A rare earth-doped modified reverse copper-based catalyst, its preparation method and application
By constructing a rare-earth-doped ReOxMOxCu three-phase interface on a porous copper surface, the CO2 adsorption and activation capacity is enhanced, the interfacial oxygen species and electronic structure are regulated, the RWGS side reaction is suppressed, and the conversion rate and selectivity of CO2 hydrogenation to methanol are improved. This solves the problem of decreased methanol selectivity at high temperatures and achieves efficient CO2 conversion and methanol production.
Patent Information
- Application Number
- CN202611379593.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing reversed copper-based catalysts exhibit decreased methanol selectivity and increased CO byproduct formation at high temperatures, making it difficult to simultaneously achieve high CO2 conversion and high methanol selectivity.
Simultaneous deposition of rare earth oxides (ReOx) and transition metal oxides (MOx) on a porous copper surface to construct a ReOxMOxCu three-phase interface enhances CO2 adsorption and activation capabilities, regulates the oxygen species and electronic structure at the interface, and suppresses the reverse water-gas shift side reaction.
It improves the conversion rate and selectivity of methanol produced by CO2 hydrogenation, solves the problem of decreased methanol selectivity at high temperatures, and is suitable for efficient conversion and high-selectivity methanol preparation in the CO2 hydrogenation methanol production reaction.
Smart Images

Figure CN123102364A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst preparation and carbon dioxide resource utilization technology, specifically relating to a rare earth-doped modified reverse copper-based catalyst, its preparation method, and its application. Background Technology
[0002] CO2 hydrogenation to methanol is an important pathway for realizing the resource utilization of CO2 and renewable hydrogen energy storage. Cu-based catalysts are one of the most classic catalytic systems for this reaction, with common components including Cu-Zn, Cu-Zn-Al, Cu-Zr, Cu-Zn-Zr, and Cu-Ce. Among them, the Cu sites are mainly responsible for H2 activation and hydrogenation, while transition metal oxides and their interfaces with Cu metal mainly participate in CO2 adsorption, activation, and the stabilization of oxygen-containing intermediates.
[0003] Research on Cu-based catalysts has revealed that by preparing porous CuO with high specific surface area and further constructing a reverse-phase Cu-based catalyst, good metal oxide-copper interfacial contact can be obtained. Among them, the Cu-based catalyst with a loading of 50 wt.% ZnO (50 wt.% ZnO / Cu) exhibits high methanol selectivity in the low-temperature CO2 hydrogenation to methanol reaction.
[0004] However, the methanol selectivity of this series of reversed Cu-based catalysts significantly decreases when the reaction temperature for methanol production is increased to >260℃. Studies have shown that this is mainly due to the increase in oxygen vacancies in the metal oxides at high temperatures, which makes CO2 more easily activated into CO, thereby enhancing the reverse water-gas shift (RWGS) reaction pathway and reducing the yield and selectivity of methanol. Summary of the Invention
[0005] To overcome the problems of decreased methanol selectivity, increased CO byproduct formation, and difficulty in simultaneously achieving high CO2 conversion and high methanol selectivity in existing reversed copper-based catalysts at higher reaction temperatures, this invention provides a rare earth-doped modified reversed copper-based catalyst, its preparation method, and its application.
[0006] Building upon previous research on reversed copper-zinc catalysts (50 wt.% ZnO / Cu), this invention utilizes the simultaneous deposition of rare earth oxides (ReO) on the surface of porous metallic copper. x ) and transition metal oxides (MO) x ), construct ReO x MO x The Cu three-phase interface enhances the adsorption and activation capacity for CO2, regulates the oxygen species and electronic structure at the interface, suppresses RWGS side reactions, and ultimately improves the conversion rate and selectivity of CO2 hydrogenation to methanol.
[0007] To achieve the above objectives, the technical solution of the present invention is as follows.
[0008] The first aspect of this invention provides a rare earth-doped modified reverse copper-based catalyst, wherein the rare earth-doped modified reverse copper-based catalyst uses porous metallic copper as a substrate, and rare earth oxides and transition metal oxides are loaded on the surface of the substrate to form ReO. x MO x Cu three-phase interface structure; ReO x Represents rare earth oxides; MO x The transition metal oxide is selected from at least one of ThO2, La2O3, CeO2 and Y2O3; the loading of the transition metal oxide accounts for 10 wt.% to 70 wt.% of the total mass of porous copper; the addition of rare earth oxide accounts for 5 wt.% to 50 wt.% of the total mass of the transition metal oxide.
[0009] This invention achieves this by simultaneously depositing rare earth oxides (ReO) on a porous copper surface. x ) and transition metal oxides (MO) x ), construct ReO x MO x The Cu three-phase interface maintains the advantages of good interfacial contact in the reversed Cu catalyst while suppressing RWGS side reactions at high temperatures and maintaining high methanol selectivity.
[0010] Preferably, the loading of transition metal oxides accounts for 30 wt.% to 70 wt.% of the total mass of porous copper; and the addition of rare earth oxides accounts for 10 wt.% to 50 wt.% of the total mass of transition metal oxides.
