Nickel-based catalysts, their preparation methods, and their application in the hydrogenation and value enhancement conversion of polyethylene terephthalate.

By preparing nickel-aluminum hydrotalcite via a urea hydrothermal method and then calcining, reducing, and passivating it, a highly dispersed small-particle nickel nanoparticle catalyst was prepared. This solved the stability and cost issues of noble metal catalysts in the hydrogenation conversion of PET, achieving efficient conversion of PET and high selectivity for PECHD, and providing an economical chemical recycling solution for PET.

CN123102353APending Publication Date: 2026-11-17PEKING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611217721.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing precious metal catalysts for PET hydrogenation conversion suffer from problems such as metal leaching, poor cycle stability, and high cost, making it difficult to achieve efficient and economical PET chemical recycling.

Method used

Nickel-aluminum hydrotalcite was prepared by urea hydrothermal method, followed by calcination, reduction treatment and passivation to prepare highly dispersed small-particle nickel nanoparticle catalyst. The non-precious metal nickel was used to replace the precious metal to form a nickel-based catalyst.

Benefits of technology

It achieves efficient conversion of PET and high selectivity of PECHD. The catalyst is easy to separate after hydrogenation, has good cycle stability, reduces costs, and provides a green and economical chemical value-added recovery path for PET.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102353A_ABST
    Figure CN123102353A_ABST
Patent Text Reader

Abstract

This application provides a nickel-based catalyst, its preparation method, and its application in the hydrogenation and value-enhancing conversion of polyethylene terephthalate (PET). The preparation method of the nickel-based catalyst includes the following steps: preparing nickel-aluminum layered double hydroxide (LTD) via a urea hydrothermal method; calcining the LTD to obtain a nickel-aluminum composite metal oxide; and subjecting the nickel-aluminum composite metal oxide to a reduction treatment and a passivation treatment to obtain the nickel-based catalyst. Applying the nickel-based catalyst of this application to the selective hydrogenation of waste PET to produce PECHD enables highly efficient conversion of PET and high selectivity for PECHD.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of catalyst preparation technology, and in particular to a nickel-based catalyst, its preparation method, and its application in the hydrogenation and value-enhancing conversion of polyethylene terephthalate. Background Technology

[0002] With the rapid development of the global economy and the continuous upgrading of consumption patterns, the annual output of plastic products has continued to climb, leading to increasingly serious waste plastic pollution problems. Statistics show that the global annual production of waste plastics has reached approximately 350 million tons, of which about 67% comes from short-life plastic products such as packaging. Polyethylene terephthalate (PET), as a high-performance and low-cost polyester plastic, is widely used in beverage bottles, textiles (such as polyester), and packaging materials. However, large quantities of discarded PET products are difficult to degrade in the natural environment, causing serious white pollution and microplastic problems, posing a potential threat to ecosystems and human health. Therefore, developing efficient and economical waste PET recycling technologies has become a research hotspot in the field of resources and environment.

[0003] Traditional PET recycling methods mainly include mechanical recycling and dissolution regeneration, but these methods often suffer from problems such as product performance degradation, severe impurity accumulation, and inability to handle mixed waste plastics. In contrast, chemical recycling technology can depolymerize PET into monomers or high-value chemicals, achieving a true circular economy. In recent years, researchers have developed various chemical recycling routes for PET, including hydrolysis, alcoholysis, pyrolysis, and hydrogenolysis. Among them, the catalytic hydrogenation route has attracted widespread attention due to its relatively mild reaction conditions and high added value of the products. Through catalytic hydrogenation, PET can be selectively converted into the hydrogenated oligomer of polyethylene terephthalate, polyethylene 1,4-cyclohexanedicarboxylate (PECHD). This process not only effectively degrades waste PET but also provides an important intermediate for subsequent conversions. Currently, noble metal catalysts (such as Ru / C) exhibit good activity in this reaction, but they suffer from problems such as metal leaching, poor cycle stability, and high cost. Therefore, developing a non-noble metal-based, highly active, and highly stable catalytic system for the selective hydrogenation conversion of PET has significant environmental and economic benefits. Summary of the Invention

[0004] The purpose of this application is to provide a nickel-based catalyst, its preparation method, and its application in the hydrogenation and upgrading conversion of polyethylene terephthalate (PET), so as to obtain a low-cost nickel-based catalyst with good activity and cycle stability, achieving efficient conversion of PET and high selectivity for PECHD. The specific technical solution is as follows:

[0005] The first aspect of this application provides a method for preparing a nickel-based catalyst, which includes the following steps: preparing nickel-aluminum hydrotalcite by a urea hydrothermal method; calcining the nickel-aluminum hydrotalcite to obtain a nickel-aluminum composite metal oxide; subjecting the nickel-aluminum composite metal oxide to a reduction treatment and a passivation treatment in sequence to obtain a nickel-based catalyst.

