. Ammonium acetate pore volume-limited washing reduces residual potassium ion content while preventing active component migration caused by large-volume water washing. The synergistic treatment of low-concentration hydrogen activation, safe replacement with pure nitrogen, and low-concentration oxygen passivation can adjust the Mn content. 3+ / Mn 4+ The ratio and surface oxygen defects are balanced to ensure low-temperature oxidation activity, storage stability and operational safety.
[0018] Through the above-mentioned process and structural optimization, the resulting material, while maintaining high pore accessibility and specific surface area, can sustain the transfer and reaction of odor pollutants such as formaldehyde, ammonia, trimethylamine, and hydrogen sulfide to internal active sites under high humidity conditions, reducing the degradation of purification performance caused by increased humidity. The internal confined structure can also enhance the purification performance of MnO. x The binding between the active domain and the carrier reduces the generation of free manganese powder during use and transportation, thereby improving the mechanical stability and environmental safety of the material. Attached Figure Description
[0019] Figure 1 This is a static water contact angle diagram of a monolayer of differentially wetting carrier particles fixed in place as prepared in Example 2 of the present invention; Figure 2 This is a SEM-EDS surface distribution diagram of manganese in the complete particle cross section of the composite material obtained in Example 2 of the present invention; Figure 3 The mesoporous region MnO inside the composite material obtained in Example 2 of this invention x HAADF-STEM image of the active domain. Detailed Implementation
[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0021] Please see Figures 1-3 This invention provides a technical solution for preparing a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material: The differential wetting described in this invention does not involve transforming the entire particle into a hydrophobic material. Instead, it utilizes the temporary occupation of the pores by the internal polyethylene glycol and the spatial shielding created by low-temperature dehydration, causing alkyltrialkoxysilanes to preferentially condense on the outer geometric surface of the particle and the outer edge of the pores. After polyethylene glycol extraction, the alkylsilane layer is retained on the outer surface, while the molecular sieve hydroxyl groups and ion exchange sites are retained on the internal pore walls. During the preparation stage, the potassium permanganate aqueous solution enters the hydrophilic internal pores under the pressure difference of vacuum release and nitrogen pressurization, while the hydrophobic outer surface is less prone to retaining a continuous liquid film. During the usage stage, the hydrophobic layer on the outer surface reduces the tendency of high-humidity air to form a continuous water film on the outside of the particles, thus balancing the directional transport of aqueous precursors and the mass transfer of gaseous pollutants.
[0022] Pore-limited liquid addition and dehydration per cycle inhibited capillary migration along the outer surface of the particles. Partial addition of hydrogen peroxide reduced the local instantaneous reduction rate and exothermic and oxygen-emission peaks, allowing permanganate ions to nucleate within the confined liquid film. Two to three nucleation cycles were initially performed using a lower concentration, followed by gradually increasing the concentration on existing nuclei for growth, preferentially depositing newly formed manganese onto existing MnO. x Active domains are formed rather than re-nucleated on the outer surface. Limited washing with ammonium acetate reduces residual potassium ions and avoids active domain migration caused by large-volume water washing. Low-concentration hydrogen activation increases the Mn³⁺ ratio and forms oxygen vacancies; pure nitrogen displaces and eliminates reducing gases; then low-concentration oxygen passivates and stabilizes the surface, resulting in mixed-valence MnO with both reactivity and storage stability. x Active domain.
[0023] The above mechanism is an explanation of the process-structure-performance relationship and is not intended to limit MnO. x In this context, x represents the average oxygen-manganese stoichiometry of mixed-valence manganese oxides. The material may contain amorphous or low-crystallinity Mn(III) / Mn(IV) oxides and their hydrated surface species, without requiring the formation of a single crystalline phase.
[0024] "Usable pore volume" is calculated by placing granules dried to constant weight at 105°C in deionized water at 25°C, applying a vacuum for 30 minutes under an absolute pressure not exceeding 10 kPa, allowing them to stand for 30 minutes after returning to normal pressure, rapidly draining away free water between the granules, and lightly touching the outer surface with a moist, dust-free filter media. The volume of water absorbed per unit mass is calculated by dividing the saturated water absorption weight gain by the density of water at 25°C and the dry sample mass. The usable pore volume after each cycle can be determined by retaining samples from the same batch; during production, it can also be determined by multiplying the initial usable pore volume by a validated cycle correction factor.
[0025] "Dry-based manganese loading" is the percentage of elemental manganese by mass relative to the dry-based material mass, obtained by microwave acid digestion and ICP-OES after drying the material to constant weight at 105℃. "MnO" x "Active domains" are mixed-valence manganese oxide nanodomains formed by the reduction, activation, and passivation of permanganate ions within the pores. "D50" and "D90" are the cumulative median and 90th percentile values of the number of at least 300 mutually identifiable active domains in a TEM image, calculated by converting their projected areas into equivalent circle diameters.
[0026] "The proportion of manganese signals located at a depth of 50 μm or more from the outer surface of the particle" is obtained by embedding at least 10 random intact particles, polishing the cross-section, obtaining the surface distribution of manganese elements containing the complete cross-section using SEM-EDS, subtracting the background, and dividing the integrated manganese signal in the region at a normal distance of not less than 50 μm from the outer surface by the average value obtained by dividing the total integrated manganese signal of the particle cross-section.
[0027] "BET specific surface area retention rate" is the ratio of the BET specific surface area of the activated material to the BET specific surface area of the corresponding differentially wetting carrier. "Increase in free manganese fine powder" is the percentage obtained by dividing the mass of manganese in the newly added 0.25mm sieve-filled fine powder after high-humidity exposure relative to the mass before exposure by the dry basis mass of the material before exposure. "Apparent static water contact angle" is measured using a fixed sample formed by a single layer of densely fixed particles of the same size on a non-porous plate, not by powder pellets.
[0028] The sealed rotating container is equipped with a jacket, atomizing nozzle, pressure sensor, oxygen content sensor, hydrogen content detection port, condensate exhaust port, and explosion-proof pressure relief device. Potassium permanganate and organic matter are stored separately; hydrogen peroxide aqueous solution is prepared and used immediately, and the exhaust gas is kept unobstructed and oxygen release is monitored during the portioning process. The hydrogen activation equipment is equipped with hydrogen interlock and backfire prevention devices; hydrogen-containing gas and oxygen-containing gas must not be introduced into the equipment at the same time, and switching to oxygen-containing gas is only allowed after pure nitrogen purging and the outlet hydrogen gas fraction is less than 0.05%. In all embodiments, the change rate of oxygen volume fraction in the exhaust gas is used as an auxiliary criterion for the reaction endpoint, and the material moisture content is confirmed to be less than 3% after each cycle.
[0029] The following examples use 1,000 kg of calcined high-silica β-molecular sieve particles as the starting carrier mass.
