A highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal and its preparation method
By preparing a PdCs/Ti-Ce3-Ox catalyst, the problem of low selectivity of 3-phenylpropanal in the selective hydrogenation reaction of cinnamaldehyde was solved, achieving efficient and stable catalytic effects, which are suitable for industrial production.
Patent Information
- Application Number
- CN202411360228.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2026-11-17
Smart Images

Figure CN123102345A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalyst technology, specifically to a highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal and its preparation method. Background Technology
[0002] The consumption of fossil fuels such as coal and oil has led to an energy crisis and environmental pollution. Therefore, it is necessary to find a green and abundant energy source to replace fossil fuels. Biomass energy, similar to solar and wind energy, is renewable and widely available, possessing enormous potential to replace fossil fuels.
[0003] Cinnamaldehyde is an important biomass resource, mainly extracted from cinnamon bark and other cinnamaldehyde-containing trees. It is a typical α,β-unsaturated aldehyde, and its hydrogenation products include phenylpropanal, phenylpropanol, and cinnamyl alcohol. However, the cinnamaldehyde molecule contains two reducible functional groups, C=C and C=O. From a thermodynamic perspective, due to the C=C double bond (bond energy 615 kJ·mol⁻¹), -1 Thermodynamically, it is more readily hydrogenated, and its bond energy with carbonyl groups is 715 kJ·mol⁻¹. -1 When these compounds coexist, the hydrogenation of the C=C double bond is more likely to yield the product. However, the C=C, C=O bonds, and benzene ring in the cinnamaldehyde molecule form a large π-bond conjugated system, and the steric effect makes the C=O bond more easily reduced. Therefore, the products of the hydrogenation reaction of cinnamaldehyde are usually a mixture of phenylpropanal, cinnamyl alcohol, and phenylpropanol (the product of complete hydrogenation of both C=C and C=O bonds). For this reaction, it is important to improve the selectivity for a single group and prevent the hydrogenation of another group. However, it is difficult to achieve 100% selectivity for a single target product, so researchers are working to synthesize and optimize novel catalysts to obtain higher yields of the target product.
[0004] Phenylacetaldehyde, the C=C hydrogenation product of cinnamaldehyde, is an important intermediate in pharmaceutical production. It is a crucial raw material in the pharmaceutical industry, particularly in the production of drugs for treating HIV. In addition, phenylpropanaldehyde is widely used as a fragrance in the food and cosmetics industries. It can be used to formulate fruit fragrances such as grape, cherry, and plum, and as a fixative in cosmetics to formulate daily-use fragrances such as hyacinth, jasmine, and rose. It can also be added to perfumes as a modifier.
[0005] In industrial production, obtaining any chemical intermediate often involves high costs. For example, in early industrial production, phenylpropanal was produced by methods such as the phenylpropionitrile process and the cinnamaldehyde diethanol acetal process. However, these methods are costly, involve complex post-processing, and cause severe environmental pollution. Currently, the main route for producing 3-phenylpropanal is the toluene chlorination and hydrolysis method. First, toluene undergoes side-chain chlorination under controlled conditions to obtain the main product, benzyl chloride. Then, 3-phenylpropanal can be obtained through acid or alkaline hydrolysis and distillation, yielding benzoic acid as a byproduct. Although the yield is high, the waste liquid (acidic) is difficult to treat, and the generated HCl easily corrodes equipment. In contrast, the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal does not produce any corrosive byproducts or waste. Furthermore, the catalytic selective hydrogenation of cinnamaldehyde to produce phenylpropanal is simple to operate, has high atom utilization, and is environmentally friendly; moreover, cinnamaldehyde is abundant in nature, the raw material is readily available, and the hydrogenation reaction product has high economic value. Therefore, researchers are focusing on improving the yield of a single reduction product with various catalysts without adding any acid or base. Developing efficient catalysts that selectively hydrogenate specific functional groups has important theoretical research significance and practical application value.
