Mn-based catalyst, preparation method thereof and application of the catalyst in catalyzing oxidation of formaldehyde at room temperature
By preparing nano-flower-like MnO2 catalysts, the problem of Mn-based catalysts requiring high temperatures was solved, achieving efficient formaldehyde oxidation at room temperature while maintaining low cost and no pollution, making it suitable for the formaldehyde purification field.
Patent Information
- Application Number
- CN202611049962.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing Mn-based catalysts require higher temperatures to achieve 100% formaldehyde removal rates. While they are low-cost, their applications are limited, as they cannot effectively catalyze the oxidation of formaldehyde at room temperature.
A mixed-phase MnO2 catalyst was prepared by adjusting the pH of a heptavalent manganese source solution with alkali and a precipitant, adding a divalent manganese salt and a reducing agent, and then calcining it in an anaerobic environment. The catalyst exhibits a nanoflower-like structure with high specific surface area and porosity.
It achieves efficient catalytic oxidation of formaldehyde at room temperature with a removal rate of over 90%, and generates no secondary pollutants. The preparation method is simple and inexpensive.
Smart Images

Figure CN123102341A_ABST
Abstract
Description
Technical Field
[0001] This application relates to a Mn-based catalyst and its preparation method, and its application in catalytic oxidation of formaldehyde at room temperature, belonging to the field of formaldehyde purification. Background Technology
[0002] Currently available formaldehyde oxidation catalysts are mainly divided into noble metal catalysts and non-noble metal catalysts. Noble metal catalysts, represented by Pt / TiO2, can catalytically oxidize formaldehyde at room temperature with a removal rate of up to 100%, but their large-scale application is limited by the cost of precious metals. Non-noble metal catalysts, represented by Mn-based catalysts, require a certain temperature to achieve a 100% formaldehyde removal rate, with a temperature window of approximately 80℃. Non-noble metal catalysts have lower costs and good formaldehyde selectivity, possessing considerable market potential. Therefore, developing Mn-based catalysts that can catalytically oxidize formaldehyde at room temperature has broad application prospects. Summary of the Invention
[0003] To address the limitation that Mn-based catalysts require high temperatures to achieve their full performance, this application provides an Mn-based catalyst that can catalyze the oxidation of formaldehyde at room temperature, exhibits excellent activity, and has a simple and low-cost synthesis method.
[0004] According to the first aspect of this application, a method for preparing a Mn-based catalyst is provided.
[0005] A method for preparing a Mn-based catalyst, the method comprising: S1. Prepare a heptavalent manganese source solution by adding alkali and precipitant, and adjust the pH to 8-10. S2. Add divalent manganese salt to the solution, add reducing agent dropwise, and react; S3. The product obtained from the reaction is separated, washed, dried, and calcined in an oxygen-free environment to obtain the Mn-based catalyst.
[0006] Optionally, in step S1, the heptavalent manganese source is selected from at least one of potassium permanganate, sodium permanganate, and ammonium permanganate.
[0007] Optionally, in step S1, the alkali is selected from at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, ammonia, potassium carbonate, and potassium hydroxide.
[0008] Optionally, in step S1, the pH is adjusted to 9-10.
[0009] Optionally, in step S1, the pH is adjusted to any value among 8, 8.5, 9, 9.5, and 10, or a range between any two.
[0010] Optionally, in step S1, the precipitant is selected from at least one of urea and ammonium chloride.
[0011] Optionally, the mass ratio of heptavalent manganese source to precipitant is 1:0.1 to 1:0.5.
[0012] Optionally, the mass ratio of heptavalent manganese source to precipitant is any value among 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or any range between the two.
[0013] Optionally, in step S2, the divalent manganese salt is selected from at least one of manganese sulfate, manganese nitrate, and manganese chloride.
[0014] Optionally, the molar ratio of heptavalent manganese source to divalent manganese salt is 1:0.8 to 1:1.2.
[0015] Optionally, the molar ratio of the heptavalent manganese source to the divalent manganese salt is any value among 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, or any range between the two.
[0016] Optionally, in step S2, the reducing agent is selected from at least one of ethanol, acetone, methanol, and acetaldehyde.