[0011] More preferably, the loading of transition metal oxides accounts for 50 wt.% of the total mass of porous copper; and the addition of rare earth oxides accounts for 20 wt.% to 30 wt.% of the total mass of transition metal oxides.
[0012] Preferably, the transition metal oxide is selected from at least one of ZnO, ZrO2 and Al2O3.
[0013] Preferably, the rare earth-doped modified reverse copper-based catalyst uses porous CuO as a precursor, on which transition metal oxide precursor salts and rare earth oxide precursor salts are simultaneously deposited or impregnated to form a co-precipitate of transition metal and rare earth metal hydroxides on the porous CuO surface; after reduction treatment, rare earth oxides and transition metal oxides are loaded onto the porous copper surface to form ReO. x MO x Cu three-phase interface structure.
[0014] This invention mainly involves adding a mixed precursor solution to a CuO suspension, adding a precipitant, and adjusting the pH of the system to allow transition metal ions such as Zn to be added.2+ Zr 4+ Y 3+ And rare earth species such as Th 3+ Ce 4+ La 3+ Simultaneous deposition on the CuO surface yields a co-precipitate of transition metals and rare earth metal hydroxides. After washing and drying, the resulting solid is reduced in an H2 atmosphere to reduce CuO to metallic Cu. The co-precipitate of transition metals and rare earth metal hydroxides is pyrolyzed into rare earth oxide-doped transition metals, thus obtaining a rare earth-doped supported reverse copper-based catalyst.
[0015] The rare earth-doped supported reverse copper-based catalyst of this invention is based on the rare earth species ReO. x transition metal oxides MO x The interfacial synergistic effect between MO and Cu improves the performance of CO2 hydrogenation to methanol. On the one hand, MO... x and ReO x Related sites can enhance CO2 adsorption and activation, promoting the formation of CO2 derivatives such as carbonates and bicarbonates; on the other hand, metallic Cu sites can participate in the adsorption, dissociation, and hydrogenation processes of H2. Meanwhile, ReO... x The introduction of [a specific substance] can regulate the oxygen species and electronic structure at the reverse phase interface, weaken the strong adsorption of CO at Cu sites, and suppress the reverse water-gas shift reaction, i.e., the RWGS side reaction, thereby improving methanol selectivity. The above CO2 activation and H2 hydrogenation processes are carried out in ReO [a specific process]. x -MO x The process proceeds synergistically at the Cu three-phase interface, ultimately achieving a highly efficient and selective conversion of CO2 to methanol.
[0016] In this invention, the deposition or impregnation method is as follows: first, the transition metal oxide precursor salt and the rare earth oxide precursor salt are added to the CuO suspension, and then precipitation is carried out; or the transition metal oxide precursor salt and the rare earth oxide precursor salt are precipitated first, and then the precipitate is added to the CuO suspension.
[0017] A second aspect of this invention provides a method for preparing the rare earth-doped modified reverse copper-based catalyst described in the first aspect, comprising the following steps: Porous CuO was dispersed in water to obtain a CuO suspension. Transition metal oxide precursor salts and rare earth oxide precursor salts were dissolved in water to obtain a mixed precursor salt solution. This mixed precursor salt solution was added to the CuO suspension, a precipitant was added, and the pH was adjusted to 8–8.5, resulting in the deposition of a co-precipitate of transition metal and rare earth metal hydroxides on the porous CuO surface. After reduction treatment, rare earth oxides and transition metal oxides were loaded onto the porous copper surface to form ReO. x MO xA three-phase interface structure of Cu was obtained to produce a rare earth-doped modified reverse copper-based catalyst.
[0018] Preferably, the transition metal oxide precursor salt is at least one selected from zinc acetate, zirconium acetate, aluminum acetate, zinc chloride, zirconium chloride, aluminum chloride, zinc nitrate, zirconium nitrate, and aluminum nitrate. Zinc acetate is the preferred transition metal precursor salt.
[0019] Preferably, the rare earth oxide precursor salt is at least one selected from thorium nitrate, cerium nitrate, lanthanum nitrate, yttrium nitrate, thorium chloride, cerium chloride, lanthanum chloride, yttrium chloride, thorium acetate, cerium acetate, lanthanum acetate, and yttrium acetate. The rare earth metal precursor salt is preferably thorium nitrate.
[0020] In this invention, the transition metal oxide precursor salt is an acetate, chloride, or nitrate of a transition metal; the rare earth oxide precursor salt is an acetate, chloride, or nitrate of a rare earth metal.
[0021] In this invention, the transition metal oxide precursor salt is a zinc salt, and the rare earth oxide precursor salt is a thorium salt.
[0022] Preferably, the reduction treatment is carried out in a reducing atmosphere containing H2 at 250℃~350℃ for 1h~3h. Preferably, the reduction treatment temperature is 300℃.
[0023] Preferably, the reducing atmosphere containing H2 is an H2 atmosphere or a mixture of H2 and an inert gas, wherein the inert gas is N2 or Ar.