[0006] In some embodiments of this application, the steps for preparing nickel-aluminum hydrotalcite by the urea hydrothermal method include: dissolving nickel salt, aluminum salt and urea in water to obtain a mixed solution; sealing the mixed solution at 100℃~140℃ for 12h~48h to obtain a precipitate; washing the precipitate until neutral; and drying it to obtain nickel-aluminum hydrotalcite.

[0007] In some embodiments of this application, the nickel salt is selected from at least one of nickel nitrate, nickel sulfate, and nickel chloride, and the aluminum salt is selected from at least one of aluminum nitrate and aluminum sulfate; in the mixed solution, the concentration of the nickel salt is 0.05 mol / L to 0.2 mol / L, the concentration of the aluminum salt is 0.025 mol / L to 0.1 mol / L, and the concentration of urea is 0.3 mol / L to 1.5 mol / L.

[0008] In some embodiments of this application, calcination includes: heating to 400°C to 600°C at a heating rate of 2°C / min to 10°C / min in an air atmosphere, and holding for 2h to 6h.

[0009] In some embodiments of this application, the reduction process includes: heating to 500°C to 700°C at a heating rate of 2°C / min to 10°C / min under a hydrogen atmosphere, and holding for 1h to 4h.

[0010] In some embodiments of this application, the passivation treatment includes: passivating for 6 h to 24 h in an inert atmosphere with an oxygen volume fraction of 0.5% to 2% at room temperature.

[0011] The second aspect of this application provides a nickel-based catalyst prepared by the preparation method provided in the first aspect of this application, wherein the nickel loading in the nickel-based catalyst is 50wt% to 70wt%.

[0012] The third aspect of this application provides the application of a nickel-based catalyst prepared by the method provided in the first aspect of this application in the hydrogenation of polyethylene terephthalate to prepare polyethylene 1,4-cyclohexanedicarboxylate.

[0013] In some embodiments of this application, the step of preparing polyethylene 1,4-cyclohexanedicarboxylate by hydrogenation of polyethylene terephthalate includes: mixing polyethylene terephthalate, solvent and nickel-based catalyst, and carrying out hydrogenation reaction under hydrogen atmosphere and continuous stirring. The hydrogenation reaction temperature is 150°C to 200°C, the time is 10h to 24h, and the hydrogen pressure is 2MPa to 6MPa.

[0014] In some embodiments of this application, the mass-to-volume ratio of polyethylene terephthalate to solvent is 1 g:10 mL to 1 g:100 mL, and the mass ratio of polyethylene terephthalate to nickel-based catalyst is 5:1 to 100:1; the solvent is selected from at least one of 1,4-dioxane, tetrahydrofuran, γ-valerolactone, and cyclohexane.

[0015] The beneficial effects of this application are:

[0016] This application provides a nickel-based catalyst, its preparation method, and its application in the hydrogenation and value-added conversion of polyethylene terephthalate (PET). The preparation method of the nickel-based catalyst includes the following steps: preparing nickel-aluminum layered double hydroxide (LTD) via a urea hydrothermal method; calcining the LTD to obtain a nickel-aluminum composite metal oxide; and subjecting the nickel-aluminum composite metal oxide to a reduction treatment and a passivation treatment to obtain the nickel-based catalyst. On the one hand, the preparation method of this catalyst is simple, easy to implement, and highly operable, and the use of non-precious metal nickel significantly reduces costs. On the other hand, applying the nickel-based catalyst obtained by this method to the selective hydrogenation of waste PET to produce PECHD enables highly efficient conversion of PET and high selectivity for PECHD. The nickel-based catalyst exhibits good activity, cycle stability, and ease of separation and recycling, providing a green, economical, and sustainable technical path for the chemical value-added recycling of waste PET.

