A method for preparing a thulium atom-dispersed Co3O4-based catalyst and its application in the catalytic decomposition of N2O in flue gas.

By atomically dispersing thulium on the surface of Co3O4, a Tm-O-Co interface structure was formed, which solved the problem of decreased activity and stability of Co3O4-based catalysts in real flue gas, and achieved efficient low-temperature decomposition of N2O and resistance to water vapor poisoning.

CN123102331APending Publication Date: 2026-11-17SOUTHEAST UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611450946.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing Co3O4-based catalysts are susceptible to competitive adsorption by water vapor, NO, SO2, etc. in real flue gas, resulting in decreased activity and stability, making it difficult to achieve low-temperature activation and efficient decomposition of N2O.

Method used

A method involving 2-methylimidazole-assisted coprecipitation and heat treatment under a protective atmosphere was adopted to achieve atomic-level dispersion and stable anchoring of thulium atoms on the Co3O4 surface, forming a Tm-O-Co interface structure, thereby improving the low-temperature reducibility and oxygen mobility of surface Co-O species.

Benefits of technology

The catalyst exhibits significantly improved low-temperature activity and resistance to water vapor poisoning. The N2O conversion rate of the catalyst in real coal-fired flue gas can reach 90%, and it maintains long-term stability in complex flue gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102331A_ABST
    Figure CN123102331A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing a thulium atomically dispersed Co3O4-based catalyst and its application in the catalytic decomposition of N2O in flue gas. The preparation method includes: dissolving cobalt salt and thulium salt in a solvent in a specific ratio, mixing with a 2-methylimidazole solution, and then co-precipitating, drying, and heat-treating under an inert atmosphere to obtain the target catalyst. The catalyst comprises spinel-type Co3O4 and atomically dispersed Tm species, with the Tm species anchored at or near-surface defect sites on the Co3O4 surface and forming a Tm-O-Co interface with adjacent Co-O units. This catalyst is used for the direct catalytic decomposition of N2O in coal-fired flue gas, achieving an N2O conversion rate of approximately 90% at 340 °C, and maintaining almost no change in catalytic efficiency in the presence of 5 vol.% water vapor. After continuous operation for 20 hours in real coal-fired flue gas, the N2O conversion rate remains above 90%, exhibiting excellent low-temperature activity, resistance to water vapor poisoning, and long-term operational stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of atmospheric pollutant treatment and heterogeneous catalysis technology, specifically relating to an atomically dispersed thulium-modified spinel-type Co3O4 catalyst and its preparation method, and also relating to the application of this catalyst in the direct catalytic decomposition of N2O in complex flue gas containing multiple pollutants in coal-fired flue gas. Background Technology

[0002] Nitrogen gas (N2O) is a long-lived greenhouse gas with a significant ozone-depleting effect. Its emissions come from sources including nitric acid and adipic acid production, fossil fuel combustion, and vehicle exhaust. Among various treatment methods, direct catalytic decomposition of N2O does not require external reducing agents and theoretically only produces N2 and O2, thus offering advantages such as simple process and minimal secondary pollution.

[0003] While existing noble metal catalysts can achieve high low-temperature activity, they suffer from high cost and limitations in thermal stability and resistance to oxidation / water. Co3O4, on the other hand, offers advantages such as low cost, structural stability, and the presence of Co... 2+ / Co 3+ It exhibits reversible redox properties, but in real flue gas, it is easily affected by competitive adsorption of water vapor, NO, SO2, etc., hydroxyl group coverage, and hindered surface oxygen migration, leading to a decrease in activity and stability.

[0004] To improve the performance of Co3O4-based catalysts, the invention patent with publication number CN117282434A attempts to adjust their electronic structure and surface properties through doping with rare earth elements (such as thulium). However, such methods typically introduce rare earth ions into the Co3O4 lattice, forming a conventional solid solution or mixed oxide structure. This lattice doping strategy makes it difficult to precisely control the dispersion state of rare earth elements on the catalyst surface, resulting in active sites being easily covered or poisoned under real-world conditions (especially in the presence of water vapor). Therefore, the low-temperature activity and long-term stability of the catalyst still need further improvement.

