A method for preparing and applying a catalyst for the hydrogenation of carbon dioxide to methanol.
Cu/M/CoWO4 composite materials were prepared by a stepwise coprecipitation-hydrothermal synthesis method, which solved the problems of low carbon dioxide conversion and poor methanol selectivity in the traditional Cu-based catalyst in the carbon dioxide hydrogenation to methanol reaction, and achieved efficient carbon dioxide conversion and methanol production.
Patent Information
- Application Number
- CN202611618420.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional Cu-based catalysts suffer from low carbon dioxide conversion, poor methanol selectivity, and insufficient catalyst stability in the carbon dioxide hydrogenation to methanol reaction.
Cu/M/CoWO4 composite materials were prepared by a stepwise coprecipitation-hydrothermal synthesis method. By adding a dispersant to the cobalt tungstate precursor and controlling the pH value, uniform nanoparticles were formed, which improved the CO2 activation capacity and methanol selectivity and suppressed the formation of by-products.
It improved carbon dioxide conversion and methanol selectivity, enhanced catalyst stability, and reduced byproduct formation.
Smart Images

Figure CN123102372A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology for the hydrogenation of carbon dioxide to methanol, specifically relating to a method for preparing and applying a catalyst for the hydrogenation of carbon dioxide to methanol. Background Technology
[0002] With industrialization, the massive burning of fossil fuels has led to a continuous rise in atmospheric CO2 concentrations, and the resulting greenhouse effect and climate change have become major challenges facing humanity. Against this backdrop, converting CO2 into high-value-added chemicals and clean fuels can not only achieve the recycling of carbon resources but also effectively reduce greenhouse gas emissions.
[0003] Methanol, as an important basic chemical raw material and a potential clean energy carrier, is widely used in the production of chemical products such as formaldehyde, acetic acid, and methyl tert-butyl ether. It can also be used directly as a fuel or a hydrogen source for fuel cells. Methanol can be directly synthesized from captured CO2 and green hydrogen through catalytic hydrogenation, realizing "electrochemical" energy conversion and storage. This is a strategic technological path to promote the circular economy and reduce greenhouse gas emissions.
[0004] Catalysts are a core factor affecting the efficiency of CO2 hydrogenation to methanol. A typical industrial Cu-based catalyst is the Cu / ZnO / Al2O3 system, where Cu acts as the main active component responsible for H2 dissociation and adsorption, ZnO synergistically promotes CO2 activation and hydrogenation of intermediate products, and Al2O3 acts as a structural aid to improve the catalyst's specific surface area and thermal stability. However, traditional Cu-based catalysts still have significant shortcomings in CO2 hydrogenation: First, low carbon dioxide conversion rate. The activation barrier of CO2 molecules is high, making activation difficult at low temperatures. Although zinc oxide can provide weakly basic sites for CO2 adsorption, the insufficient oxygen vacancy concentration on the surface of traditional catalysts leads to low CO2 activation efficiency. Second, low methanol selectivity, typically below 60%, and the formation of byproducts CO and methane reduces atom economy. Third, the reaction process can cause sintering or agglomeration of active Cu species, resulting in irreversible catalyst deactivation and long-term stability that fails to meet industrial requirements.
[0005] To address the aforementioned problems, Chinese patent CN117548113A discloses a method for preparing a copper-zinc catalyst and the copper-zinc catalyst prepared therefrom. The preparation method of this patent involves adding a surfactant to assist in the co-precipitation process of copper and zinc salts to obtain amorphous solid particles, and adding zirconium as an additive to further improve the methanol selectivity of the catalyst. However, the corresponding carbon dioxide conversion rate of this catalyst is low, and the corresponding methanol selectivity is also still low. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing a catalyst for the hydrogenation of carbon dioxide to methanol and its application. The catalyst prepared by this invention has good particle size and morphology. When the catalyst prepared by this invention is used in the reaction of hydrogenating carbon dioxide to methanol, it exhibits good stability, high carbon dioxide conversion rate, and high methanol selectivity.
