A hydrogen production catalyst, a preparation method and application thereof

Highly dispersed copper-based oxide catalysts were constructed by alkali modification and bimetallic doping, which solved the problems of low efficiency, poor stability and metal leaching of copper-based catalytic materials in biohydrogen production systems, and realized an efficient and stable biohydrogen production process.

CN123102355APending Publication Date: 2026-11-17SHANGHAI INVESTIGATION DESIGN & RES INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611370095.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing copper-based catalytic materials in bio-hydrogen production systems suffer from problems such as low hydrogen production efficiency, high electron transfer impedance, poor long-term stability, metal leaching, and difficulty in achieving microbial compatibility.

Method used

By modifying the pore structure and surface functional groups of biochar carriers with alkali, and combining this with bimetallic doping to construct highly active copper-based oxides, a highly dispersed, low-dissolution, and highly stable catalyst is formed, which is suitable for anaerobic fermentation biohydrogen production systems.

Benefits of technology

It significantly improves the efficiency of biohydrogen production, extends the service life of catalysts, ensures microbial activity and environmental safety, and achieves deep integration of organic solid waste resource utilization and clean energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a hydrogen production catalyst, its preparation method, and its application. The preparation method includes: S1, placing biomass raw materials in an alkaline modifier solution for alkaline modification impregnation, followed by solid-liquid separation and drying, and then pyrolyzing under a nitrogen atmosphere at 450-550℃. The pyrolysis product is washed with water until neutral and dried to obtain a modified support; S2, dissolving a first metal salt and a copper salt in a solvent to obtain a metal salt solution, adding the modified support for impregnation, followed by solid-liquid separation and drying, and calcining under a non-reactive gas atmosphere at 350-450℃ to obtain the hydrogen production catalyst; the molar ratio of the first metal to copper in the first metal salt and copper salt is 1:(4-6); the first metal salt includes at least one of iron salt, cobalt salt, and nickel salt. This invention enhances the extracellular electron transfer efficiency of anaerobic fermentation systems by regulating the surface functional groups and pore structure of biochar through alkaline modification and combining it with bimetallic doping to construct abundant oxygen vacancies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hydrogen production technology, specifically to a hydrogen production catalyst, its preparation method, and its application. Background Technology

[0002] Organic solid waste (such as kitchen waste) is rich in biodegradable organic matter such as carbohydrates, proteins, and lipids, making it an excellent raw material for dark fermentation bio-hydrogen production. Hydrogen-producing microorganisms generate reducing equivalents through the metabolism of organic matter, achieve interspecies electron exchange via extracellular electron transport, and ultimately reduce protons to hydrogen gas through hydrogenase action, simultaneously realizing waste resource utilization and clean energy production. However, the low efficiency of extracellular electron transport and the difficulty in controlling the redox potential within anaerobic systems are the core bottlenecks restricting the improvement of hydrogen production rates and their engineering applications.

[0003] To enhance extracellular electron transfer, existing technologies often add conductive materials (such as activated carbon, biochar, metal oxides, etc.) to the reaction system. Among them, copper-based oxides have been widely studied due to their excellent conductivity and high redox activity. However, existing copper-based catalytic materials still have many shortcomings in the application of bio-hydrogen production systems: First, the improvement in hydrogen production efficiency is limited. The electron conduction capacity of single copper-based oxides is insufficient, and the electron transfer impedance at the interface with microorganisms is large, making it difficult to construct efficient electron transfer channels. Second, the long-term operational stability is poor. Byproducts such as organic acids produced during fermentation are easily adsorbed onto the catalyst surface, covering active sites. Furthermore, surface oxygen vacancies gradually passivate during the reaction, leading to a significant decline in hydrogen production performance after 300 hours of operation. Third, the problem of metal leaching is prominent. Copper ions are easily leached and lost in weakly acidic environments, causing both loss of active components and toxicity to hydrogen-producing microorganisms that are sensitive to pH (optimal 6.0–6.5), further exacerbating performance degradation. Fourth, it is difficult to balance activity maintenance with microbial compatibility. Existing catalyst regeneration often uses strong acids, strong bases, or high temperatures, which cannot be implemented in situ under the mild conditions of anaerobic fermentation, making it difficult to meet the requirements for continuous and stable operation.