[0005] Therefore, there is an urgent need to provide a non-precious metal catalyst that can simultaneously achieve low-temperature N2O activation, rapid removal of reaction-derived oxygen, and water vapor tolerance. In particular, through atomic-scale structural design, rare earth elements can be highly dispersed and stably anchored on the Co3O4 surface to solve the aforementioned problems in the existing technology. Summary of the Invention

[0006] One of the objectives of this invention is to provide a method for preparing a thulium atom-dispersed Co3O4-based catalyst. By using 2-methylimidazole-assisted co-precipitation and heat treatment under a protective atmosphere, atomic-level dispersion and stable anchoring of Tm on the Co3O4 surface are achieved, overcoming the shortcomings of existing lattice doping strategies that make it difficult to accurately control the surface distribution of rare earth elements.

[0007] The second objective of this invention is to provide a thulium atom-dispersed Co3O4-based catalyst prepared by the above method, which has spinel-type Co3O4 and atomically dispersed Tm species anchored to surface defect sites, forming a Tm-O-Co interface structure, which can take into account both N2O low-temperature activation and water vapor tolerance.

[0008] The third objective of this invention is to provide an application of the catalyst in the catalytic decomposition of N2O in flue gas, particularly for the treatment of coal-fired flue gas containing water vapor, to achieve efficient and stable decomposition of N2O and solve the problem that existing catalysts are easily poisoned and deactivated by water vapor and acidic gases in real flue gas.

[0009] One of the technical solutions adopted by this invention to achieve its objective is to provide a method for preparing a thulium atom-dispersed Co3O4-based catalyst, comprising the following steps: S1. Dissolve cobalt salt and thulium salt in a solvent at a molar ratio of 1:0.01-0.1 to obtain a metal precursor solution; dissolve 2-methylimidazole in a solvent to obtain a 2-methylimidazole solution. S2. Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued to carry out the aging reaction so that the metal ions are fully precipitated. S3. Solid-liquid separation: the solid product is washed and dried to obtain a dried precursor. S4. The dried precursor is subjected to high-temperature treatment under a protective atmosphere to obtain a thulium atom-dispersed Co3O4-based catalyst.

[0010] The overall concept and inventive principle of this invention are as follows: This invention introduces an appropriate amount of Tm precursor into Co3O4 and employs an organic coprecipitation-thermal treatment route to stabilize Tm in an atomically dispersed state at or near-surface defect sites on the Co3O4 surface. The atomically dispersed Tm forms approximately six-coordinate Tm-O6 local units, which then connect with neighboring Co-O units via oxygen bridges to construct Tm-O-Co interfaces. These interfaces generate local charge rearrangement and Co-O orbital hybridization regulation, increasing oxygen vacancy-related defects, enhancing the low-temperature reducibility of surface Co-O species and surface oxygen mobility, while simultaneously retaining some deeper lattice / interface oxygen reservoirs, thus achieving a balance between activity and structural stability.

[0011] Specifically, this invention selects thulium (Tm) as the atomically dispersed species. Tm exists as isolated atoms on the Co3O4 surface, forming a stable Tm-O6 local coordination structure with surrounding oxygen atoms, rather than forming metallic Tm, Tm2O3 clusters or independent oxide phases. This Tm-O-Co interface can change the hybridization state of adjacent Co 3d and O 2p orbitals, promoting charge redistribution between Tm and Co3O4, and increasing the surface Co content. 2+The proportion of Tm is adjusted to create an electronic structure more conducive to N2O activation. Simultaneously, the introduction of Tm promotes the formation of oxygen vacancies and coordinated unsaturated Co-O sites, which is beneficial for N2O adsorption, NO bond breaking, reactive oxygen species migration, and active site regeneration. Regarding oxygen species behavior, Tm facilitates the migration and removal of weakly bound surface oxygen while stably retaining some deep lattice oxygen or interfacial oxygen, forming a balance between easy surface oxygen migration and relatively stable deep oxygen reservoirs, thus balancing catalytic activity and structural stability. Furthermore, under the same rare earth loading conditions, the catalyst provided by this invention exhibits significantly higher catalytic activity than catalysts doped with other rare earth elements such as Lu, Ho, and Er, indicating that the effectiveness of this invention is related to the elemental specificity of Tm and its unique regulation of the Co-O electronic structure and oxygen species behavior. DFT calculations further confirmed that the activation energy for NO bond breaking at the Tm-O-Co site decreased from 1.45 eV for Co3O4 to 0.21 eV, the OO coupling barrier decreased from 1.22 eV to 0.99 eV, and the O2 desorption free energy decreased from 0.40 eV to 0.34 eV. This theoretically supports the promoting effect of Tm on low-temperature activation of N2O, NO bond breaking, surface oxygen migration, and regeneration of active sites.

