A catalyst for the hydrolysis of carbonyl sulfur in blast furnace gas, its preparation method and application
By adopting a core-shell structure in the blast furnace gas carbonyl sulfur hydrolysis catalyst, with the core being a potassium-based active component supported by γ-Al2O3 and the outer shell being a chlorine-resistant coating, the problem of damage to the active component of the catalyst by chlorine-containing components is solved, achieving a synergistic effect of efficient dechlorination and carbonyl sulfur hydrolysis, extending the catalyst life and simplifying the process.
Patent Information
- Application Number
- CN202611364637.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
Abstract
Description
Technical Field
[0001] This invention relates to the field of blast furnace gas purification and sulfur pollutant treatment technology, and in particular to a blast furnace gas carbonyl sulfur hydrolysis catalyst, its preparation method and application. Background Technology
[0002] Blast furnace gas is a byproduct of blast furnace ironmaking, containing components such as carbon monoxide, carbon dioxide, nitrogen, hydrogen, hydrogen chloride, and carbonyl sulfide. Carbonyl sulfide readily enters subsequent gas utilization systems with the blast furnace gas, adversely affecting gas pipelines, combustion equipment, and downstream production units. Currently, carbonyl sulfide removal typically employs a combination of hydrolysis and subsequent desulfurization. This involves reacting carbonyl sulfide with water vapor under the action of a catalyst to generate hydrogen sulfide, which is then removed by subsequent desulfurization processes. However, blast furnace gas contains a small amount of hydrogen chloride, which, upon entering the catalyst channels, readily reacts with potassium-based active components, causing loss or deactivation of these components. This leads to a decrease in the catalyst's carbonyl sulfide hydrolysis activity and a shortened lifespan. Existing technologies often involve a separate dechlorination unit upstream of the catalyst, which suffers from high equipment investment, complex processes, and unstable dechlorination effects. Therefore, developing a blast furnace gas carbonyl sulfide hydrolysis catalyst that balances carbonyl sulfide hydrolysis activity and chloride resistance is crucial for improving blast furnace gas purification efficiency and extending catalyst lifespan.
[0003] Patent CN101811051B discloses a method for preparing a carbonyl sulfur hydrolysis catalyst using Co-Ni-Al type hydrotalcite as a precursor. It mainly improves the low-temperature carbonyl sulfur hydrolysis performance and hydrogen sulfide removal performance of the catalyst by controlling the metal element composition and composite oxide structure, but does not address the influence of chlorine-containing components in blast furnace gas on potassium-based active components. Patent CN113289602A discloses a catalyst for carbonyl sulfur hydrolysis in blast furnace gas, its preparation method, and its application. It uses modified alumina as a support and loads alkali metal oxides and alkaline earth metal oxides. It mainly focuses on carbonyl sulfur hydrolysis activity, gas flow efficiency, and bed pressure drop, but struggles to address the problem of chlorine-containing components preferentially entering the catalyst interior and causing deactivation of potassium-based active components. Summary of the Invention
[0004] Based on the above, this invention provides a blast furnace gas carbonyl sulfur hydrolysis catalyst, its preparation method, and its application. This invention combines a catalyst core loaded with a carbonyl sulfur hydrolysis active component (potassium-based active component) with a chlorine-resistant coating that has dechlorination properties, forming a core-shell structure. The chlorine-resistant coating pre-removes chlorine-containing components from the blast furnace gas, reducing the impact of chlorine-containing components on the potassium-based active component in the catalyst core. This maintains the carbonyl sulfur hydrolysis activity while improving the catalyst's chlorine resistance and service life.
[0005] To achieve the above objectives, the present invention provides the following solution: One of the technical solutions of the present invention is a blast furnace gas carbonyl sulfur hydrolysis catalyst, which has a core-shell structure, including a catalyst core and a shell; The catalyst core consists of a support and a potassium-based active component supported on the support; The outer shell is a chlorine-resistant coating applied to the surface of the catalyst core; the chlorine-resistant coating is made of a sacrificial agent, a binder, and a pore-forming agent.