[0004] Therefore, developing a copper-based catalytic material that is suitable for organic solid waste biohydrogen production systems, has active sites that can be maintained in situ, high hydrogen production efficiency, low metal leaching, and good biocompatibility is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a hydrogen production catalyst, its preparation method, and its application. By modifying the pore structure and surface functional groups of the biochar support with alkali, and combining this with bimetallic doping to construct a highly active copper-based oxide, a highly dispersed, low-dissolution, and highly stable catalytic effect is achieved, making it suitable for the mild reaction system of anaerobic fermentation bio-hydrogen production.

[0006] In a first aspect, the present invention provides a method for preparing a hydrogen production catalyst, comprising the following steps: S1, placing biomass raw material in an alkaline modifier solution for alkaline modification impregnation treatment, separating the solid and liquid, drying, and then pyrolyzing it under a non-reactive gas atmosphere at 450~550℃, washing the pyrolysis product with water until neutral, drying it to obtain a modified support; S2, dissolving a first metal salt and a copper salt in a solvent to obtain a metal salt solution, adding the modified support for impregnation, and calcining it under a non-reactive gas atmosphere at 350~450℃ to obtain the hydrogen production catalyst; the molar ratio of the first metal to copper in the first metal salt and copper salt is 1:(4~6); the first metal salt includes at least one of iron salt, cobalt salt, and nickel salt.

[0007] It is understandable that alkaline modifier impregnation treatment can partially dissolve the hemicellulose and lignin components in biomass raw materials (such as straw), loosen the raw material structure, and at the same time make the alkaline components uniformly loaded inside the raw material; during the subsequent pyrolysis in a non-reactive gas atmosphere, the loaded alkaline modifier generates hierarchical pores on the carbon skeleton through in-situ etching, increases the specific surface area of ​​the material, and forms a hierarchical pore structure with mesopores as the main component and macropores-mesopores-micropores interconnected.

[0008] Understandably, controlling the pyrolysis temperature at 450~550℃ ensures that the biomass is fully carbonized to form a stable carbon skeleton, while avoiding excessively high temperatures that could lead to the decomposition of a large number of oxygen-containing functional groups on the surface, thus ensuring the number of active sites for subsequent metal loading.

[0009] Understandably, during the impregnation process of the metal salt solution and the modified support, metal cations in the metal salt solution are attracted through electrostatic adsorption. Simultaneously, oxygen-containing functional groups can form coordination bonds with metal ions, uniformly anchoring and highly dispersing the metal ions in an ionic state on the support surface and pore walls through chelation. Because the metal ions diffuse uniformly into the mesopores (2–50 nm) of the support in an ionic state and are effectively anchored by the functional groups, migration and aggregation during subsequent calcination are suppressed. By controlling the metal loading and calcination conditions, the particle size of the resulting bimetallic oxide particles can be stably controlled within 2–8 nm. This size is much smaller than the pore size of the support mesopores, allowing for uniform loading on the pore walls without clogging the pores, thus avoiding the problems of large particles blocking pores and insufficient active sites.

[0010] Understandably, during the calcination process in step S2, the anchored metal salt undergoes simultaneous thermal decomposition and in-situ solid-state reaction. The first metal ions, during the CuO crystal nucleus growth process, diffuse into the crystal lattice via solid-state diffusion, replacing some Cu sites and forming spinel-type or solid-solution-type copper-based bimetallic composite oxides. Bimetallic doping induces lattice distortion, which can both enhance the electron conductivity of the oxide and reduce the dissolution tendency of copper ions at the crystal structure level, thus improving material stability. Furthermore, under the inert atmosphere and calcination temperature, some lattice oxygen is removed from the surface of the metal oxide. Lattice distortion and oxygen removal work synergistically to promote the generation of abundant oxygen vacancies on the surface of bimetallic oxides. Furthermore, setting the calcination temperature to 350–450°C ensures complete decomposition of the metal salt and sufficient generation of oxygen vacancies, while avoiding excessively high temperatures that could lead to nanoparticle aggregation and growth, and high-temperature annihilation of oxygen vacancies. This calcination temperature is also lower than the pyrolysis preparation temperature of the modified support, preventing secondary pyrolysis of the carbon framework and significant decomposition of oxygen-containing functional groups on the surface, thus maintaining the stability of the support structure and anchoring points. The calcination is performed in an oxygen-free, inert gas atmosphere, which avoids high-temperature oxidation of the carbon support and maintains a low oxygen partial pressure to promote oxygen removal from the surface lattice, ensuring the amount of oxygen vacancies generated. Nitrogen is the optimal choice due to its low cost and stable properties.