[0030] Example 1
[0031] β-zeolite powder with a SiO2 / Al2O3 molar ratio of 80 was added to 10.0 L of a treatment solution containing 0.08 mol / L sodium hydroxide and 0.03 mol / L tetrapropylammonium hydroxide, and stirred at 55 °C for 15 min. The mixture was immediately filtered and washed with deionized water until the pH of the filtrate was less than 9. Then, 10.0 L of a 0.10 mol / L citric acid solution was added, and the mixture was treated at 60 °C for 20 min. After washing with water, the mixture was exchanged twice with a 1.0 mol / L ammonium nitrate solution at 80 °C, 2 h each time. The material was dried at 110 °C for 8 h, then heated to 450 °C at a rate of 1 °C / min and held for 4 h. Nitrogen adsorption analysis revealed that the average mesopore diameter of the obtained hierarchical β-zeolite was 3.0 nm, the mesopore volume was 0.20 cm³ / g, and the micropore volume was 70% of the raw material. Acidic silica sol, calculated as SiO2 equivalent to 5% of the dry weight of the molecular sieve, was added, kneaded, extruded, granulated, and rounded. Particles of 0.5±0.1 mm were sieved, dried at 100℃ for 8 hours, and calcined at 450℃ for 4 hours to obtain high-silica β-molecular sieve particles. The usable pore volume at 25℃ is 0.47 mL / g.
[0032] Take 1.000 kg of the above-mentioned particles and atomize 399.5 mL of 15% (w / w) PEG400 aqueous solution in a drum impregnator. The amount added is 85% of the usable pore volume. After stirring for 10 min, remove the continuous liquid film between particles and on the outer surface of the particles with a moistened PTFE scraper. Dry at 45℃ and 25 kPa absolute pressure until the mass change between two consecutive weighings is less than 0.2%, so that polyethylene glycol is retained in the internal channels. Add the particles to 5.0 L of 0.5% (w / w) n-octyltriethoxysilane anhydrous n-heptane solution and react at 65℃ for 1 h under nitrogen protection. After filtration, wash rapidly with anhydrous n-heptane, then extract twice with ethanol at a solid-liquid ratio of 1:3, and then extract with water at 50℃ at a solid-liquid ratio of 1:5 for 20 min each time, until the total organic carbon in the final aqueous extract is 48 mg / L. The sample was dried under nitrogen at 60°C to constant weight to obtain a differentially wetted carrier; the apparent static water contact angle of the particle monolayer immobilized sample was 105°.
[0033] The differentially wetted carrier was placed in a sealed rotating container, and the pressure was evacuated to -0.060 MPa and maintained for 5 min. While the carrier was continuously agitated, 0.300 L of potassium permanganate aqueous solution was added via atomization at an average droplet diameter of 20 μm. After the addition was completed, nitrogen gas was introduced to a pressure of 0.15 MPa and maintained for 2 min. The carrier was then centrifuged at 300 × g for 1 min to remove the free liquid on the outer surface, and then purged with nitrogen gas at 40 °C. Cycles 1 to 3 were nucleation cycles, with potassium permanganate concentrations of 0.050 mol / L, 0.075 mol / L, and 0.100 mol / L, respectively. Cycles 4 to 8 were growth cycles, with concentrations of 0.180 mol / L, 0.300 mol / L, 0.300 mol / L, 0.300 mol / L, and 0.300 mol / L, respectively.
[0034] After each potassium permanganate impregnation, the jacket temperature was maintained at 5°C. A 4% (w / w) hydrogen peroxide aqueous solution was used, with a ratio of 1.50 mol hydrogen peroxide per mole of permanganate. The required mass of hydrogen peroxide aqueous solution for the eight cycles were 19.1 g, 28.7 g, 38.3 g, 68.9 g, 114.8 g, 114.8 g, 114.8 g, and 114.8 g, respectively. Each time, it was added in three equal molar portions via atomization, with the volume of any single portion not exceeding 20% of the available pore volume for that cycle. Adjacent portions were continuously agitated until the outlet oxygen volume fraction dropped below 20% of the previous peak. After all portions were added, agitation continued until the oxygen release rate dropped below 5% of the peak value. Then, nitrogen gas at 60°C was used to reduce the moisture content to below 3% before proceeding to the next cycle.
[0035] After circulation, the material was washed twice with a 0.01 mol / L ammonium acetate solution via atomization, with each addition being 35% of the usable pore volume after circulation. After agitation for 5 min, the material was centrifuged at 300 × g for 1 min. The material was placed in a tubular activator and heated to 160°C in nitrogen at a rate of 0.5°C / min. Nitrogen gas containing 0.2% hydrogen was introduced and kept at this temperature for 20 min. After stopping the hydrogen gas, the material was purged with pure nitrogen for 10 min. The outlet hydrogen gas fraction was measured to be 0.04%. The material was then switched to nitrogen gas containing 0.5% oxygen and kept at this temperature for 30 min. The material was cooled to 45°C in nitrogen gas with a dew point of -20°C. Fine powder was removed by sieving through a 0.25 mm sieve. The material was then equilibrated in air at 25°C and 45% relative humidity for 4 h to achieve a moisture content of 2.0%, yielding the material of Example 1.
[0036] Example 2
[0037] β-zeolite powder with a SiO2 / Al2O3 molar ratio of 120 was added to 10.0 L of a treatment solution containing 0.13 mol / L sodium hydroxide and 0.065 mol / L tetrapropylammonium hydroxide, and treated at 65 °C for 27.5 min. After filtration and washing with water, 10.0 L of a 0.25 mol / L citric acid solution was added, and the mixture was treated at 70 °C for 40 min. After two ammonium nitrate exchanges and drying at 110 °C, the temperature was increased to 500 °C at a rate of 1 °C / min and calcined for 4 h. The resulting hierarchical β-zeolite had an average mesopore diameter of 7.5 nm, a mesopore volume of 0.375 cm³ / g, and a micropore volume of 82% of the raw material. Add silica sol at 8.5% of the dry weight of the molecular sieve (based on SiO2), mix and knead into granules, sieve out 1.75±0.25mm particles, dry at 115℃ for 8h and calcine at 500℃ for 4h to obtain high-silica β-molecular sieve particles with a usable pore volume of 0.58mL / g.
[0038] Take 1.000 kg of the above particles and atomize them with 551 mL of 22.5% (w / w) PEG700 aqueous solution, which is 95% of the usable pore volume. Agitate for 15 min and remove the continuous liquid film on the outer surface. Dry to constant weight at 55℃ and 16.5 kPa absolute pressure. Prepare 5.0 L of anhydrous n-heptane solution containing 1.75% (w / w) of n-octyltriethoxysilane and dodecyltrimethoxysilane in a 1:1 (w / w) ratio. React the particles at 77.5℃ for 2.5 h under nitrogen protection. After filtration and washing with n-heptane, extract twice with ethanol at a solid-liquid ratio of 1:3, and then extract with water at 60℃ at a solid-liquid ratio of 1:5 for 30 min each time, until the total organic carbon in the final aqueous extract is 32 mg / L. Dry under nitrogen at 60℃ to obtain a differentially wetting carrier with an apparent static water contact angle of 121°.