[0006] Cinnamaldehyde selective hydrogenation catalysts can be divided into non-precious metal catalysts and precious metal catalysts. Among precious metal catalysts, Pd-based and Pt-based catalysts are the most extensively studied. Precious metal-based heterogeneous catalysts possess excellent catalytic performance and are widely used in industrial applications such as energy conversion, chemical production, and automotive exhaust purification. However, the high cost and scarcity of precious metals hinder their widespread application in these fields. Therefore, the rational design and development of precious metal catalytic materials with good activity, durability, and selectivity is essential, but it remains a significant challenge. The rapid development of nanoscience has driven in-depth research into nanocatalysis. Nanoparticle catalysts (NPCs) have small particle sizes, high specific surface areas, and abundant coordinated unsaturated surface atoms, thus exhibiting high catalytic activity. However, in precious metal NPCs, only the metal atoms on the catalyst surface participate in the reaction, leading to increased catalyst costs and reduced metal atom utilization. To achieve high atomic utilization efficiency, the size of active metals is continuously reduced from the nanoscale to the sub-nanoscale or even the atomic scale, exposing more surface active sites and enabling them to participate in catalytic reactions. This effectively improves catalyst activity and reduces catalytic costs, allowing for more efficient utilization of precious metals. This is of great significance for the sustainable development of industries related to precious metal catalysis.
[0007] Based on this, this application provides a highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal and its preparation method. Summary of the Invention
[0008] To address the problems existing in the prior art, the purpose of this invention is to provide an atomic-level Pd... Cs / Ti-Ce3-O x A catalyst for the selective hydrogenation of cinnamaldehyde and its preparation method are disclosed. This material exhibits high catalytic activity for the hydrogenation of cinnamaldehyde while also showing high selectivity for 3-phenylpropanal, one of the hydrogenation products of cinnamaldehyde. This preparation method expands the application of spray pyrolysis in the preparation of precursor morphologies supported on metal oxides. Furthermore, the equipment is readily available, the operation is simple, and the cost is low, making it more suitable for industrial production. The material prepared by this method has the advantages of controllable morphology and precise adjustment of elemental ratios and loadings.
[0009] A highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal, its preparation method, and its application are provided. The catalyst has a spherical microstructure, wherein Pd is mainly dispersed in the form of clusters in Ti-Ce3-O. x In solid solutions, the Pd loading ranges from 1% to 4%.
[0010] To achieve this objective, the present invention adopts the following technical solution:
[0011] A highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal is provided, wherein the raw materials consist of tetrabutyl titanate, cerium nitrate hexahydrate, sodium nitrate, hydrochloric acid, surfactant, H2PdCl4 and deionized water in a weight ratio of (0.3-0.4)g:(1.2-1.4)g:(0.3-0.4)g:(3-5)mL:(0.4-0.6)g:(5-6)mL:(30-40)mL.
[0012] Furthermore, the mass concentration of the hydrochloric acid is 36%-38%.
[0013] Furthermore, the molar concentration of the H2PdCl4 is 28-32 mM.
[0014] This invention also provides a method for preparing a highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal, comprising the following steps:
[0015] (1) Tetrabutyl titanate, cerium nitrate hexahydrate, sodium nitrate, hydrochloric acid and surfactant were dissolved in deionized water to obtain a mixed solution. H2PdCl4 was then added to the mixed solution to obtain the final mixed solution.
[0016] (2) The final mixture in step (1) is ultrasonically atomized, and the generated micro-droplets are introduced into a tube furnace for reaction. The powder is collected at the end of the tube furnace.
[0017] (3) The powder obtained in step (2) is heat-treated in air atmosphere;
[0018] (4) Wash the powder obtained in step (3) with deionized water and ethanol in turn to remove residual organic matter, and finally dry it in a vacuum drying oven for 12 hours to obtain the precursor powder.
[0019] (5) The powder obtained in step (4) is subjected to further heat treatment in a hydrogen-argon mixed atmosphere to finally obtain the catalyst.
[0020] Furthermore, the surfactant includes one or more of block copolymers and small organic solid molecules.
[0021] Furthermore, the surfactant includes F127 or glucose.
[0022] Furthermore, in step (2), the reaction temperature in the tubular furnace is 600-800℃.
[0023] Furthermore, in step (3), the heat treatment heating rate is 2℃ / min, the temperature is raised to 400-600℃, and the holding time is 2h.
[0024] Furthermore, in step (5), the further heat treatment involves a heating rate of 2℃ / min, raising the temperature to 200-400℃, and holding the temperature for 2 hours.
[0025] This catalyst is used in the field of organic hydrogenation.
