An XGd y Mn 1-y / CeO2@Al2O3 catalyst, its preparation method and application

By preparing a XGdyMn1-y/CeO2@Al2O3 catalyst with strong metal-support interaction (SMSI) and oxygen-rich vacancies, the problems of low activity and poor stability of existing catalysts in the simultaneous removal of Hg0 and VOCs from flue gas were solved, and a highly efficient and stable synergistic oxidation effect was achieved.

CN123102344APending Publication Date: 2026-11-17NANHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611601084.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing catalysts suffer from low activity and poor stability when simultaneously removing elemental mercury (HgO) and volatile organic compounds (VOCs) from flue gas, and are unable to achieve efficient synergistic oxidation, especially when they are difficult to adapt to the flue gas temperature conditions in non-power industries.

Method used

The XGdyMn1-y/CeO2@Al2O3 catalyst with strong metal-support interaction (SMSI) and oxygen-rich vacancies is used. By uniformly encapsulating Al2O3 with CeO2 to form a heterogeneous interface, GdMn active components are loaded, inducing the SMSI effect, regulating the electronic structure and the number of oxygen vacancies, and improving catalytic activity and stability.

Benefits of technology

It significantly improves the simultaneous oxidation efficiency of Hg0 and VOCs, enhances the thermal stability and sulfur and water resistance of the catalyst, adapts to flue gas conditions in non-power industries, and extends the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102344A_ABST
    Figure CN123102344A_ABST
Patent Text Reader

Abstract

This application provides an XGd y Mn 1‑y / CeO2@Al2O3 catalyst, its preparation method and application, wherein the catalyst exhibits strong metal-support interaction (SMSI) and oxygen-rich vacancies, with an adsorbed oxygen concentration of up to 55.43%, Mn 4+ / (Mn 4+ +Mn 3+ +Mn 2+ )=38.5%, Ce 3+ / (Ce 4+ +Ce 3+ =50.26%. In this invention, CeO2 encapsulates Al2O3 to form a heterostructure interface. Due to lattice mismatch and electronic interactions, a large number of intrinsic oxygen vacancies are spontaneously generated. This, combined with rare-earth Gd doping, further increases the number of oxygen vacancies. The SMSI and heterostructure interface effectively regulate the electronic structure of the active metal, promoting Mn... 2+ / Mn 3+ / Mn 4+ Ce 3+ / Ce 4+ Cyclic conversion and electron migration enhance its catalytic oxidation ability, thus exhibiting outstanding synergistic catalytic removal of Hg. 0 and VOCs performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of environmental catalytic materials and air pollutant purification technology, and in particular to an oxygen-rich vacancy XGd based on strong metal-support interaction. y Mn 1-y / CeO2@Al2O3 catalyst, its preparation method and application. Background Technology

[0002] Waste gases emitted from non-power industries such as steel sintering, cement production, coking, and municipal waste incineration typically contain both heavy metal mercury (Hg) and volatile organic compounds (VOCs), two typical types of air pollutants. This differs from ionic mercury (Hg) emissions. 2+ ) and particulate mercury (Hg P ) can be removed by wet desulfurization units and bag / electrostatic precipitators widely installed in enterprises, respectively, elemental mercury (Hg) 0 Highly volatile, poorly water-soluble, and highly mobile, these pollutants are difficult to remove using conventional dust removal, desulfurization, and denitrification equipment, exhibiting persistent biotoxicity and atmospheric accumulation. Typical aromatic VOCs such as benzene, toluene, and xylene are among the most abundant organic compounds in industrial flue gas, possessing carcinogenic, teratogenic, and highly chemically reactive properties. Currently, activated carbon injection is a mature and reliable method for controlling Hg. 0 Catalytic oxidation is a promising technology for VOCs treatment; however, this method, which separately controls Hg... 0 Traditional VOCs treatment processes suffer from problems such as large equipment footprint, high operating costs, and poor process coupling. Catalytic oxidation, with the aid of a suitable catalyst, can not only degrade VOCs into CO2 and H2O, but also remove Hg... 0 Oxidized into Hg, which is easily captured by wet desulfurization units. 2+ Therefore, the development of a method for the simultaneous and efficient catalytic oxidation of Hg is needed. 0 Catalysts for VOCs are currently a research hotspot and a technical challenge in air pollution control.

[0003] Currently widely used for the catalytic oxidation of Hg 0 VOCs catalysts mainly include transition / rare earth metal oxide (TRC) catalysts such as vanadium-based, manganese-based, and cerium-based catalysts. Although commercially available vanadium-based denitration catalysts (V₂O₅-WO₃(MoO₃) / TiO₂) have been shown to catalyze the oxidation of Hg... 0 It has the ability to reduce VOCs. However, its reducing ability is strong while its oxidizing ability is insufficient, leading to Hg... 0Furthermore, VOCs cannot be completely oxidized, causing secondary pollution. In addition, vanadium-based catalysts, suitable for medium to high temperatures, have a narrow active temperature window (300~400℃), far exceeding the flue gas temperature in non-electric industries (120~280℃). Heating flue gas inevitably increases costs, energy consumption, and carbon emissions, making it difficult to meet the needs of pollution reduction and carbon reduction. Manganese-based catalysts possess excellent redox properties and good low-temperature catalytic activity, and are widely used for the catalytic oxidation of Hg. 0 The research field includes VOCs. However, single-manganese-based catalysts suffer from defects such as active site aggregation, insufficient oxygen vacancies, poor high-temperature stability, and weak resistance to sulfur and water. Cerium dioxide (CeO2) has a unique oxygen storage and release capacity and is a typical rare earth oxide that easily generates oxygen vacancies. 3+ / Ce 4+ Valence state cycling constructs oxygen vacancy active sites, but its use alone suffers from problems such as small specific surface area, easy aggregation of active components, and low mechanical strength. Studies have shown that RTC catalyzes the oxidation of Hg. 0 VOCs performance and its oxygen vacancies (O2) v The concentration of reactive oxygen species (ROS) is closely related to the concentration of reactive oxygen species (ROS) and is influenced by their physicochemical properties, such as morphology, crystal facets, crystal form, acidity / basicity, and redox properties. v It can capture and activate gaseous oxygen and promote the migration of lattice oxygen, while surface-active oxygen can not only act as Hg 0 The active sites for VOC oxidation can also promote the deep oxidation of chlorine-containing VOCs and reduce chlorine poisoning caused by chlorine species deposition. Heteroatom doping has been shown to increase the O content of TRC. v Controlling the concentration of active oxygen is a simple yet effective way to solve the problems of pure manganese-based and cerium-based catalysts. Compared to the active component, the support is equally important. Unsupported catalysts lacking a support are often uneconomical for large-scale industrial applications due to their small specific surface area and high cost. Alumina (Al2O3), as a commonly used support, has advantages such as large specific surface area, well-developed pore structure, and high mechanical strength. It can serve as a rigid supporting framework, effectively preventing framework collapse and pulverization during high-temperature reactions, and is suitable for the high space velocity and complex operating conditions of industrial flue gas. Pure Al2O3 has strong surface inertness and weak anchoring ability for metal active components. Active components are prone to migration, aggregation, and detachment during high-temperature and long-term operation, leading to rapid catalyst deactivation. Furthermore, many supported catalysts have weak interfacial interactions between the metal active component and the support, poor dispersion of metal active sites, and an inability to form a stable active interface structure. The controllability of oxygen vacancy numbers is poor, making it difficult to simultaneously improve Hg oxidation efficiency and VOCs degradation efficiency, resulting in insufficient catalytic activity at low temperatures and severe deactivation during long-term operation. These shortcomings greatly limit the industrial application of the integrated technology for simultaneous mercury removal and VOCs degradation. Summary of the Invention

[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a strong metal-support interaction (SMSI) and oxygen-vacancy-rich XGd y Mn 1-y A method for preparing a / CeO2@Al2O3 catalyst, which can synergistically catalyze the oxidation of VOCs and Hg. 0 The Hg is harmless CO2 and H2O, and facilitates subsequent wet flue gas desulfurization slurry treatment. 2+ .