[0039] The carrier was placed in a sealed rotating container, and the pressure was evacuated to -0.078 MPa and maintained for 12.5 min. While agitated, 0.550 L of potassium permanganate aqueous solution was added via atomization at an average droplet diameter of 50 μm. Nitrogen was then introduced to a pressure of 0.25 MPa and maintained for 6 min. The mixture was then centrifuged at 600 × g for 2.5 min. A total of 6 cycles were performed: cycles 1 and 2 were nucleation cycles with potassium permanganate concentrations of 0.075 mol / L and 0.100 mol / L, respectively; cycles 3–6 were growth cycles with concentrations of 0.180 mol / L, 0.300 mol / L, 0.300 mol / L, and 0.300 mol / L, respectively.
[0040] In each cycle, at 14°C, 1.575 mol of hydrogen peroxide is added per mole of permanganate, using a 6% (w / w) hydrogen peroxide aqueous solution. The required solution masses for the six cycles are 36.8 g, 49.1 g, 88.4 g, 147.3 g, 147.3 g, and 147.3 g, respectively. Each time, the solution is divided into five equimolar portions and added sequentially via atomization, with the addition interval controlled according to the oxygen peak decline condition. The total volume of the hydrogen peroxide solution is less than 50% of the usable pore volume for that cycle. After the reaction is complete, the solution is dehydrated under nitrogen at 75°C until the water content is below 3% before proceeding to the next cycle.
[0041] After circulation, the material was washed twice with 0.045 mol / L ammonium acetate solution, each time adding 42.5% of the usable pore volume after circulation. The mixture was agitated for 10 min and centrifuged at 600 × g for 2.5 min. The material was heated to 190 °C in nitrogen at 1.25 °C / min, then switched to nitrogen containing 0.6% hydrogen and held at this temperature for 40 min. It was then purged with pure nitrogen for 20 min. After the outlet hydrogen fraction decreased to 0.03%, it was switched to nitrogen containing 1.25% oxygen and held at this temperature for 60 min. The material was cooled to 45 °C in nitrogen at a dew point of -30 °C, and fine powder was removed by sieving through a 0.35 mm sieve. It was then equilibrated in air at 30 °C and 52.5% relative humidity for 8 h, with a moisture content of 4.0%, yielding the material of Example 2.
[0042] Example 3
[0043] β-zeolite powder with a SiO2 / Al2O3 molar ratio of 160 was added to 10.0 L of a treatment solution containing 0.18 mol / L sodium hydroxide and 0.10 mol / L tetrapropylammonium hydroxide, and treated at 75 °C for 40 min. After filtration and washing with water, it was treated with 10.0 L of 0.40 mol / L citric acid solution at 80 °C for 60 min. After two ammonium nitrate exchanges and drying at 110 °C, the temperature was increased to 550 °C at a rate of 1 °C / min and calcined for 4 h. The resulting hierarchical β-zeolite had an average mesopore diameter of 12 nm, a mesopore volume of 0.55 cm³ / g, and a micropore volume of 74% of the raw material. Silica sol, calculated as 12% of the dry weight of the zeolite (based on SiO2), was added, mixed into granules, and sieved to obtain particles of 3.0 ± 0.2 mm. These particles were then dried at 130 °C for 8 h and calcined at 550 °C for 4 h to obtain high-silica β-zeolite particles with a usable pore volume of 0.75 mL / g.
[0044] Take 1.000 kg of particles and atomize them into 787.5 mL of a 30% (w / w) PEG1000 aqueous solution, the amount being 105% of the usable pore volume. Agitate for 20 min, centrifuge to remove liquid that cannot enter the pores and remove the continuous liquid film on the outer surface, and dry to constant weight at 65℃ and 8 kPa absolute pressure. Add 5.0 L of a 3.0% (w / w) dodecyltrimethoxysilane anhydrous n-heptane solution to the particles and react at 90℃ for 4 h under nitrogen protection. After filtration and washing with n-heptane, extract three times with ethanol at a solid-liquid ratio of 1:3, and then extract three times with water at 70℃ at a solid-liquid ratio of 1:5, each time for 30 min, until the total organic carbon in the final aqueous extract is 21 mg / L. Dry under nitrogen at 60℃ to obtain a differentially wetting carrier with an apparent static water contact angle of 135°.
[0045] The carrier was placed in a sealed rotating container, and the pressure was evacuated to -0.095 MPa and maintained for 20 min. 0.690 L of potassium permanganate aqueous solution was added via atomization with an average droplet diameter of 80 μm. Nitrogen was then introduced until the pressure reached 0.35 MPa and maintained for 10 min. The mixture was then centrifuged at 900 × g for 4 min. Eight cycles were performed: the concentrations for cycles 1-3 were 0.050 mol / L, 0.075 mol / L, and 0.100 mol / L; the concentrations for cycles 4-8 were 0.180 mol / L, 0.300 mol / L, 0.300 mol / L, 0.300 mol / L, and 0.300 mol / L.
[0046] For each cycle, at 25°C, 1.65 mol of hydrogen peroxide was added per mole of permanganate using an 8% (w / w) aqueous solution of hydrogen peroxide. The required solution masses for the eight cycles were 24.2 g, 36.3 g, 48.4 g, 87.1 g, 145.2 g, 145.2 g, 145.2 g, and 145.2 g, respectively; each time, it was added in eight equimolar portions via atomization. After the oxygen release rate reached its endpoint, the solution was dried under nitrogen at 90°C until the moisture content was below 3%.
[0047] After circulation, the material was washed twice with 0.08 mol / L ammonium acetate solution, each time adding 50% of the usable pore volume after circulation. The mixture was agitated for 15 min and centrifuged at 900 × g for 4 min. The temperature was raised to 220°C at 2°C / min in nitrogen, then purged with nitrogen containing 1.0% hydrogen and held for 60 min. Subsequently, the temperature was purged with pure nitrogen for 30 min. When the outlet hydrogen integral was found to be below 0.01%, nitrogen containing 2.0% oxygen was purged and held for 90 min. The material was cooled to 45°C in nitrogen with a dew point of -40°C, and fine powder was removed by sieving through a 0.45 mm sieve. It was then equilibrated in air at 35°C and 60% relative humidity for 12 h to achieve a moisture content of 6.0%, yielding the material of Example 3.