[0011] In one optional embodiment, in step S1, the temperature of the alkali-modified impregnation treatment is 70-85°C, and the treatment time is 3-5 hours. In one optional embodiment, in step S1, the solid-liquid ratio of the alkali-modified impregnation treatment is 1g:10-15mL; Understandably, controlling the solid-liquid ratio within this range ensures that the biomass raw materials are completely submerged in the alkali solution and that alkali ions fully penetrate into the fiber interior to achieve uniform modification. It also avoids the waste of reagents and increased drying energy consumption caused by excessive alkali solution, and is suitable for the subsequent process requirements of mild pyrolysis pore formation and functional group retention.

[0012] In one optional embodiment, in step S1, the concentration of the alkaline modifier solution is 0.8–1.2 mol / L.

[0013] In one optional implementation, in step S1, the pyrolysis includes pyrolysis for 1.5 to 2.5 hours in a non-reactive gas atmosphere.

[0014] In an optional embodiment, step S2 includes impregnation at 25–40°C for 8–12 hours with stirring. In one optional embodiment, in step S2, the solid-liquid ratio of the impregnation is 1g:10-15mL; In one optional embodiment, in step S2, the total concentration of metal ions in the metal salt solution is 0.3-0.7 mol / L; Understandably, since metal ions diffuse uniformly into the mesopores of the support in an ionic state and are effectively anchored by functional groups, migration and agglomeration during subsequent calcination are suppressed. By controlling the total concentration of the metal salt solution at 0.3–0.7 mol / L, it is possible to ensure that the support adsorption is saturated and the metal loading reaches the optimal range of 8%–15%, while avoiding particle agglomeration and excessive particle size caused by excessive metal salt.

[0015] In one optional embodiment, step S2, the calcination includes heating to the target temperature at a rate of 2-5°C / min under a non-reactive gas atmosphere and holding the temperature for 3-5 hours.

[0016] In one optional embodiment, the alkaline modifier includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, and potassium carbonate. In one optional embodiment, the copper salt includes at least one of copper nitrate, copper chloride, and copper acetate; In one optional embodiment, the iron salt includes at least one of ferric nitrate, ferric chloride, and ferric acetate; In one optional embodiment, the cobalt salt includes at least one of cobalt nitrate, cobalt chloride, and cobalt acetate; In one optional embodiment, the nickel salt includes at least one of nickel nitrate, nickel chloride, and nickel acetate; In one optional embodiment, the biomass raw material includes at least one of corn stalks, wheat stalks, rice stalks, sawdust, bamboo shavings, peanut shells, coconut shells, reeds, mushroom residue, and rice husks. In one alternative embodiment, the solvent includes at least one of water and ethanol.

[0017] And / or, in step S1, the biomass raw material before alkali modification treatment also includes washing to remove impurities, drying and then pulverizing to 40-60 mesh; And / or, in step S1, the process of washing with deionized water until neutral and drying at 60-80°C before pyrolysis is further included. And / or, in step S2, the process of drying at 90-105°C before calcination is further included; Secondly, the present invention also provides a hydrogen production catalyst prepared by the above-described preparation method.

[0018] In one optional embodiment, the hydrogen production catalyst includes a modified support and an active metal oxide supported on the surface and pore walls of the modified support. In one optional embodiment, the active metal oxide is a composite oxide of copper and a first metal; Optionally, the first metal includes at least one of Ni, Fe, and Co; In one optional embodiment, the modified carrier surface has a carboxyl content of 0.5–2.0 mmol / g and a hydroxyl content of 1.0–3.0 mmol / g.

[0019] In one optional embodiment, the total loading of the active metal oxide is 8% to 15% of the carrier mass; In one optional embodiment, the particle size distribution of the active metal oxide is in the range of 2 to 8 nm.

[0020] Thirdly, the present invention also provides the application of the hydrogen production catalyst described above in the anaerobic fermentation of organic solid waste to produce hydrogen.

[0021] In one optional embodiment, the organic solid waste includes at least one of kitchen waste, crop straw, livestock and poultry manure, and municipal sludge; In one optional embodiment, the anaerobic fermentation includes adding an alkaline agent with a concentration of 0.3 to 1.0 mol / L to the reaction system at a dropping rate of 0.1 to 2 mL / h, maintaining the pH of the system at 6.0 to 6.5; In one optional embodiment, the amount of hydrogen production catalyst added is 1.0 to 2.5 g / L.