[0017] Of course, implementing any product or method of this application does not necessarily require achieving all of the advantages described above at the same time. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other embodiments can be obtained based on these accompanying drawings.

[0019] Figure 1 The XRD pattern of the nickel-aluminum composite metal oxide prepared in Example 1 of this application;

[0020] Figure 2 The image shows the XRD pattern of the nickel-based catalyst prepared in Example 1 of this application. Detailed Implementation

[0021] The technical solutions of this application will be clearly and completely described below with reference to the embodiments and accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. All other embodiments obtained by those skilled in the art based on this application are within the scope of protection of this application.

[0022] The first aspect of this application provides a method for preparing a nickel-based catalyst, comprising the following steps: preparing nickel-aluminum hydrotalcite via a urea hydrothermal method; calcining the nickel-aluminum hydrotalcite to obtain a nickel-aluminum composite metal oxide; and subjecting the nickel-aluminum composite metal oxide to a reduction treatment and a passivation treatment sequentially to obtain a nickel-based catalyst. The inventors have discovered that Ni can be synthesized via a urea hydrothermal method. 2+ With Al 3+ Atomically uniformly dispersed layered structure, after calcination and reduction, forms a composite system in which nickel nanoparticles are highly anchored in an alumina matrix. On one hand, the strong interaction between the Ni-Al layers in the nickel-aluminum layered double hydroxide (LTD) helps suppress the migration and aggregation of nickel particles during calcination and reduction, thus obtaining highly dispersed, small-sized active centers, exhibiting excellent catalytic activity for the activation of aromatic rings in PET molecules. On the other hand, the nickel particles in the prepared catalyst are embedded in the in-situ generated alumina matrix, exhibiting excellent resistance to sintering and dissolution, and maintaining high catalytic activity even after multiple cycles. Furthermore, the use of non-precious metal nickel instead of precious metals such as ruthenium, palladium, and platinum significantly reduces the raw material cost of the catalyst. Simultaneously, the hydrothermal synthesis method is simple to operate, has mild conditions, and is easy to scale up, showing promising prospects for industrial applications. In addition, after passivation treatment, the nickel-based catalyst is stable and can be stored and transported on a large scale. In summary, this catalyst demonstrates outstanding performance in the selective hydrogenation of waste PET to prepare PECHD, exhibiting high efficiency, stability, economy, and recyclability, providing a feasible technical route for the chemical value-added recycling of waste PET.

[0023] In this application, the prepared nickel-aluminum hydrotalcite can be ground before calcination, which is beneficial for more complete calcination.

[0024] In some embodiments of this application, the steps for preparing nickel-aluminum hydrotalcite by the urea hydrothermal method include: dissolving nickel salt, aluminum salt, and urea in water to obtain a mixed solution; sealing the mixed solution and reacting it at 100℃~140℃ for 12h~48h to obtain a precipitate; washing the precipitate until neutral and drying it to obtain nickel-aluminum hydrotalcite. For example, the reaction temperature can be 100℃, 110℃, 120℃, 130℃, 140℃, or any combination of two of these values; the reaction time can be 12h, 18h, 24h, 30h, 36h, 42h, 48h, or any combination of two of these values. Controlling the reaction conditions of the urea hydrothermal method within the above range is beneficial for preparing Ni... 2+ With Al3+ The uniform dispersion of nickel-aluminum hydrotalcite at the atomic level within the layers provides a foundation for the subsequent preparation of nickel-based catalysts with good activity and cycle stability.

[0025] In this application, washing can be performed by centrifugation, and the precipitate can be washed until neutral using deionized water and / or ethanol. This application does not particularly limit the drying method, as long as it achieves the purpose of this application. For example, drying can be performed in an oven at 60°C.