[0005] Specifically, the first aspect of this application provides an XGd y Mn 1-y / CeO2@Al2O3 catalyst, XGd y Mn 1-y In the / CeO2@Al2O3 catalyst, X is 5%~20% and y is 0.1~0.9, where X is the mass fraction of Gd and Mn in the catalyst and y:(1-y) is the molar ratio of Gd:Mn.

[0006] Furthermore, XGd y Mn 1-y / CeO2@Al2O3 catalyst, adsorbed oxygen accounts for >40% of all oxygen species, which is the sum of chemically and physically adsorbed oxygen. In addition to adsorbed oxygen, all oxygen species include lattice oxygen and oxygen species derived from adsorbed water and hydroxyl groups. Mn 4+ / (Mn 4+ +Mn 3+ +Mn 2+ >30%, Ce 3+ / (Ce 3+ +Ce 4+ >40%.

[0007] A second aspect of this application provides an XGd y Mn 1-y The preparation method of / CeO2@Al2O3 catalyst includes the following steps: S1: Dissolve an appropriate amount of cerium-containing compound to form a CeO2 precursor solution, then impregnate a certain amount of active Al2O3 in the above solution, sonicate, continue to impregnate at room temperature for a preset time, and then place in a drying oven to dry to constant weight to obtain the dried modified carrier material. S2: The dried modified support material is calcined at high temperature to obtain CeO2-encapsulated Al2O3 support, labeled as CeO2@Al2O3; S3: Dissolve an appropriate amount of manganese-containing compound and gadolinium-containing compound to form a manganese and gadolinium precursor solution. Weigh a certain amount of CeO2@Al2O3 and immerse it in the manganese and gadolinium precursor solution. After ultrasonic treatment, continue to immerse at room temperature for a preset time. Then place it in a drying oven to dry to constant weight to obtain manganese and gadolinium solids. S4: The manganese and gadolinium solids are calcined at high temperature to obtain a manganese and gadolinium-modified CeO2@Al2O3 catalytic material, labeled as XGd. y Mn 1-y / CeO2@Al2O3.

[0008] Further, the cerium-containing compound in step S1 is cerium nitrate hexahydrate (Ce(NO3)3·6H2O), the dissolution is in water, the ultrasonic treatment time is 0.5~4h, the immersion time is 12h~36h, and the drying temperature is 80~110℃.

[0009] Further, the calcination temperature in step S2 is 400~600℃, and / or the heating rate of the calcination is 3~8℃ / min, and / or the calcination time is 4~6h.

[0010] Further, in step S3, the manganese-containing compound is manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O), the gadolinium-containing compound is gadolinium nitrate hexahydrate (Gd(NO3)3·6H2O), the dissolution is in water, the ultrasonic treatment time is 0.5~4h, the immersion time is 12h~36h, and the drying temperature is 80~110℃.

[0011] Furthermore, in step S4, the calcination temperature is 400-600℃, and / or the calcination heating rate is 3-8℃ / min, and / or the calcination time is 4-8h.

[0012] A third aspect of this application provides the XGd described above. y Mn 1-y / CeO2@Al2O3 catalyst for Hg removal in flue gas 0 Applications in VOCs.

[0013] Furthermore, XGd y Mn 1-y / CeO2@Al2O3 catalyst for catalytic removal of Hg in flue gas 0 The reaction temperature with VOCs is 40-400℃.

[0014] The present invention has the following beneficial effects: (1) This invention is based on the characteristics of Al2O3 substrate, which has well-developed pore structure, large specific surface area, high mechanical strength and excellent thermal stability. However, if the metal active component is directly loaded on the surface of inert Al2O3, the interface between the metal and the support is extremely weak, the anchoring ability of the metal component is weak, and the active component is prone to migration, agglomeration and detachment during high temperature and long-term operation, resulting in rapid deactivation of the catalyst. By uniformly coating CeO2 on the outer layer of Al2O3, the high specific surface area advantage of Al2O3 support is fully preserved, the diffusion and mass transfer capacity of reactants and products are improved, and sufficient attachment sites are provided for Gd and Mn bimetallic active components. It can also solve the inherent defects of pure CeO2 material, such as small specific surface area, easy agglomeration of grains and poor mechanical properties. More importantly, the CeO2 coating itself has a dual identity as a "support and active component". It can serve as a functional transition interface between the support and the active metal, inducing a high-intensity SMSI effect during the preparation of catalyst materials. This effectively anchors the active metal particles, restricts grain growth and agglomeration, enhances the dispersion uniformity of the active metal component, and significantly improves the stability of catalyst recycling and industrial operation.

[0015] (2) This invention is based on uniformly coating Al2O3 with CeO2, which is prone to oxygen defects, and then simultaneously loading GdMn bimetallic active components. This process forms numerous heterostructures, which not only spontaneously generate a large number of intrinsic oxygen vacancies due to lattice mismatch and electronic interactions, but also synergistically enhance the number of oxygen vacancies through Gd rare earth doping modification. Furthermore, these heterostructures can effectively regulate the electronic structure of the metal active components, promoting the growth of Mn... 2+ / Mn 3+ / Mn 4+ Ce 3+ / Ce 4+ Improve its redox performance by enhancing valence state cycling and electron transfer rates, and matching Hg. 0 The need for simultaneous oxidation of two pollutants, VOCs and VOCs.

