A CGPF catalyst and its preparation method

By designing a composite slurry and employing a one-time coating process, the complexity and durability issues of CGPF in the efficient capture of ultrafine particulate matter and gaseous pollutants have been resolved, achieving a synergistic improvement in efficient capture and purification, and exhibiting excellent long-term thermal durability.

CN123102346APending Publication Date: 2026-11-17FUJIAN DERI ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611010101.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing catalytic converter gasoline particulate filters (CGPF) suffer from bottlenecks in efficient capture of ultrafine particulate matter and gaseous pollutants, including complex processes, limited functionality, and poor durability. In particular, they are prone to stripping, clogging, and reduced capture efficiency under high-temperature conditions.

Method used

By employing a composite slurry design and a one-time coating process, rare earth element-modified γ-alumina and cerium-zirconium composite oxide powders are combined with precious metal precursors to form a gradient filter layer structure, achieving efficient capture of ultrafine particulate matter and active catalytic oxidation of gaseous pollutants, thereby improving durability.

Benefits of technology

It simplifies production steps, reduces costs, achieves efficient capture of ultrafine particles and efficient purification of gaseous pollutants, and possesses excellent long-term thermal durability, avoiding back pressure rise and coating peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to a method for preparing a CGPF catalyst, comprising steps S1-S7. Unlike existing technologies, this method simplifies production steps and reduces costs through composite slurry design and a one-step coating process, while achieving synergistic improvements in efficient capture of ultrafine particles, active catalytic oxidation of captured particles, and efficient purification of gaseous pollutants, and also exhibits excellent long-term thermal durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of automotive exhaust aftertreatment technology, specifically to a catalyst for a gasoline engine particulate filter (GPF) and its preparation method, and in particular to a catalytic gasoline engine particulate filter (CGPF) that can simultaneously and efficiently purify gaseous pollutants (THC, NOx, CO) and solid particulate matter (PM, PN). Background Technology

[0002] With increasingly stringent global emission regulations, gasoline vehicle exhaust pollution control faces new challenges. In particular, the "China VII" emission standard (expected to be implemented), considered the world's strictest standard, has explicitly lowered the detection limit for particulate matter (PN) from the current 23 nanometers (PN23) to 10 nanometers (PN10). This change means extremely high requirements are placed on the collection efficiency of finer particulate matter. At the same time, the regulations have further tightened the limits for gaseous pollutants such as carbon monoxide (CO), hydrocarbons (HC), and nitrogen oxides (NOx). Therefore, developing an aftertreatment technology that can simultaneously and efficiently remove ultrafine particulate matter and gaseous pollutants, while also possessing excellent durability, has become an urgent need for the industry.

[0003] Catalytic converters (CGPF) are currently the mainstream technology, which coat a porous wall-flow GPF support with a catalytic coating to integrate particulate trapping and catalytic conversion. However, existing high-efficiency CGPF technologies still have significant shortcomings in addressing the aforementioned challenges, mainly in the following two aspects:

[0004] 1. The contradiction between process complexity and functional layers: To achieve optimal performance, the ideal CGPF coating structure is usually designed as a "double layer": the inner (or bottom) layer is a high specific surface area catalytic layer, used to load active components such as noble metals to efficiently convert gaseous pollutants; the outer layer is a porous particulate trapping layer, used to physically intercept and store particulate matter (PM). However, existing technologies mostly adopt a sequential coating process, that is, first coating the catalytic layer, then curing it at high temperature, and finally coating the particulate trapping layer. This process route is lengthy, has low production efficiency, high energy consumption, and the interface between the two layers may peel off after high-temperature durability due to the mismatch of thermal expansion coefficients, affecting product life.