[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A method for preparing a catalyst for the hydrogenation of carbon dioxide to methanol includes the following steps: S1. Add a cobalt salt solution to a mixed solution of sodium tungstate and dispersant to obtain a cobalt tungstate precursor suspension. Simultaneously add a mixed solution of copper salt and nitrate and an alkaline solution to the cobalt tungstate precursor suspension and stir to obtain a coprecipitated precursor mixture. S2. The co-precipitated precursor mixture is subjected to a hydrothermal reaction, and the product is washed, dried, calcined, and reduced to obtain a catalyst for the hydrogenation of carbon dioxide to methanol.
[0008] Preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate; In the mixed solution of sodium tungstate and dispersant, the molar volume ratio of sodium tungstate in the mixed solution of sodium tungstate and dispersant is 0.012-0.016 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.02-0.8 g / 75 mL. The cobalt salt in the cobalt salt solution is one of cobalt nitrate, cobalt sulfate, cobalt chloride, or their hydrates; In the cobalt salt solution, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.01-0.015 mol / 75 mL.
[0009] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate, and the molecular weight of the dispersant is 1000-10000.
[0010] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, or ammonium polyacrylate, and the molecular weight of the dispersant is 4000-6000.
[0011] More preferably, in S1, the molar volume ratio of sodium tungstate in the sodium tungstate solution is 0.013-0.015 mol / 75 mL, and the mass-volume ratio of the dispersant in the sodium tungstate solution is 0.04-0.6 g / 75 mL.
[0012] More preferably, in S1, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.011-0.013 mol / 75 mL.
[0013] Preferably, in S1, the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution; In alkaline solutions, the concentration of alkali is 0.05-0.2 mol / L; When a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to a cobalt tungstate precursor suspension, the pH of the system is maintained between 7 and 8 by controlling the rate of addition of the alkaline solution.
[0014] More preferably, in S1, the alkaline solution is a sodium hydroxide solution.
[0015] Preferably, in S1, the copper salt in the mixed solution of copper salt and nitrate is one of copper nitrate, copper sulfate, copper chloride or their hydrate, and the nitrate is one of zinc nitrate, indium nitrate, zirconium nitrate or their hydrate; In a mixed solution of copper salt and nitrate, the molar volume ratio of copper salt in the mixed solution of copper salt and nitrate is 0.001-0.01 mol / 50 mL, and the molar volume ratio of nitrate in the mixed solution of copper salt and nitrate is 0.001-0.005 mol / 50 mL.
[0016] Preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:0.9-1.5; The mass ratio of cobalt salt in the cobalt salt solution to the dispersant in the mixed solution of sodium tungstate and dispersant is 1:0.01-0.2; The molar ratio of cobalt salt in a cobalt salt solution to copper salt in a mixed solution of copper salt and nitrate is 1-9:1; The molar ratio of cobalt salt to nitrate in a cobalt salt solution is 2-9:1.
[0017] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:1.1-1.3.
[0018] More preferably, in S1, the mass ratio of cobalt salt in the cobalt salt solution to dispersant in the mixed solution of sodium tungstate and dispersant is 1:0.01-0.17.
[0019] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to copper salt in the mixed solution of copper salt and nitrate is 1.25-8:1.
[0020] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to nitrate in the mixed solution of copper salt and nitrate is 2.5-8:1.
[0021] Preferably, in step S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 20-45°C. When adding a cobalt salt solution to a mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise. When a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to a cobalt tungstate precursor suspension, the mixed solution of copper salt and nitrate is added dropwise.
[0022] More preferably, in S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 30-40°C.
[0023] More preferably, in S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 2-10 mL / min.
[0024] More preferably, in S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 4-6 mL / min.
[0025] More preferably, in S1, when a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to the cobalt tungstate precursor suspension, the mixed solution of copper salt and nitrate is added dropwise at a rate of 2-10 mL / min.
[0026] More preferably, in S1, when a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to the cobalt tungstate precursor suspension, the mixed solution of copper salt and nitrate is added dropwise at a rate of 4-6 mL / min.
[0027] Preferably, in S1, the stirring time is 20-40 minutes.
[0028] Preferably, in S2, the hydrothermal reaction is carried out in a polytetrafluoroethylene-lined hydrothermal reactor; The hydrothermal reaction temperature is 140-180℃, and the time is 12-24h; Wash with deionized water or anhydrous ethanol 2-5 times; The drying temperature is 100-120℃, and the time is 10-12 hours; The calcination temperature is 500-550℃, and the time is 2-3 hours.
