Nickel-based magnesium aluminum spinel catalyst and its preparation method
The preparation of nickel-based magnesium-aluminum spinel catalysts by a one-step co-precipitation and one-step calcination method solves the problems of process complexity and stability of existing nickel-based catalysts, achieves stability and high activity during long-term operation at high temperatures, reduces production costs, and is suitable for industrial applications.
Patent Information
- Application Number
- CN202611019507.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing nickel-based methane dry reforming catalysts suffer from problems such as complex processes, high costs, poor stability, easy carbon deposition, and weak industrial adaptability. In particular, the agglomeration and sintering of active components caused by traditional precursors, as well as the reliance on precious metals or rare earth additives, increase costs.
Nickel-based magnesium-aluminum spinel catalysts were prepared by a one-step co-precipitation and one-step calcination method. MgAl2O4 spinel supports were synthesized by directional synthesis using hydroxide-type precursors. The nickel component was highly dispersed and anchored in the crystal lattice, avoiding high-temperature agglomeration, simplifying the process and reducing costs.
This approach achieves long-term stability and high activity of the catalyst at high temperatures, simplifies the preparation process, reduces production costs, and ensures the consistency of catalyst structure and performance, meeting industrial requirements.
Smart Images

Figure CN123102352A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of methane dry reforming reaction technology, and in particular to a nickel-based magnesium aluminum spinel catalyst and its preparation method. Background Technology
[0002] Dry reforming of methane (DRM) is a crucial process for converting methane and carbon dioxide into syngas (CO + H2), which is of great significance for achieving efficient utilization of carbon resources and carbon neutrality. Currently, nickel-based catalysts have become the mainstream candidate catalysts for dry reforming of methane due to their low cost and high catalytic activity. However, existing nickel-based catalysts generally suffer from the following technical drawbacks: (1) Existing technologies mostly use magnesium aluminum hydrotalcite with carbonate or bicarbonate as interlayer anions as precursors. CO2 is released during the calcination process, and the product is prone to forming MgO-Al2O3 solid solution with poor thermal stability, which easily leads to agglomeration and sintering of active components; (2) The preparation process generally relies on complex procedures of "multi-step precipitation, secondary calcination, and additive impregnation / coating". For example, the hydrotalcite is first calcined to obtain oxide intermediates, and then the additives are impregnated and calcined again. The process control is difficult and the production cost is high; (3) The active components have poor dispersion and are prone to carbonization and sintering under high temperature reaction conditions, which leads to rapid decay of catalytic activity and significant performance decline after the space velocity increases; (4) Some technologies use toxic coated precursors, and the waste liquid needs special treatment; core-shell structure and multi-metal alloy catalysts are difficult to guarantee the consistency of structure and performance during large-scale production, and the reliance on precious metals or rare earth additives leads to high costs.
[0003] Therefore, there is an urgent need for a nickel-based catalyst technology for dry reforming of methane that is simple in process, low in cost, has excellent stability, and is easy to industrialize. Summary of the Invention
[0004] In view of the above problems, the present invention provides a nickel-based magnesium aluminum spinel catalyst and its preparation method to solve at least one problem existing in the prior art.
[0005] In a first aspect, the present invention protects a nickel-based magnesium aluminum spinel catalyst, comprising a MgAl2O4 spinel single-phase support and a nickel component supported on the MgAl2O4 spinel single-phase support, wherein the nickel component is in the form of metallic Ni. 0 It exists in the form of NiO and / or NiO.
[0006] Further, preferably, the nickel content in the nickel-based magnesium aluminum spinel catalyst is 5-15 wt%.
[0007] Further, preferably, the catalyst has a BET specific surface area of 80~140 m² / g and a pore size of 5~15 nm.