[0024] Preferably, the precipitant is a Na₂CO₃ solution, NaOH solution, K₂CO₃ solution, KOH solution, or ammonia water; the concentration of the precipitant is 0.1 mol / L to 0.2 mol / L. The preferred precipitant is a Na₂CO₃ solution.
[0025] The third aspect of this invention provides the application of the rare earth-doped modified reverse copper-based catalyst described in the first aspect as a catalyst in the hydrogenation of CO2 to methanol.
[0026] Preferably, the reaction conditions for the hydrogenation of CO2 to methanol are: a reaction temperature of 175℃~305℃, a reaction pressure of 2MPa~5MPa, and a CO2 to H2 volume ratio of 1:2.7~3.3. More preferably, the reaction pressure is 3MPa~3.5MPa.
[0027] The beneficial effects of this invention are: 1. The rare earth-doped modified reverse copper-based catalyst of the present invention is prepared by simultaneously depositing rare earth oxides (ReO2) on the surface of porous metallic copper. x ) and transition metal oxides (MO) x ), construct ReO x MOx The Cu three-phase interface enhances the adsorption and activation capacity for CO2, regulates the oxygen species and electronic structure at the interface, suppresses RWGS side reactions, and ultimately improves the conversion rate and selectivity of CO2 hydrogenation to methanol. It effectively solves the problems of decreased methanol selectivity and increased CO by-product formation in undoped reverse-phase Cu-based catalysts at higher temperatures, and is suitable for efficient conversion and high-selectivity methanol preparation in CO2 hydrogenation to methanol reaction.
[0028] 2. This invention introduces rare earth ions simultaneously during the transition metal ion deposition process, enabling rare earth oxides (ReO) to... x ) and transition metal oxides (MO) x It forms a close-contact three-phase interface with Cu, improving the efficiency of interface control.
[0029] 3. The ReO formed by this invention x -MO x The relevant sites help enhance CO2 adsorption and activation capabilities, enabling rare earth-doped modified reverse copper-based catalysts to maintain a high CO2 conversion rate in the range of 175℃ to 305℃.
[0030] 4. This invention utilizes ReO x The introduction of [the catalyst] can regulate the adsorption behavior of interfacial oxygen species and CO, suppress RWGS side reactions, and improve methanol selectivity. Specifically, the rare-earth-doped modified reverse copper-based catalyst of this invention achieves a CO2 conversion rate of up to 35.7% and a methanol selectivity of up to 94% at 305℃, significantly improving the problem of decreased high-temperature selectivity in undoped ZnO / Cu catalysts.
[0031] 5. The rare earth-doped modified reverse copper-based catalyst of the present invention has a simple preparation process and readily available raw materials. While ensuring the performance of the catalyst, it can achieve kilogram-level scale-up of the catalyst. Attached Figure Description
[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0033] Figure 1 ThO is an embodiment of the present invention x A schematic diagram of the preparation process of the modified reverse-phase 50wt.% ZnO / Cu catalyst.
[0034] Figure 2 For different ThO xComparison of CO2 conversion rates of modified catalysts at different temperatures. (a) shows the CO2 conversion rate of the catalyst in Comparative Example 1 at different temperatures; (b) shows the CO2 conversion rate of the 10 wt.% ThO2 catalyst in Example 2. x Comparison of CO2 conversion rates of the modified catalyst at different temperatures; (c) shows the CO2 conversion rate of 20 wt.% ThO in Example 3. x Comparison of CO2 conversion rates of the modified catalyst at different temperatures; (d) is the 30 wt.% ThO2 of Example 4. x Comparison of CO2 conversion rates of the modified catalyst at different temperatures; (e) is the 40 wt.% ThO2 of Example 5. x Comparison of CO2 conversion rates of the modified catalyst at different temperatures; (f) is the CO2 conversion rate of 50 wt.% ThO in Example 6. x Comparison of CO2 conversion rates of modified catalysts at different temperatures.
[0035] Figure 3 For different ThO x Comparison of product distribution of modified catalysts at different temperatures. (a) shows the product distribution at different ThO2 concentrations. x (a) Comparison of CO2 conversion rates of modified catalysts at 175℃; (b) shows the CO2 conversion rates of different ThO catalysts. x Comparison of CO2 conversion rates of modified catalysts at 205℃; (c) shows the CO2 conversion rates of different ThO2 levels. x Comparison of CO2 conversion rates of modified catalysts at 245℃; (d) shows the CO2 conversion rates of different ThO2 levels. x Comparison of CO2 conversion rates of modified catalysts at 205℃.
[0036] Figure 4 30 wt.% ThO in Example 4 x In-situ infrared spectra of CO2 adsorption-desorption of the modified catalyst and the undoped catalyst of Comparative Example 1. Among them, (a) is the CO2 adsorption-desorption spectrum of 30 wt.% ThO2 in Example 4. x (a) In-situ infrared spectroscopy of CO2 adsorption on the modified catalyst; (b) In-situ infrared spectroscopy of CO2 adsorption on the undoped catalyst of Comparative Example 1; (c) 30 wt.% ThO2 adsorption on the catalyst of Example 4. x (d) is the in-situ infrared image of CO2 desorption of the modified catalyst; (d) is the in-situ infrared image of CO2 desorption of the undoped catalyst of Comparative Example 1.