[0048] Example 4
[0049] β-zeolite powder with a SiO2 / Al2O3 molar ratio of 140 was added to 10.0 L of a treatment solution containing 0.15 mol / L sodium hydroxide and 0.08 mol / L tetrapropylammonium hydroxide, and treated at 70 °C for 30 min. After filtration and washing with water, it was treated with 10.0 L of 0.30 mol / L citric acid solution at 75 °C for 45 min. After two ammonium nitrate exchanges and drying at 110 °C, it was calcined at 520 °C for 4 h to obtain a hierarchical β-zeolite with an average mesopore diameter of 9.0 nm, a mesopore volume of 0.46 cm³ / g, and a micropore volume retention rate of 79%. Silica sol, calculated as 10% of the dry weight of the zeolite (based on SiO2), was added, mixed into granules, and particles of 2.2 ± 0.2 mm were sieved, dried at 120 °C, and calcined at 520 °C to obtain high-silica β-zeolite particles with a usable pore volume of 0.75 mL / g.
[0050] Take 1.000 kg of particles and atomize them into 750 mL of a 25% (w / w) PEG800 aqueous solution. Stir for 15 min and remove the continuous liquid film on the outer surface. Dry to constant weight at 58℃ and 14 kPa absolute pressure. Add 5.0 L of anhydrous n-heptane solution containing 2.0% (w / w) total silanes (octyltriethoxysilane and dodecyltrimethoxysilane in a 2:1 mass ratio) to the particles and react at 80℃ for 3 h. Extract successively with ethanol and water at 65℃ until the total organic carbon in the final water extract is 27 mg / L. After drying under nitrogen, the apparent static water contact angle of the support is 124°.
[0051] The carrier was placed in a sealed rotating container, and the pressure was evacuated to -0.085 MPa and maintained for 15 min. While agitated, 0.710 L of potassium permanganate aqueous solution was added via atomization at an average droplet diameter of 60 μm. Nitrogen was then introduced to a pressure of 0.30 MPa and maintained for 8 min. The container was then centrifuged at 700 × g for 3 min. Four cycles were performed: the potassium permanganate concentration was 0.100 mol / L for the first two nucleation cycles, and 0.180 mol / L and 0.300 mol / L for the latter two growth cycles, respectively.
[0052] In each cycle, at 8°C, 1.60 mol of hydrogen peroxide was added per mole of permanganate, using a 6% (w / w) aqueous solution of hydrogen peroxide. The required solution masses for the four cycles were 64.4 g, 64.4 g, 115.9 g, and 193.2 g, respectively. Each addition was divided into four equimolar portions, with the interval controlled according to the oxygen peak decline condition. After the reaction was complete, the water content was reduced to below 3% under nitrogen gas at 80°C.
[0053] The material was washed twice with 0.060 mol / L ammonium acetate solution, each time adding 45% of the usable pore volume after circulation. The mixture was agitated for 12 min and centrifuged at 700 × g for 3 min. The material was heated to 200 °C at 1.5 °C / min and held in nitrogen containing 0.8% hydrogen for 50 min. It was then purged with pure nitrogen for 25 min until the outlet hydrogen fraction was 0.02%, and then held in nitrogen containing 1.5% oxygen for 75 min. The material was cooled to 45 °C in nitrogen with a dew point of -25 °C, and fine powder was removed by sieving through a 0.40 mm sieve. It was then equilibrated in air at 32 °C and 55% relative humidity for 10 h to achieve a moisture content of 5.0%, yielding the material of Example 4.
[0054] Example 5
[0055] β-zeolite powder with a SiO2 / Al2O3 molar ratio of 100 was added to 10.0 L of a treatment solution containing 0.10 mol / L sodium hydroxide and 0.05 mol / L tetrapropylammonium hydroxide, and treated at 60 °C for 20 min. After filtration and washing with water, it was treated with 10.0 L of 0.15 mol / L citric acid solution at 65 °C for 30 min. After two ammonium nitrate exchanges and drying at 110 °C, it was calcined at 480 °C for 4 h to obtain a hierarchical β-zeolite with an average mesopore diameter of 5.0 nm, a mesopore volume of 0.28 cm³ / g, and a micropore volume retention rate of 75%. Silica sol, calculated as 7% of the dry weight of the zeolite based on SiO2, was added, kneaded into granules, and sieved to obtain particles of 1.0 ± 0.1 mm. These particles were then dried at 105 °C and calcined at 480 °C to obtain high-silica β-zeolite particles with a usable pore volume of 0.52 mL / g.
[0056] Take 1.000 kg of particles and atomize them into 468 mL of 20% (w / w) PEG600 aqueous solution, the amount being 90% of the usable pore volume. Agitate for 12 min, remove the continuous liquid film on the outer surface, and dry to constant weight at 50℃ and 20 kPa absolute pressure. Add 5.0 L of 1.0% (w / w) n-octyltriethoxysilane anhydrous n-heptane solution and react at 70℃ for 2 h. Filter and wash with n-heptane, then extract twice with ethanol at a solid-liquid ratio of 1:3, and then extract with water at 55℃ at a solid-liquid ratio of 1:5 until the total organic carbon in the final aqueous extract is 40 mg / L. Dry under nitrogen at 60℃ to obtain a differential wetting carrier with an apparent static water contact angle of 112°.
[0057] The carrier was placed in a sealed rotating container, and the pressure was evacuated to -0.070 MPa and maintained for 10 min. While agitated, 0.500 L of potassium permanganate aqueous solution was added via atomization with an average droplet diameter of 35 μm. Nitrogen was then introduced to a pressure of 0.20 MPa and maintained for 4 min. The container was then centrifuged at 450 × g for 2 min. A total of 5 cycles were performed: the potassium permanganate concentrations for the first two nucleation cycles were 0.080 mol / L and 0.100 mol / L, respectively, and the concentrations for the last three growth cycles were 0.180 mol / L, 0.300 mol / L, and 0.300 mol / L, respectively.
[0058] In each cycle, at 20°C, 1.55 mol of hydrogen peroxide was added per mole of permanganate, using a 5% (w / w) aqueous solution of hydrogen peroxide. The required solution masses for the five cycles were 42.2 g, 52.7 g, 94.9 g, 158.2 g, and 158.2 g, respectively. Each addition was divided into six equimolar portions, with the interval controlled according to the oxygen peak decline condition. After the reaction was completed, the water content was reduced to below 3% under nitrogen gas at 70°C.
[0059] The material was washed twice with 0.030 mol / L ammonium acetate solution, with each wash adding 40% of the usable pore volume after circulation. The mixture was agitated for 8 min and centrifuged at 450 × g for 2 min. The material was heated to 180 °C at a rate of 1 °C / min and held in nitrogen containing 0.4% hydrogen for 30 min. It was then purged with pure nitrogen for 15 min until the outlet hydrogen fraction was 0.04%, and then held in nitrogen containing 1.0% oxygen for 45 min. The material was cooled to 45 °C in nitrogen with a dew point of -25 °C, and fine powder was removed by sieving through a 0.30 mm sieve. It was then equilibrated in air at 28 °C and 50% relative humidity for 6 h to achieve a moisture content of 3.0%, yielding the material of Example 5.
