An In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol
By pretreating the gasification slag support and constructing the In-O-Zr coordination structure, the problems of agglomeration and insufficient H2 dissociation capacity of In2O3-based catalysts were solved, achieving efficient CO2 conversion and methanol generation, and improving catalytic performance.
Patent Information
- Application Number
- CN202611377317.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing In2O3-based catalysts suffer from problems such as easy aggregation of In species, limited H2 dissociation ability, and the inability of co-precipitation to form a directionally coordinated In-O-Zr interface structure, resulting in unsatisfactory CO2 conversion and insufficient stability. Furthermore, the gasification residue is not effectively utilized as a support, thus affecting catalytic performance.
Using gasification slag as a carrier, a highly dispersed In2O3 nanoarray was constructed by gravity water separation and steam activation pretreatment, combined with chemical deposition. Zr4+ was introduced by ion exchange to form an In-O-Zr coordination structure, thus preparing an In-Zr/gasification slag dual-active-site catalyst.
It significantly improved the accessibility of active sites and mass transfer efficiency of the catalyst, achieving a CO2 conversion rate of 8.82%, a methanol selectivity of 70.25%, and a methanol space-time yield of 6.20 g/(gcat·h), which is superior to other schemes.
Smart Images

Figure CN123102334A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of CO2 hydrogenation to methanol technology, specifically an In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol. Background Technology
[0002] CO2 hydrogenation to methanol is one of the key technologies of "CO2 capture, storage and utilization" (CCUS), which aims to convert industrial CO2 emissions into methanol through hydrogenation, thereby achieving carbon resource recycling. Methanol, as a basic chemical raw material, can be further converted into high-value-added products such as olefins and aromatics. This technology is of great significance for achieving the "dual carbon" goal.
[0003] The C=O bond energy of the CO2 molecule is as high as 468 kJ / mol, and its activation requires a catalyst under high temperature and high pressure conditions. Methanol synthesis and the reverse water-gas shift reaction are competing pathways; both consume CO2, but the former is exothermic while the latter is endothermic. While high temperatures are beneficial for increasing CO2 conversion, they inhibit methanol formation and promote CO byproducts. Therefore, the catalyst must possess both CO2 activation capability and selectivity in suppressing side reactions.
[0004] In recent years, In₂O₃-based catalysts have attracted much attention due to their excellent selectivity for methanol. The oxygen vacancies on their surface serve as the main activation sites for CO₂ molecules, effectively promoting CO₂ adsorption and activation. However, the single In₂O₃ system suffers from drawbacks such as low specific surface area, insufficient active site density, and easy aggregation of In species under reaction conditions, leading to limited H₂ dissociation and unsatisfactory CO₂ conversion. Furthermore, the stability of this system under industrial feed gas conditions has not been fully verified. To overcome these shortcomings, researchers have attempted to construct bimetallic catalysts. Introducing Zr components into In₂O₃ has been shown to improve the dispersion state of In₂O₃, forming an In-O-Zr coordination structure to increase oxygen vacancy concentration and optimize electronic structure. However, existing In-Zr bimetallic catalysts are mostly prepared using co-precipitation methods, and Zr... 4+ Rapid hydrolysis prevents the formation of a directionally coordinated In-O-Zr interface structure, resulting in limited electronic synergistic effects and making it difficult to achieve high-speed hydrolysis at industrial space velocities (>3000 mL / (g)). cat It can operate stably for a long time under conditions of ·h) and raw gas containing impurities.
[0005] Gasification residue is a solid waste generated during coal gasification, with a huge annual output. Rich in aluminosilicates and possessing a natural hierarchical pore structure (micropore-mesopore-macropore synergy), it theoretically can serve as a catalyst support for confined dispersion of active components and enhanced mass transfer. However, in current technologies, gasification residue is mainly used in building materials, adsorbent materials, or molecular sieve synthesis, and there are no reports of its use as an In-Zr bimetallic catalyst support for CO2 hydrogenation to methanol after specific pretreatment. Furthermore, due to its low specific gravity (1.2-1.5) and loose pore structure, conventional sieving is insufficient to effectively remove ungasified residual carbon and dense mineral impurities. These impurities can easily lead to the entrapment of active components or pore blockage under high-temperature reaction conditions, affecting catalytic performance. Therefore, to address these issues, there is an urgent need to develop an In-Zr / gasification residue dual-active-site catalyst for CO2 hydrogenation to methanol. Summary of the Invention
[0006] The purpose of this invention is to provide an In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol, so as to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] A method for preparing an In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol includes the following steps:
[0009] S1. Selection and pretreatment of gasification slag carrier: Screen the gasification slag, and obtain the gasification slag carrier after water washing, steam activation and drying;
[0010] S2. Preparation of highly dispersed In2O3 / gasification slag precursor: The gasification slag support obtained in step S1 was pretreated by calcining at 300-500℃ for 2-4 hours; a highly dispersed In2O3 nanoarray was constructed on the surface of the gasification slag support by chemical deposition. After filtration, washing, and drying, it was calcined at 400-550℃ for 3-5 hours to obtain the In2O3 / gasification slag precursor.
