A composite metal compound supported noble metal catalyst, its preparation method and application

By constructing a mesoporous composite metal compound support and the synergistic effect of noble metal nanoparticles, the problems of equipment corrosion, high separation cost and low product selectivity in the HMF oxidation to FDCA process are solved, realizing the application of a highly efficient and green catalyst.

CN123102349APending Publication Date: 2026-11-17HEFEI LEAF BIOTECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611379294.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing catalysts for the oxidation of HMF to FDCA have problems such as high risk of equipment corrosion, generation of salt wastewater, high separation and purification costs, and low product selectivity. In addition, ionic liquid solvents in alkali-free systems are expensive and difficult to separate products.

Method used

A co-precipitation-calcination method was used to construct a mesoporous composite metal compound support, such as ZnO-BaCO3, which was combined with highly dispersed noble metal nanoparticles. Localized mild alkaline sites were introduced on the catalyst surface through an impregnation-reduction method to achieve efficient and selective oxidation of HMF.

Benefits of technology

This method achieves efficient conversion of HMF to FDCA under alkali-free conditions, with FDCA yields reaching up to 93% and product purity reaching up to 99.9%. It avoids equipment corrosion and salt wastewater discharge, significantly reducing separation and purification costs, and provides a new solution for the green industrial production of FDCA.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102349A_ABST
    Figure CN123102349A_ABST
Patent Text Reader

Abstract

This invention relates to the field of catalytic materials technology, specifically to a composite metal compound-supported noble metal catalyst, its preparation method, and its application. The catalyst includes a support and a noble metal active component supported on the support. The support is a composite metal compound containing zinc and a composite element selected from at least one of barium, lanthanum, or bismuth. The noble metal active component is selected from at least one of palladium, platinum, ruthenium, or gold. This catalyst can efficiently catalyze the selective oxidation of HMF to FDCA under alkaline-free conditions, effectively avoiding problems such as equipment corrosion, environmental pollution, high separation costs, and low product selectivity, thus better meeting practical application needs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalytic materials technology, specifically to a composite metal compound supported noble metal catalyst, its preparation method, and its application. Background Technology

[0002] With the increasing depletion of fossil resources and the emergence of environmental pollution problems, the development and utilization of renewable biomass resources to produce high-value-added chemicals and fuels has become a core strategy for global sustainable development. 2,5-Furfurandicarboxylic acid (FDCA), as a bio-based alternative to terephthalic acid (PTA), can be used as a monomer to synthesize polymers such as polyesters, polyurethanes, polyamides, and polyimides. Among them, PEF (polyethylene 2,5-furandicarboxylate), constructed using FDCA as a monomer, is hailed as a next-generation polyester material with the potential to replace PET (polyethylene terephthalate), possessing excellent gas barrier properties and mechanical properties, and showing broad application prospects in bottle flakes, fibers, films, and packaging.

[0003] In recent years, the green synthesis of FDCA has attracted much attention, and the thermocatalytic oxidation of 5-hydroxymethylfurfural (HMF) to FDCA is the most promising route. However, the selective oxidation of HMF to FDCA faces many challenges, such as harsh reaction conditions, high difficulty in separation and purification, and high cost. Designing efficient and stable catalysts is a key challenge in the oxidation of HMF to FDCA.

[0004] Chinese patent application (publication number CN119775236A) describes the preparation of a cobalt-based catalyst (containing platinum active metal) via a reduction-impregnation method. In the presence of this catalyst and an alkaline oxidation system, high-efficiency and highly selective oxidation of HMF to FDCA is achieved. However, most reported HMF catalytic oxidation processes are conducted in the presence of a homogeneous alkali. Although the FDCA yield is relatively ideal, the use of alkaline additives necessitates acidification and separation after the reaction. This not only poses a risk of corrosion to the reaction equipment but also generates a large amount of saline wastewater, significantly increasing the separation and purification costs and environmental burden, thus limiting its industrial application prospects. More importantly, HMF degrades under alkaline conditions, resulting in side reactions and reduced product selectivity. Therefore, developing an efficient alkali-free catalytic oxidation system is of great significance for achieving the efficient and green conversion of HMF to FDCA and promoting its large-scale industrial application. Chinese patent (authorization announcement number CN108314667B) provides a method for preparing a non-alkaline system FDCA, which uses single oxides or composite oxides of non-precious metals such as cerium, iron, and zirconium as catalysts and ionic liquids as solvents to selectively oxidize and prepare HMF. Although using ionic liquids as solvents can avoid the use of strong bases, ionic liquids are expensive, and the separation and purification of the product from high-boiling-point ionic liquids is somewhat difficult. Summary of the Invention

[0005] To address the aforementioned issues, this invention provides a composite metal compound-supported noble metal catalyst that can efficiently catalyze the selective oxidation of HMF to FDCA under alkali-free conditions, effectively avoiding problems such as equipment corrosion, environmental pollution, high separation costs, and low product selectivity, thus better meeting practical application needs.

