Preparation method and application of a carbon dioxide hydrogenation catalyst
The Cu/CoWO4 catalyst was prepared by a stepwise coprecipitation-hydrothermal synthesis method, which solved the problems of low carbon dioxide conversion and poor stability of traditional Cu-based catalysts in the CO2 hydrogenation reaction, and achieved high efficiency in carbon dioxide conversion and methanol selectivity.
Patent Information
- Application Number
- CN202611618422.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional Cu-based catalysts exhibit low carbon dioxide conversion rates, high activation energy barriers for CO2 molecules, and difficulty in activation at low temperatures during CO2 hydrogenation reactions. They also exhibit low methanol selectivity and are prone to sintering, leading to poor stability.
Cu/CoWO4 catalysts were prepared by a stepwise coprecipitation-hydrothermal synthesis method. By adding a dispersant during the cobalt tungstate precursor process, uniform nano-cobalt tungstate particles and spherical CoWO4 were formed, dispersing the Cu component, avoiding sintering, and enhancing the CO2 activation ability of the active sites.
It improved the carbon dioxide conversion rate and methanol selectivity, with the CO2 conversion rate reaching 16.83-17.24% and the CH3OH selectivity reaching 67.04-68.37%, and maintained stable catalytic performance after 127 hours of stability testing.
Smart Images

Figure CN123102373A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of carbon dioxide hydrogenation catalyst technology, specifically relating to a method for preparing and applying a carbon dioxide hydrogenation catalyst. Background Technology
[0002] With industrialization, the massive burning of fossil fuels has led to a continuous rise in atmospheric CO2 concentrations, and the resulting greenhouse effect and climate change have become major challenges facing humanity. Against this backdrop, converting CO2 into high-value-added chemicals and clean fuels can not only achieve the recycling of carbon resources but also effectively reduce greenhouse gas emissions.
[0003] Methanol, as an important basic chemical raw material and a potential clean energy carrier, is widely used in the production of chemical products such as formaldehyde, acetic acid, and methyl tert-butyl ether. It can also be used directly as fuel or a hydrogen source for fuel cells. Using captured CO2 and green hydrogen as raw materials, methanol can be directly synthesized through catalytic hydrogenation, achieving "electrochemical" energy conversion and storage. This is a strategic technological path to promote a circular economy and reduce greenhouse gas emissions.
[0004] Catalysts are a core factor affecting the efficiency of CO2 hydrogenation to methanol. A typical industrial Cu-based catalyst is the Cu / ZnO / Al2O3 system, where Cu is the main active component responsible for the dissociation and adsorption of H2, ZnO synergistically promotes CO2 activation and the hydrogenation of intermediate products, and Al2O3 acts as a structural aid to improve the catalyst's specific surface area and thermal stability. However, traditional Cu-based catalysts still have significant shortcomings in CO2 hydrogenation: First, the carbon dioxide conversion rate is low, the activation barrier of CO2 molecules is high, and carbon dioxide activation is difficult at low temperatures. Although zinc oxide can provide weak base sites for CO2 adsorption, the insufficient oxygen vacancy concentration on the surface of traditional catalysts leads to low CO2 activation efficiency. Second, methanol selectivity is low, typically below 60%, and the formation of byproducts CO and methane reduces atom economy. Third, the reaction process can lead to sintering or agglomeration of active Cu species, causing irreversible catalyst deactivation, and long-term stability cannot meet industrial requirements.
[0005] To address the aforementioned problems, Chinese patent CN117548113A discloses a method for preparing a copper-zinc catalyst and the copper-zinc catalyst prepared therefrom. The copper-zinc catalyst of this invention is used for catalyzing the hydrogenation of CO2 to methanol. The preparation method of this invention adopts a one-step co-precipitation scheme. During the one-step co-precipitation process of copper salt and zinc salt, a surfactant is added to assist in the co-precipitation preparation, which plays a dispersing role on the copper-zinc precipitate, resulting in amorphous solid particles. Zirconium is added as an additive to further improve the methanol selectivity of the catalyst, but the performance of this catalyst is poor. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing a carbon dioxide hydrogenation catalyst and its application. The catalyst prepared by this invention has good particle size and morphology. When the catalyst prepared by this invention is used in the reaction of carbon dioxide hydrogenation to methanol, it exhibits good stability, high carbon dioxide conversion rate, and high methanol selectivity.