[0037] Figure 5 30 wt.% ThO in Example 4 x Comparison of CO-TPD between the modified catalyst and the undoped catalyst in Comparative Example 1.
[0038] Figure 6 ThO is an embodiment of the present invention x- A schematic diagram of the mechanism of CO2 hydrogenation to methanol production via the ZnO-Cu three-phase interface. Detailed Implementation
[0039] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention.
[0040] This invention provides a rare-earth-doped modified reverse-phase copper-based catalyst that produces almost no CO or CH4 byproducts, its preparation method, and its application in the CO2 hydrogenation to methanol reaction. The rare-earth-doped modified reverse-phase copper-based catalyst uses porous CuO as a precursor, on which transition metal oxides (MO) are simultaneously deposited or impregnated. x ) and rare earth oxides (ReO) x The precursor salt of ) is used; wherein the transition metal oxide is preferably zinc oxide (ZnO), and the rare earth oxide is preferably thorium oxide (ThO2). After precipitation, washing, drying, and hydrogen reduction, ThO2 is formed. x -ZnO / Cu reverse interface catalyst.
[0041] In the rare earth-doped modified reverse copper-based catalyst of the present invention, the loading of transition metal oxides (such as ZnO) is preferably 50 wt.%, and the modification amount of rare earth oxides (ThO2) is preferably 30 wt.%.
[0042] Performance test results show that the 50 wt.% ZnO / Cu catalyst modified with 30 wt.% ThO2 exhibits high CO2 conversion and methanol selectivity in the temperature range of 175℃ to 305℃; specifically, at 305℃, the CO2 conversion reaches approximately 36%, and the methanol selectivity reaches approximately 90%. Compared with the undoped 50 wt.% ZnO / Cu, the rare earth-doped modified reverse copper-based catalyst of this invention can effectively maintain methanol selectivity at higher reaction temperatures, indicating that ThO2... x The introduction of [a specific substance] can regulate the oxygen species and CO2 / CO adsorption behavior at the ZnO / Cu interface, suppress the RWGS side reaction, and thus improve the performance of CO2 hydrogenation to methanol.
[0043] The rare earth-doped modified reverse copper-based catalyst of the present invention can be produced on a kilogram-scale basis, and no carbon monoxide (CO) or CH4 byproducts are produced during the reaction.
[0044] Figure 6 ThO is an embodiment of the present invention xA schematic diagram illustrating the mechanism of CO2 hydrogenation to methanol production via the ZnO-Cu three-phase interface. (See diagram for reference.) Figure 6 , with ThO x Taking the ZnO–Cu three-phase interface as an example, CO2 first appears at the ZnO / ThO interface. x Adsorption and activation occur at relevant sites, forming oxygen-containing intermediates such as carbonates and bicarbonates on the surface; simultaneously, Cu sites are responsible for the dissociation and hydrogenation of H2, providing active hydrogen species for interfacial reactions. ThO x Located in the contact region between ZnO and Cu, it can regulate the distribution and electronic structure of oxygen species at the interface, enhance the stability of CO2-derived intermediates at the interface, and promote their stepwise hydrogenation process through carbonates, bicarbonates, formates (HCOO*), formyl groups (HCO*), methoxy groups, or related oxygen-containing intermediates, ultimately generating CH3OH. Meanwhile, ThO... x The introduction of ThO weakens the strong adsorption of CO at Cu sites, reduces the tendency of CO pathway and RWGS side reactions, and allows more CO2 derivatives to be converted along the methanol formation pathway. Therefore, ThO x The ZnO-Cu three-phase interface enables synergistic coupling of CO2 adsorption activation, H2 dissociation hydrogenation, and selective conversion of oxygen-containing intermediates, which is the key structural basis for improving CO2 conversion rate and selectivity of non-CO carbon-containing products.
[0045] The rare earth-doped modified reverse copper-based catalyst of the present invention is prepared by simultaneously depositing rare earth oxides (ReO2) on the surface of porous metallic copper. x ) and transition metal oxides (MO) x ), construct ReO x MO x The Cu three-phase interface enhances the adsorption and activation capacity for CO2, regulates the oxygen species and electronic structure at the interface, suppresses RWGS side reactions, and ultimately improves the conversion rate and selectivity of CO2 hydrogenation to methanol. It effectively solves the problems of decreased methanol selectivity and increased CO by-product formation at higher temperatures for undoped reverse-phase Cu-based catalysts. It is suitable for efficient conversion and high non-CO carbon-containing product selectivity preparation in the CO2 hydrogenation to methanol reaction.
[0046] The technical solution of the present invention will be further described below through specific embodiments. Unless otherwise specified, the methods described in the following embodiments are conventional methods; the reagents and materials described are commercially available unless otherwise specified.