[0006] The present invention provides a composite metal compound supported noble metal catalyst, comprising a support and a noble metal active component supported on the support; the support is a composite metal compound containing zinc and a composite element, wherein the composite element is selected from at least one of barium, lanthanum or bismuth; and the noble metal active component is selected from at least one of palladium, platinum, ruthenium or gold.

[0007] To address the problems of high equipment corrosion risk, large amounts of salt wastewater generation, and high separation and purification costs in existing HMF oxidation processes for FDCA preparation, which generally rely on homogeneous alkali additives, as well as the easy degradation side reactions of HMF under alkaline conditions and reduced product selectivity, and the shortcomings of existing alkali-free systems such as high cost of ionic liquid solvents and difficulty in product separation, this invention constructs a composite metal compound carrier with a mesoporous structure (such as ZnO-BaCO3). By utilizing its solid alkali properties and the synergistic effect of highly dispersed noble metal nanoparticles (Au, Pt, etc.), it achieves efficient conversion of HMF to FDCA under alkali-free conditions. This effectively solves the problems of severe equipment corrosion, environmental unfriendliness, and high separation costs in traditional processes, and provides a highly promising new solution for the green industrial production of FDCA.

[0008] In one embodiment, the molar ratio of zinc to composite elements in the carrier is 1 to 10:1.

[0009] In one embodiment, the molar ratio of zinc to composite elements in the carrier is 2.5 to 6.5:1.

[0010] In one embodiment, the composite metal compound is at least one of ZnO-BaCO3, ZnO-La2O3, and ZnO-Bi2O3.

[0011] In one embodiment, the loading of the noble metal active component is 0.1% to 5% by mass of the catalyst.

[0012] In one embodiment, the loading of the noble metal active component is 0.2% to 1% by mass of the catalyst.

[0013] In one embodiment, the loading of the noble metal active component is 0.25% to 0.5% by mass of the catalyst.

[0014] In one embodiment, the catalyst satisfies at least one of the following conditions: (1) The catalyst has a mesoporous structure; (2) The average pore size of the catalyst is 2–50 nm; (3) The specific surface area of ​​the catalyst is 15-25 m². 2 / g (4) The pore volume of the catalyst is 0.100-0.150 cm³. 3 / g.

[0015] Another aspect of the present invention provides a method for preparing a noble metal catalyst supported on a composite metal compound, comprising the following steps: An alkaline solution was added to a mixed salt solution containing zinc and other elements, and the mixture was stirred, aged, precipitated, separated, and calcined to obtain a carrier. A noble metal salt solution was added to the support, followed by impregnation, separation, reduction, washing, and drying to obtain a noble metal catalyst supported on a composite metal compound.

[0016] In one embodiment, the mixed salt solution includes a zinc salt and a composite metal salt, wherein the composite metal salt is selected from at least one of barium salt, lanthanum salt, or bismuth salt.

[0017] In one embodiment, the molar ratio of the zinc salt to the composite metal salt is 1 to 10:1.

[0018] In one embodiment, the molar ratio of the zinc salt to the composite metal salt is 2.5 to 6.5:1.

[0019] In one embodiment, the alkaline solution is an aqueous solution comprising at least one alkali, such as sodium hydroxide, sodium carbonate, or ammonia.

[0020] In one embodiment, the concentration of the alkaline solution is 0.5 to 1 mol / L.

[0021] In one embodiment, the alkaline solution is at least one of an aqueous solution of sodium hydroxide, an aqueous solution of sodium carbonate, or an ammonia solution.

[0022] In one embodiment, the alkaline solution is a mixed aqueous solution comprising sodium hydroxide and sodium carbonate.