[0011] S3. Introducing a second metal active site regulator: Zirconium metal impregnation solution is prepared using zirconium pentahydrate as the zirconium source. The In2O3 / gasification slag precursor obtained in step S2 is mixed with the zirconium metal impregnation solution and ion-exchanged in a water bath at 80-85℃ for 3-6 hours. After centrifugation, washing, and drying, it is calcined at 500-700℃ for 4-9 hours to obtain an In-Zr / gasification slag dual active site catalyst.
[0012] Preferably, the gasification slag in step S1 has a particle size of 100-200 mesh and a specific gravity of 1.2-1.5; the screening is performed by first using a gravity water separator to pre-select the gasification slag raw material, and then using a vibrating filter screen for fine selection; the steam activation temperature is 300-800℃, the activation time is 3-12 hours, and the moisture content of the gasification slag carrier after drying is controlled below 10%.
[0013] Preferably, the chemical deposition method in step S2 includes: preparing an aqueous solution of indium salt and adding a precipitant to obtain a deposition solution; adding the pretreated gasified slag carrier to the deposition solution; and stirring at a constant temperature of 70-90°C for 4-12 hours; wherein the indium salt is selected from at least one of indium nitrate, indium acetate, indium chloride, indium acetylacetone, and indium sulfate; and the precipitant is urea.
[0014] Preferably, the drying temperature in steps S2 and S3 is 80-120°C, and the drying time is 6-24 hours.
[0015] Preferably, the stirring speed of the ion exchange in step S3 is 300-400 rpm, the mixing ratio of the In2O3 / gasification slag precursor to the zirconium metal impregnation solution is 1g:30mL, and the mass ratio of the Zr source to the In2O3 / gasification slag precursor is 1:0.1-1:10.
[0016] Preferably, the heating rate of calcination in step S3 is 1-5℃ / min.
[0017] The present invention also provides an In-Zr / gasification slag dual-active-site catalyst prepared by the above preparation method.
[0018] Preferably, In and Zr are combined through an In-O-Zr coordination structure.
[0019] This invention also provides the application of the catalyst in the hydrogenation of CO2 to methanol, wherein the catalyst is packed in a fixed-bed reactor, a reaction gas with a H2 to CO2 molar ratio of 3:1 is introduced, N2 is used as the equilibrium gas, the reaction temperature is 425-475℃, and the mass hourly space velocity is 3600-19200 mL / (g) cat ·h), the reaction pressure is 2-5MPa.
[0020] Preferably, the catalyst is loaded in an amount of 0.6-0.9g.
[0021] Preferably, the heating rate is 8-12℃ / min.
[0022] Compared with the prior art, the beneficial effects of the present invention are:
[0023] This invention addresses the technical shortcomings of existing In2O3-based catalysts, such as the easy aggregation of In species, limited H2 dissociation ability, and the inability of co-precipitation methods to form directionally coordinated In-O-Zr interfacial structures. It provides an In-Zr / gasification slag dual-active-site catalyst and its preparation method, achieving the following beneficial effects:
[0024] (1) After gravity water separation and steam activation pretreatment, the gasification slag effectively removed residual carbon and dense mineral impurities, and optimized the multi-level pore structure. This structure provides a gradient diffusion channel for the reactants, realizing the dual functions of confined mass transfer and dispersion of active components, and significantly improving the accessibility of active sites and mass transfer efficiency.
[0025] (2) Highly dispersed In2O3 nanoarrays were constructed on the surface of the gasification slag support using urea as a precipitant via chemical deposition. Urea was slowly hydrolyzed at a constant temperature of 70-90℃, uniformly releasing OH-. - , making In 3+ In the form of In(OH)3, it is uniformly deposited on the surface of the carrier and transformed into highly dispersed In2O3 nanoparticles after calcination, exposing abundant surface oxygen vacancies, which effectively promotes the adsorption and activation of CO2 molecules.