[0012] Meanwhile, this application employs an organic coprecipitation precursor preparation route containing a 2-methylimidazolium ligand, which can form an organic coordination / coprecipitation precursor with metal ions, promoting uniform dispersion of Co and Tm and facilitating the formation of a porous precursor. The introduction of an appropriate amount of Tm can inhibit particle agglomeration, increase the specific surface area and pore volume of the catalyst, form more accessible micropores, which is beneficial for increasing the contact between N2O and active sites and improving mass transfer capacity in the presence of water vapor and impurities in the flue gas. The heat treatment stage provides a high temperature for the 2-methylimidazolium ligand to fully decompose and form a stable Co3O4 framework. Simultaneously, the protective atmosphere prevents the rapid migration of Tm species under strong oxidizing conditions, inhibits the formation of large Tm2O3 particles, promotes the pyrolysis and defect formation of organic ligands, maintains the strong interaction between Tm and adjacent Co-O units, and forms a surface with more oxygen vacancies and coordination unsaturated sites. Existing technologies employ a sol-gel method combined with air calcination, a calcination process more closely resembling traditional oxidative calcination. This primarily facilitates the oxidative removal of organic matter from the gel, but it struggles to achieve the same atomically dispersed Tm-O6 structure. The catalyst in this application maintains a Co3O4 spinel framework, with Tm atomically dispersed on or near the surface, and no Tm2O3 crystalline phase appears. The surface Co... 2+ With the increase in proportion, the oxygen vacancy concentration increases, and the low-temperature reducibility and surface oxygen mobility are enhanced. Compared with pure Co3O4, the catalyst prepared by this invention requires a significantly lower temperature to achieve 50% and 90% N2O conversion rates, significantly improves low-temperature activity, weakens water vapor poisoning, accelerates surface oxygen circulation and active site regeneration, and exhibits better long-term stability in complex flue gas.

[0013] Furthermore, the molar ratio of cobalt to thulium is 1:0.02-0.08. Studies have found that when the Tm loading is too high, Tm2O3 phase separation, pore blockage, and active site coverage may occur, leading to a decrease in performance. Preferably, the molar ratio of cobalt to thulium is 1:0.04-0.06, more preferably 1:0.06.

[0014] Further, in step S1, the cobalt salt includes one or more of cobalt nitrate hexahydrate, cobalt acetate, and cobalt chloride; the thulium salt includes one or more of thulium nitrate hexahydrate, thulium chloride, and thulium acetate.

[0015] Preferably, the cobalt salt is cobalt nitrate hexahydrate, which is readily soluble in methanol and can provide uniform Co. 2+ The precursor, and the nitrate ions are easily decomposed during heat treatment, without introducing difficult-to-remove impurity elements. Preferably, the thulium salt is thulium nitrate hexahydrate, which is easily soluble and has a Tm... 3+ Its stable composition is beneficial for controlling the Tm / Co ratio.

[0016] Further, in step S1, the molar ratio of 2-methylimidazole to cobalt salt is 0.5:1-4:1. Studies have found that when the molar ratio of 2-methylimidazole to cobalt salt is below 0.5:1, coordination and precipitation are insufficient, leading to a decrease in precursor yield and uneven Tm distribution; while when the ratio is above 4:1, excessive organic ligands may result in increased precursor residue, unstable pore structure, and increased burden on subsequent heat treatment. Preferably, the molar ratio of 2-methylimidazole to cobalt salt is 0.8:1-2:1; more preferably, it is 1:1.

[0017] Further, the solvent is selected from methanol, ethanol, and a methanol-ethanol mixture. Preferably, the solvent is methanol, which can simultaneously dissolve cobalt nitrate, thulium nitrate, and 2-methylimidazole, and has moderate volatility, which is beneficial for organic co-precipitation. The volume ratio of the metal precursor solution to the 2-methylimidazole solution is determined based on the target molar ratio and concentration conversion. For example, when the concentration of the metal precursor solution is 0.1 mol / L and the concentration of the 2-methylimidazole solution is 0.1 mol / L, the volume ratio is approximately 1:1.

[0018] Further, the total metal concentration of the metal precursor solution is 0.01-0.50 mol / L, and the concentration of the 2-methylimidazole solution is 0.02-1.00 mol / L. Preferably, the total metal concentration of the metal precursor solution is 0.03-0.20 mol / L, and the concentration of the 2-methylimidazole solution is 0.05-0.50 mol / L. The amount of methanol used is determined to ensure complete dissolution of the metal salt and 2-methylimidazole, and to prevent localized gelation or instantaneous aggregation during the dropwise addition.