[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A method for preparing a carbon dioxide hydrogenation catalyst includes the following steps: S1. Add the cobalt salt solution to the mixed solution of sodium tungstate and dispersant to obtain a cobalt tungstate precursor suspension. Add copper salt solution and alkaline solution to the cobalt tungstate precursor suspension at the same time and stir to obtain a coprecipitated precursor mixture. S2. The coprecipitated precursor mixture is subjected to a hydrothermal reaction, and the product is washed, dried, calcined, and reduced to obtain a carbon dioxide hydrogenation catalyst.
[0008] Preferably, in S1, the cobalt salt in the cobalt salt solution is one of cobalt nitrate, cobalt sulfate, cobalt chloride, or their hydrates; In the cobalt salt solution, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.01-0.015 mol / 75 mL; The dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, or ammonium polyacrylate; In the mixed solution of sodium tungstate and dispersant, the molar volume ratio of sodium tungstate in the mixed solution of sodium tungstate and dispersant is 0.012-0.016 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.03-0.3 g / 75 mL. The copper salt in the copper salt solution is one of copper nitrate, copper sulfate, copper chloride, or their hydrates; In the copper salt solution, the molar volume ratio of copper salt in the copper salt solution is 0.001-0.02 mol / 50 mL; The alkaline solution is either sodium hydroxide solution or potassium hydroxide solution; In alkaline solutions, the concentration of alkali is 0.05-0.2 mol / L.
[0009] More preferably, in S1, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.011-0.013 mol / 75 mL.
[0010] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate, and the molecular weight of the dispersant is 1000-10000.
[0011] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, or ammonium polyacrylate, and the molecular weight of the dispersant is 4000-6000.
[0012] More preferably, in S1, the molar volume ratio of sodium tungstate to dispersant in the mixed solution of sodium tungstate and dispersant is 0.013-0.015 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.04-0.2 g / 75 mL.
[0013] More preferably, in S1, the molar volume ratio of copper salt in the copper salt solution is 0.003-0.014 mol / 50 mL.
[0014] More preferably, in S1, the alkaline solution is a sodium hydroxide solution.
[0015] Preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:(0.9-1.5). The mass ratio of cobalt salt in the cobalt salt solution to the dispersant in the mixed solution of sodium tungstate and dispersant is 1:(0.01-0.1); The molar ratio of cobalt salt in the cobalt salt solution to copper salt in the copper salt solution is (1-5):1.
[0016] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:(1.1-1.3).
[0017] More preferably, in S1, the mass ratio of cobalt salt in the cobalt salt solution to dispersant in the mixed solution of sodium tungstate and dispersant is 1:(0.01-0.04).
[0018] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to copper salt in the copper salt solution is (1-4):1.
[0019] Preferably, in S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, the pH of the system is maintained between 7 and 8 by controlling the addition rate of the alkaline solution.
[0020] Preferably, in step S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 20-45°C. When adding a cobalt salt solution to a mixed solution of sodium tungstate and a dispersant, the cobalt salt solution is added dropwise. When adding both a copper salt solution and an alkaline solution to a cobalt tungstate precursor suspension, the copper salt solution is added dropwise.
[0021] More preferably, in S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 30-40°C.
[0022] More preferably, in S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 2-10 mL / min.
[0023] More preferably, in S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 4-6 mL / min.
[0024] More preferably, in S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, the copper salt solution is added dropwise at a rate of 2-10 mL / min.
[0025] More preferably, in S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, the copper salt solution is added dropwise at a rate of 4-6 mL / min.
[0026] Preferably, in S1, the stirring time is 20-40 min.
[0027] Preferably, in S2, the hydrothermal reaction is carried out in a polytetrafluoroethylene-lined hydrothermal reactor.
[0028] The hydrothermal reaction temperature is 140-180℃, and the time is 12-24h; Wash with deionized water or anhydrous ethanol 2-5 times; The drying temperature is 90-110℃, and the time is 10-15 hours; The calcination temperature is 500-600℃, and the time is 2-3 hours.
[0029] More preferably, in S2, the calcination temperature is 500-600℃, the time is 2-3h, and the heating rate when the temperature rises to 500-550℃ is 1-5℃ / min.