[0026] (3) Using zirconium nitrate pentahydrate as a regulator, Zr is introduced via ion exchange. 4+ This forms a stable In-O-Zr coordination structure. On the one hand, this structure inhibits the aggregation of In2O3 particles through geometric confinement, maintaining a high degree of dispersion of the active component; on the other hand, it regulates the electron cloud density of In2O3 through electronic interactions, increases the oxygen vacancy concentration, enhances the CO2 adsorption and activation capacity, and enhances the stability of the reaction intermediate through interfacial synergy, promoting its directional hydrogenation into methanol.
[0027] (4) Through the synergistic effect of the above three mechanisms, the catalyst of the present invention achieves a CO2 conversion rate of 8.82%, a methanol selectivity of 70.25%, and a methanol space-time yield of 6.20 g / (g) in the CO2 hydrogenation to methanol reaction. cat Compared with unactivated carriers, single In systems without Zr, reverse addition order schemes, co-precipitation method for introducing Zr, and conventional carrier alternatives, it has significant advantages in all performance indicators. Attached Figure Description
[0028] Figure 1 This is a scanning electron microscope (SEM) image of the In-Zr / gasification slag dual-active-site catalyst prepared in Example 1 of the present invention.
[0029] Figure 2 This is an elemental distribution (EDSMapping) diagram of the In-Zr / gasification slag dual-active-site catalyst prepared in Example 1 of this invention. Detailed Implementation
[0030] The technical solution of this application will be further described in detail below with reference to specific embodiments.
[0031] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.
[0032] The core of the preparation method of the In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol provided by this invention lies in: using gasification slag as a support, after gravity water separation and steam activation pretreatment, constructing a highly dispersed In2O3 nanoarray on the support surface by chemical deposition; and then introducing Zr using zirconium pentahydrate as a zirconium source through ion exchange. 4 + An In-O-Zr coordination structure is formed, ultimately yielding an In-Zr / gasification slag dual-active-site catalyst. This includes the following steps:
[0033] S1. Selection and pretreatment of gasification slag carrier: Screen the gasification slag, and obtain the gasification slag carrier after water washing, steam activation and drying;
[0034] S2. Preparation of highly dispersed In2O3 / gasification slag precursor: The gasification slag support obtained in step S1 was pretreated by calcining at 300-500℃ for 2-4 hours; a highly dispersed In2O3 nanoarray was constructed on the surface of the gasification slag support by chemical deposition. After filtration, washing, and drying, it was calcined at 400-550℃ for 3-5 hours to obtain the In2O3 / gasification slag precursor.
[0035] S3. Introducing a second metal active site regulator: Zirconium metal impregnation solution is prepared using zirconium pentahydrate as the zirconium source. The In2O3 / gasification slag precursor obtained in step S2 is mixed with the zirconium metal impregnation solution and ion-exchanged in a water bath at 80-85℃ for 3-6 hours. After centrifugation, washing, and drying, it is calcined at 500-700℃ for 4-9 hours to obtain an In-Zr / gasification slag dual active site catalyst.
[0036] The present invention will be further described below through specific embodiments and comparative examples.
[0037] Example 1
[0038] (1) Selection and pretreatment of gasification slag carrier: First, the gasification slag raw material is initially selected by gravity water separator. The gasification slag with higher specific gravity is separated from the gasification slag with lower specific gravity. Then, it is further selected by vibrating filter screen (specifically: the gasification slag with lower specific gravity after primary separation is first selected by 100 mesh vibrating filter screen, and the gasification slag that passes through the filter screen is then selected by 200 mesh vibrating filter screen, and the gasification slag that does not pass through the filter screen is taken); the gasification slag with a particle size range of 100-200 mesh (particle size 75~150μm) and a specific gravity range of 1.25-1.5 is obtained. After being washed with water until neutral, it is activated by steam at 300℃ and dried for 12h until the moisture content is below 10% to obtain the gasification slag carrier.