[0026] The advantages of this invention are:
[0027] The Pd obtained by this invention Cs / Ti-Ce3-O x Its porous structure facilitates mass transfer in the catalytic reaction, thus enhancing the catalytic effect. The preferred 4% Pd... Cs / Ti-Ce3-O x Under the evaluation scheme, the selective hydrogenation of cinnamaldehyde achieved a conversion rate of 100% after 30 min, and the selectivity of the target product 3-phenylpropanal was 97%.
[0028] Compared to Pd / TiO2 catalysts, Ce doping can significantly modulate Pd dispersion. On Ti-Ce3-Ox, Pd mainly exists in clusters. H2 is preferentially activated on the clusters via homogeneous cleavage, generating H atoms, which then undergo addition reactions with C=C atoms adsorbed on the Pd clusters to form 3-phenylpropanal. A small portion of H atoms also spills over to single-atom sites on Pd, reacting with C=O atoms adsorbed on these sites to form a small amount of 3-phenylpropanol.
[0029] The prepared catalyst exhibits high stability, with no significant Pd agglomeration observed before and after the reaction. Furthermore, the catalyst maintains high cinnamaldehyde hydrogenation activity and 3-phenylpropanaldehyde selectivity even after five cycles, making it a highly efficient, stable catalyst capable of selectively hydrogenating specific functional groups. Attached Figure Description
[0030] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0031] Figure 1 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Scanning electron microscope image of the catalyst before performance testing;
[0032] Figure 2 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Transmission electron microscope image of catalyst before performance testing;
[0033] Figure 3 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Scanning electron microscope image after catalyst performance testing;
[0034] Figure 4 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Transmission electron microscope image after catalyst performance testing;
[0035] Figure 5 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Nitrogen adsorption / desorption curves of the catalyst;
[0036] Figure 6 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Pore size distribution diagram of the catalyst;
[0037] Figure 7 (ae) is the elemental mapping diagram of the catalysts prepared in Example 1 and Comparative Examples 1-4 of this invention;
[0038] Figure 8The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Elemental mapping diagram after catalyst performance testing;
[0039] Figure 9 The XRD patterns are of the catalysts prepared in Example 1 and Comparative Examples 1-4 of this invention.
[0040] Figure 10 The XRD patterns are of the catalysts prepared in Example 1 and Comparative Examples 5 and 6 of this invention.
[0041] Figure 11 The XRD patterns are of the catalysts prepared in Example 1 and Comparative Examples 9 and 10 of this invention.
[0042] Figure 12 (af) represents the blank control and the chromatographic data of the selectivity of the catalysts prepared in Example 1 and Comparative Examples 1-4 of this invention for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0043] Figure 13 This is a comparison chart showing the selectivity of the catalysts prepared in Example 1 and Comparative Examples 1-4 of the present invention and the commercial Pd / C catalyst for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0044] Figure 14 This is a comparison diagram of the selectivity of the catalysts prepared in Example 1 and Comparative Examples 5 and 6 of the present invention for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0045] Figure 15 This is a comparison diagram showing the selectivity of the catalysts prepared in Example 1 and Comparative Example 8 for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0046] Figure 16 This is a comparison diagram of the selectivity of the catalysts prepared in Example 1 and Comparative Examples 9 and 10 of the present invention for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0047] Figure 17 This is a comparison diagram of the selectivity of the catalysts prepared in Example 1 and Comparative Examples 11 and 12 of the present invention for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0048] Figure 18 This is a comparison diagram of the selectivity of the catalysts prepared in Example 1 and Comparative Examples 13 and 14 of the present invention for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0049] Figure 19 This is a comparison diagram of the selectivity of the catalysts prepared in Example 1 and Comparative Examples 15 and 16 of the present invention for the hydrogenation of cinnamaldehyde to 3-phenylpropanal.
[0050] Figure 20The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x A comparison of the selectivity of the catalyst in the hydrogenation of cinnamaldehyde to 3-phenylpropanal at different temperatures;
[0051] Figure 21 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x A comparison of the selectivity of the catalyst in the hydrogenation of cinnamaldehyde to 3-phenylpropanal under different pressures;
[0052] Figure 22 The Pd prepared in Example 1 of this invention Cs / Ti-Ce3-O x Cyclic performance diagram of catalyst catalyzing the hydrogenation of cinnamaldehyde to 3-phenylpropanal. Detailed Implementation
[0053] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0054] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Of course, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0055] It should be noted that the reagents used in the following examples and comparative examples are all commercially available. Among them, F127 is: polyoxypropylene polyoxyethylene polyoxypropylene triblock copolymer (EO107-PO70-EO107).