[0016] (3) The present invention XGd y Mn 1-y The / CeO2@Al2O3 catalyst can provide multiple catalytic sites through the synergistic effect of Gd-Mn-Ce, reducing the impact of Hg. 0 The simultaneous catalytic oxidation of VOCs and the competition for active sites lead to a decrease in catalytic activity. By preferentially interacting with impurities such as SO2 and water vapor in flue gas using rare earth metals Ce and Gd, an interfacial protective effect is formed, enhancing the catalyst's thermal stability, resistance to sulfur, water, and poisoning, thus improving its industrial application potential. Furthermore, this invention employs heteroatomic Gd-doped MnO. xThe defect engineering strategy involves the mutual doping and hybridization of different atomic orbitals, which induces lattice distortion, aberration, and charge imbalance in metals, generating a large number of lattice defects, oxygen vacancies, and active sites. This enhances the electron migration ability between different atoms and their different valence states, increases the quantity and mobility of surface active oxygen, and strengthens its catalytic oxidation activity, thereby benefiting VOCs and Hg. 0 Thorough degradation and deep oxidation under low-temperature conditions. This invention, through material composition design and interface structure control, aims to develop materials suitable for the complete degradation and deep oxidation of Hg in non-power industry flue gas. 0 The novel, economical, and efficient catalytic materials that synergistically catalyze the oxidation and removal of VOCs provide new ideas and directions. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of these drawings. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0018] Figure 1 The catalysts in Examples 1-7 for Hg 0 The catalytic removal performance results; Figure 2 The results show the catalytic removal performance of the catalysts in Examples 1-7 for toluene. Figure 3 The catalysts in Example 1 and Comparative Examples 1-2 and 7 synergistically catalyze the removal of Hg. 0 Performance results with toluene; Figure 4 The catalysts in Example 1 and Comparative Examples 3-6 for Hg 0 The catalytic removal performance results; Figure 5 The results show the catalytic removal performance of the catalysts in Example 1 and Comparative Examples 3-6 for toluene. Figure 6 The catalyst in Example 1 is used for the synergistic catalytic removal of Hg. 0 Results on toluene recycling performance; Figure 7 The catalyst in Example 1 is used for the synergistic catalytic removal of Hg. 0 And the stability test results of toluene; Figure 8 X-ray photoelectron spectra of the catalysts in Example 1 and Comparative Examples 1-2 Figure 1 (O 1s); Figure 9 X-ray photoelectron spectra of the catalysts in Example 1 and Comparative Example 1 Figure 2 (Mn 2p); Figure 10 X-ray photoelectron spectra of the catalysts in Example 1 and Comparative Examples 1-2 Figure 3 (Ce 3d); Figure 11 X-ray photoelectron spectra of the catalysts in Example 1 and Comparative Example 2 Figure 4 (Gd 4d); Figure 12 X-ray photoelectron spectroscopy of the catalyst in Example 1 Figure 5 (Hg 4f).

[0019] The purpose, features, and advantages of this accompanying drawing will be further explained in conjunction with the embodiments and with reference to the accompanying drawing. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of this application clearer, the following description and illustration are provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application. All other embodiments obtained by those skilled in the art based on the embodiments provided in this application without inventive effort are within the scope of protection of this application.

[0021] Obviously, the following description is merely some examples or embodiments of this application. Those skilled in the art can apply this application to other similar scenarios without any inventive effort. Furthermore, it is understood that although the effort involved in such development may be complex and lengthy, for those skilled in the art related to the content disclosed in this application, any changes to design, manufacturing, or production based on the technical content disclosed in this application are merely conventional technical means and should not be construed as insufficient disclosure of the content of this application.

[0022] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0023] To address the shortcomings of existing technologies, this invention prepares XGd with strong metal-support interaction (SMSI) and oxygen-rich vacancies. y Mn 1-y / CeO2@Al2O3 catalyst. Utilizing CeO2 to encapsulate modified Al2O3 (CeO2@Al2O3) not only fully leverages the unique oxygen storage and release properties and strong redox characteristics of CeO2, but also combines with the large specific surface area and high mechanical strength of Al2O3. It cleverly avoids the problems of small specific surface area, easy agglomeration of active components, and low mechanical strength of pure CeO2, as well as the drawbacks of strong surface inertness and extremely weak metal-support interface of pure Al2O3, making it difficult to induce electron transfer and structural modification. Subsequently, GdMn active components are simultaneously loaded onto CeO2@Al2O3. CeO2 plays a dual role as both a support and active component. The CeO2 intermediate encapsulation layer serves as a functional transition interface, connecting the Al2O3 substrate and the GdMn bimetallic active component, inducing high-strength metal-support interaction (SMSI), which can firmly anchor metal nanoparticles and inhibit their sintering. This heterogeneous interface can effectively regulate the electronic structure of the metal active component, promoting Mn... 2+ / Mn 3+ / Mn 4+ Ce 3+ / Ce 4+ Valence state cycling provides a core active interface for the efficient catalytic oxidation of the catalyst, which is the key structural guarantee for improving the catalytic activity of the catalyst in this invention. CeO2 has unique oxygen storage and release characteristics and is a typical rare earth oxide that easily generates oxygen vacancies. The heterostructure formed by CeO2 uniformly encapsulating Al2O3 will spontaneously generate a large number of intrinsic oxygen vacancies due to lattice mismatch and electronic interactions. At the same time, it can be synergistically modified by Gd rare earth doping to further controllably increase the number of oxygen vacancies. The abundant oxygen vacancies can be used as Hg 0 Adsorption active sites and VOCs oxidation reaction active centers continuously oxidize oxygen in flue gas to generate reactive oxygen species, significantly increasing Hg. 0 Oxidation efficiency and deep VOCs mineralization capability, adapted to Hg 0 This invention addresses the need for simultaneous oxidation of two pollutants, VOCs and Hg. It overcomes the limitations of traditional catalysts, which suffer from low activity, poor stability, and inability to simultaneously and efficiently oxidize Hg. 0 XGd addresses the technical challenges of VOCs. y Mn 1-y / CeO2@Al2O3 exhibits the SMSI effect and abundant oxygen vacancies, which not only increases the Hg in flue gas 0 The high efficiency of simultaneous catalytic oxidation with VOCs can also improve the thermal stability, sulfur and water resistance, and recycling performance of the catalyst, which has important engineering application value.

[0024] An embodiment of the first aspect of the present invention provides a strong metal-support interaction (SMSI) and oxygen-rich vacancy XGd y Mn 1-yIn the / CeO2@Al2O3 catalyst, X represents 5%–20%, and y represents 0.1–0.9%. X is the mass fraction of Gd and Mn in the catalyst, and y:(1-y) is the molar ratio of Gd to Mn. The catalyst exhibits SMSI and is rich in oxygen vacancies. Its adsorbed oxygen concentration accounts for >40% of the total oxygen species concentration (a key indicator for assessing oxygen vacancy concentration). Adsorbed oxygen is the sum of chemically and physically adsorbed oxygen. All oxygen species include lattice oxygen and oxygen species derived from adsorbed water and hydroxyl groups. Mn... 4+ / (Mn 4+ +Mn 3+ +Mn 2+ >30%, Ce 3+ / (Ce 4+ +Ce 3+ >40%.

[0025] Preferred, 15% Gd 0.66 Mn 0.33 / CeO2@Al2O3 catalyst , The catalyst exhibits SMSI and oxygen-rich vacancy distribution, with an adsorbed oxygen concentration of 55.43% (a key indicator for assessing oxygen vacancy concentration). Mn 4+ / (Mn 4+ +Mn 3+ +Mn 2+ )=38.57%, Ce 3+ / (Ce 4+ +Ce 3+ =50.26%.