[0026] In some embodiments of this application, the nickel salt is selected from at least one of nickel nitrate, nickel sulfate, and nickel chloride, and the aluminum salt is selected from at least one of aluminum nitrate and aluminum sulfate. In the mixed solution, the concentration of the nickel salt is 0.05 mol / L to 0.2 mol / L, the concentration of the aluminum salt is 0.025 mol / L to 0.1 mol / L, and the concentration of urea is 0.3 mol / L to 1.5 mol / L. For example, the concentration of the nickel salt can be 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, or a range of any two of these values; the concentration of the aluminum salt can be 0.025 mol / L, 0.05 mol / L, 0.1 mol / L, or a range of any two of these values; and the concentration of urea can be 0.3 mol / L, 0.5 mol / L, 0.8 mol / L, 1.2 mol / L, 1.5 mol / L, or a range of any two of these values. Controlling the concentrations of the nickel salt, aluminum salt, and urea within the above ranges is beneficial for Ni… 2+ With Al 3+ Uniform co-precipitation forms nickel-aluminum hydrotalcite with good crystallinity and uniform elemental distribution in the layers. A suitable urea concentration ensures that the ammonia release rate matches the metal ion precipitation rate during hydrothermal processes, avoiding amorphous precipitation or localized compositional segregation caused by excessive supersaturation. This facilitates precise control of the Ni / Al ratio in the layers and the complete development of the layered structure.

[0027] In some embodiments of this application, calcination includes: heating to 400℃~600℃ at a heating rate of 2℃ / min~10℃ / min in an air atmosphere and holding for 2h~6h. For example, the heating rate during calcination can be 2℃ / min, 5℃ / min, 8℃ / min, 10℃ / min, or a range of any two of these values; the calcination temperature can be 400℃, 500℃, 600℃, or a range of any two of these values; and the time can be 2h, 3h, 5h, 6h, or a range of any two of these values. Controlling the calcination parameters within the above ranges is beneficial for the orderly removal of the nickel-aluminum hydrotalcite layer structure and the uniform formation of nickel-aluminum composite metal oxides, avoiding uneven collapse of the layer structure or agglomeration of nickel species caused by local overheating due to excessively rapid heating, and promoting the growth of Ni in the layer.2+ With Al 3+ Simultaneous transformation during dehydroxylation and decarbonation forms a nickel-aluminum composite metal oxide with high specific surface area and uniform elemental distribution. At the same time, it ensures the complete collapse of the hydrotalcite layered structure and its transformation into a precursor complex of spinel and nickel oxide phases, and effectively inhibits the excessive formation of nickel-aluminum spinel phase, which is conducive to achieving the optimal content of reducible nickel species in the subsequent reduction process.

[0028] In some embodiments of this application, the reduction treatment includes: heating to 500℃~700℃ at a heating rate of 2℃ / min~10℃ / min under a hydrogen atmosphere and holding for 1h~4h. For example, the heating rate of the reduction treatment can be 2℃ / min, 5℃ / min, 8℃ / min, 10℃ / min, or any combination of two of these values; the temperature of the reduction treatment can be 500℃, 600℃, 700℃, or any combination of two of these values; and the time can be 1h, 2h, 3h, 4h, or any combination of two of these values. Adjusting the parameters of the reduction treatment within the above range is beneficial for the more complete and uniform reduction of nickel species highly dispersed in the alumina matrix in the nickel-aluminum composite metal oxide into metallic nickel nanoparticles, while maintaining their original highly dispersed state and fine particle size. This avoids insufficient reduction leading to an insufficient number of active centers, or excessively high reduction temperature or time causing migration, agglomeration, and sintering of nickel particles, thereby ensuring that the catalyst has sufficient and stable hydrogenation active sites.

[0029] In some embodiments of this application, the passivation treatment includes: passivating at room temperature in an inert atmosphere with an oxygen volume fraction of 0.5% to 2% for 6 to 24 hours. For example, the oxygen volume fraction can be 0.5%, 1%, 2%, or any combination of two of these values; the passivation time can be 6 hours, 10 hours, 15 hours, 20 hours, 24 hours, or any combination of two of these values. Adjusting the passivation parameters within the above range allows a thin oxide layer to form on the catalyst surface, preventing spontaneous combustion in air and facilitating safe storage and transfer.

[0030] In this application, the inert atmosphere includes, but is not limited to, nitrogen and argon.

[0031] The second aspect of this application provides a nickel-based catalyst prepared using the method provided in the first aspect of this application, wherein the nickel loading in the nickel-based catalyst is 50 wt% to 70 wt%. For example, the nickel loading can be 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, or a range consisting of any two of these values. By controlling the nickel loading within the above range, both the activity and cycling stability of the nickel-based catalyst can be balanced, resulting in a nickel-based catalyst exhibiting both good activity and cycling stability.