[0005] 2. Limited Functionality and Durability Bottlenecks: Existing particulate trapping layer materials (such as some macroporous alumina and cerium oxide with specific particle sizes) primarily function as physical interceptors and stores, lacking or possessing only extremely low catalytic activity. This leads to two major problems: First, particulate matter such as soot trapped in the trapping layer can only rely on active oxygen species diffused from the catalytic layer or passively regenerated at high temperatures, resulting in low oxidation efficiency. This easily causes filter pore blockage, leading to a rapid increase in back pressure and affecting engine performance and fuel economy. Second, since the trapping layer material does not participate in the catalytic reaction, its physical structure may sinter or change under long-term high-temperature, high-flow-rate exhaust gas scouring, leading to a decrease in trapping efficiency and making it difficult to meet the requirements for long-term, efficient, and stable trapping of PN10 ultrafine particles. Summary of the Invention

[0006] In view of the above problems, this application provides a CGPF catalyst with high gas-solid pollutant conversion rate and its preparation method. Through composite slurry design and one-time coating process, the production steps are simplified and costs are reduced, while achieving synergistic improvement in efficient capture of ultrafine particles, active catalytic oxidation of captured particles, and efficient purification of gaseous pollutants, and exhibiting excellent long-term thermal durability.

[0007] The first aspect of this invention provides a method for preparing a CGPF catalyst, comprising the following steps:

[0008] S1: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are pulverized to a particle size D50 of 0.5-10 μm to obtain the first powder; the mass ratio of the rare earth element modified γ-alumina and cerium-zirconium composite oxide is 1-8:2.

[0009] S2: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are mixed and then pulverized to a particle size D50 of 20-50 μm to obtain a second powder; the mass ratio of the modified γ-Al2O3 powder to the cerium-zirconium composite oxide is 1:2-8.

[0010] S3: Mix the first powder (S1) with deionized water and then ball mill for the first time for 20-180 min to obtain the first slurry; the solid content of the first slurry is 15-50 wt%, and the particle size (D50) of the particles in the first slurry is 0.5-5 μm;

[0011] S4: Add the second powder of S2 to the first slurry of S3 and then perform a second ball milling. The second ball milling time is 60-180 minutes to obtain the second slurry.

[0012] S5: Add the precious metal precursor and deionized water to the second slurry in S4, and stir for 180-600 min to obtain a composite slurry; the solid content of the composite slurry is 20-60 wt%.

[0013] S6: The S5 composite slurry is coated onto the GPF white support to form a coating, thus obtaining a wet GGPF catalyst preform.

[0014] S7: After drying the wet S6 GGPF catalyst blank, calcine it in air at 450-600℃ for 2-3 hours to obtain the CGPF catalyst.

[0015] Unlike existing technologies, this invention, through composite slurry design and a one-time coating process, simplifies production steps and reduces costs while achieving synergistic improvements in efficient capture of ultrafine particles, active catalytic oxidation of captured particles, and efficient purification of gaseous pollutants, and also possesses excellent long-term thermal durability.

[0016] Furthermore, the mass ratio of the first powder to the second powder is 1 to 5:1.

[0017] Furthermore, in the rare earth element modified γ-alumina, the rare earth element is one or more of lanthanum, cerium, praseodymium, and magnesium; its doping amount is 5-30% of the mass of alumina.

[0018] Furthermore, the particle size of the solid particles in the second slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5.

[0019] Fine particles with D10 ≤ 1.5μm can penetrate deep into the internal pores of the carrier wall with the slurry for coating, increasing the internal surface area of ​​the wall material without completely blocking the pores, which is crucial for catalytic reactions.

[0020] Coarse particles with a D90 ≥ 10μm: Their size is comparable to or slightly larger than the pore size of the carrier wall, making them easier to deposit on the inner wall surface and inlet of the pores during coating, which is beneficial for forming an interception layer for particulate matter (PM). At the same time, they constitute the main structure of the coating on the pore surface.

[0021] Wide distribution with D90 / D10>5:

[0022] Constructing a gradient filtration layer: Within the pores, a gradient structure naturally forms, with particles gradually becoming finer from the outside (pore opening) to the inside (pore wall). The large particle layer at the pore opening facilitates primary interception, while the inner small particle filling layer ensures the coating's robustness and catalytic function. This structure can efficiently capture particulate matter while avoiding the formation of dense plugs, thereby controlling the rise in back pressure.

[0023] Enhanced coating adhesion: GPF undergoes frequent carbon soot loading-regeneration (high-temperature combustion) cycles, resulting in severe thermal stress. A dense, crack-resistant coating with a wide distribution is crucial for maintaining coating integrity and preventing peeling and pore blockage under such harsh conditions.