[0026] The XGdyMn1-y / CeO2@Al2O3 catalyst, with its strong metal-support interaction (SMSI) and oxygen-vacancy-rich structure, utilizes a CeO2 interlayer as a functional transition interface to induce strong metal-support interaction (SMSI). This effectively modulates the electronic structure of the anchored metal active component, promoting the growth of Mn. 2+ / Mn 3+ / Mn 4+ Ce 3+ / Ce 4+ Valence state cycling and electron transfer rate enhance catalytic activity and catalyst stability at high temperatures and over long periods. The presence of oxygen-rich vacancies, with CeO2 uniformly coating Al2O3 to form a heterogeneous interface, leads to the spontaneous generation of numerous intrinsic oxygen vacancies due to lattice mismatch and electronic interactions. Simultaneously, synergistic modification with Gd rare earth doping further amplifies the oxygen vacancy concentration, resulting in an adsorbed oxygen content of up to 55.43% of all oxygen species.

[0027] A second aspect of the present invention provides an XGd y Mn 1-yThe preparation method of / CeO2@Al2O3 includes the following steps: S1: Dissolve an appropriate amount of cerium-containing compound to form a CeO2 precursor solution, then impregnate a certain amount of active Al2O3 in the above solution, sonicate, continue to impregnate at room temperature for a preset time, and then place in a drying oven to dry to constant weight to obtain the dried modified carrier material. S2: The dried modified support material is calcined at high temperature to obtain CeO2-encapsulated Al2O3 support, labeled as CeO2@Al2O3; S3: Dissolve an appropriate amount of manganese-containing compound and gadolinium-containing compound to form a mixed solution of manganese and gadolinium precursors. Weigh a certain amount of CeO2@Al2O3 and immerse it in the mixed solution of manganese and gadolinium precursors. After ultrasonic treatment, continue to immerse at room temperature for a preset time. Then place it in a drying oven to dry to constant weight to obtain manganese and gadolinium solids. S4: The manganese and gadolinium solids are calcined at high temperature to obtain a manganese and gadolinium-modified CeO2@Al2O3 catalytic material, labeled as XGd. y Mn 1-y / CeO2@Al2O3.

[0028] This invention utilizes CeO2 to uniformly coat Al2O3 to form a CeO2@Al2O3 heterointerface, and then loads GdMn active components onto it to prepare XGd with SMSI and oxygen-rich vacancies. y Mn 1-y The / CeO2@Al2O3 catalyst, where y:(1-y) represents the Gd:Mn molar ratio and X represents the mass percentage of Gd and Mn active metal components in the catalyst. If the active metal components are directly loaded onto the inert Al2O3 surface, it is difficult to induce electron transfer and structural changes. The metal-support interaction is extremely weak, resulting in poor anchoring ability of the active metal. The active components are prone to migration, aggregation, and detachment during high-temperature, long-term operation, leading to rapid catalyst deactivation. In contrast, the CeO2 intermediate coating layer of this invention plays a dual role as both a support and active component. It serves as a functional transition interface, precisely connecting the Al2O3 substrate and the dual active components of Gd and Mn. Under high-temperature calcination, it induces a high-intensity SMSI effect, effectively anchoring active metal particles, limiting grain growth and aggregation, and significantly improving the dispersion uniformity of the metal active components. This SMSI effect can also effectively regulate the electronic structure of the metal active components, promoting Mn... 2+ / Mn 3+ / Mn 4+ Ce 3+ / Ce 4+Valence state cycling and electron transfer rates enhance its redox properties; CeO2 possesses unique oxygen storage and release characteristics and is a typical rare earth oxide prone to oxygen vacancies. Under the SMSI effect, heterojunctions spontaneously generate a large number of intrinsic oxygen vacancies due to lattice mismatch and electronic interactions. Simultaneously, synergistic Gd rare earth doping further controllably amplifies the number of oxygen vacancies, significantly increasing Hg... 0 Oxidation efficiency and deep VOCs mineralization capability, adapted to Hg 0 The need for simultaneous oxidation of two pollutants, VOCs and VOCs.

[0029] In this embodiment, the cerium-containing compound in step S1 is cerium nitrate hexahydrate (Ce(NO3)3·6H2O), the dissolution is in water, the ultrasonic treatment time is 0.5~4h, the immersion time is 12~36h, and the drying temperature is 80~110℃.

[0030] Specifically, take a beaker, add an appropriate amount of deionized water, then weigh an appropriate amount of cerium nitrate hexahydrate (Ce(NO3)3·6H2O) using an analytical balance and put it into the aforementioned beaker. Stir thoroughly until the drug is completely dissolved to form a homogeneous solution of y mmol cerium nitrate. Sonicate the solution for 0.5~4h (preferably 2h), then impregnate it at room temperature for 12~36h (preferably 24h), and finally dry it in a drying oven at 80~110℃ (preferably 105℃) to constant weight to obtain the modified carrier material.

[0031] In this embodiment, the calcination temperature of the modified carrier material in step S2 is 400~600℃, the calcination heating rate is 3~8℃ / min, and the calcination time is 4~6h.

[0032] Specifically, the dried modified carrier material is transferred into a crucible, and then the crucible is placed in a programmed temperature tube furnace. The temperature is increased to 400-600℃ (preferably 500℃) at a heating rate of 3-8℃ / min (preferably 5℃ / min). After calcining at this temperature for 4-6 hours (preferably 5 hours), heating is stopped, and the material is cooled to room temperature to obtain the CeO2@Al2O3 modified carrier.

[0033] In this embodiment, the manganese-containing compound in step S3 is manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O), the gadolinium-containing compound is gadolinium nitrate hexahydrate (Gd(NO3)3·6H2O), the dissolution is in water, the ultrasonic treatment time is 0.5~4h, the impregnation time is 12~36h, and the drying temperature is 80~110℃.

[0034] Specifically, take a beaker, add an appropriate amount of deionized water, and then weigh an appropriate amount of gadolinium nitrate hexahydrate and manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) using an analytical balance and put them into the aforementioned beaker. Stir thoroughly until the drugs are completely dissolved to form a homogeneous solution of y mmol gadolinium nitrate and (1-y) mmol manganese acetate. Sonicate for 0.5~4h (preferably 2h), and after sonication, place at room temperature for 12~36h (preferably 24h) to soak. After soaking, place in a drying oven at 80~110℃ (preferably 105℃) to dry to constant weight to obtain manganese and gadolinium solids.

[0035] In this embodiment, the calcination temperature of the manganese and gadolinium solids in step S4 is 400~600℃, the calcination heating rate is 3~8℃ / min, and the calcination time is 4~6h.

[0036] Specifically, the dried manganese and gadolinium solids are transferred to a crucible, and then to a tube furnace for programmed temperature-controlled heat treatment. Gradient heating is performed at a constant heating rate of 3-8°C / min (preferably 5°C / min) in a flowing air atmosphere. Once the system temperature reaches the preset calcination temperature of 400-600°C (preferably 500°C), these thermodynamic conditions are maintained for 4-6 hours (preferably 5 hours), thus obtaining the manganese and gadolinium-modified CeO2@Al2O3 catalyst, named XGd. y Mn 1-y / CeO2@Al2O3.