[0017] Optionally, the mass ratio of heptavalent manganese source to reducing agent is 1:4 to 1:10.
[0018] Optionally, the mass ratio of heptavalent manganese source to reducing agent is any value from 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10 or any range between the two.
[0019] Optionally, in step S2, the reducing agent is added at a rate controlled to be completed within 30-60 minutes. Preferably, it is added within 30-50 minutes.
[0020] Optionally, in step S2, the reaction temperature is 60-90°C and the reaction time is 8-15 hours. Preferably, the reaction temperature is 70-90°C and the reaction time is 10-15 hours.
[0021] Optionally, in step S3, the oxygen-free environment is an atmosphere of inactive gas. Inactive gas includes nitrogen, helium, etc.
[0022] Optionally, in step S3, the roasting temperature is 350~450℃. Preferably, the roasting temperature is 380~420℃.
[0023] This preparation method is simple, utilizing the reducing properties of a weak organic reducing agent to undergo a redox reaction with potassium permanganate under alkaline conditions. During the reaction, the dropping rate of the reducing agent needs to be controlled, as it affects the catalyst's crystal phase formation, particle size, and the number of surface hydroxyl groups. Calcination under an inactive atmosphere is crucial; if calcination is performed under oxygen-containing conditions, some unsaturated Mn will be oxidized.3+ This reduces the number of active sites on the catalyst. The valence state transformation of Mn is a crucial pathway for electron transfer during the catalytic oxidation of formaldehyde at room temperature. The catalyst is a mixed-phase MnO2, predominantly composed of α-MnO2 and δ-MnO2, and exhibits a nanoflower-like structure under SEM microscopy.
[0024] According to a second aspect of this application, a Mn-based catalyst is provided.
[0025] The Mn-based catalyst prepared by the method described above.
[0026] Optionally, the Mn-based catalyst is δ-MnO2.
[0027] Optionally, the Mn-based catalyst has a fluffy, porous cluster structure, assembled from sheet-like or fibrous subunits, with an overall diameter of 500 nm to 2 μm for the particle clusters and a thickness of 10-20 nm for each individual substructure.
[0028] According to a third aspect of this application, an application of a Mn-based catalyst is provided.
[0029] The Mn-based catalyst prepared by the above-described method is used for the catalytic oxidation of formaldehyde at room temperature.
[0030] The beneficial effects that this application can produce include: 1) The Mn-based catalyst provided in this application has excellent room temperature catalytic activity and can be widely used in the room temperature oxidation and degradation of formaldehyde.
[0031] 2) The Mn-based catalyst provided in this application does not generate secondary pollutants during the formaldehyde removal process and can directly catalyze the degradation of formaldehyde to CO2 and H2O.
[0032] 3) The method for preparing the Mn-based catalyst provided in this application is simple and inexpensive. Attached Figure Description
[0033] Figure 1 The image shows a SEM image of catalyst A prepared in Example 1. Figure 2 The image shows the SEM image of catalyst F prepared in Comparative Example 2. Figure 3 Comparison of catalyst activity characterizations; Figure 4 XRD phase diagrams of catalysts A and F are shown. Figure 5 XRD comparison diagrams of three MnO2 crystal phases (α-MnO2, β-MnO2, δ-MnO2). Detailed Implementation
[0034] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.
[0035] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.
[0036] Unless otherwise specified, all test methods are standard and all instrument settings are those recommended by the manufacturer.
[0037] The analysis method in the embodiments of this application is as follows: The electron microscope used for analysis was a German ZEISS Sigma 360.
[0038] The XRD analysis was performed using a Thermo Fisher ARL EQUINOX instrument with the following conditions: 0° to 80°, 0.02° step size, and 4° / min.
[0039] Example 1 Potassium permanganate was used as the Mn source, urea as the precipitant, sodium carbonate as the pH adjuster, and ethanol as the reducing agent.