[0008] Secondly, this invention protects a method for preparing a nickel-based magnesium-aluminum spinel catalyst, comprising: weighing a specified amount of soluble magnesium salt, soluble aluminum salt, and soluble nickel salt to prepare a mixed salt solution; preparing an alkaline precipitant; wherein the alkaline precipitant is one or more of sodium hydroxide, potassium hydroxide, and ammonia water; adding the mixed salt solution and the alkaline precipitant dropwise together, and carrying out a co-precipitation reaction under a pH of 9.0~11.0 to obtain a precipitate slurry; aging the precipitate slurry, and washing and drying it to obtain a magnesium-aluminum-nickel layered double hydroxide precursor; calcining the magnesium-aluminum-nickel layered double hydroxide precursor in air at a temperature of 600~900℃ for 2~8 h to obtain a nickel-based magnesium-aluminum spinel catalyst.
[0009] It should be noted that the spinel support is obtained by one-step calcination and directional crystallization of a hydroxide-type magnesium aluminum nickel layered double hydroxide precursor. This directionally transforms the precursor into a support with MgAl2O4 spinel as the dominant crystalline phase, resulting in a highly dispersed nickel component anchored by the spinel lattice. Specifically, only hydroxide ions are directionally synthesized in the hydroxide-type magnesium aluminum nickel layered double hydroxide precursor. In the actual implementation process, since the precipitation preparation process does not isolate air, carbon dioxide, which accounts for approximately 0.04% of the volume in the atmosphere, can react with the alkaline precipitant to form carbonates; that is, carbonate hydroxides may also be generated due to CO2 in the air. However, the concentration of CO2 in the air is low, and the resulting carbonate impurities are present in extremely low amounts in the precursor, below the XRD phase detection limit, and will not affect the main crystalline phase of the product. Furthermore, catalyst performance evaluation data also indicate that this trace amount of carbonate has no adverse effect on catalytic activity or stability.
[0010] Further, preferably, the soluble magnesium salt is one or more of magnesium nitrate, magnesium acetate, magnesium sulfate, and magnesium chloride.
[0011] Further, preferably, the soluble nickel salt is one or more of nickel nitrate, nickel acetate, nickel sulfate, and nickel chloride.
[0012] Further, preferably, the soluble aluminum salt is one or more of aluminum nitrate, aluminum sulfate, aluminum chloride, and aluminum acetate.
[0013] Furthermore, preferably, in the step of washing and drying the magnesium-aluminum-nickel layered double hydroxide precursor and then calcining it in an air atmosphere, the calcination heating rate is 1~10℃ / min.
[0014] Further, preferably, in the step of mixing the salt solution, the molar ratio of magnesium to aluminum is 0.35 to 1.0.
[0015] Thirdly, this invention protects a dry reforming method for methane, which uses the nickel-based magnesium-aluminum spinel catalyst described above to react methane and carbon dioxide at 700-850°C.
[0016] Specifically, the catalyst is not prone to sintering or carbon buildup at high temperatures of 700-850°C in the dry reforming reaction of methane, and has long-term operational stability.
[0017] This invention provides a nickel-based magnesium-aluminum spinel catalyst and its preparation method. Addressing the shortcomings of existing nickel-based methane dry reforming catalysts, such as complex processes, high costs, poor high-temperature stability, easy carbon deposition, weak industrial adaptability, and insufficient environmental friendliness, this invention achieves a technological breakthrough through directional design of hydroxyl-type precursors and optimized, simplified processes. Specific beneficial effects are as follows: (1) The present invention can complete the catalyst preparation by one-step co-precipitation and one-step calcination. No secondary calcination, no addition of precious metals or rare earth additives, and no surface coating treatment are required. The process flow is significantly simplified and energy consumption and raw material costs are reduced. The process parameters are highly controllable. The steps that require strict process conditions, such as core-shell structure and pH swing, are eliminated in the existing technology. The catalyst structure and performance can still be kept stable during scale-up production, and it has good prospects for industrial application.
[0018] (2) The present invention uses a hydroxide-type precursor, which is different from the traditional carbonate-type precursor, to obtain a MgAl2O4 spinel single-phase support through directional synthesis. This support has a rigid crystal structure and extremely high thermal stability, which can effectively anchor nickel species and prevent them from migrating, agglomerating and sintering in the high-temperature reaction at around 800℃, thus fundamentally ensuring the long-term operational stability of the catalyst.