[0023] In one embodiment, the mass ratio of sodium hydroxide to sodium carbonate is 1:1-2.

[0024] In one embodiment, a surfactant is also added to the mixed salt solution.

[0025] In one embodiment, the surfactant includes at least one of polyethylene glycol, hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, or polyvinylpyrrolidone.

[0026] In one embodiment, the molar ratio of the surfactant to the metal salt is 0.001 to 0.2:1.

[0027] In one embodiment, the stirring aging time is 1 to 6 hours, the calcination temperature is 300 to 700°C, and the calcination time is 3 to 6 hours.

[0028] In one embodiment, the stirring and aging time is 1.5 to 3 hours; the calcination temperature is 400 to 550°C; and the calcination time is 2 to 4 hours.

[0029] In one embodiment, the noble metal salt solution is an aqueous solution of a noble metal salt including at least one of chloropalladium acid, chloroauric acid, chloroplatinic acid, and ruthenium chloride.

[0030] In one embodiment, the impregnation includes the following steps: adding the carrier to a noble metal salt solution under stirring for 3 to 5 hours.

[0031] In one embodiment, the separation includes filtration, washing, and drying.

[0032] In one embodiment, the reduction includes the following steps: reduction in a tube furnace under a hydrogen-nitrogen atmosphere for 2-6 hours at a reduction temperature of 200-400°C.

[0033] In one embodiment, the volume ratio of hydrogen to nitrogen is 1 to 19:1.

[0034] In one embodiment, the reduction temperature is 200–300°C, and the reduction time is 2–4 hours.

[0035] This invention constructs a composite metal compound support containing at least one element from Zn and Ba / La / Bi via a co-precipitation-calcination method. The solid base properties of the support introduce locally mild alkaline sites on the catalyst surface, replacing the function of traditional homogeneous bases. Then, highly dispersed noble metal nanoparticles are loaded onto the support surface via an impregnation-reduction method. Strong interactions and synergistic catalytic effects occur between the noble metal and the functionalized composite support. The alkaline sites on the support promote the adsorption of HMF and the breaking of CH and OH bonds and the oxidation of aldehyde groups, while the active sites of the noble metal promote the activation of oxygen molecules. Together, they achieve highly efficient and selective oxidation of HMF to FDCA under alkaline conditions.

[0036] The third aspect of this invention provides the application of a composite metal compound supported noble metal catalyst in the catalytic oxidation of 5-hydroxymethylfurfural to prepare 2,5-furandicarboxylic acid under alkali-free conditions.

[0037] In one embodiment, the method for preparing the 2,5-furandicarboxylic acid includes the following steps: adding the composite metal compound-supported noble metal catalyst to an aqueous solution of 5-hydroxymethylfurfural, introducing an oxygen-containing reaction gas to adjust the reaction pressure, and heating to the reaction temperature to carry out the reaction.

[0038] In one embodiment, the mass concentration of the 5-hydroxymethylfurfural aqueous solution is 1% to 10%.

[0039] In one embodiment, the mass ratio of 5-hydroxymethylfurfural to the catalyst is 1:(1-5).

[0040] In one embodiment, the reaction temperature is 80–140°C; the reaction pressure is 1–5 MPa; and the reaction time is 1–10 h.

[0041] In one embodiment, the reaction temperature is 100–120°C; the reaction pressure is 1–3 MPa; and the reaction time is 4–8 h.

[0042] In one embodiment, the oxygen-containing reactive gas is pure oxygen or air.

[0043] In one embodiment, the reaction is carried out in a high-pressure reactor.

[0044] The catalyst of this invention can efficiently catalyze the oxidation of HMF to FDCA under alkali-free, aqueous conditions, with an FDCA yield of up to 93% and a product purity of up to 99.9%. It eliminates the need for homogeneous alkali, fundamentally avoiding equipment corrosion and salt wastewater discharge, and significantly reducing subsequent separation and purification costs and environmental burden. The catalyst possesses a mesoporous structure and good structural stability, with highly dispersed precious metals and abundant active sites, providing a highly promising new catalyst solution for the green industrial production of FDCA.

[0045] Beneficial effects 1. This invention provides a composite metal compound supported noble metal catalyst, which can efficiently catalyze the selective oxidation of HMF to FDCA under alkali-free conditions, effectively avoiding problems such as equipment corrosion, environmental pollution, high separation costs, and low product selectivity, and better meeting the needs of practical applications.