[0006] The second technical solution of the present invention is a method for preparing the above-mentioned blast furnace gas carbonyl sulfur hydrolysis catalyst, comprising the following steps: The sacrificial agent, binder and pore-forming agent are mixed to obtain the chlorine-resistant coating raw material; The catalyst core is preheated at 100-110 °C for 20-60 min and then placed in a roller coating equipment. The roller speed is controlled at 10-30 r / min. First, 5%-15% of the total mass of the anti-chlorine coating material is added. Then, the remaining anti-chlorine coating material is added in 5-10 batches. During each batch addition, deionized water is atomized and sprayed. The total amount of deionized water added is 5%-20% of the total mass of the anti-chlorine coating material. At the same time, hot air at 60-90 °C is introduced for drying. After there is no visible free water on the surface of the catalyst core, the next batch of anti-chlorine coating material is added. After coating, the catalyst core is dried and calcined to obtain the blast furnace gas carbonyl sulfur hydrolysis catalyst.
[0007] The third technical solution of this invention is the application of the above-mentioned blast furnace gas carbonyl sulfur hydrolysis catalyst in the blast furnace gas carbonyl sulfur hydrolysis conversion.
[0008] Compared with the prior art, the present invention has the following beneficial effects: Using the carbonyl sulfide hydrolysis catalyst for blast furnace gas of the present invention, HCl in blast furnace gas is preferentially removed by the chlorine-resistant coating. The dechlorinated gas then enters the core for carbonyl sulfide hydrolysis, thereby achieving synergistic purification of blast furnace gas dechlorination and carbonyl sulfide hydrolysis. It has the advantages of high dechlorination efficiency, stable carbonyl sulfide hydrolysis activity, and simple preparation process.
[0009] This invention provides an anti-chlorine coating on the surface of the catalyst core (γ-Al2O3 loaded with potassium-based active components), and separates the carbonyl sulfur hydrolysis function and the chlorine-containing component removal function. This helps to reduce the direct contact between the chlorine-containing components and the potassium-based active components, slow down the deactivation of the potassium-based active components, and extend the service life of the catalyst. Detailed Implementation
[0010] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0011] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0012] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0013] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0014] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0015] This invention uses γ-Al2O3 loaded with potassium-based active components as the core of a carbonyl sulfur hydrolysis catalyst. A chlorine-resistant coating composed of a calcium-based sacrificial agent, a binder, and a pore-forming agent is coated on the surface of the catalyst core to form a core-shell structure. The chlorine-resistant coating preferentially removes chlorine-containing components from the blast furnace gas, reducing the impact of chlorine-containing components on the potassium-based active components in the core. At the same time, by controlling the composition, thickness, and pore structure of the chlorine-resistant coating, the catalyst possesses both carbonyl sulfur hydrolysis performance and chlorine resistance.
[0016] The first aspect of the present invention provides a blast furnace gas carbonyl sulfur hydrolysis catalyst, which has a core-shell structure, including a catalyst core and a shell; The catalyst core consists of a support and a potassium-based active component supported on the support; The outer shell is a chlorine-resistant coating applied to the surface of the catalyst core; the chlorine-resistant coating is made of a sacrificial agent, a binder, and a pore-forming agent.
[0017] In a preferred embodiment of the present invention, the support is γ-Al2O3; the potassium-based active component is at least one of KOH, K2CO3, KHCO3 and KNO3; and the loading of the potassium-based active component is 2% to 15% of the catalyst core mass based on K2O.
[0018] In a preferred embodiment of the present invention, the method for preparing the catalyst core includes the following steps: The potassium-based active component is dissolved in a solvent to obtain an impregnation solution; the support is impregnated in the impregnation solution, and then allowed to stand and dry to obtain the catalyst core.