[0019] Further, in step S2, the stirring speed is 300-1000 rpm; the dropping time is 10-120 min; the stirring speed continues at 200-800 rpm; the aging time is 2-24 h; and the temperature is 20-60 ℃. Preferably, the stirring speed is 500-800 rpm; the dropping time is 30-60 min; the stirring speed continues at 300-600 rpm; the aging time is 6-16 h; and the temperature is 40 ℃.

[0020] Further, in step S3, the drying temperature is 40-100 °C, and the time is 6-24 h. When the drying temperature is below 40 °C, the solvent and moisture removal is insufficient, and residual methanol in the precursor may cause local reduction or abnormal carbon deposition in subsequent heat treatment; if the drying temperature is too high, such as exceeding 100 °C, it may cause partial collapse of the precursor skeleton or ligand desorption, affecting the formation of the atomically dispersed structure in subsequent heat treatment. Preferably, the drying temperature is 50-80 °C, more preferably 60 °C; and the drying time is 8-16 h.

[0021] Further, in step S4, the high-temperature treatment temperature is 550-700 °C, the heating rate is 1-10 °C / min, and the treatment time is 1-4 h. Studies have found that treatment temperatures below 550 °C may lead to incomplete precursor decomposition and insufficient Co3O4 crystallization; while temperatures above 700 °C may cause grain growth, Tm migration, and agglomeration. Excessive heating may cause rapid decomposition of the organic precursor, localized exothermic reactions, and Tm migration; excessively slow heating increases the process time, and the prolonged residence time of the precursor in the high-temperature zone may increase the risk of Tm migration and agglomeration. Regarding the heat treatment time, too short a time will result in insufficient decomposition and structure formation, while too long a time may cause grain growth and a decrease in specific surface area. Preferably, the high-temperature treatment temperature is 600-680 °C, the heating rate is 2-8 °C / min, and the treatment time is 1.5-3 h. More preferably, the high-temperature treatment temperature is 650 °C, the heating rate is 5 °C / min, and the treatment time is 2 h.

[0022] Furthermore, the protective atmosphere includes nitrogen or argon, preferably nitrogen. Nitrogen can prevent excessive oxidation and migration of Tm during heat treatment, while promoting the decomposition of organic precursors, defect formation, and Tm-O-Co interface stability.

[0023] The second objective of this invention is to provide a thulium atom-dispersed Co3O4-based catalyst prepared by the preparation method described in the first objective of this invention, comprising: spinel-type Co3O4 and atom-dispersed Tm species, wherein the Tm species are anchored in the form of isolated atoms to defect-related sites on or near the surface of Co3O4, forming a local coordination structure dominated by Tm-O6 with surrounding oxygen atoms, and forming Tm-O-Co interface sites with adjacent Co-O units through oxygen bridges.

[0024] Furthermore, X-ray diffraction (XRD) analysis showed that the catalyst of the present invention did not exhibit the characteristic diffraction peaks of the Tm2O3 crystalline phase, indicating that Tm exists in an atomically dispersed form on the surface of Co3O4, rather than in an independent oxide crystalline phase.

[0025] The third objective of this invention is to provide an application of the thulium atom-dispersed Co3O4-based catalyst described in the second objective of this invention in the catalytic decomposition of N2O in flue gas.

[0026] Furthermore, the flue gas contains 5 vol.% or more of water vapor. Testing showed that the catalyst prepared according to this invention maintained a high N2O conversion rate even in a reaction atmosphere containing 5 vol.% water vapor, demonstrating excellent resistance to water vapor poisoning.

[0027] Furthermore, the flue gas is coal-fired flue gas, containing N2O and at least one of H2O, O2, CO2, CO, NO, SO2, and HCl. Testing showed that in real coal-fired flue gas (containing 6.2 vol.% water vapor), the catalyst operated continuously at 400 °C for 20 hours, maintaining an N2O conversion rate of approximately 90%, with no significant activity degradation observed.

[0028] Furthermore, the catalytic decomposition temperature is 200-500℃. Tests showed that the catalyst achieved an N2O conversion rate of approximately 50% at 260℃ and approximately 90% at 340℃ (compared to only about 48% conversion of pure Co3O4 at 350℃), exhibiting excellent low-temperature catalytic activity. Preferably, the catalytic decomposition temperature is 340-400℃. When the catalytic decomposition temperature is below 340℃, intermediate conversion and surface oxygen removal may still be kinetically limited; when the catalytic decomposition temperature is above 400℃, although a high conversion rate may be maintained, energy consumption increases, and particle sintering or migration of active components may occur.