[0046] 2. This invention constructs a composite metal compound carrier with a mesoporous structure (such as ZnO-BaCO3), and utilizes its solid alkali properties and the synergistic effect of highly dispersed noble metal nanoparticles (Au, Pt, etc.) to achieve efficient conversion of HMF to FDCA under alkali-free conditions. This effectively solves the problems of severe equipment corrosion, environmental unfriendliness, and high separation costs in traditional processes, and provides a highly promising new solution for the green industrial production of FDCA.

[0047] 3. This invention constructs a composite metal compound support containing at least one element from Zn and Ba / La / Bi via a co-precipitation-calcination method. The solid base properties of the support introduce locally mild alkaline sites on the catalyst surface, replacing the function of traditional homogeneous bases. Then, highly dispersed noble metal nanoparticles are loaded onto the support surface via an impregnation-reduction method. Strong interactions and synergistic catalytic effects occur between the noble metal and the functionalized composite support. The alkaline sites on the support promote the adsorption of HMF and the breaking of CH and OH bonds and the oxidation of aldehyde groups, while the active sites of the noble metal promote the activation of oxygen molecules. Together, they achieve highly efficient and selective oxidation of HMF to FDCA under alkaline conditions.

[0048] 4. The catalyst of this invention can efficiently catalyze the oxidation of HMF to FDCA under alkali-free and aqueous conditions, with an FDCA yield of up to 93% and a product purity of up to 99.9%. It eliminates the need for homogeneous alkali, fundamentally avoiding equipment corrosion and salt wastewater discharge, and significantly reducing subsequent separation and purification costs and environmental burden. The catalyst possesses a mesoporous structure and good structural stability, with highly dispersed precious metals and abundant active sites, providing a highly promising new catalyst solution for the green industrial production of FDCA. Attached Figure Description

[0049] Figure 1 The BET adsorption-desorption isotherm spectrum of the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1 of this invention; Figure 2 The XRD pattern of the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1 of this invention; Figure 3 The XPS full spectrum of the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1 of this invention; Figure 4 The fine XPS spectrum of Au 4f in the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1 of this invention; Figure 5 The image shows a 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1 of this invention under a 2 μm scale. Figure 6The image shows the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1 of this invention under a 500 nm scale. Detailed Implementation

[0050] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.

[0051] In the following examples, the purity of FDCA was determined by high performance liquid chromatography (HPLC). The detection conditions were as follows: Hitachi L2000 HPLC System, Alltech C18 column; mobile phase: methanol:0.5wt% trifluoroacetic acid aqueous solution = 20:80 (volume ratio); flow rate 1.0 mL / min; column temperature 30℃; detector: DAD, detection wavelength 264 nm.

[0052] Example 1 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), comprising a support (ZnO-BaCO3) and a noble metal active component (Au) supported on the support. The loading of the noble metal active component is 0.5% by mass of the catalyst.

[0053] Another aspect of this embodiment provides a method for preparing a noble metal catalyst supported on a composite metal compound, comprising the following steps: Zinc chloride (5.11 g, 0.037 mol), barium chloride dihydrate (3.08 g, 0.013 mol), and 0.5 g PEG-1000 were dissolved in 50 mL of pure water to prepare a mixed salt solution A. Sodium hydroxide (2 g, 0.05 mol) and sodium carbonate (4 g, 0.037 mol) were dissolved in 150 mL of pure water to prepare an alkaline solution B. Under stirring, alkaline solution B was added dropwise to mixed salt solution A for co-precipitation. The pH of the solution was measured with a pH meter, and the alkaline solution was continuously added until the pH > 11, at which point the addition was stopped. After aging with stirring for 2 hours, the precipitate was filtered, and the filter cake was washed with pure water until neutral and dried at 100 °C for 12 hours. After drying, it was calcined at 500 °C for 3 hours to obtain a composite metal oxide support. This support (5 g) was added to 40 mL of chloroauric acid aqueous solution with a concentration of 0.00108 g / mL, stirred continuously for 3 hours, filtered, and dried at 100 °C for 12 hours. After drying, the catalyst was reduced in a tube furnace at 250°C for 3 hours under an atmosphere of 10% (v / v) H2-90% (v / v) N2 to obtain a 0.5% Au / ZnO-BaCO3 catalyst.