[0056] All reagents were of AR purity. Cerium nitrate hexahydrate, palladium nitrate, F127, tetrabutyl titanate, propenylbenzene, cinnamaldehyde, 3-phenylpropanal, and ethanol were purchased from Aladdin Reagent (Shanghai) Co., Ltd. Concentrated hydrochloric acid (36%-38%) and sodium nitrate were purchased from China Pharmaceutical Chemical Reagent Co., Ltd. The resistivity of deionized water was 18.25 MΩ; the mass concentration of hydrochloric acid in the following examples and comparative examples was 37%.
[0057] Example 1
[0058] A Pd Cs / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0059] (1) 1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0060] The formula for calculating the load of Pd is as follows:
[0061]
[0062] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0063] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0064] (4) After washing the powder obtained in step (3) three times with deionized water and anhydrous ethanol respectively, place it at 60℃
[0065] Vacuum drying oven for 12 hours;
[0066] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd. Cs / Ti-Ce3-O x Composite catalyst.
[0067] In a further embodiment, the catalyst feedstock comprises (0.3-0.4) g by weight:
[0068] The mixture consists of (1.2-1.4)g: (0.3-0.4)g: (3-5)mL: (0.4-0.6)g: (5-6)mL: (30-40)mL of tetrabutyl titanate, cerium nitrate hexahydrate, sodium nitrate, hydrochloric acid, surfactant, H2PdCl4, and deionized water; the mass concentration of hydrochloric acid is 36%-38%; and the molar concentration of H2PdCl4 is 28-32mM.
[0069] In a further embodiment, the surfactant may also be glucose, and the reaction temperature in the tubular furnace in step (2) may be any value between 600-800°C; the heat treatment temperature in step (3) may be any value between 400-600°C; and the further heat treatment temperature in step (5) may be any value between 200-400°C.
[0070] Comparative Example 1
[0071] A method for preparing a Pd / TiO2-efficient catalyst for the selective hydrogenation of cinnamaldehyde:
[0072] (1) Dissolve 0.33996g NaNO3, 0.5g F127, 4mL HCl and 1.36128g tetrabutyl titanate in 34mL deionized water to obtain a mixed solution. Then add 5.334mL H2PdCl4 (30mM) to the mixed solution to obtain the final mixed solution. The Pd loading is 4%.
[0073] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0074] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0075] (4) Wash the powder obtained in step (3) three times with deionized water and anhydrous ethanol respectively, and place it at 60℃.
[0076] Vacuum drying oven for 12 hours;
[0077] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain the Pd / TiO2 composite catalyst.
[0078] Comparative Example 2
[0079] A Pd / Ti3-Ce-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0080] (1) Combine 0.43422g Ce(NO3)3·6H2O, 0.33996g NaNO 3,0.5g F127, 4mL HCl, and 1.02096g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0081] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0082] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere, and the temperature was raised to 500℃ and held for 2h, and then naturally cooled to room temperature;
[0083] (4) After washing the powder obtained in step (3) three times with deionized water and anhydrous ethanol respectively, place it at 60°C.
[0084] 12 hours in a vacuum drying oven at 0°C;
[0085] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd / Ti3-Ce-O. x Composite catalyst.
[0086] Comparative Example 3
[0087] A Pd / Ti2-Ce2-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0088] (1) Dissolve 0.86844g Ce(NO3)3·6H2O, 0.33996g NaNO3, 0.5g F127, 4mL HCl, and 0.68064g tetrabutyl titanate in 34mL of deionized water to obtain a mixed solution. Then add 5.334mL H2PdCl4 (30mM) to the mixed solution to obtain the final mixed solution. The Pd loading is 4%.
[0089] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0090] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0091] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0092] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd / Ti2-Ce2-O. x Composite catalyst.