[0037] An embodiment of the third aspect of this application provides the XGd y Mn 1-y / CeO2@Al2O3 catalyst for Hg removal in flue gas 0 Applications in VOCs.

[0038] The specific application is as follows: The above-mentioned catalyst (XGd) is loaded into a gas-solid reactor subjected to programmed temperature rise in a laboratory setting. y Mn 1-y / CeO2@Al2O3, etc.), at 150 ppm toluene, 150 μg / m 3 Hg 0 In the presence of a mixture of gases including (g), 6% O2, and 94% N2, toluene and Hg were catalytically oxidized respectively. 0 The process generates CO2 and H2O, as well as Hg, which is readily adsorbed by subsequent wet desulfurization units. 2+ .

[0039] Furthermore, XGd y Mn 1-y / CeO2@Al2O3 catalyst for catalytic removal of Hg in flue gas 0The reaction temperature with VOCs is 40-400℃.

[0040] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Constructing a heterogeneous interface to enhance the SMSI effect: Overcoming the strong inertness of the pure Al2O3 surface, the extremely weak metal-support interface interaction, and the weak anchoring ability of the active metal components, the active components are prone to migration, agglomeration, and detachment during high-temperature and long-term operation, leading to rapid catalyst deactivation. By uniformly coating Al2O3 with CeO2, CeO2 plays a dual role as "support + active component". The CeO2 coating layer serves as a functional transition interface, connecting the Al2O3 substrate and the GdMn bimetallic active components, inducing a high-intensity SMSI effect, effectively anchoring active metal particles, limiting grain growth and agglomeration, significantly improving the dispersibility of active components, and significantly improving the catalyst's cycle life and industrial operation stability. In addition, rare earth metals Ce and Gd can preferentially interact with impurities such as SO2 and water vapor in flue gas to form an interface protection effect, greatly improving the catalyst's resistance to sulfur, water, and poisoning, and solving the problem of poor operating conditions of pure manganese-based and cerium-based catalysts.

[0041] (2) Oxygen vacancy regulation: By uniformly coating Al2O3 with CeO2 to form a heterostructure interface, a large number of intrinsic oxygen vacancies will be spontaneously generated due to electronic interactions and lattice defects. At the same time, in conjunction with Gd rare earth doping modification, the number of oxygen vacancies will be further increased, providing more active sites for the activation of oxygen species and reactants, enhancing the number and mobility of reactive oxygen species, and improving Hg 0 Synergistic catalytic oxidation ability with VOCs; (3) Electronic structure optimization: The CeO2 intermediate coating layer is used as a functional transition interface to connect the Al2O3 substrate and the GdMn bimetallic active component, forming a large number of heterogeneous interfaces, effectively regulating the electronic structure of the metal active component, and promoting the Mn 2+ / Mn 3+ / Mn 4+ Ce 3+ / Ce 4+ Valence state cycling and electron transfer, together with Gd and Mn, enhance the electron transfer rate between different atoms and between different valence states of each atom through orbital hybridization, thereby enhancing the redox ability of the catalyst and improving its low-temperature catalytic oxidation activity.

[0042] (4) Reaction kinetic enhancement level: XGd y Mn 1-y The / CeO2@Al2O3 catalyst not only fully utilizes the advantages of the large specific surface area and well-developed pore structure of the Al2O3 substrate to promote the diffusion and mass transfer of reactants and products, but also exposes more types and quantities of active sites and reactive oxygen species, reducing Hg. 0The simultaneous catalytic oxidation of VOCs leads to reduced catalytic efficiency due to competition between active sites and reactive oxygen species. Abundant oxygen vacancies at heterojunctions promote the "generation-migration-consumption" cycle of reactive oxygen species, increasing their migration and conversion rates, lowering the catalytic reaction energy barrier, and enhancing their ability to catalyze Hg. 0 Synergistic catalytic oxidation performance with VOCs.

[0043] Example 1 A 15% Gd 0.66 Mn 0.33 The preparation method of / CeO2@Al2O3 catalyst includes the following steps: S1: Cerium nitrate hexahydrate was dissolved in water, and the concentration of Ce in the solution was 6.6 mmol / L. Then, a certain amount of active Al2O3 (weighed according to the calculation results) was placed in the above solution, ultrasonically treated for 2 h, then impregnated at room temperature for 24 h, and finally dried in a drying oven at 105℃ to constant weight to obtain the dried modified carrier material.

[0044] S2: Place the dried modified carrier material in a programmed temperature tube furnace and heat it to 500°C at a heating rate of 5°C / min. Hold the temperature for 5 hours, then stop heating and cool it to room temperature for later use to obtain CeO2@Al2O3.

[0045] S3: Take a beaker, add an appropriate amount of deionized water, and then use an analytical balance to weigh gadolinium hexahydrate and manganese acetate tetrahydrate and dissolve them in the beaker to form a homogeneous solution. The concentrations of Gd and Mn in the solution are 6.6 mmol / L and 3.3 mmol / L, respectively. Weigh a certain amount of CeO2@Al2O3 (weighed according to the calculation results) and immerse it in the manganese and gadolinium precursor solution. After sonication for 2 hours, it is then immersed at room temperature for 24 hours. Finally, it is dried in a drying oven at 105℃ to constant weight to obtain manganese and gadolinium solids.

[0046] S4: Manganese and gadolinium solids were calcined at a heating rate of 5℃ / min, a calcination temperature of 500℃, and a calcination time of 5h to obtain 15% Gd. 0.66 Mn 0.33 / CeO2@Al2O3.

[0047] Example 2 This embodiment is basically the same as Example 1, except that the Gd:Mn ratio in the homogeneous solution of gadolinium and manganese precursor is 0.1:0.9, and the prepared product is 15% Gd. 0.1 Mn 0.9 / CeO2@Al2O3.

[0048] Example 3 This embodiment is basically the same as Example 1, except that the Gd:Mn ratio in the homogeneous solution of gadolinium and manganese precursor is 0.25:0.75, and the prepared product is 15% Gd. 0.25 Mn 0.75 / CeO2@Al2O3.

[0049] Example 4 This embodiment is basically the same as Example 1, except that the Gd:Mn ratio in the homogeneous solution of gadolinium and manganese precursor is 0.33:0.66, and the prepared product is 15% Gd. 0.33 Mn 0.66 / CeO2@Al2O3.

[0050] Example 5 This embodiment is basically the same as Example 1, except that the Gd:Mn ratio in the homogeneous solution of gadolinium and manganese precursor is 0.5:0.5, and the prepared product is 15% Gd. 0.5 Mn 0.5 / CeO2@Al2O3.

[0051] Example 6 This embodiment is basically the same as Example 1, except that the Gd:Mn ratio in the homogeneous solution of gadolinium and manganese precursor is 0.75:0.25, and the prepared product is 15% Gd. 0.75 Mn 0.25 / CeO2@Al2O3.

[0052] Example 7 This embodiment is basically the same as Example 1, except that the Gd:Mn ratio in the homogeneous solution of gadolinium and manganese precursor is 0.9:0.1, and the prepared product is 15% Gd. 0.9 Mn 0.1 / CeO2@Al2O3.