[0019] In a preferred embodiment of the present invention, the solvent is deionized water; the potassium content in the impregnation solution is 2wt.% to 10wt.% (K2O); the impregnation is carried out using an equal-volume impregnation method, the volume of the impregnation solution is 0.8 to 1.2 times the saturated water absorption volume of the γ-Al2O3 carrier, and the impregnation is carried out at 20 to 30 °C, and the mixture is stirred for 30 to 60 min after the impregnation solution is added; the standing is specifically 8 to 16 h at 20 to 30 °C; the drying is specifically 3 to 6 h at 100 to 110 °C.
[0020] In a preferred embodiment of the present invention, the sacrificial agent is Ca(OH)2, wherein the particle size of the Ca(OH)2 is not greater than 0.15 mm, and the Ca(OH)2 with a particle size less than 0.074 mm accounts for 80% to 95% of the total mass of the Ca(OH)2; The binder is at least one of boehmite, bentonite, carboxymethyl cellulose, and polyvinyl alcohol; The pore-forming agent is at least one of starch, cellulose, ammonium bicarbonate, and polyethylene glycol.
[0021] In a preferred embodiment of the present invention, the mass ratio of the sacrificial agent, the binder and the pore-forming agent is (85-95):(2-8):(1-7).
[0022] In a preferred embodiment of the present invention, the catalyst core content in the blast furnace gas carbonyl sulfur hydrolysis catalyst is 75% to 85% by mass, with the remainder being the outer shell.
[0023] A second aspect of the present invention provides a method for preparing the above-mentioned blast furnace gas carbonyl sulfur hydrolysis catalyst, comprising the following steps: The sacrificial agent, binder and pore-forming agent are mixed to obtain the chlorine-resistant coating raw material; The catalyst core is preheated at 100–110 °C for 20–60 min and then placed in a roller coating equipment. The roller speed is controlled at 10–30 r / min. First, 5%–15% of the total mass of the anti-chlorine coating material is added. Then, the remaining anti-chlorine coating material is added in 5–10 batches. During each batch addition, deionized water is atomized and sprayed. The total amount of deionized water added is 5%–20% of the total mass of the anti-chlorine coating material. At the same time, hot air at 60–90 °C is introduced for drying. After there is no visible free water on the surface of the catalyst core, the next batch of anti-chlorine coating material is added. After coating, the catalyst core is dried and calcined to obtain the blast furnace gas carbonyl sulfur hydrolysis catalyst.
[0024] After coating, the particle size of the resulting core-shell structure catalyst is 3.4–7.0 mm, and the thickness of the chlorine-resistant coating in the catalyst is 0.2–1.0 mm.
[0025] By controlling the coating batch, the amount of water sprayed, the hot air temperature, and the coating thickness, the chlorine-resistant coating is evenly applied to the surface of the catalyst core, reducing coating cracking and peeling.
[0026] In a preferred embodiment of the present invention, the drying conditions after coating are set as follows: drying at 100-120 ℃ for 3-4 hours; the calcination conditions are set as follows: calcination at 500-550 ℃ for 4-6 hours.
[0027] The third aspect of the present invention provides the application of the above-mentioned blast furnace gas carbonyl sulfur hydrolysis catalyst in the blast furnace gas carbonyl sulfur hydrolysis conversion.
[0028] The catalyst of this invention has a core-shell structure of "core hydrolysis + outer shell chlorine resistance", which has the following advantages: (1) The contact sequence is perfectly matched with the functional positioning. The outer chlorine-resistant layer first comes into contact with HCl-containing coal gas, and utilizes the alkalinity of CaO to preferentially fix HCl, thus changing the preferential entry path through a physical barrier; The catalyst core is only exposed to low / zero HCl gas after the shell has been pretreated, thus protecting the potassium-based active components from chlorine poisoning.