[0024] Furthermore, the noble metal precursor is a soluble salt of a noble metal, and the noble metal includes one or more of Pt, Pd, Rh, and Ru.

[0025] Furthermore, the GPF white carrier is a wall-flow cordierite GPF blank carrier with a pore size of 10-20 μm.

[0026] Furthermore, carboxymethyl cellulose was added as an additive during the initial ball milling process, with an addition amount of 1-4 wt% of the first powder.

[0027] Furthermore, in step S6, vacuum suction coating is employed.

[0028] A second aspect of the present invention provides a CGPF catalyst, which is prepared using the preparation method described in the first aspect of the present invention.

[0029] Furthermore, the loading of the precious metal is 0.5-5.0 wt%.

[0030] The above description of the invention is merely an overview of the technical solution of this application. In order to enable those skilled in the art to better understand the technical solution of this application and to implement it based on the textual description, and to make the above-mentioned objectives and other objectives, features and advantages of this application easier to understand, the following description is based on the specific embodiments of this application. Detailed Implementation

[0031] To explain in detail the technical content, structural features, objectives, and effects of the technical solution, the following detailed description is provided in conjunction with specific embodiments.

[0032] To illustrate the possible application scenarios, technical principles, implementable specific solutions, and achievable objectives and effects of this application in detail, the following description is provided in conjunction with the specific embodiments listed. The embodiments described herein are merely illustrative of the technical solutions of this application and are therefore intended only as examples, not as limiting the scope of protection of this application.

[0033] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.

[0034] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.

[0035] In the description of this application, the term "and / or" is used to describe the logical relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A exists, B exists, and A and B exist simultaneously. Additionally, the character " / " in this document generally indicates that the preceding and following objects have an "or" logical relationship.

[0036] In this application, terms such as “first” and “second” are used only to distinguish one entity or operation from another, and do not necessarily require or imply any actual quantity, hierarchy or order relationship between these entities or operations.

[0037] Unless otherwise specified, the use of terms such as “comprising,” “including,” “having,” or other similar expressions in this application is intended to cover non-exclusive inclusion, which does not exclude the presence of additional elements in a process, method, or product that includes the stated elements, such that a process, method, or product that includes a list of elements may include not only those defined elements but also other elements not expressly listed, or elements inherent to such a process, method, or product.

[0038] In this application, expressions such as "greater than", "less than", and "exceeding" are understood to exclude the stated number; expressions such as "above", "below", and "within" are understood to include the stated number. Furthermore, in the description of the embodiments of this application, "multiple" means two or more (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups" and "multiple times", unless otherwise explicitly specified.

[0039] The first aspect of this invention provides a method for preparing a CGPF catalyst, comprising the following steps:

[0040] S1: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are pulverized to a particle size D50 of 0.5-10 μm to obtain the first powder; the mass ratio of the rare earth element modified γ-alumina and cerium-zirconium composite oxide is 1-8:2.

[0041] S2: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are mixed and then pulverized to a particle size D50 of 20-50 μm to obtain a second powder; the mass ratio of the modified γ-Al2O3 powder to the cerium-zirconium composite oxide is 1:2-8.

[0042] S3: Mix the first powder (S1) with deionized water and then ball mill for the first time for 20-180 min to obtain the first slurry; the solid content of the first slurry is 15-50 wt%, and the particle size (D50) of the particles in the first slurry is 0.5-5 μm;

[0043] S4: Add the second powder of S2 to the first slurry of S3 and then perform a second ball milling. The second ball milling time is 60-180 minutes to obtain the second slurry.

[0044] S5: Add the precious metal precursor and deionized water to the second slurry in S4, and stir for 180-600 min to obtain a composite slurry; the solid content of the composite slurry is 20-60 wt%.

[0045] S6: The S5 composite slurry is coated onto the GPF white support to form a coating, thus obtaining a wet GGPF catalyst preform.

[0046] S7: After drying the wet S6 GGPF catalyst blank, calcine it in air at 450-600℃ for 2-3 hours to obtain the CGPF catalyst.