[0053] The molar ratios of the components in the precursor mixture solutions of Examples 1-7 are shown in Table 1.

[0054]

[0055] Comparative Example 1 This comparative example is basically the same as Example 1, except that in step S3: manganese acetate tetrahydrate is weighed using an analytical balance and dissolved in the above beaker to form a homogeneous solution, that is, the raw material does not contain Gd, and the product obtained is 15%Mn / CeO2@Al2O3.

[0056] Comparative Example 2 This comparative example is basically the same as Example 1, except that in S3: gadolinium nitrate hexahydrate was weighed using an analytical balance and dissolved in the above beaker to form a homogeneous solution. That is, the raw material does not contain Mn, and the product obtained is 15% Gd / CeO2@Al2O3.

[0057] Comparative Example 3 This comparative example is basically the same as Example 1, except that in S3: gadolinium nitrate hexahydrate and manganese acetate tetrahydrate are weighed using an analytical balance and dissolved in the above beaker to form a homogeneous solution, wherein the mass fraction of Gd and Mn in the homogeneous solution is 5%. That is, the mass fraction of Gd and Mn in the raw materials is 5%, and the product obtained is 5% Gd. 0.66 Mn 0.33 / CeO2@Al2O3.

[0058] Comparative Example 4 This comparative example is basically the same as Example 1, except that in S3: gadolinium nitrate hexahydrate and manganese acetate tetrahydrate are weighed using an analytical balance and dissolved in the above beaker to form a homogeneous solution, wherein the mass fraction of Gd and Mn in the homogeneous solution is 10%. That is, the mass fraction of Gd and Mn in the raw materials is 10%, and the product obtained is 10% Gd. 0.66 Mn 0.33 / CeO2@Al2O3.

[0059] Comparative Example 5 This comparative example is basically the same as Example 1, except that in S3: gadolinium nitrate hexahydrate and manganese acetate tetrahydrate are weighed using an analytical balance and dissolved in the above beaker to form a homogeneous solution, wherein the mass fraction of Gd and Mn in the homogeneous solution is 12%. That is, the mass fraction of Gd and Mn in the raw materials is 12%, and the product obtained is 12% Gd. 0.66 Mn 0.33 / CeO2@Al2O3.

[0060] Comparative Example 6 This comparative example is basically the same as Example 1, except that in S3: gadolinium nitrate hexahydrate and manganese acetate tetrahydrate are weighed using an analytical balance and dissolved in the above beaker to form a homogeneous solution, wherein the mass fraction of Gd and Mn in the homogeneous solution is 17%. That is, the mass fraction of Gd and Mn in the raw materials is 17%, and the product obtained is 17% Gd. 0.66 Mn 0.33 / CeO2@Al2O3.

[0061] Comparative Example 7 This comparative example is largely the same as Example 1, except that Gd, Mn, and Ce are directly impregnated onto active Al2O3, with a Gd:Mn:Ce ratio of 0.4:0.2:0.4, resulting in a product containing 15% Gd.0.4 Mn 0.2 Ce 0.4 / Al2O3.

[0062] Test Case 1 Using 0.10g of 15% Gd from Examples 1-7 0.66 Mn 0.33 / CeO2@Al2O3、15%Gd 0.1 Mn 0.9 / CeO2@Al2O3、15%Gd 0.25 Mn 0.75 / CeO2@Al2O3、15%Gd 0.33 Mn 0.66 / CeO2@Al2O3、15%Gd 0.5 Mn 0.5 / CeO2@Al2O3、15%Gd 0.75 Mn 0.25 / CeO2@Al2O3、15%Gd 0.9 Mn 0.1 Using / CeO2@Al2O3 as the experimental subject, within a temperature range of 40-400°C, a normal simulated flue gas atmosphere (SFG) included 150 ppm toluene and 150 μg / m³. 3 Hg 0 (g), 6% O2, 94% N2, were used to test its catalytic removal of Hg. 0 The properties of toluene are as follows: Figure 1-2 As shown.

[0063] from Figure 1 It can be seen that the reaction temperature has a significant effect on the removal of Hg from all samples. 0 The performance trend is consistent. Under low-temperature conditions, the removal of Hg decreases with increasing reaction temperature. 0 The efficiency is thus improved, achieving good Hg removal at 160~280℃. 0 The effect is that as the reaction temperature continues to increase, Hg removal... 0 The performance gradually declined. Overall, the 15% Gd in Example 1... 0.66 Mn 0.33 / CeO2@Al2O3 exhibits optimal Hg removal. 0 Performance, achieving 99.6% Hg at 280℃. 0 Removal rate.

[0064] from Figure 2It can be seen that the effect of reaction temperature on the toluene removal performance of all samples shows a consistent trend. At low temperatures of 40–80°C, all samples exhibited poor toluene removal performance. Between 120–240°C, the toluene removal efficiency increased with increasing reaction temperature, and the samples showed good toluene removal performance between 240–400°C. Overall, the 15% Gd in Example 1… 0.66 Mn 0.33 / CeO2@Al2O3 exhibits the best toluene removal performance, achieving a toluene removal rate of 93.8% at 280℃.

[0065] Test Case 2 Using 0.1g of 15% Gd from Example 1 0.66 Mn 0.33 / CeO2@Al2O3 and comparative examples 1-2 and 7, containing 15% Mn / CeO2@Al2O3, 15% Gd / CeO2@Al2O3, and 15% Gd 0.4 Mn 0.2 Ce 0.4 Using Al2O3 as the experimental subject, within a temperature range of 40–400°C, a normal simulated flue gas atmosphere (SFG) included 150 ppm toluene and 150 μg / m³ of... 3 Hg 0 (g), 6% O2, 94% N2, were used to test their synergistic catalytic removal of Hg. 0 The properties of toluene are as follows: Figure 3 As shown.

[0066] from Figure 3 It can be seen that the reaction temperature has a significant effect on the catalytic removal of Hg from all samples. 0 Consistent with the trend in toluene performance, the catalytic removal performance increases with increasing reaction temperature at low temperatures, achieving good removal within a certain temperature range. However, in the high-temperature range (280~400℃), the catalytic removal performance of toluene shows slight fluctuations, while the catalytic removal performance of Hg... 0 Performance has decreased to some extent.

[0067] The general order of catalytic activity of these four catalysts is: 15% Gd 0.66 Mn 0.33 / CeO2@Al2O3 > 15%Gd 0.4 Mn 0.2 Ce 0.4 / Al2O3 > 15%Mn / CeO2@Al2O3 > 15%Gd / CeO2@Al2O3. The synergistic effect between Gd and Mn can well explain the 15% Gd content. 0.66 Mn 0.33 / CeO2@Al2O3 outperforms 15%Mn / CeO2@Al2O3 and 15%Gd / CeO2@Al2O3. 15%Gd 0.66 Mn 0.33 / CeO2@Al2O3 outperforms 15%Gd 0.4 Mn 0.2 Ce 0.4 / Al2O3 indicates that the catalytic removal of Hg by loading GdMn bimetallic active components after coating Al2O3 with CeO2 is better than that of samples directly loading GdMnCe trimetallic active components on Al2O3. 0 It exhibits better performance with toluene. This indicates that the CeO2 coating layer can leverage the dual advantages of "support + active component," inducing the SMSI effect, promoting electron transfer rates between different atoms and between different valence states, enhancing the catalyst's reducibility. The strong SMSI effect can promote the dispersion of metal oxides, inhibit their aggregation, and result in the catalyst possessing abundant oxygen vacancies, more lattice defects, and a higher active oxygen migration rate, thus exhibiting the best Hg performance. 0 The efficiency of synergistic catalytic oxidation removal with toluene.