[0039] (2) Preparation of highly dispersed In2O3 / gasification slag precursor: 2.0 g of pretreated gasification slag was weighed and activated at 500 °C for 2 h. 0.29 g of In(NO3)3·xH2O and 1.0 g of urea were dissolved in 50 mL of deionized water. The activated gasification slag was added to the solution and stirred in an oil bath at 80 °C for 8 h. After filtration and washing until the pH was neutral, the product was dried in an oven at 110 °C for 12 h and then calcined in air at 500 °C for 4 h to obtain the In2O3 / gasification slag precursor.
[0040] (3) Introducing a second metal active site regulator: 0.5 g of In2O3 / gasification slag precursor was placed in a 200 mL beaker. Zr metal impregnation solution was added dropwise according to the mass ratio of Zr source in zirconium nitrate pentahydrate to In2O3 / gasification slag precursor of 1:0.1. After the addition was completed, the sample was placed in a water bath at 80 °C for ion exchange for 3 h with the top stirring device set to 300 rpm / min. Then it was centrifuged and dried in an oven at 80 °C for 24 h. Finally, it was placed in a muffle furnace at 500 °C with an air atmosphere for calcination and activation for 9 h to obtain the In-Zr / gasification slag dual active site catalyst.
[0041] The prepared catalyst was tested, such as... Figure 1 and Figure 2 The images shown are scanning electron microscope (SEM) images and EDS elemental distribution diagrams of the catalyst obtained in this embodiment.
[0042] Example 2
[0043] (1) Selection and pretreatment of gasification slag carrier: First, the gasification slag raw material is initially selected by gravity water separator. The gasification slag with higher specific gravity is separated from the gasification slag with lower specific gravity. Then, it is further selected by vibrating filter screen (specifically: the gasification slag with lower specific gravity after primary separation is first selected by 100 mesh vibrating filter screen, and the gasification slag that passes through the filter screen is then selected by 200 mesh vibrating filter screen, and the gasification slag that does not pass through the filter screen is taken); the gasification slag with a particle size range of 100-200 mesh (particle size 75~150μm) and a specific gravity range of 1.25-1.5 is obtained. After being washed with water until neutral, it is activated by steam at 400℃ and dried for 10h until the moisture content is below 10% to obtain the gasification slag carrier.
[0044] (2) Preparation of highly dispersed In2O3 / gasification slag precursor: 1.0 g of pretreated gasification slag was weighed and activated at 400 °C for 2 h. 0.29 g of In(CH3COO)3 and 1.0 g of urea were dissolved in 50 mL of deionized water. The activated gasification slag was added to the solution and stirred in an oil bath at 80 °C for 8 h. After filtration, washing, drying at 110 °C for 12 h, and then calcining in air at 500 °C for 4 h, the In2O3 / gasification slag precursor was obtained.
[0045] (3) Introducing a second metal active site regulator: 0.5g of In2O3 / gasification slag precursor was placed in a 200mL beaker. Zr metal impregnation solution was added dropwise according to the mass ratio of Zr source in zirconium nitrate pentahydrate to In2O3 / gasification slag precursor of 1:1. After the addition was completed, the sample was placed in a water bath at 85℃ for ion exchange for 4h with the top stirring device set to 330rpm / min. Then it was centrifuged and dried in an oven at 100℃ for 12h. Then it was placed in a muffle furnace at 600℃ with air atmosphere for calcination and activation for 5h to obtain In-Zr / gasification slag dual active site catalyst.
[0046] Example 3
[0047] (1) Selection and pretreatment of gasification slag carrier: First, the gasification slag raw material is initially selected by gravity water separator. The gasification slag with higher specific gravity is separated from the gasification slag with lower specific gravity. Then, it is further selected by vibrating filter screen (specifically: the gasification slag with lower specific gravity after primary separation is first selected by 100 mesh vibrating filter screen, and the gasification slag that passes through the filter screen is then selected by 200 mesh vibrating filter screen, and the gasification slag that does not pass through the filter screen is taken); the gasification slag with a particle size range of 100-200 mesh (particle size 75~150μm) and a specific gravity range of 1.25-1.5 is obtained. After being washed with water until neutral, it is activated by steam at 600℃ and dried for 8 hours until the moisture content is below 10% to obtain the gasification slag carrier.
[0048] (2) Preparation of highly dispersed In2O3 / gasification slag precursor: 1.5g of pretreated gasification slag was weighed and activated at 500℃ for 2h. 0.48g of InCl3 and 5.0g of urea were dissolved in 50mL of deionized water. The activated gasification slag was added to the solution and stirred in an oil bath at 80℃ for 8h. After filtration, washing, drying at 110℃ for 12h, and then calcining in air at 500℃ for 4h, the In2O3 / gasification slag precursor was obtained.