[0047] Unlike existing technologies, this invention, through composite slurry design and a one-time coating process, simplifies production steps and reduces costs while achieving synergistic improvements in efficient capture of ultrafine particles, active catalytic oxidation of captured particles, and efficient purification of gaseous pollutants, and also possesses excellent long-term thermal durability.

[0048] Furthermore, the mass ratio of the first powder to the second powder is 1 to 5:1.

[0049] Furthermore, in the rare earth element modified γ-alumina, the rare earth element is one or more of lanthanum, cerium, praseodymium, and magnesium; its doping amount is 5-30% of the mass of alumina.

[0050] Furthermore, the particle size of the solid particles in the second slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5.

[0051] Fine particles with D10 ≤ 1.5μm can penetrate deep into the internal pores of the carrier wall with the slurry for coating, increasing the internal surface area of ​​the wall material without completely blocking the pores, which is crucial for catalytic reactions.

[0052] Coarse particles with a D90 ≥ 10μm: Their size is comparable to or slightly larger than the pore size of the carrier wall, making them easier to deposit on the inner wall surface and inlet of the pores during coating, which is beneficial for forming an interception layer for particulate matter (PM). At the same time, they constitute the main structure of the coating on the pore surface.

[0053] Wide distribution with D90 / D10>5:

[0054] Constructing a gradient filtration layer: Within the pores, a gradient structure naturally forms, with particles gradually becoming finer from the outside (pore opening) to the inside (pore wall). The large particle layer at the pore opening facilitates primary interception, while the inner small particle filling layer ensures the coating's robustness and catalytic function. This structure can efficiently capture particulate matter while avoiding the formation of dense plugs, thereby controlling the rise in back pressure.

[0055] Enhanced coating adhesion: GPF undergoes frequent carbon soot loading-regeneration (high-temperature combustion) cycles, resulting in severe thermal stress. A dense, crack-resistant coating with a wide distribution is crucial for maintaining coating integrity and preventing peeling and pore blockage under such harsh conditions.

[0056] Furthermore, the noble metal precursor is a soluble salt of a noble metal, and the noble metal includes one or more of Pt, Pd, Rh, and Ru.

[0057] Furthermore, the GPF white carrier is a wall-flow cordierite GPF blank carrier with a pore size of 10-20 μm.

[0058] Furthermore, carboxymethyl cellulose was added as an additive during the initial ball milling process, with an addition amount of 1-4 wt% of the first powder.

[0059] Furthermore, in step S6, vacuum suction coating is employed.

[0060] A second aspect of the present invention provides a CGPF catalyst, which is prepared using the preparation method described in the first aspect of the present invention.

[0061] Furthermore, the loading of the precious metal is 0.5-5.0 wt%.

[0062] In this embodiment, the white carrier is a wall-flow cordierite GPF blank filter with parallel channels that alternately block pores. The exhaust gas must penetrate the porous carrier wall, and the coating significantly affects the gas penetration resistance and particulate matter interception mechanism. (Specifications: Φ118.4mm×127mm, volume 1.398L, pore size 10-20μm).

[0063] The rare earth modified γ-alumina powder in this embodiment is prepared using the following steps:

[0064] Step 1: Solution preparation

[0065] The target product (based on the mass of oxides) is composed of: 80% Al2O3, 8% ZrO2, 3% La2O3, 4% BaO, and 5% MgO. The corresponding amounts of aluminum nitrate (Al(NO3)3·9H2O), zirconium oxynitrate (ZrO(NO3)2·xH2O), lanthanum nitrate (La(NO3)3·xH2O), barium nitrate (Ba(NO3)2), and magnesium nitrate (Mg(NO3)2·6H2O) are accurately weighed.

[0066] The above salts were completely dissolved in deionized water and mixed thoroughly to prepare a mixed salt solution A with a total metal ion concentration of 1.0 mol / L.

[0067] Prepare a separate 1.5 mol / L ammonium bicarbonate (NH4HCO3) aqueous solution as precipitant solution B.

[0068] Step 2: Co-precipitation

[0069] Add mixed salt solution A to the coprecipitation reactor, and slowly add precipitant solution B to the coprecipitation reactor until the pH reaches 5 ± 0.2.