[0040] Dissolve 5g of potassium permanganate in 100mL of water. Add 2g each of sodium carbonate and urea to adjust the pH to 9.0. Then add manganese sulfate at a molar ratio of potassium permanganate to manganese sulfate of 1:1. Raise the temperature to 80℃ and add ethanol at a mass ratio of potassium permanganate to ethanol of 1:5, with a dropping rate of 10mL / min (to be completed within 30 minutes). Stir in an 80℃ water bath for 12 hours. Filter and wash the precipitate until the pH of the filtrate reaches 7.0. Dry in an oven at 100℃ for 12 hours to obtain a powdered catalyst. Calcine the powdered catalyst at 400℃ under a N2 atmosphere to obtain the product catalyst, referred to as catalyst A, labeled 1-MnO2.
[0041] Example 2 Other conditions remained the same as in Example 1, but the ratio of potassium permanganate to ethanol was changed to 1:10 (mass ratio) to obtain catalyst B, which was labeled as 2-MnO2.
[0042] Example 3 Other conditions remained the same as in Example 1, except that pH was adjusted to 8.0 to obtain catalyst C, which was labeled as 3-MnO2.
[0043] Example 4 Other conditions remained unchanged as in Example 1, and the catalyst was added directly without controlling the dropping rate to obtain catalyst D, labeled as 4-MnO2.
[0044] Comparative Example 1 10g of potassium permanganate and 5g of manganese sulfate were added to a high-pressure reactor, along with 2g of KOH. The reactor was then placed in an oven at 180℃ for 12 hours. After cooling to room temperature, the solid was removed, washed, and dried to obtain catalyst E, labeled as 5-MnO2.
[0045] Comparative Example 2 Other conditions remained unchanged as in Example 1. After calcination at 400°C in air, the product catalyst was obtained, which was called catalyst F and labeled as 6-MnO2.
[0046] Comparative Example 3 Other conditions remain the same as in Example 1, except that ethanol is replaced with the organic acid ascorbic acid, referred to as catalyst G, and labeled as 7-MnO2.
[0047] Characterization test The SEM image of catalyst A prepared in Example 1 is shown below. Figure 1 As shown in the image, δ-MnO2 exhibits a fluffy, porous, clustered structure, resembling a sponge, coral, or nanoflower. This morphology is composed of numerous thin sheet-like or fibrous subunits, with a rough surface and abundant pores.
[0048] Size estimation: A scale bar of 200 nm is present at the bottom of the image. Based on this, the overall diameter of the particle cluster is approximately between 500 nm and 2 μm, while the thickness of individual substructures (such as lamellae) is likely around 10–20 nm (inferred from the fluffy appearance). This indicates that δ-MnO2 is a nanoscale material with a high specific surface area.
[0049] Surface characteristics: The structure is highly branched and porous, which may be due to self-assembly during the synthesis process. This is beneficial to improving catalyst activity because the porous structure can increase active sites and ion transport channels.
[0050] Uniformity: The sample distribution is relatively uniform, with no obvious large agglomerations, but there are slight clusters, indicating good dispersibility.
[0051] The SEM image of catalyst F prepared in Comparative Example 2 is shown below. Figure 2 As shown, it is a mixed-phase MnO2, mainly composed of α-MnO2 and δ-MnO2. Under SEM, the catalyst exhibits a coexistence of rod-like and plate-like structures. α-MnO2 exhibits a rod-like structure, while δ-MnO2 exhibits a plate-like or nano-flower-like structure, thus it is identified as a mixed-phase MnO2.
[0052] like Figure 4 and Figure 5 As shown, the XRD characteristic peaks of catalyst A are consistent with those of δ-MnO2, proving that catalyst A is δ-MnO2. The characteristic peaks of catalyst F are not obvious at 10° and 25°, indicating that the crystal phase has changed after calcination.
[0053] Application Example 1 Samples A, B, C, D, E, F, and G were compressed, ground, and sieved. 5 g of 40-60 mesh particles were then processed in a 1m... 3 Formaldehyde catalytic oxidation activity was tested in a glass-sealed chamber.
[0054] The reaction mixture consisted of: formaldehyde (HCHO) = 100 ppm, humidity 50%. The reaction temperature was 25℃.
[0055] The formula for calculating formaldehyde removal rate is: Formaldehyde removal rate (%) = (Initial formaldehyde concentration - Formaldehyde exhaust gas concentration) / Initial formaldehyde concentration 100%.