[0047] In the following embodiments, porous CuO is used as a precursor, formed by the pyrolysis of precursor salts such as copper hydroxide, copper nitrate, or copper acetate using a mechanically assisted NaCl template method. The preparation method of porous CuO is as follows:
[0048] A copper-containing precursor and NaCl, serving as a hard template, are thoroughly mixed by mechanical ball milling to uniformly disperse the copper species on the NaCl crystal surface. NaOH is then added, and ball milling continues to convert the copper-containing precursor into copper hydroxide or a basic copper salt intermediate, yielding a mixed powder. The copper-containing precursor is copper hydroxide, or a copper salt that can be converted into CuO through alkali treatment and calcination, including one or more of copper nitrate, copper acetate, and copper chloride. The mass ratio of the copper-containing precursor salt to the pore-forming agent is 1:4, resulting in a mixed powder. The mixed powder is calcined in air at a temperature of 300℃–400℃. At this high temperature, the copper-containing precursor salt decomposes to form CuO, while the presence of the NaCl template prevents the agglomeration of CuO particles and determines the final pore structure. The calcined product is washed with water to dissolve and remove the NaCl template, leaving abundant pores in the CuO structure. After drying at 60℃–80℃, porous CuO is obtained.
[0049] Example 1 like Figure 1 A method for preparing a rare earth-doped modified reverse copper-based catalyst includes the following steps: Preparation of porous CuO: CuCl2 and NaCl particles were mixed by mechanical ball milling for 40 min to uniformly disperse the copper-containing precursor (CuCl2) on the surface of the NaCl particles. Then, NaOH particles were added and ball milling continued to allow CuCl2 and NaOH to undergo a solid-phase reaction, generating Cu(OH)2 or a basic copper salt precursor, resulting in a mixed powder. The molar ratio of CuCl2 to sodium hydroxide was 1:2, and the mass ratio of CuCl2 to NaCl was 1:4.
[0050] The mixed powder was calcined in air at a temperature of 400℃. At the high temperature, Cu(OH)2 or basic copper salt precursor salt decomposed to form CuO. At the same time, the presence of NaCl template prevented the agglomeration of CuO particles and determined the final pore structure. The calcined product was washed with deionized water to dissolve and remove the NaCl template, thereby leaving abundant pores in the CuO structure. After drying at 70℃, porous CuO was obtained.
[0051] Preparation of rare earth-doped modified reverse copper-based catalyst: Porous CuO was dispersed in deionized water and subjected to ultrasonic and mechanical stirring to form a homogeneous CuO suspension. Then, zinc acetate aqueous solution was added according to the theoretical loading of 50 wt.% ZnO / Cu (ZnO loading accounts for 50 wt.% of the mass percentage of porous metallic Cu), and an additional thorium nitrate aqueous solution equivalent to 5 wt.% ThO2 modification (ThO2 modification accounts for 5 wt.% of the mass percentage of ZnO) was added to co-disperse the Zn and Th sources on the porous CuO surface. Subsequently, 0.1 mol / L Na2CO3 solution was added dropwise until the pH of the system was approximately 8, allowing Zn and Th species to deposit simultaneously on the porous CuO surface. After washing and drying, the obtained solid was reduced at 300℃ for 2 hours in a 5 vol.% H2 / N2 atmosphere (H2 accounts for 5 vol.% of the volume of H2 / N2 atmosphere). ThO2 and ZnO were then loaded onto the porous metal Cu surface to obtain a rare earth-doped modified reverse copper-based catalyst.
[0052] The sample obtained in Example 1 is designated as a 50 wt.% ZnO / Cu-5 wt.% ThO2 catalyst. The loading of ZnO accounts for 50 wt.% of the mass percentage of porous metal Cu; the modification amount of ThO2 accounts for 5 wt.% of the mass percentage of ZnO.
[0053] Example 2 A method for preparing a rare-earth-doped modified reverse-phase copper-based catalyst was carried out according to the preparation method of Example 1, except that the amount of thorium nitrate aqueous solution added was adjusted according to the 10 wt.% ThO2 modification amount, while the rest of the method was the same as in Example 1. The sample obtained in Example 2 was designated as a 50 wt.% ZnO / Cu-10 wt.% ThO2 catalyst. The ZnO loading amount accounted for 50 wt.% of the mass percentage of porous metal Cu; the ThO2 modification amount accounted for 10 wt.% of the mass percentage of ZnO.
[0054] Example 3 A method for preparing a rare-earth-doped modified reverse-phase copper-based catalyst was carried out according to the preparation method of Example 1, except that the amount of thorium nitrate aqueous solution added was adjusted to a 20 wt.% ThO2 modification amount, while the other conditions were the same as in Example 1. The sample obtained in Example 2 was designated as a 50 wt.% ZnO / Cu-20 wt.% ThO2 catalyst. The ZnO loading accounted for 50 wt.% of the mass percentage of porous metal Cu; the ThO2 modification amount accounted for 20 wt.% of the mass percentage of ZnO.