[0093] Comparative Example 4
[0094] A method for preparing a Pd / CeO2 catalyzed selective hydrogenation catalyst for cinnamaldehyde:
[0095] (1) Combine 1.73688g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5 g F127 was dissolved in 4 mL HCl in 34 mL deionized water to obtain a mixed solution. Then, 5.334 mL H2PdCl4 (30 mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0096] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0097] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0098] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0099] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain the Pd / CeO2 composite catalyst.
[0100] Comparative Example 5
[0101] A Pd Cs / Ti-Ce3-O x Preparation method of (F127-free) effective catalyst for selective hydrogenation of cinnamaldehyde:
[0102] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3,4 mL HCl and 0.34032 g tetrabutyl titanate were dissolved in 34 mL deionized water to obtain a mixed solution. Then, 5.334 mL H2PdCl4 (30 mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0103] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0104] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0105] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0106] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd. Cs / Ti-Ce3-O x (F127-free) composite catalyst.
[0107] Comparative Example 6
[0108] A Pd Cs / Ti-Ce3-O x Preparation method of (NaNO3-free) effective catalyst for selective hydrogenation of cinnamaldehyde:
[0109] (1) 1.30266g Ce(NO3)3·6H2O, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0110] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0111] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0112] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0113] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd. Cs / Ti-Ce3-O x (NaNO3-free) composite catalyst.
[0114] Comparative Example 7
[0115] A Pd Cs / Ti-Ce3-O x Preparation method of (HCl-free) effective catalyst for selective hydrogenation of cinnamaldehyde:
[0116] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0117] Because of the lack of HCl, tetrabutyl titanate cannot dissolve and cannot form a clear solution.
[0118] Comparative Example 8
[0119] A Pd Cs / Ti-Ce3-O x Preparation method of (glucose) effective catalyst for selective hydrogenation of cinnamaldehyde:
[0120] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5 g glucose, 4 mL HCl, and 0.34032 g tetrabutyl titanate were dissolved in 34 mL deionized water to obtain a mixed solution. Then, 5.334 mL H2PdCl4 (30 mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0121] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0122] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0123] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0124] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd. Cs / Ti-Ce3-O x (Glucose) composite catalyst.
[0125] Comparative Example 9
[0126] A Pd Cs / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0127] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0128] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0129] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0130] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0131] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 200℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd. Cs / Ti-Ce3-O x Composite catalyst.
[0132] Comparative Example 10
[0133] A Pd Cs / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0134] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0135] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0136] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0137] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0138] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 400℃ and held for 2h. Then it is naturally cooled to room temperature to obtain Pd. Cs / Ti-Ce3-O x Composite catalyst.
[0139] Comparative Example 11
[0140] A 1% Pd / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0141] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 1.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 1%.
[0142] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0143] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0144] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0145] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain 1% Pd / Ti-Ce3-O. x Composite catalyst.
[0146] Comparative Example 12
[0147] A 2% Pd / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0148] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 2.667mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 2%.
[0149] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0150] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0151] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0152] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain 2% Pd / Ti-Ce3-O. x Composite catalyst.
[0153] Comparative Example 13
[0154] A 4% Pd / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0155] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0156] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. Powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 600℃.
[0157] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0158] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0159] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain 4% Pd / Ti-Ce3-O. x Composite catalyst.
[0160] Comparative Example 14
[0161] A 4% Pd / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0162] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3,0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0163] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 800℃.
[0164] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 500℃ and held for 2 hours, and then naturally cooled to room temperature.
[0165] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0166] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain 4% Pd / Ti-Ce3-O. x Composite catalyst.
[0167] Comparative Example 15
[0168] A 4% Pd / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0169] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution to obtain the final mixed solution. The Pd loading was 4%.
[0170] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0171] (3) The above powder was heat-treated for 2 hours at a heating rate of 2℃ / min in air at a temperature of 400℃.
[0172] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0173] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain 4% Pd / Ti-Ce3-O. x Composite catalyst.
[0174] Comparative Example 16
[0175] A 4% Pd / Ti-Ce3-O x Preparation method of effective catalyst for selective hydrogenation of cinnamaldehyde:
[0176] (1)1.30266g Ce(NO3)3·6H2O, 0.33996g NaNO 3, 0.5g F127, 4mL HCl, and 0.34032g tetrabutyl titanate were dissolved in 34mL deionized water to obtain a mixed solution. Then, 5.334mL H2PdCl4 (30mM) was added to the mixed solution, and the Pd loading was 4%.