[0029] More preferably, in S2, the calcination temperature is 500-550℃, the time is 2-3h, and the heating rate when the temperature is raised to 500-550℃ is 1-5℃ / min.
[0030] In a further preferred embodiment, in S2, the calcination temperature is 500-550℃, the time is 2-3h, and the heating rate when the temperature is raised to 500-550℃ is 1-3℃ / min.
[0031] Preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen. The reduction temperature is 300-350℃, and the time is 2-3 hours.
[0032] More preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 2-20% and argon accounts for 80-98%.
[0033] In a further preferred embodiment, during S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 5-10% and argon accounts for 90-95%.
[0034] Furthermore, in S2, the product is washed, dried, calcined, and reduced before being granulated to a particle size of 20-50 mesh.
[0035] Application of a catalyst prepared by the aforementioned method in the reaction of carbon dioxide hydrogenation to methanol.
[0036] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) A method for preparing a catalyst for the hydrogenation of carbon dioxide to methanol according to the present invention is to prepare a Cu / M / CoWO4 composite material by stepwise coprecipitation-hydrothermal synthesis. The oxygen vacancies of cobalt tungstate in the composite material can serve as CO2 active sites, weakening the C=O bond of CO2, solving the problem of poor CO2 capture and activation ability in the hydrogenation of carbon dioxide to methanol reaction at lower temperatures, and improving the carbon dioxide conversion rate.
[0037] (2) A method for preparing a carbon dioxide hydrogenation catalyst according to the present invention uses a stepwise coprecipitation-hydrothermal synthesis method to obtain a Cu / M / CoWO4 composite material. By adding a dispersant during the first step of the stepwise coprecipitation process of cobalt tungstate metathesis reaction, the viscosity of the dispersion system is increased, the diffusion and migration rate of metal ions and hydrolysis precursors are reduced, and the steric hindrance is increased after the instantaneous nucleation of CoWO4, so that ions cannot aggregate on large crystal nuclei for secondary growth, and a large number of small crystal nuclei are frozen, reducing the agglomeration of CoWO4 precursors. The composite material consists of near-spherical particles with a diameter of 200-500 nm, with uniform particle size, and is not easily sintered during the reaction, and the catalyst has good stability.
[0038] (3) A method for preparing a carbon dioxide hydrogenation catalyst according to the present invention involves co-precipitating Cu and auxiliary metal M onto CoWO4. Metal Cu dissociates and activates H2 into surface H, and auxiliary metal M induces more surface oxygen vacancies at the copper-tungstate interface, enhancing CO2 adsorption activation. This synergistic effect with the H2 dissociation activation of Cu sites inhibits RWGS sites, reduces CO generation, and promotes the reaction of CO2 with surface H to generate formate (HCOO) intermediates. Subsequently, hydrogenation is carried out via methoxy (CH3O) to generate methanol, thereby improving methanol selectivity. Attached Figure Description
[0039] Figure 1 Scanning electron microscope (SEM) images of the catalysts for the hydrogenation of carbon dioxide to methanol prepared in Examples 1, 1, 2, and 4. In the picture, Figure 1 (a) A scanning electron microscope (SEM) image of the catalyst prepared in Example 1 for the hydrogenation of carbon dioxide to methanol. Figure 1 (b) A scanning electron microscope (SEM) image of the catalyst prepared for the hydrogenation of carbon dioxide to methanol prepared in Comparative Example 1. Figure 1 (c) is a scanning electron microscope (SEM) image of the catalyst prepared for the hydrogenation of carbon dioxide to methanol prepared in Comparative Example 2. Figure 1 (d) is a scanning electron microscope (SEM) image of the catalyst prepared for the hydrogenation of carbon dioxide to methanol prepared in Comparative Example 4.
[0040] Figure 2 The elemental distribution diagram is shown for the catalyst prepared in Example 5 for the hydrogenation of carbon dioxide to methanol. Detailed Implementation
[0041] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0042] In all the embodiments and comparative examples, the chemicals used were commercially available chemically pure reagents.