[0054] The third aspect of this embodiment provides a method for preparing FDCA by supporting a noble metal catalyst with a composite metal compound, comprising the following steps: HMF (0.6 g, 4.8 mmol), 30 g of water, and 1.5 g of the above-mentioned composite metal compound-supported noble metal catalyst were added to a reaction vessel and reacted at 110 °C and 1 MPa O2 for 4 h. After the reaction was completed, the catalyst was separated by filtration, and the reaction solution was analyzed by HPLC. The FDCA yield was 91%, and the purity was 99.8%. Example 2 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-La2O3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-La2O3) and a noble metal active component (Au) supported on the support. In the preparation method, barium chloride dihydrate (3.08 g, 0.013 mol) is replaced with lanthanum nitrate hexahydrate (6.93 g, 0.016 mol) to prepare the 0.5% Au / ZnO-La2O3 catalyst. The 0.5% Au / ZnO-La2O3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 87%, and the purity is 99.6%.

[0055] Example 3 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-Bi2O3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-Bi2O3) and a noble metal active component (Au) supported on the support. In the preparation method, barium chloride dihydrate (3.08 g, 0.013 mol) is replaced with bismuth nitrate pentahydrate (5.34 g, 0.011 mol) to prepare the 0.5% Au / ZnO-Bi2O3 catalyst. The 0.5% Au / ZnO-Bi2O3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 77%, and the purity is 99.8%.

[0056] Example 4 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Pt / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-BaCO3) and a noble metal active component (Pt) supported on the support. In the preparation method, the 0.00108 g / mL chloroauric acid aqueous solution is replaced with a 0.0013 g / mL chloroplatinic acid aqueous solution to prepare the 0.5% Pt / ZnO-BaCO3 catalyst. The 0.5% Pt / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 89%, and the purity is 99.9%.

[0057] Example 5 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Ru / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-BaCO3) and a noble metal active component (Ru) supported on the support. In the preparation method, the 0.00108 g / mL chloroauric acid aqueous solution is replaced with a 0.00128 g / mL ruthenium chloride aqueous solution to prepare the 0.5% Ru / ZnO-BaCO3 catalyst. The 0.5% Ru / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 80%, and the purity is 99.7%.

[0058] Example 6 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Pd / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-BaCO3) and a noble metal active component (Pd) supported on the support. In the preparation method, the 0.00108 g / mL chloroauric acid aqueous solution is replaced with a 0.00147 g / mL chloropalladic acid aqueous solution to prepare the 0.5% Pd / ZnO-BaCO3 catalyst. The 0.5% Pd / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 81%, and the purity is 98.9%.

[0059] Example 7 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Pt / ZnO-La2O3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-La2O3) and a noble metal active component (Pt) supported on the support. In the preparation method, barium chloride dihydrate (3.08 g, 0.013 mol) is replaced with lanthanum nitrate hexahydrate (6.93 g, 0.016 mol), and the 0.00108 g / mL chloroauric acid aqueous solution is replaced with a 0.0013 g / mL chloroplatinic acid aqueous solution to prepare the 0.5% Pt / ZnO-La2O3 catalyst. The 0.5% Pt / ZnO-La2O3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 85%, and the purity is 99.2%.

[0060] Example 8 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Pt / ZnO-Bi2O3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-Bi2O3) and a noble metal active component (Pt) supported on the support. In the preparation method, barium chloride dihydrate (3.08 g, 0.013 mol) is replaced with bismuth nitrate pentahydrate (5.34 g, 0.011 mol), and the 0.00108 g / mL chloroauric acid aqueous solution is replaced with a 0.0013 g / mL chloroplatinic acid aqueous solution to prepare the 0.5% Pt / ZnO-Bi2O3 catalyst. The 0.5% Pt / ZnO-Bi2O3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 71%, and the purity is 99.8%.

[0061] Example 9 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Ru / ZnO-La2O3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-La2O3) and a noble metal active component (Ru) supported on the support. In the preparation method, barium chloride dihydrate (3.08 g, 0.013 mol) is replaced with lanthanum nitrate hexahydrate (6.93 g, 0.016 mol), and the 0.00108 g / mL chloroauric acid aqueous solution is replaced with a 0.00128 g / mL ruthenium chloride aqueous solution to prepare the 0.5% Ru / ZnO-La2O3 catalyst. The 0.5% Ru / ZnO-La2O3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 79%, and the purity is 98.8%.