[0177] (2) The final mixture in step (1) is ultrasonically atomized, and the droplets are introduced into a high-temperature tube furnace for reaction. The powder is collected at the other end of the tube furnace. The heating zone of the tube furnace is 30cm long and the temperature is 700℃.
[0178] (3) The above powder was subjected to heat treatment at a heating rate of 2℃ / min in air atmosphere. The temperature was raised to 600℃ and held for 2 hours, and then naturally cooled to room temperature.
[0179] (4) The powder obtained in step (3) was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for 12 hours.
[0180] (5) The powder from step (4) is further heat-treated at a heating rate of 2℃ / min in an H2 / Ar atmosphere with a volume fraction of 5%, and the temperature is raised to 300℃ and held for 2h. Then it is naturally cooled to room temperature to obtain 4% Pd / Ti-Ce3-O. x Composite catalyst.
[0181] To illustrate Pd Cs / Ti-Ce3-O x Its highly efficient catalytic activity and excellent selectivity, along with its application and evaluation techniques, are as follows:
[0182] The selective hydrogenation reaction of cinnamaldehyde was carried out in a 100 mL stainless steel autoclave. The specific steps were as follows: 20 mg of catalyst, 60 mL of ethanol, 3 mmol of cinnamaldehyde, and 1 mmol of propylbenzene (internal standard, used for calibration and to eliminate the influence of fluctuations in operating conditions on the analytical results) were ultrasonically dispersed in a quartz beaker (the quartz beaker was used to avoid excessive heat transfer due to an excessively thick PTFE liner). The mixture was then transferred to the autoclave and sealed. The autoclave was purged three times with 2.0 MPa N2 to replace any residual air, followed by three purgings with 1.0 MPa H2. Subsequently, H2 was introduced to a certain pressure (0.5 MPa, 1.0 MPa, 1.5 MPa, 2.0 MPa), the magnetic stirrer was adjusted to 500 rpm, and the temperature was programmed (heating rate of 2 °C / min) to reach the set reaction temperature (50 °C, 70 °C, 90 °C). Every 15 minutes, 1 mL of the reaction solution was extracted using a syringe with a filter membrane, and the organic composition of the reaction solution was analyzed using gas chromatography (GC9790Plus, Zhejiang Fuli).
[0183] After each reaction, the catalyst was collected by centrifugation, washed with ethanol, dried, and then subjected to a cycle experiment.
[0184] The method for calculating the selectivity of 3-phenylpropanal is as follows:
[0185]
[0186] Figure 1-4 These are Pd prepared according to Example 1 of the present invention. Cs / Ti-Ce3-O x Scanning electron microscope and transmission electron microscope images before and after catalyst performance testing. Figure 7 (d) and 8 are Pd prepared in Example 1 of the present invention. Cs / Ti-Ce3-O x Elemental mapping diagrams before and after catalyst performance testing. Figure 1 and Figure 3 , Figure 2 and Figure 4 The comparison shows that the Pd prepared by this invention... Cs / Ti-Ce3-O x The catalyst structure did not collapse before and after the performance test. Figure 7 (d) Comparison with 8 shows that Pd in the catalyst after the reaction did not agglomerate. Figure 22 In terms of cycle performance, the Pd prepared in this invention Cs / Ti-Ce3-O x The catalyst exhibits high stability.
[0187] Based on the N2 adsorption isotherm ( Figure 5 ), PdCs / Ti-Ce3-O x The catalyst has 87.101m 2 ·g -1 The specific surface area and pore size of 20.291 nm ( Figure 6 This provides sufficient surface for Pd deposition.
[0188] Figure 7 (ae) is the elemental mapping diagram of the catalysts prepared in Example 1 and Comparative Examples 1-4 of this invention. The comparison shows that as the Ce ratio increases, the dispersion of Pd also increases.
[0189] Figure 9 The XRD patterns of the catalysts prepared in Example 1 and Comparative Examples 1-4 of this invention, as well as the commercial Pd / C catalyst, are shown in the figures. It can be seen from the figures that Pd... Cs / Ti-Ce3-O x The 28.5° shift relative to the (111) crystal plane of the CeO2 standard card indicates the formation of a solid solution.