[0022] In one optional embodiment, the hydrogen production catalyst is added in either a suspended or fixed-bed state.

[0023] Specifically, suspended addition is suitable for stirred anaerobic reactors and fermentation systems for high-suspended-solids organic solid waste. The catalyst is directly added to the reaction system at a dosage of 1.0–2.5 g / L, and stirring ensures the catalyst is uniformly suspended in the fermentation liquid, allowing for sufficient contact with the substrate and hydrogen-producing microorganisms. During the reaction, the system is maintained at pH 6.0–6.5, anaerobic conditions in the dark, and a temperature of 35±1℃. This method is simple to operate, requires no modification to existing anaerobic equipment, and ensures sufficient mass transfer and contact.

[0024] Specifically, fixed-bed loading is suitable for continuous flow fermentation systems and low-suspended-matter liquid fermentation substrates. The catalyst is filled into a fixed bed in the reactor, and the fermentation broth flows through the catalyst bed to complete the reaction at a set hydraulic residence time; the catalyst is fixed and retained in the bed, and is not easily lost with the discharge, allowing for long-term continuous operation.

[0025] The technical solution of this invention has the following advantages: 1. The present invention provides a method for preparing a hydrogen production catalyst, comprising the following steps: S1, modifying biomass raw material with an alkaline modifier and pyrolyzing it at 450~550℃ to obtain a modified support; S2, dissolving a first metal salt and a copper salt in a solvent to obtain a metal salt solution, adding the modified support for impregnation, and calcining it at 350~450℃ under a non-reactive gas atmosphere to obtain the hydrogen production catalyst; wherein the molar ratio of the first metal to copper in the first metal salt and copper salt is 1:(4~6); the first metal salt includes at least one of iron salt, cobalt salt, and nickel salt.

[0026] The method for preparing the hydrogen production catalyst provided by this invention involves impregnating and pyrolyzing biomass raw materials with an alkaline modifier. This process modifies the surface functional groups of the resulting alkaline-modified biochar support, enhancing its ability to anchor metal ions. By controlling the molar ratio of the first metal salt to the copper salt to be 1:(4~6), uniform dispersion and interfacial synergy of the metal components are achieved. Combined with calcination under a non-reactive gas atmosphere, a synergistic structure of a first metal-oxygen-copper bimetallic composite oxide is formed. Simultaneously, stable surface oxygen vacancies are controllably constructed. These two elements synergistically enhance electron transfer capabilities, significantly improving the efficiency of bio-hydrogen production. Furthermore, the surface buffering properties and reaction characteristics of the alkaline-modified biochar support are utilized... The system's pH is precisely controlled to achieve phase adaptation, enabling in-situ removal of byproducts from the surface of bimetallic composite oxides and gentle protection of active sites, thus extending the catalyst's lifespan without introducing external reagents. Furthermore, the physical immobilization of metal particles by the modified support, the stable crystalline phase structure formed between metals, and the anchoring and complexation of metal ions by functional groups on the support surface after alkali modification work together to effectively inhibit the dissolution of copper ions and the first metal ion, ensuring microbial activity and system environmental safety. Ultimately, this achieves a deep coupling between the resource utilization of organic solid waste and efficient biohydrogen production, providing a feasible technical solution for large-scale, stable, and green biohydrogen production.

[0027] In this process, controlling the molar ratio of the first metal to copper in the first metal salt and copper salt to 1:(4-6) ensures that the doping amount is within the optimal range, which fully utilizes the regulatory effect of lattice distortion and avoids excessive doping leading to phase separation and a reduction in active sites. The first metal salt includes at least one of iron salt, cobalt salt, and nickel salt, all of which can form a stable composite oxide with copper, improving conductivity and structural stability. In step S1, the pyrolysis temperature is 450-550℃, which ensures that the biomass is fully carbonized to form a stable carbon skeleton and avoids excessive temperature leading to the decomposition of a large number of oxygen-containing functional groups on the surface, thus ensuring the number of active sites for subsequent metal loading. In step S2, the calcination temperature is 350-450℃, which ensures that the metal salt is completely decomposed, the composite oxide crystal phase is formed, and oxygen vacancies are fully generated, while avoiding nanoparticle aggregation and oxygen vacancy annihilation.