[0043] The present invention provides a method for preparing a catalyst for the hydrogenation of carbon dioxide to methanol, comprising the following steps: S1. Add a cobalt salt solution to a mixed solution of sodium tungstate and dispersant to obtain a cobalt tungstate precursor suspension. Simultaneously add a mixed solution of copper salt and nitrate and an alkaline solution to the cobalt tungstate precursor suspension and stir to obtain a coprecipitated precursor mixture. S2. The co-precipitated precursor mixture is subjected to a hydrothermal reaction, and the product is washed, dried, calcined, and reduced to obtain a catalyst for the hydrogenation of carbon dioxide to methanol.
[0044] Preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate.
[0045] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate, and the molecular weight of the dispersant is 1000-10000.
[0046] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, or ammonium polyacrylate, and the molecular weight of the dispersant is 4000-6000.
[0047] Preferably, in S1, the molar volume ratio of sodium tungstate to dispersant in the mixed solution of sodium tungstate and dispersant is 0.012-0.016 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.02-0.8 g / 75 mL.
[0048] More preferably, in S1, the molar volume ratio of sodium tungstate in the sodium tungstate solution is 0.013-0.015 mol / 75 mL, and the mass-volume ratio of the dispersant in the sodium tungstate solution is 0.04-0.6 g / 75 mL.
[0049] Preferably, in S1, the cobalt salt in the cobalt salt solution is one of cobalt nitrate, cobalt sulfate, cobalt chloride, or their hydrates.
[0050] Preferably, in S1, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.01-0.015 mol / 75 mL.
[0051] More preferably, in S1, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.011-0.013 mol / 75 mL.
[0052] Preferably, in S1, the copper salt in the mixed solution of copper salt and nitrate is one of copper nitrate, copper sulfate, copper chloride or their hydrates, and the nitrate is one of zinc nitrate, indium nitrate, zirconium nitrate or their hydrates.
[0053] Preferably, in S1, the molar volume ratio of copper salt in the mixed solution of copper salt and nitrate is 0.001-0.01 mol / 50 mL, and the molar volume ratio of nitrate in the mixed solution of copper salt and nitrate is 0.001-0.005 mol / 50 mL.
[0054] Preferably, in S1, the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution.
[0055] More preferably, in S1, the alkaline solution is a sodium hydroxide solution.
[0056] Preferably, in S1, the concentration of the alkali in the alkaline solution is 0.05-0.2 mol / L.
[0057] Preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:0.9-1.5.
[0058] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:1.1-1.3.
[0059] Preferably, in S1, the mass ratio of cobalt salt in the cobalt salt solution to dispersant in the mixed solution of sodium tungstate and dispersant is 1:0.01-0.2.
[0060] More preferably, in S1, the mass ratio of cobalt salt in the cobalt salt solution to dispersant in the mixed solution of sodium tungstate and dispersant is 1:0.01-0.17.
[0061] Preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to copper salt in the mixed solution of copper salt and nitrate is 1-9:1.
[0062] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to copper salt in the mixed solution of copper salt and nitrate is 1.25-8:1.
[0063] Preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to nitrate in the mixed solution of copper salt and nitrate is 2-9:1.
[0064] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to nitrate in the mixed solution of copper salt and nitrate is 2.5-8:1.
[0065] Preferably, in S1, when a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to the cobalt tungstate precursor suspension, the pH of the system is maintained between 7 and 8 by controlling the rate of addition of the alkaline solution.
[0066] In S1, maintaining the pH of the system between 7 and 8 with an alkaline solution helps to form nano-cobalt tungstate particles with uniform particle size and morphology, while ensuring that copper ions in the copper salt solution and metal ions in the nitrate solution can form uniform precipitates.
[0067] Preferably, in step S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 20-45°C.
[0068] More preferably, in S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 30-40°C.
[0069] Preferably, in S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise.
[0070] More preferably, in S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 2-10 mL / min.
[0071] More preferably, in S1, when adding the cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 4-6 mL / min.
[0072] Preferably, in S1, when a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to the cobalt tungstate precursor suspension, the mixed solution of copper salt and nitrate is added dropwise.