[0070] Ammonia water was then added to adjust the pH, so that the pH value of the reaction system was precisely stabilized at 8.5±0.2. After the addition was completed, the mixture was kept warm and stirred for another 30 minutes to obtain the precursor slurry.

[0071] Step 3: Aging treatment

[0072] The precursor slurry obtained in step 2 was transferred to an aging tank, heated to 70°C, and stirred continuously at this temperature for 4 hours to promote the crystallization and aging of the precipitate.

[0073] Step 4: Filtration and Washing

[0074] The aged slurry is pumped into a plate and frame filter press for filtration to obtain filter cake.

[0075] Step 5: Drying and roasting

[0076] The washed filter cake was placed in an oven and dried at 120°C for 12 hours.

[0077] The dried lumpy material was ground and placed in a calcining furnace. Under a ventilated atmosphere, the temperature was increased to 600°C at a rate of 5°C / min, and calcined at this temperature for 4 hours. After natural cooling, the rare earth modified γ-alumina powder of this embodiment was obtained.

[0078] In this embodiment, the cerium-zirconium rare earth composite oxide comprises the following components by mass percentage: 30% CeO2, 60% ZrO2, 5% La2O3, and 5% Y2O3.

[0079] In this embodiment, the noble metal precursors are platinum nitrate and palladium nitrate, wherein the mass ratio of platinum to palladium is 1:1:1.

[0080] Example 1

[0081] S1: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are pulverized to a particle size D50=10μm to obtain the first powder; the mass ratio of the rare earth element modified γ-alumina and cerium-zirconium composite oxide is 1:2.

[0082] S2: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are mixed and then pulverized to a particle size D50=30μm to obtain a second powder; the mass ratio of the modified γ-Al2O3 powder to the cerium-zirconium composite oxide is 2:1.

[0083] The mass ratio of the first powder to the second powder is 3:1.

[0084] S3: Mix 84g of the first powder, 1.7g of carboxymethyl cellulose auxiliary agent, and deionized water, and then ball mill for the first time for 180min to obtain the first slurry; the solid content of the first slurry is 30wt%, and the particle size D50 of the particles in the first slurry is 0.5-5μm;

[0085] S4: Add 28g of the second powder to the first slurry and then perform a second ball milling for 60 minutes to obtain the second slurry; the particle size of the solid particles in the second slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5;

[0086] S5: After mixing platinum nitrate, palladium nitrate, and deionized water, the mixture is added to the second slurry and stirred for 300 minutes to obtain a composite slurry; the solid content of the composite slurry is 40 wt%.

[0087] S6: The composite slurry is suction-coated from the gas inlet end of the GPF carrier, and the suction rate is controlled so that the slurry penetration length is about 60% of the total length of the carrier. After draining and pre-drying at 120°C for 2 hours, the carrier is flipped over and suction-coated again from the gas outlet end under the same conditions to optimize the uniformity of the coating distribution along the axial direction of the carrier; thus obtaining the wet GGPF catalyst preform.

[0088] S7: After drying the wet GGPF catalyst blank at 120℃, it was placed in a muffle furnace and calcined in air at 550℃ for 3 hours to obtain the CGPF catalyst. (Total coating loading is approximately 80 g / L, and total noble metal loading is approximately 5 g / ft) 3 。

[0089] Example 2

[0090] S1: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are pulverized to a particle size D50=5μm to obtain the first powder; the mass ratio of the rare earth element modified γ-alumina and cerium-zirconium composite oxide is 1:1.

[0091] S2: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are mixed and then pulverized to a particle size D50=20μm to obtain a second powder; the mass ratio of the modified γ-Al2O3 powder to the cerium-zirconium composite oxide is 1:1.

[0092] The mass ratio of the first powder to the second powder is 1:1.

[0093] S3: Mix 56g of the first powder, 1g of carboxymethyl cellulose auxiliary agent, and deionized water, and then ball mill for the first time for 180 minutes to obtain the first slurry; the solid content of the first slurry is 50wt%, and the particle size D50 of the particles in the first slurry is 0.5-5μm;

[0094] S4: Add 56g of the second powder to the first slurry and then perform a second ball milling for 60min to obtain the second slurry; the particle size of the solid particles in the second slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5;

[0095] S5: Platinum nitrate, palladium nitrate, and deionized water are mixed, and the mixture is added to the second slurry. After stirring for 300 minutes, a composite slurry is obtained; the solid content of the composite slurry is 60 wt%.