[0028] 2. In the preparation method provided by the present invention, in step S1, the carboxyl content on the surface of the modified carrier is 0.5-2.0 mmol / g and the hydroxyl content is 1.0-3.0 mmol / g, which can provide sufficient chelation sites for metal ions, ensure high dispersion of active components, and inhibit the dissolution of metal ions through complexation.

[0029] 3. The hydrogen production catalyst provided by this invention, when applied to anaerobic fermentation of organic solid waste for biohydrogen production, overcomes the technical limitations of traditional catalysts, which require strong acid and alkali treatment for active regeneration and cannot adapt to microbial-sensitive environments. Through a dynamic pH compensation strategy using trace amounts of continuous alkali, the catalyst surface organic acid byproducts are removed in situ and oxygen vacancies are passivated and slowed down while strictly maintaining the optimal growth environment for microorganisms. This effectively extends the catalyst's lifespan and resolves the core contradiction of the incompatibility between dynamic repair of active sites and protection of microbial activity. Simultaneously, through the triple synergistic effect of bimetallic crystal phase bonding, biochar functional group chelation, and mild pH inhibition of excessive dissolution, the concentration of heavy metal ions leaching is stably controlled at a level far below the microbial toxicity threshold, significantly improving the system's biocompatibility and environmental safety, and overcoming the inherent defects of copper-based catalysts, such as easy dissolution and easy poisoning of microorganisms. Detailed Implementation

[0030] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having” and any variations thereof in the text of this application are intended to cover non-exclusive inclusion.

[0032] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0033] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers from a to b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed herein, and "0-5" is merely a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥ 2, it is equivalent to disclosing that the parameter can be, for example, integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0034] In the description of the embodiments of this application, the term "and / or" is merely a description of the relationship between related objects, indicating that there can be three relationships. For example, A and / or B can represent three situations: A exists alone, A and B exist simultaneously, and B exists alone.

[0035] In the description of the embodiments of this application, the term "at least one" refers to one or more (including two).

[0036] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0037] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0038] Example 1 This embodiment provides a hydrogen production catalyst, and the specific operation and parameter settings are as follows: S1. Take corn stalks, wash to remove impurities, dry at 80℃ for 24 hours, and pulverize to 40 mesh. Place the pulverized corn stalks in a 1.0 mol / L KOH solution (solid-liquid ratio 1 g:10 mL) and perform alkali modification impregnation treatment at 80℃ for 4 hours. After filtration, dry at 80℃ for 12 hours. Place the dried material in a tube furnace and pyrolyze at 500℃ under a nitrogen atmosphere at a rate of 5℃ / min for 2 hours. After natural cooling to room temperature, remove the material, wash with deionized water until neutral, and dry at 80℃ for 12 hours to obtain the modified carrier.

[0039] S2, nickel nitrate and copper nitrate (Ni to Cu molar ratio of 1:5) were dissolved in deionized water to prepare a metal salt solution with a total metal ion concentration of 0.5 mol / L. A modified support was added to the above solution, controlling the solid-liquid ratio at 1 g:12 mL. The mixture was stirred and impregnated at room temperature for 10 h, dried at 105 °C for 12 h, placed in a tube furnace, and calcined at 400 °C under a nitrogen atmosphere at a rate of 5 °C / min for 4 h. The mixture was then naturally cooled to room temperature to obtain the hydrogen production catalyst.

[0040] Example 2 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in the first metal and the calcination parameters. The specific operation is as follows: Step S2: Replace nickel nitrate with cobalt nitrate, and the molar ratio of Co to Cu in the metal salt solution is 1:4; In step S2, the roasting temperature is 350℃ and the roasting time is 5 h.

[0041] Example 3 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in the first metal and the calcination parameters. The specific operation is as follows: In step S2, nickel nitrate is replaced with ferric nitrate, and the molar ratio of Fe to Cu in the metal salt solution is 1:6. In step S2, the roasting temperature is 450℃ and the roasting time is 3 hours.

[0042] Example 4 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that the molar ratio of Ni to Cu in the metal salt solution is 1:4.

[0043] Example 5 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that the molar ratio of Ni to Cu in the metal salt solution is 1:6.

[0044] Example 6 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that the pyrolysis temperature in step S1 is 450°C.

[0045] Example 7 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that the pyrolysis temperature in step S1 is 550°C.