[0068] Test Case 3 Using 0.1g of 15% Gd from Example 1 0.66 Mn 0.33 / CeO2@Al2O3 and 5% Gd in Comparative Examples 3-6 0.66 Mn 0.33 / CeO2@Al2O3、10%Gd 0.66 Mn 0.33 / CeO2@Al2O3、12%Gd 0.66 Mn 0.33 / CeO2@Al2O3、17%Gd 0.66 Mn 0.33 Using / CeO2@Al2O3 as the experimental subject, within a temperature range of 40–400°C, a normal simulated flue gas atmosphere (SFG) included 150 ppm toluene and 150 μg / m³. 3 Hg 0 (g), 6% O2, 94% N2, tested its catalytic removal of Hg 0 The properties of toluene are as follows: Figure 4-5 As shown.

[0069] from Figure 4and Figure 5 It can be seen that, under low loading conditions, increasing the loading helps to improve the catalytic removal of Hg by the catalyst. 0 Compared to toluene, the sample with a 15% loading exhibited the best catalytic removal of Hg. 0 The properties of toluene were observed, and subsequently, further increasing the loading actually led to the catalytic removal of Hg from the sample. 0 The performance of toluene decreases accordingly. This is because, at low loading levels, further increasing the loading allows for the loading of more metal-active components onto the support, providing more metal-active sites. However, at high loading levels, metal oxides aggregate and overlap, damaging the pore structure and thus reducing the number of exposed metal-active sites. 15% Gd 0.66 Mn 0.33 / CeO2@Al2O3 possesses the best physicochemical properties, achieving the best catalytic removal of Hg. 0 Properties of toluene.

[0070] Test Case 4 While maintaining a reaction temperature of 280℃, under a normal simulated flue gas atmosphere (SFG) including 150 ppm toluene and 150 μg / m³... 3 Hg 0 (g), 6% O2, 94% N2, tested with 15% Gd 0.66 Mn 0.33 / CeO2@Al2O3 catalytic removal of Hg 0 The recycling performance of toluene was as follows: Figure 6 As shown in the figure, the annotations are as follows: Run1, Run2, and Run3 correspond to the first, second, and third performance tests of the sample, respectively; EHg is the removal efficiency of mercury (Hg); Etoluene is the removal efficiency of toluene; and the removal efficiency of 15% Gd is calculated using SFG and SFG + 8% vol H2O(g) + 300 ppm SO2, respectively. 0.66 Mn 0.33 / CeO2@Al2O3 co-catalytic oxidation of Hg 0 The stability of the compound with toluene was tested. The test results are as follows: Figure 7 As shown, Figure 7 In this context, EHg represents the removal efficiency of mercury (Hg), and Etoluene represents the removal efficiency of toluene (toluene).

[0071] The simulated flue gas (SFG) included 150 ppm toluene, 150 μg / m3 Hg0(g), 6% O2, and 94% N2; The simulated flue gas (SFG + 8% H2O + 300ppm SO2) includes 150ppm toluene, 150μg / m3 Hg0(g), 6% O2, 94% N2, 8% H2O, and 300ppm SO2.

[0072] from Figure 6 It can be seen that under SFG conditions, 15% Gd 0.66 Mn 0.33 / CeO2@Al2O3 three-stage catalytic removal of Hg 0 The performance results were almost identical to those of toluene, with no significant decrease, indicating that 15% Gd 0.66 Mn 0.33 / CeO2@Al2O3 exhibits excellent recyclability. Compared to SFG conditions, adding 8% H2O + 300ppm SO2 results in a 15% reduction in Gd. 0.66 Mn 0.33 / CeO2@Al2O3 co-catalytic oxidation of Hg 0 Its performance with toluene showed a significant decrease, but its ability to remove Hg continuously for 36 hours remained unchanged. 0 Both efficiencies for Gd and toluene remained above 81.3% and 78%, respectively. 0.66 Mn 0.33 / CeO2@Al2O3 synergistically removes Hg under SFG + 8% H2O + 300ppm SO2 conditions 0 The performance degradation of toluene is a result of the synergistic inhibitory effect of water vapor and SO2. Water vapor has a significant inhibitory effect on 15% Gd... 0.66 Mn 0.33 / CeO2@Al2O3 co-catalytic oxidation of Hg 0 SO2 exhibits a slight inhibitory effect on the properties of toluene. Although the hydroxyl groups (-OH) generated by the dissociation of H2O can promote the oxidation reaction, this slight inhibitory effect may stem from the fact that the inhibitory effect caused by the competition between water vapor and reactants for active sites outweighs the promoting effect of the generated hydroxyl groups; SO2 has a slight inhibitory effect on 15% Gd. 0.66 Mn 0.33 / CeO2@Al2O3 co-catalytic oxidation of Hg 0 SO2 exhibits a certain inhibitory effect on the properties of toluene, possibly because SO2 not only reacts with Hg... 0 It competes with toluene for active sites and can also react with active metal oxides to produce metal sulfates or sulfites, leading to active site coverage, pore blockage, and a decrease in specific surface area, thus hindering its catalytic oxidation of Hg. 0 The performance of Gd is reduced, along with that of toluene. (15% Gd) 0.66Mn 0.33 / CeO2@Al2O3 still exhibits good synergistic catalytic oxidation of Hg in the presence of both SO2 and water vapor. 0 It exhibits good resistance to water and sulfur, and has potential for industrial applications.

[0073] Test Case 5 To investigate 15% Gd 0.66 Mn 0.33 The / CeO2@Al2O3 catalyst exhibits excellent synergistic catalytic oxidation of Hg. 0 The intrinsic mechanism of the properties of toluene, with 15% Gd before and after the reaction in Example 1. 0.66 Mn 0.33 / CeO2@Al2O3-fresh, 15%Gd 0.66 Mn 0.33 The / CeO2@Al2O3-used catalyst and the 15%Mn / CeO2@Al2O3 and 15%Gd / CeO2@Al2O3 catalysts in Comparative Examples 1-2 were used as experimental subjects, and their X-ray photoelectron spectroscopy (XPS) characterization was performed. The results are shown in the figure. Figure 8-12 .