[0019] (3) The present invention enables the nickel active component to be highly dispersed in an ultrafine state through the atomic-level uniform dispersion of the precursor and the spinel lattice confinement effect, and forms a strong interaction with the spinel support. It is not easy to migrate or agglomerate at high temperatures of 700~850℃. At the same time, the stable support surface structure can inhibit the deep cracking of methane and significantly reduce the carbon deposition rate. It overcomes the defect of easy carbon deposition and deactivation of single metal nanosheet catalysts in the prior art, and ensures that the catalyst can maintain high activity under high space velocity and high temperature industrial conditions.
[0020] (4) The entire preparation process of the present invention uses only conventional inorganic salts and alkalis, without using toxic or expensive organometallic precursors such as aluminum isopropoxide and tetrabutyl titanate, and does not rely on precious metals or rare earth additives such as ruthenium and yttrium; the roasting process only releases water vapor and there is no emission of toxic gases. The production process is green and safe, which is in line with the development trend of low carbon and clean chemical industry.
[0021] (5) By strictly controlling the core parameters in the precipitation process, this invention can stably obtain a carrier structure with highly crystalline MgAl2O4 spinel as the dominant crystal phase and extremely low impurity phase content, which solves the problem of catalyst performance fluctuation caused by existing complex processes and ensures the consistency and reproducibility of product performance in large-scale production. Attached Figure Description
[0022] Figure 1 The N2 adsorption-desorption isotherm of the nickel-based magnesium-aluminum spinel catalyst prepared in Example 1.
[0023] Figure 2 The stability graph shows the nickel-based magnesium-aluminum spinel catalyst prepared in Example 1 after nearly 800 hours of operation in a methane dry reforming process.
[0024] Figure 3 The XRD patterns are those of the nickel-based magnesium-aluminum spinel catalyst prepared in Example 1 and the nickel-based magnesium-aluminum spinel catalyst prepared in Comparative Example 1. Detailed Implementation
[0025] The present invention will be described in more detail with reference to the following embodiments. However, the scope of protection of the present invention is not limited to the following embodiments.
[0026] The MgAl2O4 spinel single-phase support was analyzed by X-ray diffraction (XRD). Its diffraction pattern showed only characteristic peaks of MgAl2O4 spinel; characteristic peaks of MgO, Al2O3 or MgO-Al2O3 solid solutions, and carbonate hydroxides were not observed. MgAl2O4 spinel is the dominant crystalline phase of the support. The total content of MgO, Al2O3, and impurity phases such as carbonate hydroxides and MgO-Al2O3 solid solutions that may form due to the presence of CO2 in the air is extremely low, and does not affect the catalyst's high-temperature stability, anti-sintering properties, or anti-coking performance.
[0027] Example 1
[0028] S1. Weigh out the specified amounts of soluble magnesium salt, soluble aluminum salt, and soluble nickel salt to prepare a mixed salt solution. At room temperature, take 0.52g Ni(NO3)2·6H2O, 2.0g Mg(NO3)2·6H2O, and 3.65g Al(NO3)3·9H2O, dissolve them in an appropriate amount of deionized water to obtain a mixed metal salt solution, such that the molar ratio of Mg / Al is 0.8.
[0029] S2. Prepare an alkaline precipitant; wherein the alkaline precipitant is one or more of sodium hydroxide, potassium hydroxide, and ammonia water. In this embodiment, 1.5 mol·L⁻¹ is selected. -1 NaOH solution is used as an alkaline precipitant.
[0030] S3. The mixed salt solution and the alkaline precipitant are added dropwise together to carry out a co-precipitation reaction under conditions of pH 9.0~11.0 to obtain a precipitate slurry. In this embodiment, the mixed metal salt solution prepared in step S1 and the 1.5 mol·L⁻¹ alkaline precipitant solution prepared in step S2 are used together. -1 NaOH solution was added dropwise to the base solution, and the pH was controlled at 9.2-9.8 during the stirring process. After the titration was completed, stirring was continued for 1 hour to obtain the precipitated slurry.