[0029] (2) The outer shell (chlorine-resistant coating) and the catalyst core have a clear division of labor. The outer shell acts as a sacrificial / consumption layer: CaO is consumed by the reaction with HCl, but this does not affect the activity of the core. The core acts as a persistent active layer: the potassium-based components continue to perform COS hydrolysis under a protected environment.
[0030] This invention fundamentally solves the technical contradiction of "chlorine-containing components preferentially causing the deactivation of potassium-based active components" by placing the anti-chlorination function externally and the hydrolysis function internally in a spatial layout. This is consistent with the logic of "setting a separate dechlorination device at the front end of the catalyst" in industry. However, this invention integrates the two into a single catalyst particle, avoiding the problems of "large equipment investment and complex process flow".
[0031] This invention enables the chlorine-resistant coating to have good dechlorination ability by controlling the particle size and addition ratio of Ca(OH)2; by adding an appropriate proportion of binder and pore-forming agent, the adhesion strength and porosity of the chlorine-resistant coating are improved, which is conducive to the entry of blast furnace gas into the chlorine-resistant coating and its full contact with the sacrificial agent.
[0032] Unless otherwise specified, the technical solutions described in this invention are all conventional solutions in the field, and the reagents or raw materials used are all purchased from commercial channels or are publicly available unless otherwise specified.
[0033] The γ-Al₂O₃ used in this embodiment of the invention was purchased from Pingxiang Huanqiu New Material Technology Co., Ltd. It is a KA405-1 activated alumina catalyst support, spherical in shape with a particle size of 3–5 mm, an Al₂O₃ content of not less than 94%, and a specific surface area of not less than 170 m². 2 / g, pore volume not less than 0.40 mL / g, single particle compressive strength not less than 110 N, Na2O content not more than 0.20%, and the saturated water absorption of the γ-Al2O3 carrier was measured to be 0.50 mL / g; the cellulose used was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., model C434461, in powder form, with a nominal particle size of about 20 μm.
[0034] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0035] In all embodiments of the present invention, γ-Al2O3 is used as the catalyst support, the catalyst core is prepared using potassium-based active components, and an anti-chlorine coating (shell) is formed on the surface of the catalyst core by roller coating.
[0036] In this embodiment of the invention, simulated blast furnace gas is used as the reactant gas. The simulated blast furnace gas, by volume fraction, comprises: N2 54.96%, CO 24%, CO2 20%, H2O 1%, HCl 0.02%, COS 0.015%, and H2S 0.005%. The temperature of the simulated blast furnace gas entering the fixed-bed reactor is 130 °C, and the gas hourly space velocity (HSV) within the fixed-bed reactor is 5000 h⁻¹. -1 .
[0037] Example 1 The catalyst core uses γ-Al₂O₃ as a support and K₂CO₃ as the potassium-based active component, with the loading of the potassium-based active component (calculated as K₂O) controlled at 8% of the catalyst core mass. 13.30 g of anhydrous K₂CO₃ was weighed and dissolved in deionized water, then diluted to 50 mL to obtain a K₂CO₃ impregnation solution with a mass concentration of 0.266 g / mL. 50 mL of the impregnation solution was added evenly to 100 g of γ-Al₂O₃ support in equal-volume batches, with a solid-liquid ratio of 100 g:50 mL. The addition of the impregnation solution was completed at 25 °C, followed by stirring and mixing for 30 min. The impregnated γ-Al₂O₃ was then sealed and allowed to stand at 25 °C for 12 h, followed by drying at 105 °C for 4 h to obtain the K / γ-Al₂O₃ catalyst core. Based on the total catalyst mass, the catalyst core accounts for 85%, and the chlorine-resistant coating accounts for 15%. The chlorine-resistant coating is composed of Ca(OH)₂, bentonite, and cellulose. Ca(OH)₂ accounts for 85% of the total mass of the chlorine-resistant coating raw material, bentonite 8%, and cellulose 7%. The Ca(OH)₂ particle size is no greater than 0.15 mm, with 80 wt.% of the particle size smaller than 0.074 mm. The bentonite particle size is no greater than 0.074 mm. The median particle size (D50) of the cellulose is 20 μm. Ca(OH)₂, bentonite, and cellulose are mixed according to the above mass percentages to obtain the chlorine-resistant coating raw material. The catalyst core is preheated at 100 °C for 40 min and then placed in a roller coating equipment, with the roller speed controlled at 10 r / min. First, 15% of the total mass of the chlorine-resistant coating raw material is added. Then, the remaining chlorine-resistant coating raw material is added in 5 batches, with deionized water atomized and sprayed during each batch addition. The total amount of deionized water added is 5% of the total mass of the chlorine-resistant coating raw material. Simultaneously, hot air at 60 °C is introduced for drying. The obtained chlorine-resistant coating had an average thickness of 0.2 mm and an average catalyst particle size of 4 mm. After coating, the obtained catalyst was dried at 100 °C for 3.5 h and calcined at 525 °C for 5 h to obtain a core-shell structured blast furnace gas carbonyl sulfur hydrolysis catalyst.