[0096] S6: The composite slurry is suction-coated from the gas inlet end of the GPF carrier, and the suction rate is controlled so that the slurry penetration length is about 60% of the total length of the carrier. After draining and pre-drying at 120°C for 2 hours, the carrier is flipped over and suction-coated again from the gas outlet end under the same conditions to optimize the uniformity of the coating distribution along the axial direction of the carrier; thus obtaining the wet GGPF catalyst preform.

[0097] S7: After drying the wet GGPF catalyst blank at 120℃, it was placed in a muffle furnace and calcined in air at 450℃ for 3 hours to obtain the CGPF catalyst. (Total coating loading is approximately 80 g / L, and total noble metal loading is approximately 5 g / ft) 3 。

[0098] Example 3

[0099] S1: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are pulverized to a particle size D50=0.5μm to obtain the first powder; the mass ratio of the rare earth element modified γ-alumina and cerium-zirconium composite oxide is 4:1.

[0100] S2: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are mixed and then pulverized to a particle size D50=30μm to obtain a second powder; the mass ratio of the modified γ-Al2O3 powder to the cerium-zirconium composite oxide is 4:1.

[0101] The mass ratio of the first powder to the second powder is 5:1.

[0102] S3: Mix 100g of the first powder, 2g of carboxymethyl cellulose additive, and deionized water, and then ball mill for the first time for 180 minutes to obtain the first slurry; the solid content of the first slurry is 20wt%, and the particle size D50 of the particles in the first slurry is 0.5-5μm;

[0103] S4: Add 20g of the second powder to the first slurry and then perform a second ball milling for 180min to obtain the second slurry; the particle size of the solid particles in the second slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5;

[0104] S5: After mixing platinum nitrate, palladium nitrate, and deionized water, the mixture is added to the second slurry and stirred for 600 minutes to obtain a composite slurry; the solid content of the composite slurry is 50 wt%.

[0105] S6: The composite slurry is suction-coated from the gas inlet end of the GPF carrier, and the suction rate is controlled so that the slurry penetration length is about 60% of the total length of the carrier. After draining and pre-drying at 120°C for 2 hours, the carrier is flipped over and suction-coated again from the gas outlet end under the same conditions to optimize the uniformity of the coating distribution along the axial direction of the carrier; thus obtaining the wet GGPF catalyst preform.

[0106] S7: After drying the wet GGPF catalyst blank at 120℃, it was placed in a muffle furnace and calcined in air at 550℃ for 3 hours to obtain the CGPF catalyst. (Total coating loading is approximately 85 g / L, and total noble metal loading is approximately 5 g / ft) 3 。

[0107] Comparative Example 1: (Traditional two-layer sequential coating)

[0108] Step 1: Prepare a first slurry containing catalytic material (La / γ-Al2O3: cerium-zirconium composite material), coat it onto the same GPF support, dry it, and calcine it at 550℃ to form an inner catalytic layer.

[0109] The La / γ-Al2O3 is a commercially available material, with a composition of (4.5% La2O3, 95.5% Al2O3).

[0110] Step 2: Prepare a second slurry containing only coarse-grained alumina (D50=30μm), coat it onto the calcined inner catalyst support, dry it, and calcinate it again at 550℃ to form an outer trapping layer.

[0111] The total coating load and precious metal load in Comparative Example 1 are the same as those in Example 1.

[0112] Comparative Example 2:

[0113] The difference between Comparative Example 2 and Comparative Example 1 is that: after mixing the first and second slurries, they are ground to D10=0.8um, and the catalyst support is coated, dried and sintered.

[0114] Performance Testing and Result Analysis

[0115] Initial back pressure test: The exhaust back pressure of the fresh catalyst was measured under standard conditions (25°C, air flow rate 900 kg / h) using SUPERFLOW's SF-1020 back pressure testing equipment.