[0073] More preferably, in S1, when a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to the cobalt tungstate precursor suspension, the mixed solution of copper salt and nitrate is added dropwise at a rate of 2-10 mL / min.
[0074] More preferably, in S1, when a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to the cobalt tungstate precursor suspension, the mixed solution of copper salt and nitrate is added dropwise at a rate of 4-6 mL / min.
[0075] Preferably, in S1, the stirring time is 20-40 minutes.
[0076] Preferably, in S2, the hydrothermal reaction is carried out in a polytetrafluoroethylene-lined hydrothermal reactor.
[0077] Preferably, in S2, the hydrothermal reaction temperature is 140-180℃ and the time is 12-24h.
[0078] Preferably, in S2, the washing process involves washing with deionized water or anhydrous ethanol 2-5 times.
[0079] Preferably, in step S2, the drying temperature is 100-120℃ and the time is 10-12h.
[0080] Preferably, in S2, the calcination temperature is 500-550℃ and the time is 2-3h.
[0081] More preferably, in S2, the calcination temperature is 500-550℃, the time is 2-3h, and the heating rate when the temperature is raised to 500-550℃ is 1-5℃ / min.
[0082] In a further preferred embodiment, in S2, the calcination temperature is 500-550℃, the time is 2-3h, and the heating rate when the temperature is raised to 500-550℃ is 1-3℃ / min.
[0083] Preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen.
[0084] More preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 2-20% and argon accounts for 80-98%.
[0085] In a further preferred embodiment, during S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 5-10% and argon accounts for 90-95%.
[0086] Preferably, in S2, the reduction temperature is 300-350℃ and the time is 2-3h.
[0087] Furthermore, in S2, the product is washed, dried, calcined, and reduced before being granulated to a particle size of 20-50 mesh.
[0088] Embodiments of the present invention also provide the application of the catalyst prepared by the said preparation method in the reaction of carbon dioxide hydrogenation to methanol.
[0089] Example 1 Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.740 g of copper nitrate trihydrate and 1.438 g of zinc nitrate hexahydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0090] Place the beaker containing solution B in a thermostatic magnetic stirrer at 40°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.05 mol / L sodium hydroxide solution and solution C dropwise simultaneously using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 30 min after the addition is complete to obtain the coprecipitated precursor.
[0091] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixture (8% hydrogen + 92% argon) to obtain the synthesized product.
[0092] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / Zn / CoWO4=3:2:5.
[0093] Example 2 Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.354 g of sodium tungstate and 0.1104 g of polyacrylic acid (PAA) with a molecular weight of 5000 into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.798 g of copper sulfate pentahydrate and 1.531 g of indium nitrate monohydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0094] Place the beaker containing solution B on a thermostatic magnetic stirrer at 35°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, simultaneously add 0.2 mol / L sodium hydroxide solution and solution C using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 20 minutes after the addition is complete to obtain the coprecipitated precursor.
[0095] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 140 °C for 24 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with anhydrous ethanol and then placed in a drying oven and dried at 110 °C for 10 h. The dried product was then placed in a muffle furnace and calcined at 500 °C for 2 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 320 °C for 3 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0096] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / In / CoWO4=3:2:5.
[0097] Example 3 Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 3.958 g of sodium tungstate and 0.184 g of ammonium polyacrylate (40 wt% purity, PAA-NH4) into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.227 g of copper chloride dihydrate and 2.061 g of zirconium nitrate pentahydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0098] Place the beaker containing solution B in a thermostatic magnetic stirrer at 30°C. Then, add solution A dropwise to the mixed aqueous solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.05 mol / L sodium hydroxide solution and solution C dropwise simultaneously using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 25 min after the addition is complete to obtain the coprecipitated precursor.
[0099] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 180 °C for 12 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 120 °C for 11 h. The dried product was then placed in a muffle furnace and calcined at 530 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 350 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0100] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / Zr / CoWO4=3:2:5.
[0101] Example 4 Weigh 3.373 g of cobalt sulfate heptahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.552 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 0.375 g of copper sulfate pentahydrate and 0.446 g of zinc nitrate hexahydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0102] Place beaker B in a thermostatic magnetic stirrer at 35°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, simultaneously add 0.15 mol / L sodium hydroxide solution and solution C using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 35 min after the addition is complete to obtain the coprecipitated precursor.