[0030] In a further preferred embodiment, in S2, the calcination temperature is 500-550℃, the time is 2-3h, and the heating rate when the temperature is raised to 500-550℃ is 1-3℃ / min.
[0031] Preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen. The reduction temperature is 300-350℃, and the time is 2-3 hours.
[0032] More preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 2-20% and argon accounts for 80-98%.
[0033] In a further preferred embodiment, during S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 5-10% and argon accounts for 90-95%.
[0034] Furthermore, in S2, the product is washed, dried, calcined, and reduced before being granulated to a particle size of 20-50 mesh.
[0035] Application of a carbon dioxide hydrogenation catalyst prepared by the aforementioned method in the reaction of carbon dioxide hydrogenation to methanol.
[0036] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) The preparation method of the carbon dioxide hydrogenation catalyst of the present invention adopts the stepwise coprecipitation-hydrothermal synthesis method to prepare Cu / CoWO4 catalyst. The oxygen vacancy of cobalt tungstate in the catalyst can be used as CO2 active site, weakening the C=O bond of CO2, solving the problem of poor CO2 capture and activation ability in the carbon dioxide hydrogenation to methanol reaction at low temperature, and improving the carbon dioxide conversion rate.
[0037] (2) The preparation method of the carbon dioxide hydrogenation catalyst of the present invention uses a stepwise coprecipitation-hydrothermal synthesis method to prepare Cu / CoWO4 catalyst. By adding a dispersant in the first step of the stepwise coprecipitation, namely the metathesis reaction to prepare cobalt tungstate, the viscosity of the dispersion system is increased, the steric hindrance is increased, and the diffusion and migration rate of metal ions and precursors is reduced. When CoWO4 is generated and nucleation occurs, ions cannot aggregate on large crystal nuclei for secondary growth, and a large number of small crystal nuclei are frozen, reducing the agglomeration of CoWO4 precursors. The composite material is a spherical particle with a diameter of 200-500 nm and uniform particle size. In addition, by adding a dispersant in the stepwise coprecipitation process, a good CoWO4 morphology is obtained, and it also plays a dispersing role in the precipitation of Cu component in the second step, so that the active metal Cu is uniformly dispersed, and it is not easy to sinter during the reaction. The catalyst has good stability.
[0038] (3) When the carbon dioxide hydrogenation catalyst prepared in this invention is used in the reaction of carbon dioxide hydrogenation to methanol, the CO2 conversion rate can reach 16.83-17.24%, the CH3OH selectivity can reach 67.04-68.37%, and the catalytic performance remains stable after a 127-hour stability test. Attached Figure Description
[0039] Figure 1Scanning electron microscope (SEM) images of the carbon dioxide hydrogenation catalysts prepared in Example 1 and Comparative Example 2. In the picture, Figure 1 (a) A scanning electron microscope (SEM) image of the carbon dioxide hydrogenation catalyst prepared in Example 1; Figure 1 (b) is a scanning electron microscope (SEM) image of the carbon dioxide hydrogenation catalyst prepared in Comparative Example 2.
[0040] Figure 2 The graph shows the stability evaluation of the carbon dioxide hydrogenation catalysts prepared in Example 1 and Comparative Example 2. Detailed Implementation
[0041] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. In all embodiments and comparative examples, the chemicals used are commercially available chemically pure reagents.
[0042] An embodiment of the present invention provides a method for preparing a carbon dioxide hydrogenation catalyst, comprising the following steps: S1. Add the cobalt salt solution to the mixed solution of sodium tungstate and dispersant to obtain a cobalt tungstate precursor suspension. Add copper salt solution and alkaline solution to the cobalt tungstate precursor suspension at the same time and stir to obtain a coprecipitated precursor mixture. S2. The coprecipitated precursor mixture is subjected to a hydrothermal reaction, and the product is washed, dried, calcined, and reduced to obtain a carbon dioxide hydrogenation catalyst.
[0043] Preferably, in S1, the cobalt salt in the cobalt salt solution is one of cobalt nitrate, cobalt sulfate, cobalt chloride, or their hydrates.
[0044] Preferably, in S1, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.01-0.015 mol / 75 mL.
[0045] More preferably, in S1, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.011-0.013 mol / 75 mL.
[0046] Preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate.
[0047] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate, and the molecular weight of the dispersant is 1000-10000.
[0048] More preferably, in S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, or ammonium polyacrylate, and the molecular weight of the dispersant is 4000-6000.