[0029] Furthermore, the catalyst prepared by this invention exhibits excellent stability in the catalytic decomposition of N2O in flue gas. The catalyst Tm prepared under preferred conditions... 0.06Co maintained a conversion rate of approximately 90% for 20 consecutive hours in real coal-fired flue gas at 400 °C. In a simulated atmosphere test at 400 °C, the conversion rate remained above 95% for 26 hours with CO or H2O present. After the introduction of NO or SO2, the conversion rate decreased to approximately 84% and 88%, respectively, and could be restored to nearly 100% after removing impurities. This indicates that the inhibition was mainly due to reversible adsorption rather than irreversible deactivation.

[0030] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The present invention provides a method for preparing a thulium-atom-dispersed Co3O4-based catalyst. A MOF precursor is constructed through the coordination of 2-methylimidazole with metal ions, achieving uniform mixing and spatial confinement of Co and Tm at the molecular scale. After pyrolysis under an inert atmosphere, Tm is anchored to defect sites on the Co3O4 surface, achieving atomic-level dispersion. Single-atom dispersion is maintained even at a Tm / Co molar ratio of 0.06, with the Tm2O3 crystalline phase appearing only at a ratio of 0.10, significantly expanding the non-agglomeration dispersion window. Compared to lattice-doped products obtained by the traditional sol-gel method, the method of the present invention can precisely control the dispersion state of Tm on the catalyst surface, is simple to operate, and is suitable for industrial production.

[0031] (2) The thulium atom-dispersed Co3O4-based catalyst prepared in this invention is applied to the catalytic decomposition of N2O in flue gas. The atom-dispersed structure avoids the agglomeration of large-size Tm oxides, while achieving synergistic regulation of adjacent Co sites, oxygen vacancies, and surface oxygen migration, forming a balance of "easy surface oxygen migration and relatively stable deep oxygen reservoir," thus taking into account both catalytic activity and structural stability. Furthermore, the irreversible hydroxylation caused by water vapor is suppressed through the Tm-O6 structure and the Tm-O-Co interface. In a simulated atmosphere, the catalyst achieves an N2O conversion rate of approximately 50% at 260 °C and approximately 90% at 340 °C, which is significantly better than the conversion rate of unmodified Co3O4 (only about 48% at 350 °C). In the presence of 5 vol.% water vapor, the N2O conversion rate of the catalyst is almost unaffected. In a 10 kW circulating fluidized bed coal combustion unit, real coal combustion flue gas was introduced into the catalyst bed and operated continuously for 20 hours at 400 °C and a flue gas flow rate of 1 L / min. The N2O conversion rate remained at approximately 90%, and no significant deactivation was observed. This indicates that the catalyst of this invention possesses excellent low-temperature activity, resistance to water vapor poisoning, and long-term operational stability. These effects stem from the synergistic effect of 2-methylimidazole-assisted co-precipitation, controlled nitrogen heat treatment, and the Tm loading window. Attached Figure Description

[0032] Figure 1 Tm obtained in Example 4 0.06 AC-HAADF-STEM image of Co catalyst; Figure 2 Tm obtained in Example 4 0.06 EDS-Mapping diagram of Co catalyst; Figure 3 Tm obtained in Example 4 0.06 Co's Tm L3 edge EXAFS fitting results; Figure 4 Tm obtained in Example 4 0.06 Co and Tm prepared in Example 6 0.1 XRD pattern of Co; Figure 5 The N2O catalytic efficiency of catalysts with different Tm / Co molar ratios prepared in various embodiments and comparative examples of the present invention is shown in the graph at 350 °C. Figure 6 The graph shows the N2O catalytic efficiency of catalysts with different Tm / Co molar ratios prepared in various embodiments and comparative examples of the present invention at different temperatures. Figure 7 Tm obtained in Example 4 of this invention 0.06 Comparison of N2O catalytic efficiency of Co catalyst under anhydrous and water vapor conditions; Figure 8 Tm obtained in Example 4 of this invention 0.06 The catalytic efficiency of Co catalyst for N2O in a 10 kW circulating fluidized bed coal-fired flue gas is shown in the figure. Detailed Implementation

[0033] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] This invention provides a method for preparing a thulium atom-dispersed Co3O4-based catalyst, comprising the following steps: Step 1: Dissolve cobalt nitrate hexahydrate and thulium nitrate hexahydrate in methanol according to a cobalt to thulium molar ratio of 1:0.01-0.1 to obtain a metal precursor solution with a total metal concentration of 0.03-0.20 mol / L.