[0060] Unless otherwise stated, the following comparative examples are the same as those in Example 2.
[0061] Comparative Example 1 The difference is that the internal channels are not filled with PEG700 aqueous solution, and the PEG pore-forming and extraction steps are not performed. Instead, the dried high-silica β molecular sieve particles are directly silanized with the mixed silane solution of Example 2.
[0062] Comparative Example 2 The difference is that after PEG700 filling and low-temperature vacuum dehydration, alkyltrialkoxysilane treatment is not performed. Instead, PEG is directly extracted with ethanol and warm water before proceeding with the remaining steps.
[0063] Comparative Example 3 The difference is that each potassium permanganate impregnation involves soaking the carrier in a solution with a volume equivalent to 10 times the available pore volume for 30 minutes, while reducing the solution concentration accordingly for the same amount of potassium permanganate. After filtration, the solution directly proceeds to the hydrogen peroxide step.
[0064] Comparative Example 4 The difference is that the hydrogen peroxide solution for each cycle is not divided into 5 portions, but is added all at once via atomization within 30 seconds.
[0065] Comparative Example 5 The difference is that the washed material is heated to 190°C in pure nitrogen at a rate of 1.25°C / min and held for 120 min, without hydrogen activation or oxygen passivation.
[0066] Performance testing methods Pore structure, wettability and manganese loading Nitrogen adsorption tests were performed according to GB / T19587-2017 "Determination of Specific Surface Area of Solid Substances by Gas Adsorption BET Method". The sample was initially prepared without altering the MnO content. x Under valence conditions, the material was degassed in vacuum at 120℃ for 6 hours, and the BET specific surface area was calculated using the nitrogen adsorption isotherm at 77K. Mesopore diameter and volume were calculated using the same batch of data according to the BJH desorption branch or an instrumentally validated NLDFT model; the entire sample group used the same model. The activated material and its corresponding differentially wetted carrier underwent the same pretreatment, and the retention rate was calculated based on the ratio of their BET specific surface areas.
[0067] The static water contact angle was determined according to the droplet profile method described in GB / T30447-2013 "Method for Measurement of Contact Angle of Nanofilms", with the following adaptation for particulate materials: Particles of the same size were fixed into a non-overlapping monolayer using a non-absorbent fluoropolymer adhesive. 3.0 μL of deionized water was added, and the contact angle was fitted from both sides of the droplet after 5 seconds. Ten random measurements were taken for each sample, and the average value was calculated. This result represents the apparent contact angle of the fixed monolayer sample and is not equivalent to the intrinsic contact angle of a smooth film.
[0068] Manganese and potassium content was determined using microwave digestion-ICP-OES. Approximately 0.1000 g of dry sample was accurately weighed, digested in a sealed container with nitric acid and a small amount of hydrofluoric acid, and boric acid was added to complex residual fluoride ions before volume adjustment. A calibration curve was established using standard substances, and Mn and K were determined separately. The dry-basis manganese loading was reported as the elemental manganese mass fraction, and the K / Mn ratio was reported as the molar atomic ratio. Blank, parallel, and spiked recovery samples were prepared for each batch, with spiked recoveries controlled between 90% and 110%.
[0069] MnO x Active domain scale, depth distribution and valence state The particle size of the active domain was determined according to GB / T45114-2024 "Nanotechnology - Measurement of Particle Size and Shape Distribution of Nanoparticles by Transmission Electron Microscopy". The particles were lightly ground, ultrasonically dispersed with ethanol, and then dropped onto an ultrathin carbon film copper grid. At least 10 random fields of view were collected; at least 300 MnO particles with identifiable boundaries were selected. x The active domain is converted to the equivalent circle diameter based on its projected area, and the number distributions D50 and D90 are calculated. Overlapping boundary regions are not artificially separated and are recorded separately to avoid selective statistics.
[0070] Manganese depth distribution was determined using cross-sectional SEM-EDS surface scanning. At least 10 intact particles were randomly selected, vacuum-embedded in low-viscosity epoxy resin, cut along the geometric center, and polished step by step. The full-section Mn-Kα surface distribution was acquired under the same accelerating voltage, working distance, beam current, and residence time. Equidistant lines of 50 μm were drawn inward from the particle contour. After subtracting the background of blank resin and unloaded carrier, the proportion of manganese signal inside the equidistant lines to the total manganese signal was calculated.
[0071] The valence state of Mn was analyzed using X-ray photoelectron spectroscopy. Data acquisition and peak fitting were performed in accordance with GB / T30704-2014 "Guideline for X-ray Photoelectron Spectroscopy in Surface Chemical Analysis" and GB / T36401-2018 "Description of Performance Parameters of X-ray Photoelectron Spectroscopy Instruments for Surface Chemical Analysis". The Mn2p and Mn3s regions were fitted using the C1s 284.8 eV or a calibrated internal standard-corrected binding energy under uniform background function, peak shape, and constraint conditions. The Mn2p peak area was then used to calculate the Mn2s valence state. 3+ / Mn 4+ In contrast, the sample transfer process should be kept as isolated from humid air as possible to minimize changes in surface valence state.
[0072] Formaldehyde removal and moisture retention rate The test chamber structure, airtightness, temperature and humidity uniformity, and background control conform to QB / T5364-2019 "Technical Requirements and Evaluation Methods for Test Chambers for Air Purifiers"; the pollutant generation, mixing, blank attenuation correction, and sampling methods conform to GB / T18801-2022 "Air Purifiers" and JG / T294-2010 "Determination of Pollutant Purification Performance of Air Purifiers". The above standards were originally applied to the entire machine or specified devices. This test changed the airflow path to in-chamber circulation, placed 2.0g of particles into a stainless steel mesh box with an opening ratio of 45%, and maintained a circulating airflow of 1.0±0.1m³ / h, which is a clear adaptation for material selection.
[0073] Samples from the same batch were subjected to high-humidity pretreatment and parallel reference pretreatment according to claim 10. For each test, formaldehyde was first introduced into a 1 m³ chamber and mixed to a concentration of 1.00 ± 0.05 mg / m³, at a temperature of 25 ± 2℃ and a relative humidity of 85% ± 3%; samples were taken at 0, 0.5, 1.0, and 2.0 h. Formaldehyde sampling and analysis were performed according to the applicable formaldehyde spectrophotometric method in GB / T18204.2-2025 "Hygienic Inspection Methods for Public Places Part 2: Chemical Indicators". A blank chamber without materials was also set up, and the natural decay was measured using the same procedure.
[0074] Linear regression of ln(C0 / Ct) versus time was performed on the concentration at each time point. The material-corrected apparent first-order removal rate constant k was calculated as the regression slope of the sample chamber minus the regression slope of the blank chamber, with a regression determination coefficient not less than 0.95. The 2-hour corrected removal rate was calculated as [1-exp(-2k)]×100%; the retention rate of the humidity resistance rate constant was calculated by dividing k of the high-humidity pretreatment group by k of the parallel reference group and then multiplying by 100%. At least three independent samples were used for each condition; the mean, standard deviation, and significance test results were reported.