[0062] Example 10 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Ru / ZnO-Bi2O3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that it includes a support (ZnO-Bi2O3) and a noble metal active component (Ru) supported on the support. In the preparation method, barium chloride dihydrate (3.08 g, 0.013 mol) is replaced with bismuth nitrate pentahydrate (5.34 g, 0.011 mol), and 0.00108 g / mL chloroauric acid aqueous solution is replaced with 0.00128 g / mL ruthenium chloride aqueous solution to prepare the 0.5% Ru / ZnO-Bi2O3 catalyst. The 0.5% Ru / ZnO-Bi2O3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are the same as in Example 1. After the reaction, the FDCA yield is measured to be 69%, and the purity is 98.6%.

[0063] Example 11 This embodiment provides a composite metal compound supported noble metal catalyst (0.25% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the concentration of 0.00108 g / mL chloroauric acid aqueous solution is replaced with 0.00054 g / mL to prepare the 0.25% Au / ZnO-BaCO3 catalyst. The 0.25% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 85%, and the purity is 99.6%.

[0064] Example 12 This embodiment provides a composite metal compound supported noble metal catalyst (0.35% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the concentration of the 0.00108 g / mL chloroauric acid aqueous solution is replaced with 0.00077 g / mL to prepare the 0.35% Au / ZnO-BaCO3 catalyst. The 0.35% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 93%, and the purity is 98.4%.

[0065] Example 13 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the aging time is replaced with 1 hour to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the other conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 83%, and the purity is 99.4%.

[0066] Example 14 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the aging time is replaced with 5 hours to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 86%, and the purity is 98.5%.

[0067] Example 15 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the calcination temperature is replaced with 350℃ to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 88%, and the purity is 98.4%.

[0068] Example 16 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the calcination temperature is replaced with 600℃ to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 72%, and the purity is 99.5%.

[0069] Example 17 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the calcination time is replaced with 4 hours to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 88%, and the purity is 99.1%.

[0070] Example 18 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the calcination time is replaced with 5 hours to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 83%, and the purity is 99.0%.

[0071] Example 19 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the stirring time for adding the composite metal oxide support to the chloroauric acid aqueous solution is replaced with 5 hours to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 88%, and the purity is 99.7%.

[0072] Example 20 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the reduction temperature is replaced with 200℃ to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the other conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 83%, and the purity is 98.3%.

[0073] Example 21 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the reduction temperature is replaced with 350℃ to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 86%, and the purity is 98.8%.

[0074] Example 22 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the reduction time is replaced by 2 hours to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the other conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 83%, and the purity is 99.7%.

[0075] Example 23 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the reduction time is replaced with 4.5 h to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 87%, and the purity is 99.5%.

[0076] Example 24 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that PEG-1000 is replaced with hexadecyltrimethylammonium bromide to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst is used in the catalytic preparation of FDCA, and the remaining conditions are consistent with Example 1. After the reaction, the FDCA yield is measured to be 85%, and the purity is 98.5%.

[0077] Example 25 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that PEG-1000 is replaced with sodium dodecylbenzenesulfonate to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst was used in the catalytic preparation of FDCA, and the remaining conditions were consistent with Example 1. After the reaction, the FDCA yield was measured to be 79%, and the purity was 99.7%.

[0078] Example 26 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method, and its application. The specific implementation method is the same as in Example 1, except that the mass of PEG-1000 is replaced with 5g to prepare the 0.5% Au / ZnO-BaCO3 catalyst. The 0.5% Au / ZnO-BaCO3 catalyst was used in the catalytic preparation of FDCA, and the remaining conditions were consistent with Example 1. After the reaction, the FDCA yield was measured to be 93%, and the purity was 98.3%.

[0079] Example 27 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that 30g of water is replaced with 60g in the catalytic preparation of FDCA. The other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 89% and the purity was 98.5%.

[0080] Example 28 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that 30g of water is replaced with 7.5g in the catalytic preparation of FDCA. The other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 82% and the purity was 99.4%.

[0081] Example 29 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that in the catalytic preparation of FDCA, 1.5g of composite metal compound supported noble metal catalyst is replaced with 0.6g. The other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 74% and the purity was 97.8%.