[0055] Example 4 A method for preparing a rare-earth-doped modified reverse-phase copper-based catalyst was carried out according to the preparation method of Example 1, except that the amount of thorium nitrate aqueous solution added was adjusted to a 30 wt.% ThO2 modification amount, while the other conditions were the same as in Example 1. The sample obtained in Example 2 was designated as a 50 wt.% ZnO / Cu-30 wt.% ThO2 catalyst. The ZnO loading accounted for 50 wt.% of the mass percentage of porous metal Cu; the ThO2 modification amount accounted for 30 wt.% of the mass percentage of ZnO.
[0056] Example 5 A method for preparing a rare-earth-doped modified reverse-phase copper-based catalyst was carried out according to the preparation method of Example 1, except that the amount of thorium nitrate aqueous solution added was adjusted to 30 wt.% ThO2 modification, while the other conditions were the same as in Example 1. The sample obtained in Example 2 was designated as a 50 wt.% ZnO / Cu-40 wt.% ThO2 catalyst. The ZnO loading accounted for 50 wt.% of the mass percentage of porous metal Cu; the ThO2 modification accounted for 40 wt.% of the mass percentage of ZnO.
[0057] Example 6 A method for preparing a rare-earth-doped modified reverse-phase copper-based catalyst was carried out according to the preparation method of Example 1, except that the amount of thorium nitrate aqueous solution added was adjusted to 50 wt.% ThO2 modification, while the other conditions were the same as in Example 1. The sample obtained in Example 2 was designated as a 50 wt.% ZnO / Cu-50 wt.% ThO2 catalyst. The ZnO loading accounted for 50 wt.% of the mass percentage of porous metal Cu; the ThO2 modification accounted for 50 wt.% of the mass percentage of ZnO.
[0058] Comparative Example 1 A method for preparing a rare-earth-doped modified reverse-phase copper-based catalyst is disclosed. A 50 wt.% reverse-phase ZnO / Cu catalyst was prepared according to the method in Example 4, except that thorium nitrate was not added; only zinc acetate was added as the Zn source. After precipitation with Na2CO3, washing, drying, and reduction with H2, an undoped Th-modified 50 wt.% reverse-phase ZnO / Cu catalyst was obtained. The sample obtained in Comparative Example 1 is designated as the 50 wt.% ZnO / Cu catalyst. The ZnO loading accounts for 50 wt.% of the mass of porous metallic Cu.
[0059] The samples prepared in Examples 1-6 and Comparative Example 1 were used as catalysts for CO2 hydrogenation to methanol performance testing. The volume ratios and test conditions were as follows: catalyst dosage was 100 mg; in-situ reduction at 300°C for 2 h in a 5 vol.% H2 / N2 atmosphere before reaction; the reaction gas composition, by volume percentage, was CO2 24 vol.%, H2 72 vol.%, and N2 4 vol.%, totaling 100 vol.%; that is, the volume ratio of CO2 to H2 was 1:3. The reaction pressure was 3 MPa, and the weight hourly space velocity (WHSV, representing the volume of feed gas passing through per gram of catalyst per hour) was 6000 mL·g. cat -1 ·h -1 The products were analyzed by online gas chromatography. CO2 conversion and methanol selectivity were calculated based on the contents of CO2, CO, CH4, and CH3OH in the products. The results are shown in Tables 1-6 below. Figures 2-3 As shown.
[0060] Table 1 Performance test results of the sample prepared in Example 1 at different temperatures Note: The sample obtained in Example 1 is recorded as 50wt.%ZnO / Cu-5wt.%ThO2 catalyst.
[0061] Table 2. Performance test results of the sample prepared in Example 2 at different temperatures. Note: The sample obtained in Example 2 is recorded as a 50wt.%ZnO / Cu-10wt.%ThO2 catalyst.
[0062] Table 3. Performance test results of the samples prepared in Example 3 at different temperatures. Note: The sample obtained in Example 3 is denoted as 50wt.%ZnO / Cu-20wt.%ThO2 catalyst.
[0063] Table 4. Performance test results of the sample prepared in Example 4 at different temperatures. Note: The sample obtained in Example 4 is denoted as 50wt.%ZnO / Cu-30wt.%ThO2 catalyst.
[0064] Table 5. Performance test results of the sample prepared in Example 5 at different temperatures. Note: The sample obtained in Example 5 is recorded as a 50wt.%ZnO / Cu-40wt.%ThO2 catalyst. Table 6. Performance test results of the sample prepared in Example 6 at different temperatures. Note: The sample obtained in Example 6 is denoted as 50wt.%ZnO / Cu-50wt.%ThO2 catalyst.
[0065] Table 7 Performance test results of the undoped ThO2 sample in Comparative Example 1 at different temperatures Note: The sample obtained in Comparative Example 1 is recorded as 50 wt.% ZnO / Cu catalyst.