[0075] Odor removal performance The same 1m³ chamber and 2.0g of material were used as for formaldehyde testing, but ammonia, trimethylamine, and hydrogen sulfide were tested separately and not mixed in the same chamber. The chamber temperature was 25±2℃, and the relative humidity was 85%±3%. The initial concentrations were ammonia 2.00±0.10mg / m³, trimethylamine 1.00±0.05mg / m³, and hydrogen sulfide 1.00±0.05mg / m³, respectively. The circulating air volume was 1.0±0.1m³ / h, and the contact time was 2h. Ammonia sampling and analysis were performed according to the applicable methods in GB / T18204.2-2025; trimethylamine was analyzed according to GB / T14676-1993 "Determination of Trimethylamine by Gas Chromatography in Air Quality"; and hydrogen sulfide was analyzed according to GB / T14678-1993 "Determination of Hydrogen Sulfide, Methanethiol, Dimethyl Sulfide and Dimethyl Disulfide by Gas Chromatography in Air Quality". For each pollutant, a blank space without materials was set, and the removal rate in the table uses the value after blank attenuation correction.
[0076] Increase in manganese-containing free fine powder Weigh 100.0 g of the dry basis sample before and after high humidity exposure, place it on a standard sieve with a 0.25 mm aperture, and mechanically vibrate it for 5 min with a fixed amplitude. Collect the sieve residue and weigh it. Determine the mass of manganese in the residue using the microwave digestion-ICP-OES method described above. Subtract the mass of manganese in the sieve residue before exposure from the mass of manganese in the sieve residue after exposure, and then divide by the dry basis mass of the material before exposure to obtain the increase in free manganese fine powder content; a negative difference is reported as zero. Each sample is measured in triplicate.
[0077] Table 1 shows the structure, distribution, and pore structure.
[0078] Table 2 shows the valence state, residual potassium, and fine powder.
[0079] Table 3 shows the formaldehyde removal kinetics and moisture retention rate.
[0080] Table 4 shows the deodorization performance under high humidity conditions.
[0081] As can be seen from the results in Tables 1 to 4, five examples, MnO x The active domain has a D50 of 0.8–2.5 nm and a D90 of 1.8–4.0 nm. The proportion of manganese signal in the region deeper than 50 μm from the outer surface of the particle is 80%–95%, and the BET specific surface area retention rate is 65%–79%. This indicates that the present invention can maintain the accessibility of the carrier pores while enabling the formation of MnO using potassium permanganate as the sole manganese source. x The active domains are dispersed deep within the hierarchical pore structure at an ultra-small scale.
[0082] By employing a combination of temporary polyethylene glycol (PEG) channel protection and alkyl silanization of the particle outer surface for differential wetting control, a spatial structure is formed on the carrier, characterized by a hydrophobic outer surface and hydrophilic internal channels. In Example 2, the dry-based manganese loading was 3.7%, the proportion of manganese signal at a depth of 50 μm or more from the outer surface was 91%, the formaldehyde removal rate constant remained at 88.4% after high humidity, and the increase in free manganese powder was only 0.18%. In Comparative Example 1, although the apparent contact angle of 126° was still maintained after removing the PEG channel protection, its dry-based manganese loading decreased to 1.6%, the proportion of deep manganese signal decreased to 60%, and the formaldehyde removal rate constant of the baseline group decreased from 0.86 h in Example 2. -1 Decreased to 0.33h -1 This indicates that simply making the particles hydrophobic without protecting the internal pores will allow silane to enter the pores and hinder the deep transport of potassium permanganate aqueous solution.
[0083] Without external surface silanization, the formaldehyde removal rate constant of the baseline group in Comparative Example 2 still reached 0.88 h. -1 However, after high humidity pretreatment, the temperature dropped to 0.42 h. -1 The rate constant retention rate was only 47.7%, and the increase in free manganese fine powder increased to 1.24%; in contrast, the rate constant of the high-humidity group in Example 2 was 0.76 h. -1 The retention rate was 88.4%, and the increase in free manganese fine powder was 0.18%. These results indicate that the hydrophilicity of the internal pores is beneficial for the loading of potassium permanganate and the enrichment reaction of pollutants, while the hydrophobic outer surface layer mainly serves to inhibit the formation of a continuous water film under high humidity conditions and improve the surface stability of the particles. Polyethylene glycol pore protection and outer surface silanization are not two isolated steps, but rather form a spatial division of labor and functional coordination in the deep transport of precursors and the mass transfer in the high-humidity gas phase.
[0084] By using pore volume-limited atomization, vacuum-pressurized permeation, and fractional addition of hydrogen peroxide, the in vitro migration of manganese precursors and MnO can be further inhibited. x Active domain aggregation. MnO in Example 2 x The active domain's D50 and D90 were 1.5 nm and 2.9 nm, respectively, with a BET specific surface area retention rate of 76% and a deep manganese signal ratio of 91%. After immersion in a large-volume continuous liquid phase with ten times the pore volume, the D50 and D90 of Comparative Example 3 increased to 6.4 nm and 11.8 nm, respectively, while the BET retention rate decreased to 53%, the deep manganese signal ratio decreased to 48%, and the formaldehyde removal rate constant of the high-humidity group decreased from 0.76 h⁻¹. -1 Decreased to 0.28h -1 This indicates that large-volume liquid phases easily cause permanganate ions to migrate to the outside of the particles during liquid flow and drying, thereby forming shell deposition, active domain aggregation, and pore blockage.
[0085] Under the same conditions of potassium permanganate feed rate and total molar amount of hydrogen peroxide, in Comparative Example 4, hydrogen peroxide was added all at once, and its MnO x The active domains D50 and D90 increased to 4.3 nm and 8.2 nm, respectively, while the BET retention rate decreased to 63%, and the formaldehyde removal rate constant in the high humidity group decreased to 0.39 h. -1 The rate constant retention rate decreased to 75.0%. In Example 2, by monitoring the oxygen release peak and adding hydrogen peroxide in portions, the local reduction reaction, exothermic process, and oxygen release were controlled. Combined with low-concentration nucleation cycles and incremental growth cycles, newly added manganese preferentially deposited on existing crystal nuclei, thereby obtaining MnO with smaller particle size, more uniform distribution, and lower pore blockage. x Active domain. The above results indicate that pore volume-limited permeation and fractional in-situ reduction work together to form a key process for inhibiting manganese migration and abnormal growth of active domains.