[0049] (3) Introducing a second metal active site regulator: 0.5g of In2O3 / gasification slag precursor was placed in a 200mL beaker, and Zr metal impregnation solution was added dropwise according to the mass ratio of Zr source in zirconium nitrate pentahydrate to In2O3 / gasification slag precursor of 1:6. After the addition was completed, the sample was placed in a water bath at 80℃ for ion exchange for 5h with the top stirring device set to 360rpm / min. Then it was centrifuged and dried in an oven at 100℃ for 12h. Then it was placed in a muffle furnace at 550℃ with air atmosphere for calcination and activation for 9h to obtain In-Zr / gasification slag dual active site catalyst.
[0050] Example 4
[0051] (1) Selection and pretreatment of gasification slag carrier: First, the gasification slag raw material is initially selected by gravity water separator. The gasification slag with higher specific gravity is separated from the gasification slag with lower specific gravity. Then, it is further selected by vibrating filter screen (specifically: the gasification slag with lower specific gravity after primary separation is first selected by 100 mesh vibrating filter screen, and the gasification slag that passes through the filter screen is then selected by 200 mesh vibrating filter screen, and the gasification slag that does not pass through the filter screen is taken); the gasification slag with a particle size range of 100-200 mesh (particle size 75~150μm) and a specific gravity range of 1.25-1.5 is obtained. After being washed with water until neutral, it is activated by steam at 700℃ and dried for 6 hours until the moisture content is below 10% to obtain the gasification slag carrier.
[0052] (2) Preparation of highly dispersed In2O3 / gasification slag precursor: 2.0 g of pretreated gasification slag was weighed and activated at 500 °C for 2 h. 0.29 g of In(acac)3 (indium acetylacetone) and 1.0 g of urea were dissolved in 50 mL of deionized water. The activated gasification slag was added to the solution and stirred in an oil bath at 80 °C for 8 h. After filtration, washing, drying at 110 °C for 12 h, and then calcining in air at 500 °C for 4 h, the In2O3 / gasification slag precursor was obtained.
[0053] (3) Introducing a second metal active site regulator: 0.5g of In2O3 / gasification slag precursor was placed in a 200mL beaker, and Zr metal impregnation solution was added dropwise according to the mass ratio of Zr source in zirconium nitrate pentahydrate to In2O3 / gasification slag precursor of 1:3. After the addition was completed, the sample was placed in a water bath at 80℃ for ion exchange for 6h with the top stirring device set to 330rpm / min. Then it was centrifuged and dried in an oven at 100℃ for 12h. Then it was placed in a muffle furnace at 700℃ with air atmosphere for calcination and activation for 4h to obtain In-Zr / gasification slag dual active site catalyst.
[0054] Example 5
[0055] (1) Selection and pretreatment of gasification slag carrier: First, the gasification slag raw material is initially selected by gravity water separator. The gasification slag with higher specific gravity is separated from the gasification slag with lower specific gravity. Then, it is further selected by vibrating filter screen (specifically: the gasification slag with lower specific gravity after primary separation is first selected by 100 mesh vibrating filter screen, and the gasification slag that passes through the filter screen is then selected by 200 mesh vibrating filter screen, and the gasification slag that does not pass through the filter screen is taken); the gasification slag with a particle size range of 100-200 mesh (particle size 75~150μm) and a specific gravity range of 1.25-1.5 is obtained. After being washed with water until neutral, it is activated by steam at 800℃ and dried for 3h until the moisture content is below 10% to obtain the gasification slag carrier.
[0056] (2) Preparation of highly dispersed In2O3 / gasification slag precursor: 2.0 g of pretreated gasification slag was weighed and activated at 500 °C for 2 h. 0.29 g of In2(SO4)3 and 1.0 g of urea were dissolved in 50 mL of deionized water. The activated gasification slag was added to the solution and stirred in an oil bath at 80 °C for 8 h. After filtration, washing, drying at 110 °C for 12 h, and then calcining in air at 500 °C for 4 h, the In2O3 / gasification slag precursor was obtained.