[0031] S4. The precipitated slurry is aged to obtain a magnesium-aluminum-nickel layered double hydroxide precursor; wherein the interlayer anion of the magnesium-aluminum-nickel layered double hydroxide precursor is a directionally synthesized hydroxide ion. In this embodiment, after aging for 24 hours, it is filtered and washed with deionized water until neutral. It is then dried in a drying oven at 125°C for 12 hours to obtain the magnesium-aluminum layered double hydroxide.
[0032] S5. The magnesium-aluminum-nickel layered double hydroxide precursor is calcined in air at a temperature of 600-900°C for 2-8 hours to obtain a nickel-based magnesium-aluminum spinel catalyst. In this embodiment, the dried magnesium-aluminum-nickel layered double hydroxide is placed in a muffle furnace and heated to 850°C at a heating rate of 5°C / min, and calcined for 6 hours to obtain a catalyst in which the nickel component is highly dispersed in the magnesium-aluminum spinel structure. The particle size of the Ni oxide is 6.5 nm.
[0033] It should be noted that no surfactant is added during the entire preparation process from steps S1 to S5; and the alkaline precipitant in step S2 is strictly free of carbonate and bicarbonate ions.
[0034] The above catalyst was ground and sieved to obtain a catalyst with a mesh size of 40-60, denoted as C-1. The C-1 catalyst obtained in Example 1 has a specific surface area of 100² / g, which belongs to mesoporous materials with medium specific surface area.
[0035] Figure 1 The N2 adsorption-desorption isotherm of the catalyst prepared in Example 1 is shown. As can be seen from the figure, this isotherm belongs to a typical type IV adsorption isotherm, with a significant H2-type hysteresis loop appearing between 0.4 and 0.9 relative pressures (P / P0), which is a characteristic feature of mesoporous materials.
[0036] The nickel-based magnesium aluminum spinel catalyst (C-1) of Example 1 has a specific surface area of 100 m² / g calculated by the BET method and an average pore size of approximately 7.8 nm calculated by the BJH method.
[0037] To investigate the stability of the catalyst, a long-term stability test was conducted on the nickel-based magnesium-aluminum spinel catalyst (C-1) of Example 1, which was used in the dry reforming reaction of methane. The test was carried out in a fixed-bed reactor, which was a microreactor consisting of a quartz tube (15 mm) filled with a mixture of 0.2 g of catalyst (40-60 mesh) and quartz sand. The test procedure was as follows: first, H2 / N2 was introduced at 800°C to reduce the catalyst, followed by the introduction of reaction gases. The catalyst stability test conditions were: reaction temperature 900°C, reaction pressure 0.1 MPa, CH4 / CO2 = 1, a mixed gas of 4.5% CO, 48% H2, and a small amount of O2, and a space velocity of 60000 mL·gca. t-1 ·h -1 The composition of the outlet gas was analyzed in a chromatograph equipped with a TCD detector. The conversion rates of CH4 and CO2 were calculated, such as... Figure 2 As shown. After nearly 800 hours of operation, the conversion rate of CH4 was >90%, the conversion rate of CO2 was >85%, and there were no signs of decreased catalyst activity. That is, the nickel-based magnesium-aluminum spinel catalyst (C-1) of Example 1 exhibits high resistance to sintering and coking, as well as long-term stability under the high-temperature conditions of methane dry reforming.
[0038] Example 2
[0039] S1. Weigh 0.89 g of Ni(NO3)2 at room temperature. 6H2O, 1.38 g Mg(NO3)2 6H2O, 5.78 g Al(NO3)3 9H2O is dissolved in an appropriate amount of deionized water to obtain a mixed metal salt solution, such that the molar ratio of Mg / Al is 0.35.
[0040] S2, Choose 1 mol·L -1 KOH solution is used as an alkaline precipitant.
[0041] S3. The mixed metal salt solution prepared in step S1 and the KOH solution prepared in step S2 as an alkaline precipitant solution are added dropwise to the base liquid in parallel. The pH is controlled at 10.5~11 during the stirring process. After the titration is completed, stirring is continued for 1 h to obtain the precipitated slurry.