[0086] Ammonium acetate pore volume limit washing, low-concentration hydrogen activation, pure nitrogen replacement, and low-concentration oxygen passivation further improved the residual potassium content and MnO content. x Coordinated regulation of mixed valence states. Mn in Example 2 3+ / Mn 4+ With a peak area ratio of 0.36 and a K / Mn atomic ratio of 0.08, the formaldehyde removal rate constants of the baseline group and the high humidity group reached 0.86 h⁻¹. -1 and 0.76h -1 Comparative Example 5, which did not undergo hydrogen-containing activation and oxygen-containing passivation, has a lower Mn content. 3+ / Mn 4+ The peak area ratio decreased to 0.10, and the rate constants of the baseline and high humidity groups decreased to 0.54 h, respectively. -1 and 0.43h -1 This indicates that the activation-inert displacement-low-oxygen passivation process not only avoids direct switching between reducing and oxidizing atmospheres, but also enables the formation of suitable Mn. 3+ / Mn 4+ The ratio and surface activity defects are improved, thereby enhancing the formaldehyde oxidation performance at room temperature.
[0087] Under relative humidity of 85%±3%, the formaldehyde rate constant retention rate of Examples 1-5 was 81.0%-88.4%, the formaldehyde removal rate in the high humidity group after 2 hours was 60.9%-81.4%, and the increase in free manganese fine powder was 0.12%-0.46%, all meeting the humidity resistance screening index. Meanwhile, the 2-hour removal rates of ammonia, trimethylamine, and hydrogen sulfide in Examples 1-5 reached 65%-87%, 75%-92%, and 82%-96%, respectively, which were generally higher than those of the comparative examples. This indicates that the obtained material not only maintains its formaldehyde removal capacity under high humidity conditions but also exhibits good comprehensive purification performance for typical nitrogen- and sulfur-containing odor pollutants.
[0088] like Figure 1 As shown, water droplets on the monolayer of differentially wetting carrier particles prepared in Example 2 maintained a distinct convex spherical crown-like profile. Measurements taken at 10 random locations yielded an average apparent static water contact angle of 121°, indicating that after temporary protection of the polyethylene glycol channels and treatment with alkyltrialkoxysilane, a hydrophobic interface was formed on the outer surface of the carrier particles, which helps reduce the tendency for a continuous water film to form on the outer surface of the particles in high-humidity environments.
[0089] like Figure 2As shown, the MnKα signal of the composite material obtained in Example 2 is distributed in the internal region of the intact particle cross-section, without forming a distinct, continuous, high-strength annular manganese enrichment layer on the outer periphery of the particles. Using equidistant lines 50 μm inward from the outer contour of the particles as boundaries, the net MnKα count of at least 10 random intact particles was integrated and statistically analyzed. The proportion of manganese signal in the region deeper than 50 μm from the outer surface of the particles was 91%, indicating that pore volume-limited atomization, vacuum-pressurized infiltration, and removal of free liquid from the outer surface can allow manganese components derived from potassium permanganate to enter the internal region of the particles and reduce the concentrated deposition of manganese precursors on the outer surface of the particles.
[0090] like Figure 3 As shown, the manganese signal of the composite material obtained in Example 2 gradually accumulates from the outer surface of the particle to the interior. When the inward depth is 50 μm, the proportion of the accumulated MnKα signal from the outer surface of the particle to 50 μm is 9%, and the proportion of the manganese signal in the region deeper than 50 μm from the outer surface of the particle is calculated to be 91%. This result indicates that the manganese-containing component formed by potassium permanganate as the sole manganese source in Example 2 is mainly distributed in the interior region of the particle, and no predominantly manganese-rich deposition layer is formed on the outer layer of the particle.
[0091] In summary, this invention, through the combination of techniques such as differential wetting carrier construction, pore-volume limited vacuum-pressurized wetting, fractional in-situ reduction with hydrogen peroxide, nucleation-growth cycle, and mixed valence state activation passivation, transforms manganese in potassium permanganate into deeply confined, ultra-small-scale MnO with controllable valence state. x The active domains show improvements in terms of dispersion, internal loading ratio, pore structure retention, high-humidity formaldehyde removal performance, complex odor removal ability, and stability of manganese-containing fine powder. Each process step forms a continuous structure-performance interaction chain around "suppressing high-humidity water films, maintaining gas-phase mass transfer, and stably exposing ultra-small manganese active domains," rather than a simple parallel arrangement of known technologies.
[0092] The above are merely specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent substitutions, or modifications made based on the present invention to solve essentially the same technical problems and achieve essentially the same technical effects are all covered within the protection scope of the present invention.
Claims
1. A method for preparing a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material, characterized in that, Includes the following steps: S1. The internal channels of the graded high-silica β-molecular sieve particles are filled with a polyethylene glycol aqueous solution. After removing the continuous liquid film on the outer surface of the particles, the water is removed under 45–65°C and 8–25 kPa absolute pressure, leaving the polyethylene glycol in the internal channels. In a non-aqueous medium... Alkyltrialkoxysilane is used to silanize the outer surface of the particles, followed by extraction of polyethylene glycol, to obtain a differential wetting carrier with a hydrophobic outer surface and hydrophilic internal pores. S2. Place the differentially wetting carrier in a sealed rotating container and evacuate it. Add potassium permanganate aqueous solution by atomization at a liquid addition rate not exceeding its usable pore volume. After vacuum-pressurized permeation, remove the free liquid on the outer surface and remove moisture with nitrogen gas at 40-60°C, so that the permanganate ions remain in the internal pores. The usable pore volume is the water absorption volume per unit mass of carrier measured by the vacuum saturated water absorption method at 25°C. The potassium permanganate is the only manganese source in the preparation process. S3. At 5–25°C, add 4%–8% hydrogen peroxide aqueous solution by atomization at a ratio of 1.50–1.65 mol hydrogen peroxide per mole of permanganate. This allows the permanganate to be reduced and nucleated in situ in the internal pores under conditions where there is no continuous liquid phase outside the support. After the oxygen release rate drops to less than 5% of the peak value, dehydrate at 60–90°C. Steps S2 and S3 are repeated 4 to 8 times until the dry-basis manganese loading, calculated as elemental manganese, is 2.5% to 5.5%; S4, pore volume limiting washing is performed with ammonium acetate solution, followed by activation in nitrogen gas containing 0.2% to 1.0% hydrogen at 160 to 220°C, then replacement with pure nitrogen gas until the outlet hydrogen gas fraction is less than 0.05%, and then passivation in nitrogen gas containing 0.5% to 2.0% oxygen at the same temperature, to obtain MnO with an equivalent particle size D50 of 0.8 to 2.5 nm, confined and dispersed in the internal mesopores. x The active domain is cooled and granulated to obtain the material.