[0057] (3) Introducing a second metal active site regulator: 0.5 g of In2O3 / gasification slag precursor was placed in a 200 mL beaker. Zr metal impregnation solution was added dropwise according to the mass ratio of Zr source in zirconium nitrate pentahydrate to In2O3 / gasification slag precursor of 1:10. After the addition was completed, the sample was placed in a water bath at 80 °C for ion exchange for 6 h with the top stirring device set to 400 rpm / min. Then it was centrifuged and dried in an oven at 100 °C for 12 h. Then it was placed in a muffle furnace at 700 °C with air atmosphere for calcination and activation for 4 h to obtain In-Zr / gasification slag dual active site catalyst.
[0058] Comparative Example 1
[0059] A gasification slag carrier without steam activation pretreatment was used for comparison. In the selection and pretreatment of the gasification slag carrier, only a fine gasification slag with a particle size of 100~200 mesh and a specific gravity of 1.25~1.5 was obtained by gravity water separator and vibrating filter screen (100 mesh and 200 mesh). After being washed with water until neutral, it was directly dried at 110℃ for 12h (without steam activation treatment) to obtain an unactivated gasification slag carrier. The rest was the same as in Example 1.
[0060] Comparative Example 2
[0061] A comparative study was conducted on the preparation of a single In2O3 / gasification slag catalyst without the addition of a second metal, Zr. The synthesis steps without the addition of metal Zr were as follows: First, following step (1) in Example 1, the gasification slag was pretreated by washing with water, sieving, and steam activation to obtain a gasification slag support; then, following step (2) in Example 1, 2.0 g of the pretreated gasification slag was weighed and activated at 500 °C for 2 h, 0.29 g of In2O3·xH2O and 1.0 g of urea were dissolved in 50 mL of deionized water, and the activated gasification slag was added to the solution. The mixture was stirred in an oil bath at 80 °C for 8 h, filtered, washed until pH neutral, dried at 110 °C for 12 h, and then calcined in an air atmosphere at 500 °C for 4 h to obtain a single metal In modified In2O3 / gasification slag catalyst (without the Zr introduction step).
[0062] Comparative Example 3
[0063] A Zr-In / gasification slag catalyst was prepared by controlling the order of In and Zr addition for comparison. The pretreatment of the gasification slag support in the preparation process still followed the step (1) in Example 1. Then, 0.5g of the pretreated gasification slag was placed in a 200mL beaker, and Zr metal impregnation solution was added dropwise according to the mass ratio of Zr source in zirconium nitrate pentahydrate to gasification slag support of 1:0.1. Ion exchange was carried out in an 80℃ water bath for 3h with stirring at 300rpm / min. After centrifugation, it was dried at 80℃ for 24h and then calcined in air atmosphere at 500℃ for 4h to obtain Zr / gasification slag intermediate. Subsequently, the loading of metallic In was carried out: the above Zr / gasification slag sample was added to 50 mL of deionized water containing 0.29 g In(NO3)3·xH2O and 1.0 g urea, stirred in an oil bath at 80 °C for 8 h, filtered and washed until pH neutral, dried at 110 °C for 12 h, and then calcined in air at 500 °C for 4 h to obtain Zr-In / gasification slag catalyst (the loading order of In-Zr is reversed in Example 1).
[0064] Comparative Example 4
[0065] The introduction of metallic Zr was controlled, and the traditional co-precipitation method was used for comparison. The pretreatment of the gasification slag carrier and the preparation of the highly dispersed In2O3 / gasification slag precursor were carried out using steps (1) and (2) in Example 1. Then, 0.5g of the pretreated In2O3 / gasification slag precursor was placed in a 200mL beaker. Zirconium nitrate pentahydrate was dissolved in 50mL of deionized water according to a Zr source to In2O3 / gasification slag carrier mass ratio of 1:0.1. In2O3 / gasification slag was added, and the mixture was vigorously stirred to form a suspension. At room temperature and with stirring at 300rpm / min, 1.0mol / L ammonia solution was added dropwise to adjust the pH of the system to 9.0~10.0, allowing Zr to be introduced. 4+ The Zr(OH)4 precipitate completely on the surface and in the pores of the precursor. After the addition is complete, the mixture is stirred and aged for another 2 hours. The suspension is centrifuged, and the precipitate is repeatedly washed with deionized water until the pH is neutral. The resulting solid is dried at 80°C for 24 hours and then calcined in air at 500°C for 4 hours to obtain the In-Zr / gasification slag catalyst (different from the method of introducing the second metal Zr in Example 1).