[0038] The carbonyl sulfur hydrolysis catalyst for blast furnace gas prepared in this embodiment, when applied to a fixed bed, still showed a carbonyl sulfur hydrolysis conversion rate of more than 95% after 50 hours of continuous reaction.
[0039] Example 2 The catalyst core was prepared in the same manner as in Example 1. By total catalyst mass, the catalyst core accounted for 80%, and the anti-chlorine coating accounted for 20%. The anti-chlorine coating consisted of Ca(OH)₂, bentonite, and cellulose, with Ca(OH)₂ accounting for 90% of the total mass of the anti-chlorine coating raw materials, bentonite accounting for 5%, and cellulose accounting for 5%. The Ca(OH)₂ particle size was no greater than 0.15 mm, with the portion smaller than 0.074 mm accounting for 80 wt.%. The bentonite particle size was no greater than 0.074 mm; the median particle size (D50) of the cellulose used was 20 μm. Ca(OH)₂, bentonite, and cellulose were mixed according to the above mass percentages to obtain the anti-chlorine coating raw material. The catalyst core was preheated at 105°C for 40 min and then placed in a roller coating equipment, with the roller speed controlled at 20 r / min. First, 10% of the total mass of the chlorine-resistant coating raw material was added. Then, the remaining chlorine-resistant coating raw material was added in seven batches, with deionized water atomized and sprayed during each batch addition. The total amount of deionized water added was 12% of the total mass of the chlorine-resistant coating raw material. Simultaneously, hot air at 75 °C was introduced for drying. The resulting chlorine-resistant coating had an average thickness of 0.6 mm, and the catalyst had an average particle size of 7 mm. After coating, the resulting catalyst was dried at 105 °C for 3.5 h and calcined at 525 °C for 5 h to obtain a core-shell structured blast furnace gas carbonyl sulfur hydrolysis catalyst.
[0040] The carbonyl sulfur hydrolysis catalyst for blast furnace gas prepared in this embodiment, when applied to a fixed bed, still showed a carbonyl sulfur hydrolysis conversion rate of more than 95% after 72 hours of continuous reaction.