[0035] Step 2: Dissolve 2-methylimidazole in methanol to obtain a 2-methylimidazole solution; the molar ratio of 2-methylimidazole to cobalt nitrate hexahydrate is 0.8:1-2:1; the concentration of the 2-methylimidazole solution is 0.05-0.50 mol / L.

[0036] Step 3: Under stirring conditions of 500-800 rpm, add the metal precursor solution dropwise to the 2-methylimidazole solution, controlling the addition time at 30-60 min. Continue stirring at 300-600 rpm to carry out the aging reaction for 6-16 h at a temperature of 30-50℃, so that the metal ions can be fully precipitated.

[0037] Step 4: Solid-liquid separation, the solid product is washed and dried to obtain the dried precursor; the drying temperature is 50-80 ℃ and the time is 8-16 h.

[0038] Step 5: The dried precursor is subjected to high-temperature treatment under a nitrogen atmosphere at a temperature of 600-680℃, a heating rate of 2-8℃ / min, and a treatment time of 1.5-3 h, finally obtaining a thulium atom-dispersed Co3O4-based catalyst.

[0039] The present invention will be further described below with reference to specific embodiments, but these are not intended to limit the scope of the invention.

[0040] Example 1 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.001 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.1 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued and the mixture is aged to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and dried overnight at 60 °C; (5) The dried precursor was heated to 650 °C at a rate of 5 °C / min under a nitrogen atmosphere and held for 2 hours to obtain Tm. 0.01 Co catalyst.

[0041] Example 2 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.002 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.1 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued and the mixture is aged to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and dried overnight at 60 °C; (5) The dried precursor was heated to 650 °C at a rate of 5 °C / min under a nitrogen atmosphere and held for 2 hours to obtain Tm. 0.02Co catalyst.

[0042] Example 3 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.004 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.1 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued and the mixture is aged to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and dried overnight at 60 °C; (5) The dried precursor was heated to 650 °C at a rate of 5 °C / min under a nitrogen atmosphere and held for 2 hours to obtain Tm. 0.04 Co catalyst.

[0043] Example 4 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.006 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.1 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued and the mixture is aged to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and dried overnight at 60 °C; (5) The dried precursor was heated to 650 °C at a rate of 5 °C / min under a nitrogen atmosphere and held for 2 hours to obtain Tm. 0.06 Co catalyst.

[0044] Example 5 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.008 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.1 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued and the mixture is aged to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and dried overnight at 60 °C; (5) The dried precursor was heated to 650 °C at a rate of 5 °C / min under a nitrogen atmosphere and held for 2 hours to obtain Tm. 0.08 Co catalyst.

[0045] Example 6 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.01 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.1 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued and the mixture is aged to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and dried overnight at 60 °C; (5) The dried precursor was heated to 650 °C at a rate of 5 °C / min under a nitrogen atmosphere and held for 2 hours to obtain Tm. 0.1 Co catalyst.

[0046] Example 7 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.006 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.08 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring and aging are continued to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and then dried at 50 °C for 16 h. (5) The dried precursor was heated to 600 °C at a rate of 2 °C / min under a nitrogen atmosphere and held at that temperature for 1.5 h to obtain Tm. 0.06 Co catalyst.

[0047] Example 8 (1) Dissolve 0.1 mol cobalt nitrate hexahydrate and 0.006 mol thulium nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.2 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring and aging are continued to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and then dried at 80 °C for 8 h. (5) The dried precursor was heated to 680 °C at a rate of 8 °C / min under a nitrogen atmosphere and held for 3 h to obtain Tm. 0.06 Co catalyst.

[0048] Comparative Example (1) Dissolve 0.1 mol of cobalt nitrate hexahydrate in methanol and stir to obtain a homogeneous metal precursor solution; (2) Dissolve 0.1 mol of 2-methylimidazole in methanol and stir; (3) Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued and the mixture is aged to allow the metal ions to precipitate fully; (4) The obtained solid was centrifuged, washed repeatedly with ethanol, and dried overnight at 60 °C; (5) The dry precursor was heated to 650 °C at 5 °C / min under a nitrogen atmosphere and kept at the temperature for 2 hours to obtain the Co3O4 catalyst.

[0049] Structural characterization and analysis To further verify the dispersion state and local coordination structure of Tm in Co3O4, the Tm prepared in Example 4 was subjected to further analysis. 0.06 The Co catalyst was characterized by AC-HAADF-STEM, EDS-Mapping, EXAFS, and XRD.