[0066] Comparative Example 5
[0067] A catalyst was prepared by replacing gasification slag with a composite oxide support of γ-Al2O3 and SiO2 for comparison. In the preparation process, commercial γ-Al2O3 and mesoporous SiO2 (SBA-15) were uniformly mixed at a mass ratio of 1:1 and then ground in a grinder. The mixture was then passed through 100-mesh and 200-mesh standard inspection sieves to obtain particle components with a particle size range of 100-200 mesh (75-150 μm). The sieved composite oxide support was placed in an oven and dried at 300℃ for 12 hours to reduce its moisture content to below 10%. After cooling, it was placed in a sealed sample bag for later use. The preparation of the highly dispersed In2O3 / composite oxide support and the preparation of the second metal active site regulator were carried out using steps (2) and (3) in Example 1. That is, firstly, a highly dispersed In2O3 nanoarray was constructed on the surface of the composite oxide support by urea homogeneous deposition, and then Zr was introduced by ion exchange. 4+ An In-Zr / (γ-Al2O3+SBA-15) catalyst was prepared (different from the support type in Example 1).
[0068] Catalyst performance evaluation
[0069] The In-Zr / gasification slag dual-active-site catalysts obtained in Examples 1-5 and the catalysts obtained in Comparative Examples 1-5 were subjected to CO2 hydrogenation to methanol reaction. The reaction steps were as follows: 200 mg of catalyst was weighed and placed in the constant temperature zone of the reaction tube. Quartz wool was plugged at both ends of the reaction tube, and the catalyst was fixed in place with quartz wool and quartz sand to prevent catalyst loss and backmixing. Then, N2 was introduced into the reaction tube for purging for more than 30 min (50 mL / min) to remove the initial gas, and combustion pressure was checked. To ensure a leak-free reaction pathway, a reducing gas (a hydrogen-nitrogen mixture with a 20% H2 volume fraction) is introduced at atmospheric pressure at a rate of 50 mL / min. The temperature is then increased to 300 °C at a rate of 2 °C / min. After reduction for 2 hours, the temperature is purged with N2 to 220 °C. Once the specified temperature is reached, the N2 flow rate is switched to a reaction gas (with a H2 to CO2 molar ratio of 3:1 and nitrogen as the equilibrium gas) to initiate the reaction. The reaction space velocity is 16800 mL / (g⁻¹). cat The system pressure was increased to 3 MPa to begin performance evaluation of the CO2 hydrogenation reaction. After the temperature and pressure of the reaction system stabilized, the gaseous products were detected online using a gas chromatograph. The results are shown in Table 1.
[0070] Table 1 Comparison of catalytic results of the prepared catalysts in the CO2 hydrogenation to methanol reaction.
[0071]
[0072] In summary, the In-Zr / gasification slag dual-active-site catalyst prepared by this invention exhibits excellent catalytic performance in the CO2 hydrogenation to methanol reaction, as shown in Table 1. Compared with Comparative Examples 1-5, Examples 1-4 show significantly improved CO2 conversion and methanol selectivity. Example 1 achieved a CO2 conversion of 8.82%, a methanol selectivity of 70.25%, and a methanol space-time yield of 6.20%, all significantly better than Comparative Example 1 (without steam activation), Comparative Example 2 (without the introduction of the second metal Zr), Comparative Example 3 (with the metal addition order reversed), Comparative Example 4 (using the conventional co-precipitation method to introduce Zr), and Comparative Example 5 (using a conventional composite oxide support instead of the gasification slag). These results indicate that the Zr in Comparative Example 4... 4+Because the hydrolysis is too rapid, it cannot form a directionally coordinated In-O-Zr interface structure with In2O3, resulting in the loss of the bimetallic electronic synergistic effect. In Comparative Example 5, the conventional support lacks the microporous-mesoporous-macroporous synergistic multi-level pore structure unique to gasification slag, failing to achieve the gradient mass transfer enhancement effect. The catalytic performance of both examples is far lower than that of Example 1, further demonstrating that the introduction method of Zr and the selection of the gasification slag support in this invention are non-obvious. The In-Zr / gasification slag catalyst prepared by the technical solution of this application precisely controls the matching relationship between the metal active sites and acid active centers on the catalyst surface through a triple synergistic mechanism of mass transfer enhancement via the multi-level pore structure of the gasification slag support, In-Zr bimetallic electronic synergy, and surface acid redistribution: on the one hand, gravity-water separation coupled with steam activation treatment constructs a suitable multi-level pore structure for the gasification slag support, significantly improving the diffusion efficiency of reactants / products; on the other hand, In... 3+ With Zr 4+ The In-O-Zr coordination structure formed by ion exchange effectively suppressed indium species aggregation and adjusted the electron cloud density of indium species, while also optimizing the ratio of Brønsted acid to Lewis acid on the catalyst surface. Under these synergistic effects, the catalyst effectively suppressed the reverse water-gas shift reaction (CO selectivity only 26.18%) and the methanation reaction (CH4 selectivity only 3.57%), significantly improving methanol selectivity and overall catalyst performance, showing broad prospects for industrial application in CO2 hydrogenation to methanol.