[0032] The third aspect of this application provides the application of a nickel-based catalyst prepared by the method provided in the first aspect of this application in the hydrogenation of polyethylene terephthalate to prepare polyethylene 1,4-cyclohexanedicarboxylate.

[0033] In some embodiments of this application, the step of preparing polyethylene terephthalate (PET) by hydrogenation includes: mixing PET, a solvent, and a nickel-based catalyst, and carrying out a hydrogenation reaction under a hydrogen atmosphere and continuous stirring. The hydrogenation reaction temperature is 150°C to 200°C, the time is 10h to 24h, and the hydrogen pressure is 2MPa to 6MPa. For example, the hydrogenation reaction temperature can be 150°C, 160°C, 180°C, 200°C, or any combination of two of these values; the time can be 10h, 15h, 20h, 24h, or any combination of two of these values; and the hydrogen pressure can be 2MPa, 3MPa, 5MPa, 6MPa, or any combination of two of these values. Controlling the temperature, time, and hydrogen pressure of the PET hydrogenation reaction within the above ranges is beneficial for improving the conversion rate of PET and the selectivity of PECHD.

[0034] In some embodiments of this application, the mass-to-volume ratio of polyethylene terephthalate (PET) to solvent is 1 g:10 mL to 1 g:100 mL, and the mass ratio of PET to nickel-based catalyst is 5:1 to 100:1; the solvent is selected from at least one of 1,4-dioxane, tetrahydrofuran, γ-valerolactone, and cyclohexane. For example, the mass-to-volume ratio of PET to solvent can be 1 g:10 mL, 1 g:20 mL, 1 g:50 mL, 1 g:70 mL, 1 g:100 mL, or any combination of two such values; the mass ratio of PET to nickel-based catalyst can be 5:1, 10:1, 20:1, 40:1, 50:1, 70:1, 85:1, 100:1, or any combination of two such values. By controlling the mass-volume ratio of PET to solvent and the mass ratio of PET to nickel-based catalyst within the above ranges, PET can be more fully and uniformly dispersed in the solvent, and the nickel-based catalyst can provide sufficient active sites. These factors are all beneficial to promoting the hydrogenation conversion of PET to PECHD.

[0035] This application does not specifically limit the source of PET, as long as it achieves the purpose of this application. For example, commercial PET powder or waste PET products (such as beverage bottles, polyester textiles, etc.) can be used as raw materials. When using waste PET products as raw materials, the waste PET products need to undergo pretreatment such as crushing, washing, and drying.

[0036] In this application, after the PET hydrogenation reaction is completed, the nickel-based catalyst can be separated from the reaction products by magnetic separation or filtration. The separated nickel-based catalyst can be recycled while retaining a small amount of liquid wetting.

[0037] Example

[0038] The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.

[0039] Test methods and equipment:

[0040] X-ray diffraction (XRD):

[0041] An X-ray diffractometer, model D8 powder diffractometer, manufactured by Bruker GmbH, Germany, was used. The parameters were set to 35kV, 40mA, continuous mode, and a scan rate of 10. o The scanning range is 20-80° per minute, and tests are conducted using a copper target.

[0042] Nickel metal loading test:

[0043] The catalyst was digested using a microwave digestion system, specifically the UltraWAVE ECR model manufactured by Milestone, Italy. After digestion, the samples were analyzed for elemental composition using an inductively coupled plasma optical emission spectrometer (ICP-OES), specifically the Prodigy 7 model manufactured by Leeman, USA. Wavelength range: 165nm-1100nm; Instrument type: full-spectrum direct reading; Detector: CMOS solid-state detector.

[0044] Catalytic performance testing of nickel-based catalysts:

[0045] The method for calculating PET conversion rate is as follows:

[0046] Conv.(PET) = 1 - [m(residual solids) - m(catalyst feed)] / m(PET feed)

[0047] Where m(PET added) is the mass of PET weighed before the reaction starts, m(catalyst added) is the mass of catalyst weighed before the reaction starts, and m(remaining solids) is the total mass of solids filtered out after the reaction.