[0041] Example 3 The catalyst core was prepared in the same manner as in Example 1. By total catalyst mass, the catalyst core accounted for 75%, and the anti-chlorine coating accounted for 25%. The anti-chlorine coating consisted of Ca(OH)₂, bentonite, and cellulose, with Ca(OH)₂ accounting for 95% of the total mass of the anti-chlorine coating raw materials, bentonite accounting for 3%, and cellulose accounting for 2%. The Ca(OH)₂ particle size was no greater than 0.15 mm, with the portion smaller than 0.074 mm accounting for 80 wt.%. The bentonite used had a particle size no greater than 0.074 mm; the median particle size D50 of the cellulose used was 20 μm. Ca(OH)₂, bentonite, and cellulose were mixed according to the above mass percentages to obtain the anti-chlorine coating raw material. The catalyst core was preheated at 110°C for 40 min and then placed in a roller coating equipment, with the roller speed controlled at 30 r / min. First, 5% of the total mass of the anti-chlorine coating raw material was added. Then, the remaining anti-chlorine coating raw material was added in 10 batches, with deionized water atomized and sprayed during each batch addition. The total amount of deionized water added was 20% of the total mass of the anti-chlorine coating raw material. Simultaneously, hot air at 75 °C was introduced for drying. The resulting anti-chlorine coating had an average thickness of 1.0 mm, and the catalyst had an average particle size of 8 mm. After coating, the resulting catalyst was dried at 105 °C for 3.5 h and calcined at 525 °C for 5 h to obtain a core-shell structured blast furnace gas carbonyl sulfur hydrolysis catalyst.
[0042] The carbonyl sulfur hydrolysis catalyst for blast furnace gas prepared in this embodiment, when applied to a fixed bed, still showed a carbonyl sulfur hydrolysis conversion rate of more than 95% after 130 hours of continuous reaction.
[0043] Comparative Example 1 The only difference from Example 1 is that the catalyst core was not coated with an antichlorine layer; instead, the catalyst core was treated according to the drum rotation, drying, and calcination process of Example 1. When the obtained carbonyl sulfur hydrolysis catalyst was applied to a fixed bed, the carbonyl sulfur hydrolysis conversion rate was 90% after 50 hours of continuous reaction.
[0044] Comparative Example 2 The only difference from Example 1 is that no bentonite binder was added to the chlorine-resistant coating raw material. Specifically, the chlorine-resistant coating raw material consisted of Ca(OH)₂ and cellulose, with a Ca(OH)₂ to cellulose mass ratio of 93:7. The proportion of the chlorine-resistant coating to the total catalyst mass, as well as the particle size of Ca(OH)₂ and cellulose, roller coating, spraying with deionized water, hot air drying, and subsequent heat treatment conditions were all the same as in Example 1. During the preparation process, it was observed that without the addition of bentonite binder, the bonding strength between the chlorine-resistant coating and the catalyst core was significantly reduced, resulting in a relatively loose coating on the catalyst surface. During continuous aeration in the fixed bed, the chlorine-resistant coating exhibited significant pulverization and localized detachment, and fine powder entrainment was observed at the reactor outlet.
[0045] Comparative Example 3 The only difference from Example 1 is that no cellulose pore-forming agent is added to the chlorine-resistant coating raw material. An equal mass of Ca(OH)₂ replaces the cellulose in Example 1, meaning the chlorine-resistant coating raw material consists of Ca(OH)₂ and bentonite, with Ca(OH)₂ accounting for 92% of the total mass and bentonite accounting for 8%. The proportion of the chlorine-resistant coating to the total catalyst mass, as well as the particle size of Ca(OH)₂ and bentonite, the roller coating, the spraying of deionized water, the hot air drying, and the subsequent heat treatment conditions are all the same as in Example 1. After the obtained carbonyl sulfur hydrolysis catalyst was applied to a fixed bed, the carbonyl sulfur hydrolysis conversion rate was 92% after 50 hours of continuous reaction.
[0046] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A catalyst for the hydrolysis of carbonyl sulfur in blast furnace gas, characterized in that, It has a core-shell structure, including a catalyst core and an outer shell; The catalyst core consists of a support and a potassium-based active component supported on the support; The outer shell is a chlorine-resistant coating applied to the surface of the catalyst core; the chlorine-resistant coating is made of a sacrificial agent, a binder, and a pore-forming agent.
2. The blast furnace gas carbonyl sulfur hydrolysis catalyst according to claim 1, characterized in that, The support is γ-Al2O3; the potassium-based active component is at least one of KOH, K2CO3, KHCO3 and KNO3; the loading of the potassium-based active component is 2% to 15% of the catalyst core mass based on K2O.