[0066] As can be seen from Tables 1 to 7, when no Th species are introduced, the reverse-phase 50 wt.% ZnO / Cu catalyst of Comparative Example 1 exhibits high methanol selectivity under low-temperature conditions, for example, the methanol selectivity can reach 98.9% at 170℃. However, when the reaction temperature is increased to 260℃, the selectivity of non-CO carbon-containing products decreases significantly to 56%. This indicates that the ZnO / Cu catalyst without ThO2 doping is prone to reverse water-gas shift reaction at higher temperatures (260℃), leading to an increase in the formation of CO byproducts.
[0067] Introducing ThO2 species into the 50 wt.% ZnO / Cu reverse-phase catalyst improved both CO2 conversion and methanol selectivity. As the ThO2 modification amount increased from 5 wt.% to 30 wt.%, the CO2 conversion at the same temperature gradually increased, while the selectivity for non-CO carbonaceous products remained at a high level. Among them, the 30 wt.% ThO2-modified 50 wt.% ZnO / Cu reverse-phase catalyst in Example 4 exhibited the best overall performance, achieving a CO2 conversion of 35.7% and a non-CO carbonaceous product selectivity of 93.7% at 305°C.
[0068] When the ThO2 modification amount was increased to 40 wt.%, the apparent total CO2 conversion rate of the sample in Example 5 at 305 °C was 32.1%, the selectivity of non-CO carbon-containing products was 82.4%, and the CH3OH yield was 6.4%, showing a downward trend compared to the 30 wt.% ThO2 modified sample. Further increasing the ThO2 modification amount to 50 wt.%, the apparent total CO2 conversion rate of the sample in Example 6 at 305 °C decreased to 30.1%, and the selectivity of non-CO carbon-containing products decreased to 66.8%.
[0069] The above results indicate that appropriate ThO2 modification is beneficial for constructing effective ThO2. x –ZnO–Cu three-phase interface, while excessive ThO2 species may lead to ThO xEnrichment, interfacial coverage, or strong adsorption of CO2 derivatives can weaken interfacial synergy and reduce the selectivity of non-CO carbonaceous products.
[0070] Therefore, there is an optimal range for ThO2 modification. At low ThO2 content, ThO... x The insufficient construction of the ZnO-Cu three-phase interface makes it difficult to fully regulate the adsorption behavior of oxygen species and CO at the ZnO / Cu interface; when the ThO2 content is too high, excessive ThO2... x It may cover part of the Cu or ZnO-Cu interface, reducing the utilization rate of effective hydrogenation sites. The preferred amount of Th modification is 10 wt.% to 30 wt.%. In particular, 30 wt.% Th modification can form a better balance between CO2 adsorption activation, H2 hydrogenation and CO side reaction inhibition, thus exhibiting the highest CO2 conversion rate and high selectivity for non-CO carbon-containing products.
[0071] The 30 wt.% ThO2-modified reverse-phase 50 wt.% ZnO / Cu catalyst prepared in Example 4 of this invention, compared with the undoped 50 wt.% ZnO / Cu catalyst prepared in Comparative Example 1, can significantly suppress the decrease in methanol selectivity at a higher reaction temperature (305 °C). This is because thorium nitrate and zinc acetate are added simultaneously during the deposition stage, forming a tightly connected ThO2-ZnO-Cu three-phase interface between the ThO2 species and ZnO and Cu. On the one hand, the ZnO and ThO2-related sites can enhance CO2 adsorption activation; on the other hand, the introduction of ThO2 can regulate the stability of interfacial oxygen species, weakening the strong adsorption of CO at Cu sites, thereby suppressing RWGS side reactions and improving the selectivity of non-CO carbonaceous products.
[0072] Figure 4 30 wt.% ThO in Example 4 x In-situ infrared spectra of CO2 adsorption-desorption of the modified catalyst and the undoped catalyst of Comparative Example 1. Figure 4 As shown in (a) and (b), compared to the unmodified 50 wt.% ZnO / Cu of Comparative Example 1, the 30 wt.% ThO of Example 4... x The modified catalyst exhibits stronger HCO3- concentration during CO2 adsorption. - , m-CO3, m / b-CO3, bridged / b-CO3 and v s Characteristic absorption peaks such as CO3 indicate that ThO x The introduction of [the catalyst] enhances the adsorption and activation capacity of CO2 on the catalyst surface.
[0073] like Figure 4 As shown in (c) and (d), compared with the unmodified 50 wt.% ZnO / Cu of Comparative Example 1, the 30 wt.% ThO of Example 4...x The modified catalyst retains significant carbonate and bicarbonate-related peaks during CO2 desorption, indicating its ability to stabilize more CO2-derived oxygen-containing intermediates. This result demonstrates that ThO x The oxygen species and acid-base properties at the ZnO / Cu interface can be controlled, making it easier for CO2 to form surface species in the interface region that can be further hydrogenated and converted, thereby improving the conversion rate and selectivity of non-CO carbon-containing products in the CO2 hydrogenation to methanol reaction.