[0046] Example 8 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that the calcination temperature in step S2 is 350°C.

[0047] Example 9 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that the calcination temperature in step S2 is 450°C.

[0048] Example 10 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that nickel nitrate in the metal salt solution is replaced with an equimolar amount of iron nitrate.

[0049] Example 11 This embodiment provides a hydrogen production catalyst, which differs from Example 1 only in that nickel nitrate in the metal salt solution is replaced with an equimolar amount of cobalt nitrate.

[0050] Example 12 This embodiment provides a hydrogen production catalyst, and the specific operation and parameter settings are as follows: S1. Take rice straw, wash to remove impurities, dry at 80℃ for 24 hours, and pulverize to 40 mesh. Place the pulverized rice straw in a 1.2 mol / L NaOH solution (solid-liquid ratio 1 g:10 mL) and perform alkali modification impregnation treatment at 85℃ for 3 hours. After filtration, dry at 80℃ for 12 hours. Place the dried material in a tube furnace and pyrolyze at 550℃ under a nitrogen atmosphere at a rate of 5℃ / min for 1.5 hours. Allow it to cool naturally to room temperature, remove the material, wash with deionized water until neutral, and dry at 80℃ for 12 hours to obtain the modified carrier.

[0051] S2, ferric chloride and copper acetate (Fe to Cu molar ratio of 1:6) were dissolved in deionized water to prepare a metal salt solution with a total metal ion concentration of 0.3 mol / L. A modified support was added to the above solution, controlling the solid-liquid ratio at 1 g:15 mL. The mixture was stirred and impregnated at 25°C for 12 h, dried at 105°C for 12 h, placed in a tube furnace, and calcined at 450°C under a nitrogen atmosphere at a rate of 2°C / min for 3 h. The mixture was then naturally cooled to room temperature to obtain the hydrogen production catalyst.

[0052] Example 13 This embodiment provides a hydrogen production catalyst, and the specific operation and parameter settings are as follows: S1. Take reeds, wash to remove impurities, dry at 80℃ for 24 hours, and pulverize to 60 mesh. Place the pulverized reeds in a 0.8 mol / L K2CO3 solution (solid-liquid ratio 1 g:15 mL) and perform alkali modification impregnation treatment at 70℃ for 5 hours. After filtration, dry at 80℃ for 12 hours. Place the dried material in a tube furnace and pyrolyze at 450℃ under a nitrogen atmosphere at a rate of 5℃ / min for 2.5 hours. Allow to cool naturally to room temperature, remove the material, wash with deionized water until neutral, and dry at 80℃ for 12 hours to obtain the modified carrier.

[0053] S2, nickel acetate and copper chloride (Ni to Cu molar ratio of 1:4) were dissolved in deionized water to prepare a metal salt solution with a total metal ion concentration of 0.7 mol / L. A modified support was added to the above solution, controlling the solid-liquid ratio at 1 g:10 mL. The mixture was stirred and impregnated at 40 °C for 8 h, dried at 105 °C for 12 h, placed in a tube furnace, and calcined at 350 °C under a nitrogen atmosphere at a rate of 5 °C / min for 5 h. The mixture was then naturally cooled to room temperature to obtain the hydrogen production catalyst.

[0054] Comparative Example 1 This comparative example provides a hydrogen production catalyst, which differs from Example 1 only in that the support is unmodified and there is no first metal in the metal salt solution. The specific operation is as follows: S1. Take corn stalks, wash and remove impurities, dry at 80℃ for 24 hours, crush to 40 mesh, place the dried material in a tube furnace, heat to 500℃ at 5℃ / min under nitrogen atmosphere, keep at constant temperature for 2 hours, cool naturally to room temperature, wash with water and dry to obtain the carrier.

[0055] S2, copper nitrate was dissolved in deionized water to prepare a metal salt solution with a total metal ion concentration of 0.5 mol / L. A support was added to the solution, controlling the solid-liquid ratio at 1 g:12 mL. The solution was stirred and impregnated at room temperature for 10 h, dried at 105 °C for 12 h, placed in a tube furnace, and calcined at 400 °C under a nitrogen atmosphere at a rate of 5 °C / min for 4 h. The solution was then naturally cooled to room temperature to obtain the hydrogen production catalyst.