[0116] Particulate matter (PN) capture efficiency test: On a vehicle chassis, using equipment capable of detecting particles with a PN of 10 or higher, the initial particulate matter capture efficiency of the catalyst is measured under specific operating conditions. GB18352.6 - Emission limits and measurement methods for pollutants from light-duty vehicles (China Stage VI) (Exhaust emission test after cold start at ambient temperature (Type I)).

[0117] The test results are shown in the table below:

[0118]

[0119] The test results show that Example 1 achieves both low back pressure and high capture rate. This invention precisely controls the particle size distribution of the coating material to match the average pore size of the selected GPF white carrier. During the coating process, smaller particles can enter the carrier pores and adhere to the pore walls, primarily functioning to purify gaseous pollutants; while larger particles are intercepted on the outer walls and inlet areas of the carrier pores, forming a loose, porous interception layer for particle capture. Crucially, this interception layer itself possesses catalytic activity, not only efficiently capturing particulate matter including PN10, but also catalytically oxidizing the captured carbon soot particles, achieving "passive regeneration," and participating in the purification reaction of gaseous pollutants. Thus, a gradient functional structure of "inner catalysis, outer capture and catalysis" is spontaneously constructed through a single coating process.

[0120] Finally, it should be noted that although the above embodiments have been described in the description of this application, this should not limit the scope of patent protection of this application. Any technical solutions that are based on the essential concept of this application, utilize the content described in this application's description to make equivalent structural or procedural substitutions or modifications, or directly or indirectly implement the technical solutions of the above embodiments in other related technical fields, are all included within the scope of patent protection of this application.

Claims

1. A method for preparing a CGPF catalyst, characterized in that, Includes the following steps: S1: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are pulverized to a particle size D50 of 0.5-10 μm to obtain the first powder; the mass ratio of the rare earth element modified γ-alumina and cerium-zirconium composite oxide is 1-8:

2. S2: Rare earth element modified γ-alumina and cerium-zirconium composite oxide are mixed and then pulverized to a particle size D50 of 20-50 μm to obtain a second powder; the mass ratio of the modified γ-Al2O3 powder to the cerium-zirconium composite oxide is 1-8:

2. S3: Mix the first powder (S1) with deionized water and then ball mill for the first time for 20-180 min to obtain the first slurry; the solid content of the first slurry is 15-50 wt%, and the particle size (D50) of the particles in the first slurry is 0.5-5 μm; S4: Add the second powder of S2 to the first slurry of S3 and then perform a second ball milling. The second ball milling time is 60-180 minutes to obtain the second slurry. S5: Add the precious metal precursor and deionized water to the second slurry in S4, and stir for 180-600 min to obtain a composite slurry; the solid content of the composite slurry is 20-60 wt%. S6: The S5 composite slurry is coated onto the GPF white support to form a coating, thus obtaining a wet GGPF catalyst preform. S7: After drying the wet S6 GGPF catalyst blank, calcine it in air at 450-600℃ for 2-3 hours to obtain the CGPF catalyst.

2. The preparation method according to claim 1, characterized in that, The mass ratio of the first powder to the second powder is 1 to 5:

1.

3. The preparation method according to claim 1, characterized in that, In the rare earth element modified γ-alumina, the rare earth element is one or more of lanthanum, cerium, praseodymium, and magnesium; its doping amount is 5-30% of the mass of alumina.

4. The preparation method according to claim 1, characterized in that, The solid particles in the second slurry have a particle size of D10≤1.5μm, D90≥10μm, and D90 / D10>5.

5. The preparation method according to claim 1, characterized in that, The noble metal precursor is a soluble salt of a noble metal, and the noble metal includes one or more of Pt, Pd, Rh, and Ru.

6. The preparation method according to claim 1, characterized in that, The GPF white carrier is a wall-flow cordierite GPF blank carrier with a pore size of 10-20 μm.

7. The preparation method according to claim 1, characterized in that, Carboxymethyl cellulose was added as an additive during the first ball milling process, with an addition amount of 1-4 wt% of the first powder.

8. The preparation method according to claim 1, characterized in that, Step S6 involves vacuum suction coating.

9. A CGPF catalyst, characterized in that, The CGPF catalyst is prepared using the preparation method described in any one of claims 1-8.

10. The CGPF catalyst according to claim 9, characterized in that, The loading of the precious metal is 0.5-5.0 wt%.