3. The blast furnace gas carbonyl sulfur hydrolysis catalyst according to claim 1, characterized in that, The method for preparing the catalyst core includes the following steps: The potassium-based active component is dissolved in a solvent to obtain an impregnation solution; the support is impregnated in the impregnation solution, and then allowed to stand and dry to obtain the catalyst core.
4. The blast furnace gas carbonyl sulfur hydrolysis catalyst according to claim 3, characterized in that, The solvent is deionized water; the potassium content in the impregnation solution is 2wt.% to 10wt.% (K2O); the impregnation is carried out using an equal-volume impregnation method, with the volume of the impregnation solution being 0.8 to 1.2 times the saturated water absorption volume of the carrier, and the impregnation is carried out at 20 to 30 °C, with mixing for 30 to 60 min after the impregnation solution is added; the standing is specifically for 8 to 16 h at 20 to 30 °C; the drying is specifically for 3 to 6 h at 100 to 110 °C.
5. The blast furnace gas carbonyl sulfur hydrolysis catalyst according to claim 1, characterized in that, The sacrificial agent is Ca(OH)2, and the particle size of the Ca(OH)2 is no greater than 0.15 mm, wherein Ca(OH)2 with a particle size less than 0.074 mm accounts for 80% to 95% of the total mass of the Ca(OH)2; The binder is at least one of boehmite, bentonite, carboxymethyl cellulose, and polyvinyl alcohol; The pore-forming agent is at least one of starch, cellulose, ammonium bicarbonate, and polyethylene glycol.
6. The blast furnace gas carbonyl sulfur hydrolysis catalyst according to claim 1, characterized in that, The mass ratio of the sacrificial agent, binder and pore-forming agent is (85-95):(2-8):(1-7).
7. The blast furnace gas carbonyl sulfur hydrolysis catalyst according to claim 1, characterized in that, The catalyst core content in the blast furnace gas carbonyl sulfur hydrolysis catalyst is 75% to 85% by mass, with the remainder being the outer shell.
8. A method for preparing a blast furnace gas carbonyl sulfur hydrolysis catalyst according to any one of claims 1 to 7, characterized in that, Includes the following steps: The sacrificial agent, binder and pore-forming agent are mixed to obtain the chlorine-resistant coating raw material; The catalyst core is preheated at 100-110 °C for 20-60 min and then placed in a roller coating equipment. The roller speed is controlled at 10-30 r / min. First, 5%-15% of the total mass of the anti-chlorine coating material is added. Then, the remaining anti-chlorine coating material is added in 5-10 batches. During each batch addition, deionized water is atomized and sprayed. The total amount of deionized water added is 5%-20% of the total mass of the anti-chlorine coating material. At the same time, hot air at 60-90 °C is introduced for drying. After there is no visible free water on the surface of the catalyst core, the next batch of anti-chlorine coating material is added. After coating, the catalyst core is dried and calcined to obtain the blast furnace gas carbonyl sulfur hydrolysis catalyst.
9. The preparation method according to claim 8, characterized in that, The drying conditions after coating are set as follows: drying at 100-120 ℃ for 3-4 hours; the calcination conditions are set as follows: calcination at 500-550 ℃ for 4-6 hours.
10. The application of the blast furnace gas carbonyl sulfur hydrolysis catalyst as described in any one of claims 1 to 7 in the carbonyl sulfur hydrolysis conversion of blast furnace gas.
Citation Information
Patent Citations
Carbonyl sulfide hydrolysis catalyst prepared by using cobalt(Co)-nickel(Ni)-aluminum(Al) hydrotalcites as precursor and preparation method thereof
CN101811051B
Catalyst for hydrolysis of carbonyl sulfide in blast furnace gas as well as preparation method and application of catalyst
CN113289602A