[0056] Comparative Example 2 This comparative example provides a hydrogen production catalyst, which differs from Example 1 only in that the metal salt solution does not contain a first metal. The specific operation is as follows: In step S2, copper nitrate is dissolved in deionized water to prepare a metal salt solution with a total metal ion concentration of 0.5 mol / L. A carrier is added to the solution to control the solid-liquid ratio at 1 g: 12 mL.

[0057] Comparative Example 3 This comparative example provides a hydrogen production catalyst, which differs from Example 1 only in that it does not undergo alkali modification. The specific operation is as follows: In step S1, corn stalks are taken, washed to remove impurities, dried at 80℃ for 24 hours, pulverized to 40 mesh, and the dried material is placed in a tube furnace. Under a nitrogen atmosphere, the temperature is increased to 500℃ at 5℃ / min, and pyrolyzed at a constant temperature for 2 hours. After naturally cooling to room temperature, the carrier is obtained after washing and drying.

[0058] Comparative Example 4 This comparative example provides a hydrogen production catalyst that differs from Example 1 only in that the pyrolysis temperature in step S1 is 400°C.

[0059] Comparative Example 5 This comparative example provides a hydrogen production catalyst that differs from Example 1 only in that the pyrolysis temperature in step S1 is 600°C.

[0060] Comparative Example 6 This comparative example provides a hydrogen production catalyst that differs from Example 1 only in that the calcination temperature in step S2 is 300°C.

[0061] Comparative Example 7 This comparative example provides a hydrogen production catalyst that differs from Example 1 only in that the calcination temperature in step S2 is 500°C.

[0062] Comparative Example 8 This comparative example provides a hydrogen production catalyst, which differs from Example 1 only in that the calcination is not performed under a nitrogen atmosphere. The specific operation is as follows: In step S2, after impregnation, the sample is placed in a tube furnace and heated to 400°C at 5°C / min under an argon atmosphere, and then calcined for 4 hours.

[0063] Comparative Example 9 This comparative example provides a hydrogen production catalyst, which differs from Example 1 only in that the molar ratio of Ni to Cu in the metal salt solution is 1:3.

[0064] Comparative Example 10 This comparative example provides a hydrogen production catalyst, which differs from Example 1 only in that the molar ratio of Ni to Cu in the metal salt solution is 1:7.

[0065] Comparative Example 11 This comparative example provides a hydrogen production catalyst, which differs from Example 1 only in that cobalt nitrate is replaced with an equimolar amount of palladium nitrate.

[0066] Experimental Example 1 The modified supports and hydrogen production catalysts prepared in each embodiment and comparative example were subjected to performance tests. The specific test methods are as follows: (1) Performance testing of the modified carrier: The carboxyl and hydroxyl content on the carrier surface was determined by Boehm titration.

[0067] (2) Performance testing of hydrogen production catalysts: The relative concentration of oxygen vacancies was characterized using X-ray photoelectron spectroscopy (XPS). The microstructure of the catalyst was observed using transmission electron microscopy (TEM). Multiple TEM images with different fields of view were randomly selected for each sample. The particle size of no less than 300 independent active metal oxide particles with clear boundaries and no obvious agglomeration was measured and statistically analyzed using ImageJ software to obtain the particle size distribution range of the active metal oxides. During the statistical process, particles of the carrier matrix and particles with severe agglomeration and overlapping whose boundaries could not be distinguished were not included in the statistics.

[0068] The total loading of active metal oxides was determined using inductively coupled plasma optical emission spectroscopy (ICP-OES).

[0069] The specific test results are shown in Table 1: Table 1 Performance data of support and hydrogen production catalyst

[0070] Experimental Example 2 Kitchen waste (5% total solids) was used as the substrate, inoculated with anaerobic hydrogen-producing sludge (10% v / v). The reactor had an effective volume of 5 L, an initial pH of 6.0, a temperature of 35 ± 1 °C, and operated anaerobically in the dark. The catalyst dosage was 2 g / L. During the reaction of all groups, 0.5 mol / L NaOH solution was added dropwise in real time using a peristaltic pump to maintain the pH at 6.0–6.5, with the drop rate dynamically adjusted according to the real-time pH. The reactor was run continuously for 300 h, and samples were taken periodically to determine the hydrogen production rate and the concentration of dissolved metal ions. The maximum hydrogen production rate, 300-hour hydrogen production retention rate, Cu ion dissolution, and first metal ion dissolution were measured.