[0103] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with anhydrous ethanol and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 2 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 320 °C for 3 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0104] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / Zn / CoWO4=1:1:8.
[0105] Example 5 Weigh 2.855 g of cobalt chloride hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.184 g of ammonium polyacrylate (40 wt% purity, PAA-NH4) into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 2.31 g of copper nitrate trihydrate and 0.714 g of zinc nitrate hexahydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0106] Place beaker B in a thermostatic magnetic stirrer at 30°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, simultaneously add 0.1 mol / L sodium hydroxide solution and solution C using the peristaltic pump, with the flow rate of solution C set to 5 mL / min. Adjust the flow rate of the sodium hydroxide solution in real time to maintain the pH between 7 and 8. Continue stirring for 20 min after the addition is complete to obtain the coprecipitated precursor.
[0107] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 140 °C for 24 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 10 h. The dried product was then placed in a muffle furnace and calcined at 500 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0108] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / Zn / CoWO4=4:1:5.
[0109] Comparative Example 1 Compared with Example 1, the carrier in this comparative example is Al2O3.
[0110] Weigh 3.853 g of aluminum nitrate hexahydrate and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 and add them to a beaker. Add 150 mL of deionized water and stir well to obtain solution B. Weigh 1.740 g of copper nitrate trihydrate and 1.438 g of zinc nitrate hexahydrate and add them to a beaker. Add 50 mL of deionized water and stir well to obtain solution C.
[0111] Place the beaker containing solution B on a thermostatic magnetic stirrer at 30°C. Then, add solution C dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. Simultaneously, add 0.05 mol / L sodium hydroxide solution dropwise using the peristaltic pump, maintaining the pH at 7-8 by adjusting the flow rate of the sodium hydroxide solution in real time. After the addition is complete, continue stirring for 20 min to obtain the coprecipitated precursor.
[0112] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0113] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / Zn / Al=3:2:5.
[0114] Comparative Example 2 Compared with Example 1, the dispersant addition steps are different in this comparative example.
[0115] Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.740 g of copper nitrate trihydrate, 1.438 g of zinc nitrate hexahydrate, and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0116] Place the beaker containing solution B on a thermostatic magnetic stirrer at 40°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.05 mol / L sodium hydroxide solution and solution C simultaneously using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 30 min after the addition is complete to obtain the coprecipitated precursor.
[0117] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0118] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / Zn / CoWO4=3:2:5.
[0119] Comparative Example 3 Compared with Example 1, no nitrate additive was added in this comparative example.
[0120] Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.740 g of copper nitrate trihydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0121] Place the beaker containing solution B in a thermostatic magnetic stirrer at 40°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.05 mol / L sodium hydroxide solution and solution C dropwise simultaneously using the peristaltic pump at a flow rate of 5 mL / min. Adjust the flow rate of the sodium hydroxide solution in real time to maintain the pH between 7 and 8. Continue stirring for 30 min after the addition is complete to obtain the coprecipitated precursor.
[0122] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0123] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / CoWO4=3:5.
[0124] Comparative Example 4 Compared with Example 1, this comparative example does not involve a hydrothermal reaction; that is, the coprecipitated precursor is directly washed with deionized water after being obtained.
[0125] Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.740 g of copper nitrate trihydrate and 1.438 g of zinc nitrate hexahydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0126] Place the beaker containing solution B on a thermostatic magnetic stirrer at 40°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.05 mol / L sodium hydroxide solution and solution C simultaneously using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 30 min after the addition is complete to obtain the coprecipitated precursor.
[0127] The coprecipitated precursor was washed three times with deionized water. After washing, the product was placed in a drying oven and dried at 100°C for 12 hours. Then, the dried product was placed in a muffle furnace and calcined at 550°C for 3 hours at a heating rate of 2°C / min. After calcination, the product was cooled to room temperature and then transferred to a tube furnace. It was reduced at 300°C for 2 hours in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0128] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a catalyst for the hydrogenation of carbon dioxide to methanol, denoted as Cu / Zn / CoWO4=3:2:5.