[0042] S4. In this embodiment, after aging for 24 hours, the mixture is filtered and washed with deionized water until neutral. It should be noted that during the washing process, special attention should be paid to strengthening the removal of potassium ions. The mixture is then dried in a drying oven at 125°C for 12 hours to obtain a magnesium-aluminum-nickel layered double hydroxide.
[0043] S5. The dried magnesium-aluminum-nickel layered double hydroxide was placed in a muffle furnace and heated to 600°C at a heating rate of 1°C / min, and calcined for 8 hours to obtain a catalyst in which the nickel component is highly dispersed in the magnesium-aluminum spinel structure.
[0044] The above catalyst was ground and sieved to obtain a catalyst with a mesh size of 40-60, denoted as C-2. The C-2 catalyst obtained in Example 2 has a specific surface area of 142 m² / g and an average pore size of 10.26 nm, belonging to mesoporous materials.
[0045] Example 3
[0046] S1. At room temperature, weigh 0.29 g Ni(CH3COO)2·4H2O, 2.7 g MgCl2·6H2O, and 3.2 g AlCl3·6H2O, dissolve them in an appropriate amount of deionized water to obtain a mixed metal salt solution, such that the molar ratio of Mg / Al is 1.
[0047] S2, Choose 1.0 mol·L -1 Ammonia solution is used as an alkaline precipitant.
[0048] S3. Combine the mixed metal salt solution prepared in step S1 with the 1.0 mol·L⁻¹ solution prepared in step S2 as an alkaline precipitant. -1 Ammonia water was added dropwise to the base solution in parallel flow. The pH was controlled at 9.2-10 during the stirring process. After titration, stirring was continued for 1 hour to obtain a precipitated slurry.
[0049] S4. In this embodiment, after aging for 24 hours, the product is filtered and washed with deionized water until neutral. It should be noted that during the washing process, attention should be paid to strengthening the removal of chloride ions. Then, it is placed in a drying oven at 125°C and dried for 12 hours to obtain magnesium aluminum nickel layered double hydroxide.
[0050] S5. The dried magnesium-aluminum-nickel layered double hydroxide was placed in a muffle furnace and heated to 900°C at a heating rate of 10°C / min, and calcined for 2 hours to obtain a catalyst in which the nickel component is highly dispersed in the magnesium-aluminum spinel structure.
[0051] The above catalyst was ground and sieved to obtain a catalyst with a mesh size of 40-60, denoted as C-3. The C-3 catalyst obtained in Example 3 has a specific surface area of 80 m² / g and an average pore size of 13 nm, belonging to mesoporous materials.
[0052] Isotherms were obtained for the nickel-based catalysts prepared in Examples 2 and 3. The results showed that the catalysts exhibited a type IV isotherm, an H2-type hysteresis loop, a high specific surface area (>80 m² / g), and uniform mesoporous pore size (5–15 nm). This structure facilitates the high dispersion of the active component nickel and the rapid diffusion of reactants / products, and is an important structural basis for the excellent activity and stability of the catalysts in methane dry reforming.
[0053] The activity of the nickel-based catalysts prepared in Examples 1-3 was determined under conditions conducive to induced coking. The catalyst activity and stability tests were conducted in a fixed-bed reactor. The results of the catalyst activity and coking conditions are as follows: Table 1
[0054] As can be seen from the data in Table 1, the nickel-based magnesium-aluminum spinel catalysts prepared in Examples 1-3 of this invention all have a CO2 conversion rate of over 98.5% and a coking amount of less than 0.8% / mg under reaction conditions of 900℃, which fully demonstrates that the catalysts of this invention have both excellent catalytic activity and outstanding anti-coking ability in high-temperature methane dry reforming systems.