[0048] The method for calculating PECHD selectivity is as follows:

[0049] Sel.(PECHD)=[1-yield(PX)-yield(DCHM)]×[A(PECHD) / (A(PECHD)+A(aromatic))] / Conv.(PET)

[0050] Yield(PX) and yield(DCHM) represent the yields of the two small byproducts, p-xylene (PX) and p-dimethylcyclohexane (DCHM), quantified using gas chromatography (GC 7020A, Agilent). A(PECHD) and A(aromatic) correspond to the peak areas of the ethylene glycol segment and the aromatic ring segment (corresponding to incomplete hydrogenation) of PECHD in the NMR spectrum of the products, respectively, quantified using 1H NMR spectroscopy. 1 Quantification was performed using HNMR (Bruker 500MHz).

[0051] Example 1

[0052] <Preparation of Nickel-Based Catalysts>

[0053] At room temperature, 2.91 g of nickel nitrate hexahydrate, 1.87 g of aluminum nitrate nonahydrate, and 4.5 g of urea were weighed and dissolved in 100 mL of deionized water. The solution was stirred and sonicated to form a uniform, green, transparent solution. The solution was transferred to a 100 mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene and placed in a sealed oven at 120 °C for 24 h. After the reaction, a precipitate was obtained. The precipitate was centrifuged, washed with deionized water until neutral, and dried overnight at 60 °C in a vacuum oven to obtain nickel-aluminum hydrotalcite. The nickel-aluminum hydrotalcite was then ground. The ground nickel-aluminum hydrotalcite was calcined in a muffle furnace at a heating rate of 5 °C / min to 500 °C, held for 4 h, and then naturally cooled to room temperature to obtain a nickel-aluminum composite metal oxide. The nickel-aluminum composite metal oxide was placed in a tube furnace for reduction activation. The temperature was raised to 600°C in a pure hydrogen atmosphere at a heating rate of 3°C / min and held for 3 hours. Then, the temperature was lowered to room temperature in the hydrogen atmosphere and then switched to an Ar atmosphere with an O2 volume fraction of 0.5% at room temperature for passivation treatment for 12 hours to obtain the nickel-based catalyst.

[0054] <Preparation of PECHD from PET by Hydrogenation>

[0055] 2.9923 g of PET powder was weighed and added to 50.0 mL of 1,4-dioxane as a solvent, followed by 315.8 mg of the nickel-based catalyst prepared above. The mixture was transferred to a high-pressure reactor, and the air inside the reactor was replaced with hydrogen five times. Then, hydrogen was introduced to a pressure of 4.0 MPa. The reactor was sealed and reacted at 180.0 °C for 15.0 h with continuous stirring at a stirring speed of 600 r / min. After the reaction, the nickel-based catalyst was separated from the reaction solution by magnetic separation. The conversion rate of PET was 100%, and the selectivity for PECHD was 97.2%.

[0056] <Cyclic Stability of Nickel-Based Catalysts>

[0057] The nickel-based catalyst obtained above was retained in a small amount of liquid, and the PET hydrogenation reaction was repeated until the reaction was repeated four times. Testing showed that after four cycles, the PET conversion rate was 99.4%, and the selectivity for PECHD was 96.5%.

[0058] Comparative Example 1

[0059] 2.9923 g of PET powder was weighed and added to 50.0 mL of 1,4-dioxane as a solvent, followed by 313.2 mg of 5% Ru / C commercial catalyst (Ru / C catalyst with a Ru loading of 5 wt%). The mixture was transferred to a high-pressure reactor, and the air inside the reactor was replaced with hydrogen five times. Then, hydrogen was introduced to a pressure of 4.0 MPa. The reactor was sealed and reacted at 180.0 °C for 15.0 h with continuous stirring at a stirring speed of 600 r / min. After the reaction, the 5% Ru / C commercial catalyst was separated from the reaction solution by filtration. The initial PET conversion rate was 99.0%, and the PECHD selectivity was 99.5%. However, after four cycles of the above PET hydrogenation, the PET conversion rate was only 85.0%, and the PECHD selectivity was 95.2%.