[0049] Preferably, in S1, the molar volume ratio of sodium tungstate to dispersant in the mixed solution of sodium tungstate and dispersant is 0.012-0.016 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.03-0.3 g / 75 mL.
[0050] More preferably, in S1, the molar volume ratio of sodium tungstate to dispersant in the mixed solution of sodium tungstate and dispersant is 0.013-0.015 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.04-0.2 g / 75 mL.
[0051] Preferably, in S1, the copper salt in the copper salt solution is one of copper nitrate, copper sulfate, copper chloride, or their hydrates.
[0052] Preferably, in S1, the molar volume ratio of copper salt in the copper salt solution is 0.001-0.02 mol / 50 mL.
[0053] More preferably, in S1, the molar volume ratio of copper salt in the copper salt solution is 0.003-0.014 mol / 50 mL.
[0054] Preferably, in S1, the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution.
[0055] More preferably, in S1, the alkaline solution is a sodium hydroxide solution.
[0056] Preferably, in S1, the concentration of the alkali in the alkaline solution is 0.05-0.2 mol / L.
[0057] Preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:(0.9-1.5).
[0058] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:(1.1-1.3).
[0059] Preferably, in S1, the mass ratio of cobalt salt in the cobalt salt solution to dispersant in the mixed solution of sodium tungstate and dispersant is 1:(0.01-0.1).
[0060] More preferably, in S1, the mass ratio of cobalt salt in the cobalt salt solution to dispersant in the mixed solution of sodium tungstate and dispersant is 1:(0.01-0.04).
[0061] Preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to copper salt in the copper salt solution is (1-5):1.
[0062] More preferably, in S1, the molar ratio of cobalt salt in the cobalt salt solution to copper salt in the copper salt solution is (1-4):1.
[0063] Preferably, in S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, the pH of the system is maintained between 7 and 8 by controlling the addition rate of the alkaline solution.
[0064] In S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, by controlling the addition rate of alkaline solution and maintaining the pH of the system between 7 and 8, it helps to form nano-cobalt tungstate particles with uniform particle size and morphology, while ensuring that copper ions in the copper salt solution can form a uniform precipitate.
[0065] Preferably, in step S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 20-45°C.
[0066] More preferably, in S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 30-40°C.
[0067] Preferably, in S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise.
[0068] More preferably, in S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 2-10 mL / min.
[0069] More preferably, in S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the cobalt salt solution is added dropwise at a rate of 4-6 mL / min.
[0070] Preferably, in S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, the copper salt solution is added dropwise.
[0071] More preferably, in S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, the copper salt solution is added dropwise at a rate of 2-10 mL / min.
[0072] More preferably, in S1, when copper salt solution and alkaline solution are added to the cobalt tungstate precursor suspension at the same time, the copper salt solution is added dropwise at a rate of 4-6 mL / min.
[0073] Preferably, in S1, the stirring time is 20-40 min.
[0074] Preferably, in S2, the hydrothermal reaction is carried out in a polytetrafluoroethylene-lined hydrothermal reactor.
[0075] Preferably, in S2, the hydrothermal reaction temperature is 140-180℃ and the time is 12-24h.
[0076] Preferably, in S2, the washing process involves washing with deionized water or anhydrous ethanol 2-5 times.
[0077] Preferably, in step S2, the drying temperature is 90-110℃ and the time is 10-15h.
[0078] Preferably, in S2, the calcination temperature is 500-600℃ and the time is 2-3h.
[0079] More preferably, in S2, the calcination temperature is 500-600℃, the time is 2-3h, and the heating rate when the temperature rises to 500-550℃ is 1-5℃ / min.
[0080] In a further preferred embodiment, in S2, the calcination temperature is 500-550℃, the time is 2-3h, and the heating rate when the temperature is raised to 500-550℃ is 1-3℃ / min.
[0081] Preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen.
[0082] More preferably, in S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 2-20% and argon accounts for 80-98%.
[0083] In a further preferred embodiment, during S2, the reduction is carried out in a mixed atmosphere of argon and hydrogen, wherein hydrogen accounts for 5-10% and argon accounts for 90-95%.
[0084] Preferably, in S2, the reduction temperature is 300-350℃ and the time is 2-3h.