[0190] Figure 12 (a) is the blank control. Figure 12 (bf) shows the chromatographic data for the hydrogenation of cinnamaldehyde catalyzed by the catalysts prepared in Example 1 and Comparative Examples 1-4 of this invention. The selectivity of the catalysts prepared in all cases of this invention for 3-phenylpropanal was calculated after subtracting the blank control.
[0191] Figure 13 This is a comparison of the selectivity of the catalysts prepared in Example 1 and Comparative Examples 1-4 of this invention, and the commercial Pd / C catalyst, for the hydrogenation of cinnamaldehyde to 3-phenylpropanal. We can observe that the selectivity of 3-phenylpropanal gradually increases and then decreases with increasing Ce content. Therefore, the Pd / C catalyst prepared in this invention... Cs / Ti-Ce3-O x The catalyst exhibits far greater selectivity for the target product 3-phenylpropanal than commercial Pd / C.
[0192] Figure 17 , 18 The figures show a comparison of the catalysts prepared in Example 1 and Comparative Examples 13, 14, 15, and 16 of this invention, as well as the conversion and selectivity of the catalysts in the hydrogenation of cinnamaldehyde to 3-phenylpropanal. As can be seen from the figures, the catalyst prepared under the conditions of Example 1 exhibits the highest conversion rate of cinnamaldehyde and the highest selectivity for 3-phenylpropanal.
[0193] The applicant declares that the present invention is illustrated by the above embodiments to demonstrate the product and detailed preparation method of the present invention, but the present invention is not limited to the above product and detailed preparation method, that is, it does not mean that the present invention must rely on the above product and detailed preparation method to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of excipients, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0194] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention. These simple modifications all fall within the protection scope of the present invention.
[0195] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0196] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal, characterized in that, The raw materials consist of tetrabutyl titanate, cerium nitrate hexahydrate, sodium nitrate, hydrochloric acid, surfactant, H2PdCl4 and deionized water in a weight ratio of (0.3-0.4)g:(1.2-1.4)g:(0.3-0.4)g:(3-5)mL:(0.4-0.6)g:(5-6)mL:(30-40)mL.
2. The highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal according to claim 1, characterized in that, The hydrochloric acid has a mass concentration of 36%-38%.
3. The highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal according to claim 1, characterized in that, The molar concentration of H2PdCl4 is 28-32 mM.
4. A method for preparing a highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal as described in any one of claims 1-3, characterized in that the step... include: (1) Tetrabutyl titanate, cerium nitrate hexahydrate, sodium nitrate, hydrochloric acid and surfactant were dissolved in deionized water to obtain a mixed solution. H2PdCl4 was then added to the mixed solution to obtain the final mixed solution. (2) The final mixture in step (1) is ultrasonically atomized, and the generated micro-droplets are introduced into a tube furnace for reaction. The powder is collected at the end of the tube furnace. (3) The powder obtained in step (2) is heat-treated in air atmosphere; (4) Wash the powder obtained in step (3) with deionized water and ethanol in turn to remove residual organic matter, and finally dry it in a vacuum drying oven for 12 hours to obtain the precursor powder. (5) The powder obtained in step (4) is subjected to further heat treatment in a hydrogen-argon mixed atmosphere to finally obtain the catalyst.
5. The method for preparing the highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal according to claim 4, characterized in that, The surfactant includes block copolymers and small organic solid molecules.
6. The method for preparing the highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal according to claim 4, characterized in that, The surfactant includes F127 or glucose.
7. The method for preparing the highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal according to claim 4, characterized in that, In step (2), the reaction temperature in the tubular furnace is 600-800℃.
8. The method for preparing the highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal according to claim 4, characterized in that, In step (3), the heat treatment heating rate is 2℃ / min, the temperature is raised to 400-600℃, and the holding time is 2h.
9. The method for preparing the highly efficient catalyst for the selective hydrogenation of cinnamaldehyde to 3-phenylpropanal according to claim 4, characterized in that, In step (5), the further heat treatment involves a heating rate of 2℃ / min, raising the temperature to 200-400℃, and holding it for 2 hours.
10. A catalyst as described in claims 1-3 applied in the field of organic hydrogenation.