[0129] Application examples The catalysts for the hydrogenation of carbon dioxide to methanol prepared in Examples 1-5 and Comparative Examples 1-4 were subjected to performance testing and evaluation. The methods and results of the testing and evaluation are as follows: In a continuous flow fixed-bed reactor, the reaction of carbon dioxide hydrogenation to methanol was carried out. First, a small amount of quartz wool was inserted into the middle of a high-temperature resistant quartz glass tube with an inner diameter of 12 mm. Then, 0.3 g of catalyst and 0.3 g of quartz sand were mixed and filled into the quartz glass tube. Finally, a small amount of quartz wool was inserted into the other side of the catalyst to fix it, resulting in a quartz glass tube filled with catalyst. A quartz glass tube containing the catalyst was inserted into a stainless steel reaction tube, which was then installed in a fixed-bed reactor. A small amount of nitrogen was introduced to purge the reactor and replace the air. The catalyst was then reduced using an argon-hydrogen mixture (8% hydrogen + 92% argon) at a gas velocity of 40 mL / min. The temperature was set at 300℃, and the reduction time was 2 hours. After reduction, the system was allowed to cool naturally and then pressurized with N2 at a pressure of 3 MPa. Once the system pressure stabilized, a feed gas mixture of CO2 and H2 with a volume ratio of 1:3 was introduced. The temperature was then raised to the reaction temperature of 220℃, and the space velocity of the feed gas mixture during the reaction was 10000 mL / (g). cat •h), after 6h of reaction, the performance of the catalyst (CO2 conversion rate and product selectivity) in the reaction was evaluated, and the evaluation results are shown in Table 1.
[0130] Table 1 Catalyst performance evaluation results
[0131] In Table 1, the formulas for calculating CO2 conversion rate and product selectivity are as follows:
[0132] As can be seen from the data in Table 1 for Example 1 and Comparative Example 1, when the CoWO4 catalyst was replaced with the conventional catalyst Al2O3, the carbon dioxide conversion rate was only 12.75%, a significant decrease compared to Example 1. This indicates that adding CoWO4 can significantly improve the carbon dioxide conversion rate. Analysis shows that the oxygen vacancies in CoWO4 can serve as active sites for CO2, weakening the C=O bonds of CO2 at lower reaction temperatures. This solves the problem of poor CO2 capture and activation ability in the carbon dioxide hydrogenation to methanol reaction, thereby improving the carbon dioxide conversion rate.
[0133] As can be seen from the data in Table 1 for Example 1 and Comparative Example 2, the order in which the dispersant is added affects the catalyst performance during the catalyst preparation process. Adding a dispersant during the preparation of the cobalt tungstate precursor ensures good dispersibility of the prepared cobalt tungstate support, thus providing a good foundation for the effective dispersion of the catalyst's active components. This results in a composite catalyst with good morphology after subsequent hydrothermal reaction, calcination, and reduction. Without adding a dispersant during the preparation of the cobalt tungstate precursor, the catalyst's active components exhibit significant particle agglomeration, poor morphology, and reduced exposed active sites, leading to a decrease in carbon dioxide conversion rate.
[0134] As can be seen from the data in Table 1 for Examples 1, 2, 3 and Comparative Example 3, the addition of Zn, In, and Zr additives to the catalyst can significantly reduce CO selectivity and thus improve methanol selectivity. Among them, the methanol selectivity corresponding to the Zn additive is the best, reaching 86.26%.
[0135] Figure 1 SEM images of the catalysts for the hydrogenation of carbon dioxide to methanol prepared in Examples 1, 1, 2, and 4. Figure 1 (a) It can be seen that the catalyst prepared in Example 1 for the hydrogenation of carbon dioxide to methanol has significant particle morphology and dispersibility; Figure 1 (b) It can be seen that the Cu / Zn / Al2O3 catalyst prepared in Comparative Example 1 for the hydrogenation of carbon dioxide to methanol exhibits a clearly amorphous polymeric morphology; Figure 1 (c) It can be seen that the dispersant in Comparative Example 2 was not added during the preparation of the cobalt tungstate precursor, resulting in the catalyst prepared in Comparative Example 2 for the hydrogenation of carbon dioxide to methanol having a poor morphology and obvious agglomeration, although it has a particulate morphology. Figure 1 (d) It can be seen that Comparative Example 4 does not undergo hydrothermal reaction. The catalyst prepared in Comparative Example 4 for the hydrogenation of carbon dioxide to methanol exhibits agglomeration and has no clearly defined particle morphology. Figure 2 The elemental distribution diagram of the catalyst for the hydrogenation of carbon dioxide to methanol prepared in Example 5 is shown below. Figure 2 It can be seen that the Cu and Zn elements are evenly distributed in the catalyst for the hydrogenation of carbon dioxide to methanol prepared in Example 5.