[0071] The specific test results are shown in Table 2: Table 2 Performance data of hydrogen production catalysts

[0072] As shown in Tables 1 and 2, the catalyst prepared using the process of this invention has small active metal particle size, good dispersibility, and high oxygen vacancy content. When applied to anaerobic fermentation of kitchen waste for hydrogen production, it exhibits high hydrogen production rate, good long-term operational stability, and metal leaching levels far below the microbial toxicity threshold. Comparative examples deviating from the parameter range of this invention all showed varying degrees of performance degradation, verifying the scientific validity and effectiveness of the technical solution of this invention.

[0073] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing a hydrogen production catalyst, characterized in that, Includes the following steps: S1, the biomass raw material is placed in an alkaline modifier solution for alkaline modification impregnation treatment, and after solid-liquid separation and drying, it is then pyrolyzed at 450~550℃ under a nitrogen atmosphere. The pyrolysis product is washed with water until neutral and dried to obtain the modified carrier. S2, dissolve the first metal salt and copper salt in a solvent to obtain a metal salt solution, add a modified support for impregnation, separate the solid and liquid, dry, and calcine at 350-450°C under a non-reactive gas atmosphere to obtain the hydrogen production catalyst. The molar ratio of the first metal to copper in the first metal salt and copper salt is 1:(4-6); The first metal salt includes at least one of iron salt, cobalt salt, and nickel salt.

2. The preparation method according to claim 1, characterized in that, In step S1, the temperature of the alkali-modified impregnation treatment is 70-85°C, and the treatment time is 3-5 hours. And / or, in step S1, the solid-liquid ratio of the alkali-modified impregnation treatment is 1g:10-15mL; And / or, in step S1, the concentration of the alkaline modifier solution is 0.8 to 1.2 mol / L.

3. The preparation method according to claim 1 or 2, characterized in that, In step S1, the pyrolysis includes pyrolysis for 1.5 to 2.5 hours in a non-reactive gas atmosphere.

4. The preparation method according to any one of claims 1-3, characterized in that, In step S2, the impregnation step includes stirring and impregnating at 25-40°C for 8-12 hours; And / or, in step S2, the solid-liquid ratio of the impregnation is 1g:10-15mL; And / or, in step S2, the total concentration of metal ions in the metal salt solution is 0.3-0.7 mol / L.

5. The preparation method according to any one of claims 1-4, characterized in that, In step S2, the calcination is carried out under a non-reactive gas atmosphere, with a heating rate of 2-5°C / min and a calcination time of 3-5 hours.

6. The preparation method according to any one of claims 1-5, characterized in that, The alkaline modifier includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, and potassium carbonate. And / or, the copper salt includes at least one of copper nitrate, copper chloride, and copper acetate; And / or, the iron salt includes at least one of ferric nitrate, ferric chloride, and ferric acetate; And / or, the cobalt salt includes at least one of cobalt nitrate, cobalt chloride, and cobalt acetate; And / or, the nickel salt includes at least one of nickel nitrate, nickel chloride, and nickel acetate; And / or, the biomass raw materials include at least one of corn stalks, wheat stalks, rice stalks, sawdust, bamboo shavings, peanut shells, coconut shells, reeds, mushroom residue, and rice husks; And / or, the solvent includes at least one of water and ethanol.

7. A hydrogen production catalyst prepared by the method according to any one of claims 1-6.

8. The hydrogen production catalyst according to claim 7, characterized in that, The hydrogen production catalyst includes a modified support and an active metal oxide supported on the surface and pore walls of the modified support. And / or, the active metal oxide is a composite oxide of copper and a first metal; Optionally, the first metal includes at least one of Ni, Fe, and Co; And / or, the total loading of the active metal oxide is 8% to 15% of the carrier mass; And / or, the particle size distribution range of the active metal oxide is 2~8 nm.

9. The application of the hydrogen production catalyst according to any one of claims 7-8 in the anaerobic fermentation of organic solid waste for hydrogen production.

10. The application according to claim 9, characterized in that, The organic solid waste includes at least one of kitchen waste, crop straw, livestock and poultry manure, and municipal sludge; And / or, the anaerobic fermentation includes adding an alkaline agent with a concentration of 0.3 to 1.0 mol / L to the reaction system at a dropping rate of 0.1 to 2 mL / h, maintaining the pH of the system at 6.0 to 6.5; And / or, the amount of hydrogen production catalyst added is 1.0 to 2.5 g / L.