[0074] Figure 5 This is a comparison of CO-TPD between the 30 wt.% Th-modified catalyst of Example 4 and the undoped catalyst of Comparative Example 1. CO-TPD represents CO temperature-programmed desorption. Figure 5 As shown, the unmodified 50 wt.% ZnO / Cu catalyst of Comparative Example 1 exhibited a strong CO desorption peak in the mid-to-high temperature range, indicating that its surface has many strong CO adsorption sites, which easily promote CO accumulation and enhance the RWGS side reaction. Compared with the undoped catalyst of Comparative Example 1, the 30 wt.% ThO catalyst of Example 4... x The modified catalyst showed a significant decrease in the intensity of the CO desorption peak, especially a significant weakening of the high-temperature strong adsorption CO peak, indicating that ThO x This can weaken the strong adsorption of CO at Cu-related sites. This result indicates that ThO x Modification can adjust the electronic structure of the ZnO / Cu interface and the CO adsorption strength, thereby reducing the tendency of CO byproduct formation and improving the selectivity of non-CO carbon-containing products in the CO2 hydrogenation reaction.
[0075] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A rare earth-doped modified reverse copper-based catalyst, characterized in that, The rare earth-doped modified reverse copper-based catalyst uses porous metallic copper as a substrate, with rare earth oxides and transition metal oxides loaded on the substrate surface to form ReO. x MO x Cu three-phase interface structure; ReO x Represents rare earth oxides; MO x Indicates transition metal oxides; The rare earth oxides are selected from at least one of ThO2, La2O3, CeO2, and Y2O3; The loading of transition metal oxides accounts for 10 wt.% to 70 wt.% of the total mass of porous copper. The amount of rare earth oxides added accounts for 5 wt.% to 50 wt.% of the total mass of transition metal oxides.
2. The rare earth-doped modified reverse copper-based catalyst according to claim 1, characterized in that, The loading of transition metal oxides accounts for 30 wt.% to 70 wt.% of the total mass of porous copper; the addition of rare earth oxides accounts for 10 wt.% to 50 wt.% of the total mass of transition metal oxides.
3. The rare earth-doped modified reverse copper-based catalyst according to claim 1, characterized in that, The transition metal oxide is selected from at least one of ZnO, ZrO2 and Al2O3.
4. The rare earth-doped modified reverse copper-based catalyst according to claim 1, characterized in that, The rare earth-doped modified reverse copper-based catalyst uses porous CuO as a precursor, and simultaneously deposits or impregnates transition metal oxide precursor salts and rare earth oxide precursor salts on the surface of the precursor to form a co-precipitate of transition metal and rare earth metal hydroxides on the surface of porous CuO. After reduction treatment, rare earth oxides and transition metal oxides are loaded onto the porous copper surface to form ReO. x MO x Cu three-phase interface structure.
5. A method for preparing a rare earth-doped modified reverse copper-based catalyst according to any one of claims 1 to 4, characterized in that, Includes the following steps: Porous CuO is dispersed in water to obtain a CuO suspension; Transition metal oxide precursor salts and rare earth oxide precursor salts are dissolved in water to obtain a mixed precursor salt solution. A mixed precursor salt solution was added to a CuO suspension, a precipitant was added, and the pH was adjusted to 8–8.
5. This resulted in the deposition of a co-precipitate of transition metal and rare earth metal hydroxides on the porous CuO surface. Following reduction treatment, rare earth oxides and transition metal oxides were loaded onto the porous copper surface to form ReO. x MO x A three-phase interface structure of Cu was obtained to produce a rare earth-doped modified reverse copper-based catalyst.
6. The method for preparing the rare earth-doped modified reverse copper-based catalyst according to claim 5, characterized in that, The transition metal oxide precursor salt is at least one of zinc acetate, zirconium acetate, aluminum acetate, zinc chloride, zirconium chloride, aluminum chloride, zinc nitrate, zirconium nitrate, and aluminum nitrate. The rare earth oxide precursor salt is at least one of thorium nitrate, cerium nitrate, lanthanum nitrate, yttrium nitrate, thorium chloride, cerium chloride, lanthanum chloride, yttrium chloride, thorium acetate, cerium acetate, lanthanum acetate, and yttrium acetate.
7. The method for preparing the rare earth-doped modified reverse copper-based catalyst according to claim 5, characterized in that, The reduction treatment is carried out in a reducing atmosphere containing H2 at 250℃~350℃ for 1h~3h.
8. The method for preparing the rare earth-doped modified reverse copper-based catalyst according to claim 5, characterized in that, The precipitant is a Na2CO3 solution, NaOH solution, K2CO3 solution, KOH solution, or ammonia water; the concentration of the precipitant is 0.1mol / L to 0.2mol / L.
9. The application of the rare earth-doped modified reverse copper-based catalyst according to any one of claims 1 to 4 as a catalyst in the hydrogenation of CO2 to methanol.
10. The application of the rare earth-doped modified reverse copper-based catalyst according to claim 9 as a catalyst in the hydrogenation of CO2 to methanol, characterized in that, The reaction conditions for the hydrogenation of CO2 to methanol are: reaction temperature 175℃~305℃, reaction pressure 2MPa~5MPa, and the volume ratio of CO2 to H2 is 1:2.7~3.3.