[0055] Phase structure characterization of the catalysts was conducted. XRD results showed that the calcined precursor, magnesium aluminum nickel layered double hydroxide, could be directionally transformed into a structurally stable magnesium aluminum spinel phase, verifying the reliability and feasibility of the preparation route of this invention. Furthermore, the catalysts in all embodiments possessed complete mesoporous structures, with specific surface areas maintained in the range of 80–140 m² / g. Relying on this stable spinel support and excellent pore structure, the catalysts exhibited excellent anti-sintering and anti-coking properties under the high-temperature conditions of methane dry reforming, enabling long-term stable operation.
[0056] Comparative Example 1
[0057] S1. Weigh 0.78g of Ni(NO3)2 at room temperature. 6H2O, 7.32g Mg(NO3)2 6H2O, 4.28g Al(NO3)3 9H2O is dissolved in an appropriate amount of deionized water to obtain a mixed metal salt solution, such that the molar ratio of Mg / Al is 2.5.
[0058] S2, Choose 1.5 mol·L -1 NaOH solution is used as an alkaline precipitant.
[0059] S3. Combine the mixed metal salt solution prepared in step S1 with the 1.5 mol·L⁻¹ solution prepared in step S2 as an alkaline precipitant. -1NaOH solution was added dropwise to the base solution in a parallel flow. The pH was controlled at 8.8-9.2 during the stirring process. After the titration was completed, stirring was continued for 1 hour to obtain a precipitated slurry.
[0060] S4. In this embodiment, after aging for 24 hours, the product is filtered and washed with deionized water until neutral. It is then dried in a drying oven at 125°C for 12 hours to obtain magnesium aluminum nickel layered double hydroxide.
[0061] S5. The dried magnesium-aluminum-nickel layered double hydroxide was placed in a muffle furnace and heated to 850°C at a heating rate of 5°C / min, and calcined for 6 hours to obtain a catalyst in which the nickel component is highly dispersed in the magnesium-aluminum spinel structure.
[0062] The above catalyst was ground and sieved to obtain a catalyst with a mesh size of 40-60, denoted as C-4. The C-4 catalyst obtained in Comparative Example 1 has a specific surface area of 100 m² / g and an average pore size of 12 nm, belonging to mesoporous materials with medium specific surface area.
[0063] Table 2
[0064] Table 2 shows that the catalysts of Example 1 and Comparative Example 1 exhibit similar catalytic activities when applied to the dry reforming reaction of methane; however, the catalyst with a magnesium-aluminum molar ratio of 2.5, under the same reaction conditions, has a coking rate approximately 60 times that of the sample with a magnesium-aluminum molar ratio of 0.8. XRD spectra of the nickel-based magnesium-aluminum spinel catalyst (C-1) of Example 1 and the nickel-based magnesium-aluminum spinel catalyst (C-4) of Comparative Example 1 were obtained, and the results are as follows: Figure 3 As shown.
[0065] Through observation Figure 3 It can be seen that the nickel-based magnesium-aluminum spinel catalyst (C-1) prepared in Example 1 has a spinel structure, while the main crystalline phase of the nickel-based magnesium-aluminum spinel catalyst (C-4) in Comparative Example 1 is an oxide solid solution.
[0066] Comparative Example 2
[0067] S1. At room temperature, take 0.52g Ni(NO3)2·6H2O, 2.0g Mg(NO3)2·6H2O, and 3.65g Al(NO3)3·9H2O, dissolve them in an appropriate amount of deionized water to obtain a mixed metal salt solution, such that the molar ratio of Mg / Al is 0.8.
[0068] S2, Choose 1.5 mol·L -1 NaOH solution is used as an alkaline precipitant.
[0069] S3. Combine the mixed metal salt solution prepared in step S1 with the 1.5 mol·L⁻¹ solution prepared in step S2 as an alkaline precipitant. -1 NaOH solution was added dropwise to the base solution in a parallel flow. The pH was controlled at 8.8-9.2 during the stirring process. After the titration was completed, stirring was continued for 1 hour to obtain a precipitated slurry.
[0070] S4. In this embodiment, after aging for 24 hours, the product is filtered and washed with deionized water until neutral. It is then dried in a drying oven at 125°C for 12 hours to obtain magnesium aluminum nickel layered double hydroxide.