[0074] Depend on Figure 8 It can be seen that 15%Mn / CeO2@Al2O3, 15%Gd / CeO2@Al2O3, and 15%Gd 0.66 Mn 0.33 / CeO2@Al2O3-fresh, 15%Gd 0.66 Mn 0.33 The adsorbed oxygen in / CeO2@Al2O3-used groups accounted for 45.08%, 27.19%, 55.43%, and 35.85% of all oxygen species, respectively, and 15% of Gd. 0.66 Mn 0.33 The relative proportion of adsorbed oxygen in / CeO2@Al2O3-fresh was significantly higher than that in other samples. Adsorbed oxygen is a key indicator for assessing oxygen vacancy concentration. The low-temperature catalytic activity of a catalyst is related to its adsorbed oxygen ratio because adsorbed oxygen is the most active oxygen species with a high mobility, which is beneficial for Hg. 0 Adsorption and activation of toluene. Therefore, 15% Gd 0.66 Mn 0.33 / CeO2@Al2O3 exhibits good low-temperature synergistic catalytic oxidation of Hg 0 Properties of toluene.

[0075] Depend on Figure 9 It can be seen that 15% Mn / CeO2@Al2O3 contains Mn 4+ / Mnn+ (Mn) n+ =Mn 4+ +Mn 3+ +Mn 2+ The percentage was 22.01%, and after Gd doping, it was 15% Gd. 0.66 Mn 0.33 / CeO2@Al2O3-fresh Mn 4+ / Mn n+ It rose to 38.57%, and 15% Gd after the reaction. 0.66 Mn 0.33 / CeO2@Al2O3-used Mn 4+ / Mn n+ It decreased to 28.45%. This indicates that the catalyst Mn content decreased after Gd doping. 4+ The increased content of Hg results in the highest concentration of oxygen vacancies, giving it superior redox properties. This facilitates the adsorption and activation of gaseous oxygen molecules, promoting synergistic catalytic oxidation of Hg. 0 And toluene. Figure 9 In the middle, note: O latt O represents lattice oxygen, Oads represents adsorbed oxygen, O H Represents oxygen species derived from adsorbed water and hydroxyl groups; O t =O latt +O ads +O H .

[0076] Depend on Figure 10 It can be seen that 15%Mn / CeO2@Al2O3, 15%Gd / CeO2@Al2O3, and 15%Gd 0.66 Mn 0.33 / CeO2@Al2O3-fresh, 15%Gd 0.66 Mn 0.33 / CeO2@Al2O3-used Ce 3+ / (Ce 3+ +Ce 4+ The values ​​were 15.26%, 20.94%, 50.26%, and 17.34%, respectively, with 15% Gd. 0.66 Mn 0.33 / CeO2@Al2O3-fresh Ce 3+ The proportion was significantly higher than that of other samples. 3+ It can induce unsaturated chemical coordination environments, generating more oxygen vacancies and promoting the adsorption and activation of gaseous oxygen, which helps to increase Hg. 0 And the catalytic oxidation efficiency of toluene.

[0077] Depend on Figure 11It can be seen that, compared to 15% Gd / CeO2@Al2O3, 15% Gd 0.66 Mn 0.33 The position and shape of the Gd 4d peak in / CeO2@Al2O3-fresh change, indicating a change in the environment after Gd doping with Mn. This is because Gd doping with Mn helps induce more oxygen vacancies in its lattice defects and increases the electron transfer rates of Mn and Ce in different valence states, promoting Hg... 0 Low-temperature catalytic oxidation performance of toluene.

[0078] Depend on Figure 12 It can be known that 15% Gd 0.66 Mn 0.33 The Hg 4f of / CeO2@Al2O3-used exhibits three peaks, located at 106.41, 104.53, and 101.77 eV. The peak at 106.41 eV is characteristic of HgO, indicating that some Hg... 0 During the reaction, it is catalytically oxidized to HgO and remains on the catalyst surface.

[0079] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. An XGd y Mn 1-y / CeO2@Al2O3 catalyst, characterized in that, The XGd y Mn 1-y In the XGd / CeO2@Al2O3 catalyst, X is 5% to 20%, y is 0.1 to 0.9, X is the mass fraction of Gd and Mn in the catalyst, and y:(1-y) is the molar ratio of Gd:Mn.

2. The XGd according to claim 1 y Mn 1-y / CeO2@Al2O3 catalyst, characterized in that, Adsorbed oxygen accounts for >40% of all oxygen species, which is the sum of chemically and physically adsorbed oxygen. Besides adsorbed oxygen, all oxygen species include lattice oxygen and oxygen species derived from adsorbed water and hydroxyl groups. Mn 4+ / (Mn 4+ +Mn 3+ +Mn 2+ >30%, Ce 3+ / (Ce 3+ +Ce 4+ >40%.

3. An XGd according to claim 1 or 2 y Mn 1-y The method for preparing the / CeO2@Al2O3 catalyst is characterized by, Includes the following steps: S1: Dissolve an appropriate amount of cerium-containing compound to form a CeO2 precursor solution, then impregnate a certain amount of active Al2O3 in the precursor solution, sonicate it, continue to impregnate it at room temperature for a preset time, and then place it in a drying oven to dry to constant weight to obtain the dried modified carrier material. S2: The dried modified support material is calcined at high temperature to obtain CeO2-encapsulated Al2O3 support, labeled as CeO2@Al2O3; S3: Dissolve an appropriate amount of manganese-containing compound and gadolinium-containing compound to form a manganese and gadolinium precursor solution. Weigh a certain amount of CeO2@Al2O3 and immerse it in the manganese and gadolinium precursor solution. After ultrasonic treatment, continue to immerse at room temperature for a preset time. Then place it in a drying oven to dry to constant weight to obtain manganese and gadolinium solids. S4: The manganese and gadolinium solids are calcined at high temperature to obtain a manganese and gadolinium-modified CeO2@Al2O3 catalytic material, labeled as XGd. y Mn 1-y / CeO2@Al2O3.

4. The method for preparing the catalyst according to claim 3, characterized in that, The cerium-containing compound in step S1 is cerium nitrate hexahydrate (Ce(NO3)3·6H2O). The dissolution is carried out in water, with ultrasonic treatment time of 0.5~4h, immersion time of 12h~36h, and drying temperature of 80~110℃.

5. The preparation method according to claim 3, characterized in that, The calcination temperature in step S2 is 400-600℃, and / or The heating rate for calcination is 3-8℃ / min, and / or The calcination time is 4-6 hours.

6. The preparation method according to claim 3, characterized in that, The manganese-containing compound in step S3 is manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O), and the gadolinium-containing compound is gadolinium nitrate hexahydrate (Gd(NO3)3·6H2O). The dissolution is carried out in water, the ultrasonic treatment time is 0.5~4h, the immersion time is 12h~36h, and the drying temperature is 80~110℃.

7. The preparation method according to claim 3, characterized in that, In step S4, the calcination temperature of the manganese and gadolinium solids is 400-600℃, and / or The heating rate of the calcination is 3-8°C / min, and / or The roasting time is 4-6 hours.

8. An XGd as described in claim 1 or 2 y Mn 1-y / CeO2@Al2O3 catalyst for Hg removal in flue gas 0 Applications in VOCs.

9. The application according to claim 8, characterized in that, XGd y Mn 1-y / CeO2@Al2O3 catalytic removal of Hg in flue gas 0 The reaction temperature with VOCs is 40-400℃.