[0085] Furthermore, in S2, the product is washed, dried, calcined, and reduced before being granulated to a particle size of 20-50 mesh.
[0086] Embodiments of the present invention also provide the application of the carbon dioxide hydrogenation catalyst prepared by the preparation method in the carbon dioxide hydrogenation to methanol reaction.
[0087] Example 1 Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.450 g of copper nitrate trihydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0088] Place the beaker containing solution B on a thermostatic magnetic stirrer at 40°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, simultaneously add 0.05 mol / L sodium hydroxide solution and solution C using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 30 min after the addition is complete to obtain the coprecipitated precursor.
[0089] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0090] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a carbon dioxide hydrogenation catalyst, denoted as Cu / CoWO4=1:2 (this ratio is the molar ratio of Cu to CoWO4, the same below).
[0091] Example 2 Weigh 3.373 g of cobalt sulfate heptahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.1104 g of polyacrylic acid (PAA) with a molecular weight of 5000 into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 3.332 g of copper sulfate pentahydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0092] Place the beaker containing solution B in a thermostatic magnetic stirrer at 35°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.1 mol / L sodium hydroxide solution and solution C dropwise simultaneously using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 35 min after the addition is complete to obtain the coprecipitated precursor.
[0093] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 180 °C for 12 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with anhydrous ethanol and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 2 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 320 °C for 3 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0094] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a carbon dioxide hydrogenation catalyst, denoted as Cu / CoWO4=1:1.
[0095] Example 3 Weigh 2.855 g of cobalt chloride hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate and 0.184 g of ammonium polyacrylate (existing as an aqueous solution of ammonium polyacrylate with a mass fraction of 40 wt%, PAA-NH4) into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 0.511 g of copper chloride dihydrate into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0096] Place beaker B in a thermostatic magnetic stirrer at 30°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.2 mol / L sodium hydroxide solution and solution C dropwise simultaneously using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 20 min after the addition is complete to obtain the coprecipitated precursor.
[0097] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 140 °C for 24 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 10 h. The dried product was then placed in a muffle furnace and calcined at 500 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0098] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a carbon dioxide hydrogenation catalyst, denoted as Cu / CoWO4=1:4.
[0099] Comparative Example 1 Compared with Example 1, the carrier in this comparative example is Al2O3.
[0100] Weigh 7.709 g of aluminum nitrate hexahydrate and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 and add them to a beaker. Add 150 mL of deionized water and stir well to obtain solution B. Weigh 1.450 g of copper nitrate trihydrate and add it to a beaker. Add 50 mL of deionized water and stir well to obtain solution C.
[0101] Place the beaker containing solution B in a thermostatic magnetic stirrer at 30°C. Then, add solution C dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. Simultaneously, add 0.05 mol / L sodium hydroxide solution dropwise using the same peristaltic pump. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. After the addition is complete, continue stirring for 30 min to obtain the coprecipitated precursor.
[0102] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0103] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a carbon dioxide hydrogenation catalyst, denoted as Cu / Al2O3=1:2.
[0104] Comparative Example 2 The dispersant addition steps are different in this comparative example compared to Example 1.
[0105] Weigh 3.492 g of cobalt nitrate hexahydrate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution A. Weigh 4.156 g of sodium tungstate into a beaker, add 75 mL of deionized water, and stir until homogeneous to obtain solution B. Weigh 1.450 g of copper nitrate trihydrate and 0.042 g of sodium polyacrylate (PAAS) with a molecular weight of 5000 into a beaker, add 50 mL of deionized water, and stir until homogeneous to obtain solution C.
[0106] Place the beaker containing solution B in a thermostatic magnetic stirrer at 40°C. Then, add solution A dropwise to solution B using a peristaltic pump at a flow rate of 5 mL / min. After the addition is complete, continue to add 0.05 mol / L sodium hydroxide solution and solution C containing a dispersant dropwise using the peristaltic pump at a flow rate of 5 mL / min. Maintain the pH between 7 and 8 by adjusting the flow rate of the sodium hydroxide solution in real time. Continue stirring for 30 min after the addition is complete to obtain the coprecipitated precursor.