[0082] Example 30 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that in the catalytic preparation of FDCA, 1.5g of composite metal compound supported noble metal catalyst is replaced with 2.6g. The other conditions are the same as in Example 1. After the reaction, the yield of FDCA is measured to be 88% and the purity is 98.6%.

[0083] Example 31 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that the reaction pressure is replaced with 2 MPa in the catalytic preparation of FDCA, and the other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 92% and the purity was 98.7%.

[0084] Example 32 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that the reaction pressure is replaced with 4 MPa in the catalytic preparation of FDCA, and the other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 88% and the purity was 98.9%.

[0085] Example 33 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that the reaction temperature is replaced with 90℃ in the catalytic preparation of FDCA, and the other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 75% and the purity was 99.6%.

[0086] Example 34 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that the reaction temperature is replaced with 140℃ in the catalytic preparation of FDCA, and the other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 83% and the purity was 99.7%.

[0087] Example 35 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that oxygen is replaced with air in the catalytic preparation of FDCA. The other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 75% and the purity was 98.0%.

[0088] Example 36 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that the reaction time in the catalytic preparation of FDCA is replaced with 3h, and the other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 85% and the purity was 98.2%.

[0089] Example 37 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as that in Example 1, except that the reaction time in the catalytic preparation of FDCA is replaced with 6 hours. The other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 93% and the purity was 99.3%.

[0090] Example 38 This embodiment provides a composite metal compound supported noble metal catalyst (0.5% Au / ZnO-BaCO3 catalyst), its preparation method and application. The specific implementation method is the same as in Example 1, except that the reaction time in the catalytic preparation of FDCA is replaced with 9 hours. The other conditions are the same as in Example 1. After the reaction, the yield of FDCA was measured to be 86% and the purity was 99.7%.

[0091] Performance testing The catalyst samples prepared in the examples were subjected to performance tests, and the test results were analyzed. Taking the catalyst in Example 1 as an example, the following results were obtained: Figures 1-6 Characterization diagram.

[0092] Figure 1 This is the BET (Brunauer-Emmett-Teller) adsorption-desorption isotherm spectrum of the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1. Figure 1 The characterization results show that the specific surface area of ​​this catalyst is 18.27 m². 2 / g, pore volume is 0.121 cm³ 3The catalyst exhibits a surface area of ​​approximately 27.60 nm / g, with an average pore size falling within the mesoporous range of 2-50 nm. Simultaneously, the adsorption-desorption isotherm displays typical Type IV characteristics with a distinct hysteresis loop, indicating that the catalyst is a mesoporous material formed by the stacking of nanoparticles, with a well-developed mesoporous network within the support. The moderate specific surface area and well-developed mesoporous structure facilitate mass transfer between reactants and products within the catalyst and provide suitable space for the dispersion of active gold nanoparticles.

[0093] Figure 2 This is the XRD (X-ray diffraction) pattern of the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1. Figure 2 The characterization results show that the main diffraction peaks of the catalyst highly match the standard cards of BaCO3 and ZnO. Strong diffraction peaks appearing at 24°, 28-29°, 42°, 45°, 52°, 55°, 60°, 68°, 73°, and 79° in the spectrum are consistent with the characteristic peaks of orthorhombic BaCO3 in terms of position and relative intensity. Diffraction peaks at 47.6°, 56.6°, 62.9°, 66.4°, 68.0°, and 69.1° in the spectrum are consistent with the standard diffraction data of hexagonal ZnO. This indicates the presence of well-crystallized BaCO3 and ZnO with well-defined crystal structures in the sample. Furthermore, no characteristic diffraction peaks of Au were observed in the spectrum, indicating that Au exists in the form of highly dispersed ultrasmall nanoparticles or atomic clusters.

[0094] Figure 3 This is the X-ray photoelectron spectroscopy (XPS) spectrum of the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1. The spectrum shows multiple distinct peaks, indicating the presence of various elements in the catalyst. The characteristic photoelectron peaks of Zn 2p, Ba 3d, O 1s, C 1s, and Au 4f are clearly visible in the spectrum, indicating the presence of Zn, Ba, O, C, and Au elements in the catalyst. Based on the fine spectrum of Au 4f (… Figure 4 It can be seen that the gold element in the sample is mainly in the elemental metallic state (Au). 0 The presence of these elements results in the formation of gold nanoparticles.