Claims
1. A method for preparing a catalyst for the hydrocarbon monoxide of carbon dioxide, characterized by, Includes the following steps: S1. Add a cobalt salt solution to a mixed solution of sodium tungstate and dispersant to obtain a cobalt tungstate precursor suspension. Simultaneously add a mixed solution of copper salt and nitrate and an alkaline solution to the cobalt tungstate precursor suspension and stir to obtain a coprecipitated precursor mixture. S2. The co-precipitated precursor mixture is subjected to a hydrothermal reaction, and the product is washed, dried, calcined, and reduced to obtain a catalyst for the hydrogenation of carbon dioxide to methanol.
2. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate. In the mixed solution of sodium tungstate and dispersant, the molar volume ratio of sodium tungstate in the mixed solution of sodium tungstate and dispersant is 0.012-0.016 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.02-0.8 g / 75 mL. The cobalt salt in the cobalt salt solution is one of cobalt nitrate, cobalt sulfate, cobalt chloride, or their hydrates; In the cobalt salt solution, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.01-0.015 mol / 75 mL.
3. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S1, the copper salt in the mixed solution of copper salt and nitrate is one of copper nitrate, copper sulfate, copper chloride or their hydrate, and the nitrate is one of zinc nitrate, indium nitrate, zirconium nitrate or their hydrate; In a mixed solution of copper salt and nitrate, the molar volume ratio of copper salt in the mixed solution of copper salt and nitrate is 0.001-0.01 mol / 50 mL, and the molar volume ratio of nitrate in the mixed solution of copper salt and nitrate is 0.001-0.005 mol / 50 mL.
4. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S1, the alkaline solution is either sodium hydroxide solution or potassium hydroxide solution; In alkaline solutions, the concentration of alkali is 0.05-0.2 mol / L; When a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to a cobalt tungstate precursor suspension, the pH of the system is maintained between 7 and 8 by controlling the rate of addition of the alkaline solution.
5. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:0.9-1.5; The mass ratio of cobalt salt in the cobalt salt solution to the dispersant in the mixed solution of sodium tungstate and dispersant is 1:0.01-0.2; The molar ratio of cobalt salt in a cobalt salt solution to copper salt in a mixed solution of copper salt and nitrate is 1-9:1; The molar ratio of cobalt salt to nitrate in a cobalt salt solution is 2-9:
1.
6. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S1, when adding cobalt salt solution to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 20-45℃. When adding a cobalt salt solution to a mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise. When a mixed solution of copper salt and nitrate and an alkaline solution are added simultaneously to a cobalt tungstate precursor suspension, the mixed solution of copper salt and nitrate is added dropwise.
7. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S1, the stirring time is 20-40 minutes.
8. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S2, the hydrothermal reaction is carried out in a polytetrafluoroethylene-lined hydrothermal reactor. The hydrothermal reaction temperature is 140-180℃, and the time is 12-24h; Washing is washing 2-5 times with deionized water or anhydrous ethanol; The temperature of drying is 100-120℃, and the time is 10-12h; The temperature of calcination is 500-550℃, and the time is 2-3h.
9. The method for preparing a catalyst for carbon dioxide hydrogenation to methanol according to claim 1, characterized by, In S2, the reduction is carried out under a mixed atmosphere of argon and hydrogen; The temperature of reduction is 300-350℃, and the time is 2-3h.
10. Use of the catalyst prepared by the preparation method of any one of claims 1-9 in the reaction of carbon dioxide hydrogenation to methanol.
Citation Information
Patent Citations
Preparation method of copper-zinc catalyst and prepared copper-zinc catalyst
CN117548113A