[0107] The coprecipitated precursor was transferred to a 500 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 160 °C for 16 h. After heating, the reactor was allowed to cool naturally to room temperature. The product was washed three times with deionized water and then placed in a drying oven and dried at 100 °C for 12 h. The dried product was then placed in a muffle furnace and calcined at 550 °C for 3 h at a heating rate of 2 °C / min. After calcination, the product was allowed to cool to room temperature and then transferred to a tube furnace. It was reduced at 300 °C for 2 h in an argon-hydrogen mixed atmosphere (8% hydrogen + 92% argon) to obtain the synthesized product.
[0108] The synthesized product was loaded into a tableting mold, tableted and granulated using a tableting machine, and then sieved through a 20-mesh stainless steel standard sieve to obtain a carbon dioxide hydrogenation catalyst, denoted as Cu / CoWO4=1:2.
[0109] Application examples The performance of the carbon dioxide hydrogenation catalysts prepared in Examples 1-3 and Comparative Examples 1-2 was tested and evaluated according to the following methods: The reaction of carbon dioxide hydrogenation to methanol was carried out in a continuous flow fixed bed reactor. First, a small amount of quartz wool was inserted into the middle of a high-temperature resistant quartz glass tube with an inner diameter of 12 mm. 0.3 g of carbon dioxide hydrogenation catalyst was mixed with 0.3 g of quartz sand and then filled into the quartz glass tube. Then, a small amount of quartz wool was inserted into the other side of the catalyst to fix it, and a quartz glass tube filled with catalyst was obtained.
[0110] Then, the quartz glass tube containing the catalyst was placed into a stainless steel reaction tube, and the stainless steel reaction tube was installed into a fixed-bed reactor. A small amount of nitrogen was introduced to purge and replace the air in the fixed-bed reactor. The catalyst was then reduced with an argon-hydrogen mixture (8% hydrogen + 92% argon). The gas flow rate of the argon-hydrogen mixture was 40 mL / min, the temperature was set at 300℃, and the reduction time was 2 hours.
[0111] After reduction, the system was naturally cooled and then pressurized with N2 at a pressure of 3 MPa. Once the system pressure stabilized, a feed gas mixture of CO2 and H2 with a volume ratio of 1:3 was introduced, and the temperature was raised to 220℃ with a feed gas hourly space velocity of 10000 mL / (g). cat •h), the reaction was carried out for 6 hours. After the reaction was completed, the catalyst performance was evaluated. The evaluation results are shown in Table 1.
[0112] Table 1 Catalyst performance evaluation results
[0113] In Table 1, the formulas for calculating CO2 conversion rate and product selectivity are as follows: CO2 conversion rate:
[0114] Product selectivity:
[0115] As can be seen from the data in Table 1 for Example 1 and Comparative Example 1, when the catalyst Cu / CoWO4 was replaced with the conventional catalyst Cu / Al2O3, the carbon dioxide conversion was only 11.92%, a significant decrease compared to Example 1. This comparison demonstrates that adding CoWO4 can significantly improve the carbon dioxide conversion rate. This is mainly because the oxygen vacancies in the CoWO4 of the composite catalyst prepared by this method can serve as active sites for CO2. Under lower reaction temperatures, this weakens the C=O bonds of CO2, solving the problem of poor CO2 capture and activation ability in the carbon dioxide hydrogenation to methanol reaction, thereby improving the carbon dioxide conversion rate.
[0116] As can be seen from the data in Table 1 for Example 1 and Comparative Example 2, the order in which the dispersant is added affects the catalyst performance during catalyst preparation. Adding a dispersant during the preparation of the cobalt tungstate precursor enables the cobalt tungstate support to have good dispersibility, thus providing a good foundation for the effective dispersion of the active component in the second step. This results in a composite catalyst with good morphology after subsequent hydrothermal synthesis, calcination, and reduction. When no dispersant is added during the preparation of the cobalt tungstate precursor, the catalyst particles agglomerate significantly, resulting in poor morphology and a reduction in exposed active sites, leading to a decrease in carbon dioxide conversion rate.
[0117] SEM images of the carbon dioxide hydrogenation catalysts prepared in Example 1 and Comparative Example 2 are shown below. Figure 1 As shown, by Figure 1 (a) It can be seen that the carbon dioxide hydrogenation catalyst prepared in Example 1 has significant particle morphology and dispersibility; Figure 1 (b) It can be seen that the dispersant of the carbon dioxide hydrogenation catalyst prepared in Comparative Example 2 was not added during the preparation of the cobalt tungstate precursor. Although it has a particle morphology, the morphology is poor and obvious agglomeration occurs.