[0056] Catalyst activity characterization such as Figure 3 As shown in Table 1, the specific analysis results are as follows.
[0057] Table 1
[0058] Catalyst A exhibits the most robust performance in the figure. It maintains a removal rate above 90% for approximately 1.1 hours, and after deactivation, the curve flattens out around 2.5 hours, eventually stabilizing at a steady-state removal rate of approximately 22%. This "long-tail" phenomenon may suggest the existence of two types of active sites on the catalyst surface: one type is highly active sites susceptible to product poisoning, and the other type is stable sites with lower activity but stronger resistance to poisoning. Catalyst B's activity is very close to that of catalyst A, due to the different concentrations of organic reducing agents, which affect crystal phase formation, resulting in insufficient formation of active sites and a significant decrease in the deactivation rate. The rapid activity decay of catalyst C is due to the different mechanisms of action between permanganate and reducing agent at pH below 9, leading to the absence of highly active reaction sites on the product catalyst. The poor activity of catalyst D is due to the excessively rapid addition of the reducing agent during the reaction, resulting in insufficient time for manganese oxide crystal growth and insufficient formation of active sites. The activity of catalyst E shows a precipitous drop after 0.4 hours, indicating that its surface active sites are easily covered by reaction intermediates. After calcination under aerobic conditions, the active sites of catalyst F are oxidized, resulting in a significant decrease in catalytic activity. Catalyst G uses ascorbic acid as a reducing agent, and the MnO2 generated under acidic conditions is mainly α-MnO2, which has fewer active sites and therefore poorer activity.
[0059] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a Mn-based catalyst, characterized in that, The preparation method includes: S1. Prepare a heptavalent manganese source solution by adding alkali and precipitant, and adjust the pH to 8-10. S2. Add divalent manganese salt to the solution, add reducing agent dropwise, and react; S3. The product obtained from the reaction is separated, washed, dried, and calcined in an oxygen-free environment to obtain the Mn-based catalyst.
2. The preparation method according to claim 1, characterized in that, In step S1, the heptavalent manganese source is selected from at least one of potassium permanganate, sodium permanganate, and ammonium permanganate.
3. The preparation method according to claim 1, characterized in that, In step S1, the alkali is selected from at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, ammonia, potassium carbonate, and potassium hydroxide. Preferably, in step S1, the pH is adjusted to 9-10; Preferably, in step S1, the precipitant is selected from at least one of urea and ammonium chloride; Preferably, the mass ratio of heptavalent manganese source to precipitant is 1:0.1 to 1:0.
5.
4. The preparation method according to claim 1, characterized in that, In step S2, the divalent manganese salt is selected from at least one of manganese sulfate, manganese nitrate, and manganese chloride; Preferably, the molar ratio of heptavalent manganese source to divalent manganese salt is 1:0.8 to 1:1.
2.
5. The preparation method according to claim 1, characterized in that, In step S2, the reducing agent is selected from at least one of ethanol, acetone, methanol, and acetaldehyde; Preferably, the mass ratio of heptavalent manganese source to reducing agent is 1:4 to 1:10; Preferably, in step S2, the reducing agent is added at a rate controlled within 30 to 60 minutes.
6. The preparation method according to claim 1, characterized in that, In step S2, the reaction temperature is 60~90℃ and the reaction time is 8~15h.
7. The preparation method according to claim 1, characterized in that, In step S3, the oxygen-free environment is an inactive gas atmosphere; Preferably, in step S3, the calcination temperature is 350~450℃.
8. The Mn-based catalyst prepared by the preparation method according to any one of claims 1 to 7.
9. The Mn-based catalyst according to claim 8, characterized in that, The Mn-based catalyst is δ-MnO2; Preferably, the Mn-based catalyst has a fluffy, porous cluster structure, assembled from sheet-like or fibrous sub-units, with an overall diameter of 500 nm to 2 μm for the particle cluster and a thickness of 10 to 20 nm for each individual sub-structure.
10. The application of the Mn-based catalyst prepared by the preparation method according to any one of claims 1 to 7 for the catalytic oxidation of formaldehyde at room temperature.