[0050] like Figure 1 As shown in the AC-HAADF-STEM image, isolated bright spots dispersed in the background of the Co3O4 lattice can be observed. No continuous bright bands or granular bright spots were observed, indicating that Tm exists in an atomically dispersed form.

[0051] like Figure 2 As shown in the EDS-Mapping diagram, Tm can be observed to be uniformly dispersed in the Co3O4 lattice, further confirming the atomic-level dispersion state of Tm.

[0052] like Figure 3 As shown, the EXAFS fitting results of the Tm L3 edge show that the Tm-O coordination number is 6.5±0.5 and the bond length is 2.23±0.02 Å. No Tm-Tm scattering path was detected above 3 Å, indicating that Tm mainly forms isolated Tm-O6 local coordination structures, and does not form Tm metal or Tm2O3 clusters.

[0053] like Figure 4 As shown in the XRD pattern, Tm 0.06 Co only shows spinel Co3O4 diffraction peaks, without the characteristic diffraction peaks of Tm2O3; while Tm 0.1 The presence of Tm2O3 diffraction peaks in Co indicates that an appropriate amount of Tm (Tm / Co molar ratio of 0.01-0.08) can better achieve atomic-level dispersion, while excess Tm will result in phase separation.

[0054] The above characterization results collectively confirm that in the catalyst of the present invention, Tm is anchored in the form of isolated atoms at defect-related sites on or near the surface of Co3O4, forming a local coordination structure dominated by Tm-O6 with the surrounding oxygen atoms, and forming Tm-O-Co interface sites with adjacent Co-O units through oxygen bridges.

[0055] Application Example 1 The catalytic N2O decomposition capabilities of the thulium atomically dispersed cobalt oxide catalysts prepared in Examples 1-6 and the comparative examples were verified on a fixed-bed catalytic test bench. The test conditions were as follows: inlet N2O concentration of 2000 ppm, inner diameter of quartz tube reactor of 10 mm, catalyst dosage of 200 mg, catalytic temperature of 200 °C to 500 °C, and total gas flow rate of 1 L / min.

[0056] The N2O conversion rates of the catalysts in each embodiment and comparative example at 350 °C are shown in the attached figures. Figure 5 As shown. From the appendix Figure 5 It can be seen that the N2O conversion rate first increases and then decreases with the increase of the Tm / Co molar ratio. A Tm / Co molar ratio in the range of 0.02-0.08 significantly improves the catalytic activity (conversion rate of approximately 80%-94%), with 0.06 being the optimal value. When the Tm / Co molar ratio exceeds 0.08, the activity begins to decrease, indicating that excess Tm leads to phase separation and reduces catalytic performance. Specifically, the Tm prepared in Example 4... 0.06 The Co catalyst exhibited the best activity, with the highest N2O conversion rate at 350 °C.

[0057] The N2O conversion rates of the catalysts in each embodiment and comparative example at different temperatures are shown in the attached figures. Figure 6 As shown. From the appendix Figure 6 It can be seen that the Tm prepared in Example 4 0.06 The Co catalyst exhibited optimal activity across the entire test temperature range, with an N2O conversion rate of approximately 50% at 260 °C and approximately 90% at 340 °C, significantly outperforming the comparative example and other embodiments.

[0058] Application Example 2 The N2O catalytic decomposition performance of the catalyst prepared in Example 4 under water vapor conditions was verified on a fixed-bed catalytic test bench. The test conditions were as follows: inlet N2O concentration of 2000 ppm, water vapor content of 5 vol.%, inner diameter of quartz tube reactor of 10 mm, catalyst dosage of 200 mg, catalytic temperature of 200 °C to 500 °C, and total gas flow rate of 1 L / min.

[0059] Tm prepared in Example 4 0.06 Comparison of N2O conversion rates of Co catalysts under anhydrous and steam-containing conditions is shown in the attached figure. Figure 7 As shown. From the appendix Figure 7 It can be seen that the catalytic efficiency of the catalyst for N2O remains almost unchanged in the presence of 5 vol.% water vapor, indicating that the catalyst of the present invention has excellent resistance to water vapor poisoning.

[0060] Application Example 3 On a 10 kW circulating fluidized bed coal-fired experimental device, the Tm prepared in Example 4 was tested. 0.06 The N2O catalytic decomposition performance and long-term stability of the Co catalyst under real coal-fired flue gas conditions were verified.

[0061] After the coal-fired experimental apparatus reached a stable operating state, 1 L / min of flue gas was drawn from the furnace outlet and fed into the Tm prepared in Example 4. 0.06 A fixed-bed reactor with Co catalyst was used, and the reactor temperature was maintained at 400 °C. The actual flue gas composition was: 95 ppm N2O, 6.2% water vapor, 8.5% O2, 10.2% CO2, 850 ppm CO, 75 ppm NO, 300 ppm SO2, and 18 ppm HCl.