[0095] Figure 5-6 These are scanning electron microscope (SEM) images of the 0.5% Au / ZnO-BaCO3 catalyst prepared in Example 1. Figure 5-6 Characterization results show that the catalyst support is composed of a large number of irregularly shaped nanoparticles that are tightly packed and aggregated, forming micron-sized secondary particles. High-resolution images show that these primary nanoparticles are nearly spherical or short rod-shaped, and the stacking between the nanoparticles forms abundant interparticle pores, providing a large number of surface sites for loading the active metal gold.

[0096] This catalyst, with its unique mesoporous structure, synergistic effect between the supports, and highly dispersed active centers, can efficiently catalyze the oxidation of HMF to FDCA. HMF molecules can rapidly reach the interior of the catalyst through the well-developed mesoporous network and be adsorbed and activated by the basic sites of BaCO3 on the support surface. BaCO3, as a solid base, can activate the hydroxyl and aldehyde groups of HMF under conditions without added base (such as NaOH) or under mild conditions, while the presence of carbonate helps to inhibit the formation of acidic byproducts (such as levulinic acid). ZnO, as a hexagonal semiconductor, forms a stable interface with BaCO3, improving the structural stability of the catalyst in the reaction system. In addition, Au nanoparticles are highly dispersed on the support surface, improving the adsorption capacity for oxygen and HMF. Therefore, this synergistic effect between the support and the noble metal makes it possible to efficiently convert HMF under alkaline conditions.

Claims

1. A composite metal compound supported noble metal catalyst, characterized in that, It includes a carrier and a noble metal active component loaded on the carrier; the carrier is a composite metal compound containing zinc and a composite element, wherein the composite element is selected from at least one of barium, lanthanum or bismuth; the noble metal active component is selected from at least one of palladium, platinum, ruthenium or gold.

2. The composite metal compound supported noble metal catalyst according to claim 1, characterized in that, The molar ratio of zinc to composite elements in the carrier is 1 to 10:

1.

3. The composite metal compound supported noble metal catalyst according to claim 1, characterized in that, The composite metal compound is at least one of ZnO-BaCO3, ZnO-La2O3, and ZnO-Bi2O3.

4. The composite metal compound supported noble metal catalyst according to claim 1, characterized in that, The loading of the noble metal active component is 0.1% to 5% by mass of the catalyst.

5. The composite metal compound supported noble metal catalyst according to claim 1, characterized in that, The catalyst satisfies at least one of the following conditions: (1) The catalyst has a mesoporous structure; (2) The average pore size of the catalyst is 2–50 nm; (3) The specific surface area of ​​the catalyst is 15-25 m². 2 / g (4) The pore volume of the catalyst is 0.100-0.150 cm³. 3 / g.

6. A method for preparing a noble metal catalyst supported on a composite metal compound according to any one of claims 1-5, characterized in that, Includes the following steps: An alkaline solution was added to a mixed salt solution containing zinc and other elements, and the mixture was stirred, aged, precipitated, separated, and calcined to obtain a carrier. A noble metal salt solution was added to the support, followed by impregnation, separation, reduction, washing, and drying to obtain a noble metal catalyst supported on a composite metal compound.

7. The preparation method according to claim 6, characterized in that, The mixed salt solution also contains a surfactant, which includes at least one of polyethylene glycol, hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, or polyvinylpyrrolidone.

8. The preparation method according to claim 6, characterized in that, The stirring and aging time is 1 to 6 hours, and the calcination temperature is 300 to 700°C; the calcination time is 3 to 6 hours.

9. The application of a composite metal compound supported noble metal catalyst according to any one of claims 1-5 in the catalytic oxidation of 5-hydroxymethylfurfural to prepare 2,5-furandicarboxylic acid under alkali-free conditions.

10. The application according to claim 9, characterized in that, The preparation method of the 2,5-furandicarboxylic acid includes the following steps: adding the composite metal compound supported on a noble metal catalyst to an aqueous solution of 5-hydroxymethylfurfural, introducing an oxygen-containing reaction gas to adjust the reaction pressure, and heating to the reaction temperature to carry out the reaction.

Citation Information

Patent Citations

  • A method for preparing bio-based 2,5-furandicarboxylic acid in a non-alkaline system

    CN108314667B

  • A method for synthesizing 2,5-furandicarboxylic acid by highly selective oxidation of 5-hydroxymethylfurfural

    CN119775236A