[0118] The carbon dioxide hydrogenation catalysts prepared in Example 1 and Comparative Example 2 were subjected to a 127-hour stability test. The stability evaluation graph is shown below. Figure 2 As shown, from Figure 2 It can be seen that changing the order in which the dispersant is added affects the stability of the catalyst. Combined with... Figure 1 (a) and Figure 1 (b) By comparison, it is shown that the addition of dispersant in the second precipitation process of Comparative Example 2 failed to better disperse the cobalt tungstate precursor, resulting in the cobalt tungstate agglomeration, poorer catalytic performance, and easier deactivation.
Claims
1. A method for preparing a carbon dioxide hydrogenation catalyst, characterized in that, Includes the following steps: S1. Add the cobalt salt solution to the mixed solution of sodium tungstate and dispersant to obtain a cobalt tungstate precursor suspension. Add copper salt solution and alkaline solution to the cobalt tungstate precursor suspension at the same time and stir to obtain a coprecipitated precursor mixture. In S1, the dispersant in the mixed solution of sodium tungstate and dispersant is one of sodium polyacrylate, polyacrylic acid, and ammonium polyacrylate. S2. The coprecipitated precursor mixture is subjected to a hydrothermal reaction, and the product is washed, dried, calcined, and reduced to obtain a carbon dioxide hydrogenation catalyst.
2. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, characterized in that, In S1, the cobalt salt in the cobalt salt solution is one of cobalt nitrate, cobalt sulfate, cobalt chloride, or their hydrates; In the cobalt salt solution, the molar volume ratio of cobalt salt in the cobalt salt solution is 0.01-0.015 mol / 75 mL; In the mixed solution of sodium tungstate and dispersant, the molar volume ratio of sodium tungstate in the mixed solution of sodium tungstate and dispersant is 0.012-0.016 mol / 75 mL, and the mass volume ratio of dispersant in the mixed solution of sodium tungstate and dispersant is 0.03-0.3 g / 75 mL. The copper salt in the copper salt solution is one of copper nitrate, copper sulfate, copper chloride, or their hydrates; In the copper salt solution, the molar volume ratio of copper salt in the copper salt solution is 0.001-0.02 mol / 50 mL; The alkaline solution is either sodium hydroxide solution or potassium hydroxide solution; In alkaline solutions, the concentration of alkali is 0.05-0.2 mol / L.
3. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, characterized in that, In S1, the molar ratio of cobalt salt in the cobalt salt solution to sodium tungstate in the mixed solution of sodium tungstate and dispersant is 1:(0.9-1.5); The mass ratio of cobalt salt in the cobalt salt solution to the dispersant in the mixed solution of sodium tungstate and dispersant is 1:(0.01-0.1); The molar ratio of cobalt salt in the cobalt salt solution to copper salt in the copper salt solution is (1-5):
1.
4. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, characterized in that, In S1, when copper salt solution and alkaline solution are added simultaneously to the cobalt tungstate precursor suspension, the pH of the system is maintained between 7 and 8 by controlling the rate of addition of the alkaline solution.
5. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, characterized in that, In S1, when the cobalt salt solution is added to the mixed solution of sodium tungstate and dispersant, the mixed solution of sodium tungstate and dispersant is stirred at a temperature of 20-45℃. When adding a cobalt salt solution to a mixed solution of sodium tungstate and a dispersant, the cobalt salt solution is added dropwise. When adding both a copper salt solution and an alkaline solution to a cobalt tungstate precursor suspension, the copper salt solution is added dropwise.
6. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, characterized in that, In S2, the hydrothermal reaction temperature is 140-180℃ and the time is 12-24h; Wash with deionized water or anhydrous ethanol 2-5 times; The drying temperature is 90-110℃, and the time is 10-15 hours; The calcination temperature is 500-600℃, and the time is 2-3 hours.
7. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, characterized in that, In S2, reduction is carried out in a mixed atmosphere of argon and hydrogen. The reduction temperature is 300-350℃, and the time is 2-3 hours.
8. The application of a carbon dioxide hydrogenation catalyst prepared by the preparation method according to any one of claims 1-7 in the reaction of carbon dioxide hydrogenation to methanol.
Citation Information
Patent Citations
Preparation method of copper-zinc catalyst and prepared copper-zinc catalyst