[0071] S5. The dried magnesium-aluminum-nickel layered double hydroxide was placed in a muffle furnace and heated to 1000℃ at a heating rate of 16℃ / min, and calcined for 9h to obtain a catalyst in which the nickel component is highly dispersed in the magnesium-aluminum spinel structure.
[0072] The above catalyst was ground and sieved to obtain a catalyst with a mesh size of 40-60, denoted as C-5. The C-5 catalyst obtained in Comparative Example 2 had a specific surface area of 45 m² / g and an average pore size of 16 nm. The specific surface area of the catalyst at this temperature was significantly lower than that of the catalysts prepared at the temperatures of Examples 1-3.
[0073] For the various experimental supplies (including but not limited to chemical reagents, biological products, cells, organisms, instruments, etc.) mentioned in this article, the manufacturers, references or detailed preparation methods have been noted for those that are special or difficult to obtain; unless otherwise specified, they are all conventional experimental supplies that could be easily obtained through various means (such as purchase, self-preparation, etc.) before the date of this application.
[0074] Although the present invention has been described in detail above with general descriptions, specific embodiments, and experiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications and improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.
Claims
1. A nickel-based magnesium aluminate spinel catalyst, characterized in that, comprise a MgAl204spinel monophase support and a nickel component supported on the MgAl204spinel monophase support, wherein the nickel component is present in the form of metallic Ni 0 and / or NiO.
2. The nickel-based magnesium aluminum spinel catalyst according to claim 1, characterized in that, The nickel-based magnesium aluminum spinel catalyst has a nickel content of 5-15 wt%.
3. The nickel-based magnesium aluminum spinel catalyst according to claim 1, characterized in that, The catalyst has a BET specific surface area of 80~140 m² / g and a pore size of 5~15 nm.
4. A process for the preparation of a nickel-based magnesium aluminate spinel catalyst, characterized in that, include: Weigh out the specified amounts of soluble magnesium salt, soluble aluminum salt and soluble nickel salt to prepare a mixed salt solution; Prepare an alkaline precipitant; wherein the alkaline precipitant is one or more of sodium hydroxide, potassium hydroxide, and ammonia water; The mixed salt solution and the alkaline precipitant were added dropwise together, and a co-precipitation reaction was carried out under conditions of pH 9.0~11.0 to obtain a precipitated slurry; After aging, washing and drying the precipitated slurry, a magnesium-aluminum-nickel layered double hydroxide precursor was obtained. The magnesium-aluminum-nickel layered double hydroxide precursor was calcined in air at a temperature of 600-900°C for 2-8 hours to obtain a nickel-based magnesium-aluminum spinel catalyst.
5. The process for the preparation of a nickel-based magnesium aluminate spinel catalyst according to claim 4, characterized in that, The soluble magnesium salt is one or more of magnesium nitrate, magnesium acetate, magnesium sulfate, and magnesium chloride.
6. The process for the preparation of a nickel-based magnesium aluminate spinel catalyst according to claim 4, characterized in that, The soluble nickel salt is one or more of nickel nitrate, nickel acetate, nickel sulfate, and nickel chloride.
7. The method for preparing the nickel-based magnesium aluminum spinel catalyst according to claim 4, characterized in that, The soluble aluminum salt is one or more of aluminum nitrate, aluminum sulfate, aluminum chloride, and aluminum acetate.
8. The method for preparing the nickel-based magnesium aluminum spinel catalyst according to claim 4, characterized in that, In the step of washing and drying the magnesium-aluminum-nickel layered double hydroxide precursor and then calcining it in air, the calcination heating rate is 1~10℃ / min.
9. The method for preparing the nickel-based magnesium aluminum spinel catalyst according to claim 4, characterized in that, In the step of preparing the mixed salt solution, the molar ratio of magnesium to aluminum is 0.35 to 1.
0.
10. A method for dry reforming methane, characterized in that, Using any one of the nickel-based magnesium-aluminum spinel catalysts according to claims 1 to 3, methane and carbon dioxide are reacted at 700 to 850°C.