[0062] Tm prepared in Example 4 0.06 The N2O conversion rate of the Co catalyst after 20 hours of continuous operation under real coal-fired flue gas conditions is shown in the attached figure. Figure 8 As shown. From the appendix Figure 8 It can be seen that the N2O conversion rate remained at approximately 90% during 20 hours of continuous operation, and no significant activity decay was observed, indicating that the catalyst of this invention still maintains excellent long-term operational stability under complex real flue gas conditions.

[0063] In summary, this invention provides a thulium atom-dispersed Co3O4-based catalyst, its preparation method, and its applications. This catalyst, through an organic co-precipitation-thermal treatment route, anchors thulium (Tm) in an atomically dispersed form at defect sites on the Co3O4 surface, forming a Tm-O-Co interface structure, exhibiting both excellent low-temperature activity and resistance to water vapor poisoning. Compared with existing technologies, the catalyst of this invention achieves an N2O conversion rate of over 90% in coal-fired flue gas containing more than 5 vol.% water vapor within a temperature range of 340-400 °C, and shows no significant deactivation after 20 hours of continuous operation, demonstrating promising prospects for industrial application.

[0064] The above are merely preferred embodiments of the present invention and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should recognize that any equivalent substitutions and obvious changes made based on the content of this specification should be included within the protection scope of the present invention.

Claims

1. A method for preparing a thulium atom-dispersed Co3O4-based catalyst, characterized in that, Includes the following steps: S1. Dissolve cobalt salt and thulium salt in a solvent according to a molar ratio of cobalt to thulium of 1:0.01-0.1 to obtain a metal precursor solution; 2-Methylimidazole was dissolved in a solvent to obtain a 2-methylimidazole solution; S2. Under stirring conditions, the metal precursor solution is added dropwise to the 2-methylimidazole solution, and stirring is continued to carry out the aging reaction so that the metal ions are fully precipitated. S3. Solid-liquid separation: the solid product is washed and dried to obtain a dried precursor. S4. The dried precursor is subjected to high-temperature treatment under a protective atmosphere to obtain a thulium atom-dispersed Co3O4-based catalyst.

2. The preparation method according to claim 1, characterized in that, In step S1, the cobalt salt includes one or more of cobalt nitrate hexahydrate, cobalt acetate, and cobalt chloride; the thulium salt includes one or more of thulium nitrate hexahydrate, thulium chloride, and thulium acetate.

3. The preparation method according to claim 1, characterized in that, In step S1, the molar ratio of 2-methylimidazole to cobalt salt is 0.5:1-4:1; the solvent is selected from methanol, ethanol, and methanol-ethanol mixed solvent.

4. The preparation method according to claim 1, characterized in that, In step S2, the stirring speed is 300-1000 rpm; the dropping time is 10-120 min; the stirring speed is 200-800 rpm; the aging time is 2-24 h; and the temperature is 20-60 ℃.

5. The preparation method according to claim 1, characterized in that, In step S3, the drying temperature is 40-100℃ and the time is 6-24 h.

6. The preparation method according to claim 1, characterized in that, In step S4, the protective atmosphere is nitrogen or argon; the high-temperature treatment temperature is 550-700 ℃, the heating rate is 1-10 ℃ / min, and the treatment time is 1-4 h.

7. A thulium atom-dispersed Co3O4-based catalyst prepared by the method according to any one of claims 1-6, characterized in that, include: Spinel-type Co3O4 and atomically dispersed Tm species, wherein the Tm species are anchored in the form of isolated atoms at defect-related sites on or near the surface of Co3O4, forming a local coordination structure dominated by Tm-O6 with surrounding oxygen atoms, and forming Tm-O-Co interface sites with adjacent Co-O units through oxygen bridges.

8. The application of a thulium atom-dispersed Co3O4-based catalyst according to claim 7 in the catalytic decomposition of N2O in flue gas.

9. The application according to claim 8, characterized in that, The flue gas contains 5 vol.% or more of water vapor.

10. The application according to claim 8, characterized in that, The flue gas is coal-fired flue gas, containing N2O and at least one of H2O, O2, CO2, CO, NO, SO2 and HCl.

Citation Information

Patent Citations

  • Rare earth doped cobalt-based catalyst for catalytic decomposition of N2O and preparation method and application thereof

    CN117282434A