[0073] The above are merely preferred embodiments of the present invention. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention, and these should also be considered within the scope of protection of the present invention. These will not affect the effectiveness of the implementation of the present invention or the practicality of the patent.
Claims
1. A method for preparing an In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol, characterized in that, Includes the following steps: S1. Selection and pretreatment of gasification slag carrier: Screen the gasification slag, and obtain the gasification slag carrier after water washing, steam activation and drying; S2. Preparation of highly dispersed In2O3 / gasification slag precursor: The gasification slag support obtained in step S1 was pretreated by calcining at 300-500℃ for 2-4 hours; a highly dispersed In2O3 nanoarray was constructed on the surface of the gasification slag support by chemical deposition. After filtration, washing, and drying, it was calcined at 400-550℃ for 3-5 hours to obtain the In2O3 / gasification slag precursor. S3. Introducing a second metal active site regulator: Zirconium metal impregnation solution is prepared using zirconium pentahydrate as the zirconium source. The In2O3 / gasification slag precursor obtained in step S2 is mixed with the zirconium metal impregnation solution and ion-exchanged in a water bath at 80-85℃ for 3-6 hours. After centrifugation, washing, and drying, it is calcined at 500-700℃ for 4-9 hours to obtain an In-Zr / gasification slag dual active site catalyst.
2. The preparation method of the In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol according to claim 1, characterized in that, The gasification slag in step S1 has a particle size of 100-200 mesh and a specific gravity of 1.2-1.5; the screening process involves first performing a gravity water separator to pre-select the gasification slag raw material, and then using a vibrating filter screen for further selection; the steam activation temperature is 300-800℃, and the activation time is 3-12 hours.
3. The preparation method of the In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol according to claim 1, characterized in that, The chemical deposition method in step S2 includes: preparing an aqueous solution of indium salt and adding a precipitant to obtain a deposition solution; adding the pretreated gasified slag carrier to the deposition solution; and stirring at a constant temperature of 70-90°C for 4-12 hours; wherein the indium salt is selected from at least one of indium nitrate, indium acetate, indium chloride, indium acetylacetone, and indium sulfate; and the precipitant is urea.
4. The method for preparing the In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol according to claim 1, characterized in that, The drying temperature in steps S2 and S3 is 80-120°C, and the time is 6-24 hours.
5. The method for preparing the In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol according to claim 1, characterized in that, In step S3, the stirring speed for ion exchange is 300-400 rpm, the mixing ratio of the In2O3 / gasification slag precursor to the zirconium metal impregnation solution is 1g:30mL, and the mass ratio of the Zr source to the In2O3 / gasification slag precursor is 1:0.1-1:
10.
6. The method for preparing the In-Zr / gasification slag dual-active-site catalyst for CO2 hydrogenation to methanol according to claim 1, characterized in that, The heating rate for calcination in step S3 is 1-5℃ / min.
7. The In-Zr / gasification slag dual-active-site catalyst prepared by the preparation method according to any one of claims 1-6, characterized in that, The In and Zr are combined through an In-O-Zr coordination structure.
8. The application of the In-Zr / gasification slag dual-active-site catalyst as described in claim 7 in CO2 hydrogenation to methanol, characterized in that, The catalyst was packed into a fixed-bed reactor, and a reaction gas with a H2 to CO2 molar ratio of 3:1 was introduced, with N2 as the equilibrium gas. The reaction temperature was 425-475℃, and the mass hourly space velocity was 3600-19200 mL / (g). cat ·h), the reaction pressure is 2-5MPa.
9. The application according to claim 8, characterized in that, The catalyst is loaded in an amount of 0.6-0.9g.
10. The application according to claim 8, characterized in that, The heating rate is 8-12℃ / min.