[0060] As can be seen from Example 1 and Comparative Example 1, the nickel-based catalyst of this application can achieve high efficiency conversion of PET and high selectivity for PECHD. After four hydrogenation cycles, the nickel-based catalyst can still maintain a high PET conversion rate and PECHD selectivity, indicating that the nickel-based catalyst of this application has good cycle stability. Moreover, the nickel-based catalyst of this application does not contain precious metals and has low cost. Although the 5%Ru / C commercial catalyst can also achieve high efficiency conversion of PET and high selectivity for PECHD, after four hydrogenation cycles, its PET conversion rate is significantly reduced and its PECHD selectivity is also lower than that of the nickel-based catalyst in Example 1. This indicates that the 5%Ru / C commercial catalyst has poor cycle stability and contains the precious metal Ru, which significantly increases the cost.

[0061] from Figure 1It can be seen that the XRD pattern shows characteristic diffraction peaks matching those of the standard card JCPDS 44-1159 NiO, indicating that the nickel-aluminum composite metal oxide prepared in Example 1 contains nickel oxide; from Figure 2 It can be seen that only the characteristic diffraction peaks matching the standard card JCPDS 04-0850 Ni appeared in the XRD pattern, indicating that the nickel-based catalyst prepared in Example 1 does not contain nickel oxide, but only metallic nickel. This indicates that after reduction treatment, the nickel oxide in the nickel-aluminum composite metal oxide was reduced to nickel.

[0062] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.

Claims

1. A method for preparing a nickel-based catalyst, comprising the following steps: Nickel-aluminum hydrotalcite was prepared by a urea hydrothermal method. The nickel-aluminum hydrotalcite was calcined to obtain a nickel-aluminum composite metal oxide. The nickel-aluminum composite metal oxide is subjected to reduction and passivation treatments in sequence to obtain the nickel-based catalyst.

2. The production method according to claim 1, wherein The steps for preparing nickel-aluminum hydrotalcite by the urea hydrothermal method include: dissolving nickel salt, aluminum salt and urea in water to obtain a mixed solution; sealing the mixed solution at 100℃~140℃ for 12h~48h to obtain a precipitate; washing the precipitate until neutral and drying it to obtain the nickel-aluminum hydrotalcite.

3. The production method according to claim 2, wherein, The nickel salt is selected from at least one of nickel nitrate, nickel sulfate, and nickel chloride, and the aluminum salt is selected from at least one of aluminum nitrate and aluminum sulfate; in the mixed solution, the concentration of the nickel salt is 0.05 mol / L to 0.2 mol / L, the concentration of the aluminum salt is 0.025 mol / L to 0.1 mol / L, and the concentration of the urea is 0.3 mol / L to 1.5 mol / L.

4. The production method according to claim 1, wherein The calcination process includes: heating to 400°C to 600°C at a heating rate of 2°C / min to 10°C / min in an air atmosphere, and holding for 2h to 6h.

5. The production method according to claim 1, wherein The reduction process includes: heating to 500℃~700℃ at a heating rate of 2℃ / min~10℃ / min under a hydrogen atmosphere, and holding for 1h~4h.

6. The preparation method according to claim 1, wherein, The passivation treatment includes: passivating for 6 to 24 hours at room temperature in an inert atmosphere with an oxygen volume fraction of 0.5% to 2%.

7. A nickel-based catalyst prepared by the method according to any one of claims 1 to 6, wherein, In the nickel-based catalyst, the nickel loading is 50wt%~70wt%.

8. The application of the nickel-based catalyst prepared by the method according to any one of claims 1 to 6 in the hydrogenation of polyethylene terephthalate to prepare polyethylene 1,4-cyclohexanedicarboxylate.

9. The application according to claim 8, wherein, The step of preparing polyethylene 1,4-cyclohexanedicarboxylate by hydrogenation of polyethylene terephthalate includes: The polyethylene terephthalate, solvent, and nickel-based catalyst are mixed and subjected to a hydrogenation reaction under a hydrogen atmosphere and continuous stirring. The hydrogenation reaction is carried out at a temperature of 150°C to 200°C for 10 to 24 hours and at a hydrogen pressure of 2 MPa to 6 MPa.

10. The application according to claim 9, wherein, The mass-to-volume ratio of the polyethylene terephthalate to the solvent is 1g:10mL to 1g:100mL, and the mass ratio of the polyethylene terephthalate to the nickel-based catalyst is 5:1 to 100:1; the solvent is selected from at least one of 1,4-dioxane, tetrahydrofuran, γ-valerolactone, and cyclohexane.