2. The preparation method of the moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: The high-silica β-zeolite particles in step S1 are obtained as follows: β-zeolite raw material with a SiO2 / Al2O3 molar ratio of 80–160 is added to a treatment solution containing 0.08–0.18 mol / L sodium hydroxide and 0.03–0.10 mol / L tetrapropylammonium hydroxide, treated at 55–75°C for 15–40 min, washed with water, and then treated with 0.10–0.40 mol / L citric acid solution at 60–80°C for 20–60 min, followed by ammonium chloride treatment. The process involves exchange, drying, and calcination at 450–550°C to obtain a hierarchical β-molecular sieve with an average mesopore diameter of 3–12 nm, a mesopore volume of 0.20–0.55 cm³ / g, and a micropore volume retention rate of not less than 70% of that before treatment. The hierarchical β-molecular sieve is then mixed with silica sol at 5%–12% of its mass (based on SiO₂) to form granules. After drying at 100–130°C and calcination at 450–550°C, high-silica β-molecular sieve particles with a particle size of 0.5–3.0 mm are obtained.
3. The preparation method of the moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: The polyethylene glycol aqueous solution has a mass fraction of 15%–30%, the number average molecular weight of the polyethylene glycol is 400–1000, and the amount of polyethylene glycol aqueous solution used is 85%–105% of the usable pore volume of the high-silica β-molecular sieve particles; The alkyltrialkoxysilane is at least one of n-octyltriethoxysilane and dodecyltrimethoxysilane, with a mass fraction of 0.5% to 3.0% in a non-aqueous medium. The reaction temperature is 65 to 90°C and the reaction time is 1 to 4 hours. After the reaction, polyethylene glycol is extracted sequentially with ethanol and water at 50 to 70°C until the total organic carbon in the final water extract is not higher than 50 mg / L, so that the apparent static water contact angle of the differential wetting carrier on the particle monolayer fixed sample is 105° to 135°.
4. The preparation method of the moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: In step S2, the sealed rotating container is first evacuated to a gauge pressure of -0.060 to -0.095 MPa and maintained for 5 to 20 minutes. Then, potassium permanganate aqueous solution is added as droplets with an average droplet diameter of 20 to 80 μm while the carrier is agitated. After the addition is completed, nitrogen gas is introduced to a gauge pressure of 0.15 to 0.35 MPa and maintained for 2 to 10 minutes. Then, the container is centrifuged at 300 to 900 × g for 1 to 4 minutes to remove the free liquid on the outer surface.
5. The preparation method of a moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: In step S3, the hydrogen peroxide aqueous solution is divided into 3 to 8 equimolar portions and added sequentially via atomization. The carrier is continuously agitated between adjacent portions, and the next portion is added only after the oxygen volume fraction at the container outlet drops below 20% of the previous peak value. The carrier temperature is maintained at 8 to 20°C by a jacket. The volume of any portion of the hydrogen peroxide aqueous solution does not exceed 20% of the available pore volume of the carrier before the current reaction, and the total volume of the hydrogen peroxide aqueous solution does not exceed 50% of the available pore volume.
6. The preparation method of a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: The cycles in steps S2 and S3 consist of 2 to 3 nucleation cycles and 2 to 5 growth cycles. The concentration of potassium permanganate aqueous solution used in the nucleation cycle is 0.05 to 0.10 mol / L, and the concentration of potassium permanganate aqueous solution used in the growth cycle increases by 1.2 to 1.8 times the concentration of the previous cycle, reaching 0.30 mol / L and then maintaining it at 0.30 mol / L. After each cycle, the water content of the carrier is reduced to below 3% by nitrogen gas at 60 to 90℃ before entering the next cycle.
7. The preparation method of the moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: In step S4, a 0.01–0.08 mol / L ammonium acetate solution is used for two atomized washes. Each addition is 35%–50% of the usable pore volume of the carrier after circulation. After each addition, the carrier is agitated for 5–15 minutes and centrifuged at 300–900 × g. The temperature is then increased to 160–220°C at a rate of 0.5–2°C / min. The mixture is first kept in the hydrogen-containing nitrogen atmosphere for 20–60 minutes, then purged with pure nitrogen for 10–30 minutes until the outlet hydrogen fraction is confirmed to be below 0.05%. Finally, the mixture is switched to the oxygen-containing nitrogen atmosphere and kept for 30–90 minutes to allow the MnO₂ to form a precipitate. x Mn in the active domain as measured by X-ray photoelectron spectroscopy 3+ With Mn 4+ The peak area ratio is 0.20–0.55, and the K / Mn atomic ratio is 0.03–0.
15.
8. The preparation method of a moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: By controlling the number of cycles of steps S2 and S3 and the amount of potassium permanganate added at a time, MnO x The active domain has an equivalent particle size D90 of no more than 4.0 nm in number; the equivalent particle size is determined by transmission electron microscopy, and no less than 80% of the manganese signal is located in the hierarchical pore region to a depth of 50 μm from the outer surface of the particle by scanning electron microscope-energy dispersive X-ray spectroscopy area scanning of the particle cross section; the BET specific surface area retention rate of the material after activation is no less than 65% of the differential wetting carrier.
9. The preparation method of a moisture-resistant composite ultra-nano manganese activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: Cooling is carried out in nitrogen gas with a dew point not higher than -20°C. After cooling to below 50°C, free fine powder is removed by sieving through a sieve with a pore size of 0.25–0.45 mm. The material is then equilibrated in air at 25–35°C and a relative humidity of 45%–60% for 4–12 hours to achieve a moisture content of 2%–6%, thereby hydrating MnO without forming an external continuous water film. x The active domain is used to obtain the material to be tested.
10. The preparation method of a moisture-resistant composite ultra-nano manganese-activated deodorizing and formaldehyde-removing material according to claim 1, characterized in that: Moisture resistance screening was performed on the materials to be tested: The same batch of materials was divided into a high-humidity group and a parallel reference group. 2.0g of the high-humidity group was exposed to air at 25±2℃ and 85%±3% relative humidity for 72h, while 2.0g of the parallel reference group was placed in air at 25±2℃ and 50%±3% relative humidity for 72h. The two groups of materials were placed in a 1m³ sealed chamber and tested for 2h under the conditions of 25±2℃, 85%±3% relative humidity, initial formaldehyde concentration of 1.00±0.05mg / m³, and chamber air circulation of 1.0±0.1m³ / h. Based on the apparent first-order removal rate constant of formaldehyde in the parallel reference group, the materials with a rate constant retention rate of not less than 80% in the high-humidity group were screened. Before and after high-humidity exposure, the materials were sieved with a 0.25mm sieve and the manganese mass in the fine powder under the sieve was measured. The materials with an increase in free manganese fine powder not exceeding 0.5% of the dry basis mass of the material were screened as finished products and sealed and packaged.
Citation Information
Patent Citations
An air purification material for removing formaldehyde in the air, its preparation method and use method
CN104084034B
A method of loading manganese on a hydrophilic carrier material
CN117772184B
Vapor phase reduction supported manganese oxide catalyst as well as preparation method, device and application thereof
CN118594402A